Powder containing ground cement clinker
A powder containing ground cement clinker with specific phase proportions and additives enhances early strength development in low-temperature environments, addressing the limitations of existing curing accelerators and ensuring effective cement performance.
Patent Information
- Application Number
- JP2021029802
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Cement compositions experience reduced early strength development in low-temperature environments, and existing curing accelerators are expensive and less effective in such conditions, leading to delayed formwork removal and increased costs.
A powder containing ground cement clinker, mixed with quicklime powder, is formulated with specific proportions of alite, belite, aluminate, ferrite phases, and free lime, along with controlled crystallite size and potassium content, to enhance early strength development in low-temperature conditions.
The formulation achieves superior early strength development in both low-temperature and room-temperature environments, reducing the degree of property deterioration and maintaining fluidity in uncured cement compositions.
Smart Images

Figure 0007576994000001 
Figure 0007576994000002 
Figure 0007576994000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder containing ground cement clinker. [Background technology]
[0002] For more economical and rational construction, there is a need for a technique that allows cement compositions to quickly develop their strength. As an example of a hardening accelerator for accelerating the hardening of cement, Patent Document 1 describes a hardening accelerator containing hydrated lime and at least one selected from thiosulfate salts, formate salts, nitrate salts, and nitrite salts. Furthermore, as an example of a cement with excellent early strength development, Patent Document 2 describes a cement composition having a clinker mineral composition in which the C3S content is 60-71%, the C2S content is 1% or more, the combined content of C3S and C2S is 70-80%, and the C3S / C2S content ratio is at least 5, as determined by the Bogue formula, and which is obtained by adding gypsum to an alite-rich clinker with a free lime content of 1.0-4.0% by weight, to which is added 2-10% by weight of limestone fine powder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-277111 A [Patent Document 2] JP 2017-154904 A Summary of the Invention [Problem to be solved by the invention]
[0004] The strength development of a cement composition is affected by temperature. In a low-temperature environment such as winter or cold region, the early strength development of the cement composition decreases, and there is a problem that the time until the formwork can be removed from the cement composition is delayed. In addition, the effect of the hardening accelerator for quickly developing the strength of the cement composition is also easily affected by temperature, so that the effect of the hardening accelerator is not sufficient in a low-temperature environment, and therefore, the hardening accelerator cannot be used in winter or in cold regions, etc. Another problem is that the hardening accelerator is expensive. The object of the present invention is to provide a powder containing pulverized cement clinker, which can produce cement that has excellent early strength development in a low temperature (e.g., 10°C) environment and exhibits a small degree of decline in early strength development compared to the early strength development in a room temperature (e.g., 20°C) environment. [Means for solving the problem]
[0005] As a result of intensive research to solve the above problems, the present inventors have found that the above object can be achieved by using a powder containing ground cement clinker, which is a mixture of ground cement clinker or ground cement clinker and quicklime powder, and which has a rate of alite (C3S) of 42 to 65 mass%, a rate of belite (C2S) of 12 to 40 mass%, a rate of aluminate phase (C3A) of 12 to 18 mass%, and a rate of ferrite phase (C4AF) of 0.5 to 12 mass%, and a rate of free lime (f.CaO) of 0.7 to 3.0 mass%, as calculated by a specific Bogue formula, and have completed the present invention. That is, the present invention provides the following [1] to [5]. [1] A powder containing ground cement clinker, which is a mixture of ground cement clinker or ground cement clinker and quicklime powder, characterized in that the value calculated by the Bogue formula (wherein the value of the proportion of CaO used in calculating alite (C3S) is the total CaO proportion contained in the ground cement clinker powder minus the proportion of free lime (f.CaO)) is 42-65% by mass for alite (C3S), 12-40% by mass for belite (C2S), 12-18% by mass for aluminate phase (C3A), and 0.5-12% by mass for ferrite phase (C4AF), and the proportion of free lime (f.CaO) is 0.7-3.0% by mass.
[0006] [2] The powder containing ground cement clinker according to [1], wherein the proportion of potassium is 0.40 to 0.80 mass% calculated as oxide (K2O). [3] The powder containing ground cement clinker according to [1] or [2], wherein the crystallite diameter of the ferrite phase (C4AF) measured by X-ray diffraction is 30 to 90 nm. [4] A cement containing the powder containing pulverized cement clinker according to any one of [1] to [3] above, and gypsum, wherein the proportion of sulfur is 3.0 to 3.5 mass% in terms of SO3, and the Blaine specific surface area is 4,800 to 6,000 cm 2 / g. [5] A method for producing a hardened cement composition, comprising: a mixing step of mixing the cement according to [4] above with other materials including water at a temperature of 10°C or less to obtain an unhardened cement composition; and a curing step of curing the unhardened cement composition to obtain a hardened cement composition. Effect of the Invention
[0007] According to the powder containing ground cement clinker of the present invention, it is possible to obtain cement that has excellent early strength development in a low temperature (e.g., 10°C) environment and that shows a small degree of decline in early strength development compared to the early strength development in a room temperature (e.g., 20°C) environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The powder containing ground cement clinker of the present invention is a powder containing ground cement clinker, which is a mixture of ground cement clinker or ground cement clinker and quicklime powder, and is characterized in that the value calculated by the Bogue formula (wherein the value of the proportion of CaO used in calculating alite (C3S) is the proportion of the total CaO contained in the ground cement clinker powder minus the proportion of free lime (f.CaO)) is 42 to 65 mass% of alite (C3S), 12 to 40 mass% of belite (C2S), 12 to 18 mass% of aluminate phase (C3A), and 0.5 to 12 mass% of ferrite phase (C4AF), and the proportion of free lime (f.CaO) is 0.7 to 3.0 mass%.
[0009] The proportion of alite (3CaO·SiO2; abbreviated as C3S) in the powder containing ground cement clinker, calculated by the Bogue formula (wherein the value of the proportion of CaO used in calculating alite (C3S) is the proportion of the total CaO contained in the powder containing ground cement clinker minus the proportion of free lime (f.CaO)), is 42 to 65 mass%, preferably 44 to 65 mass%, more preferably 50 to 64.5 mass%, further preferably 55 to 64 mass%, and particularly preferably 56 to 64 mass%. If the proportion is less than 42 mass%, the early strength development of the cement containing the powder containing ground cement clinker is reduced. If the proportion exceeds 65 mass%, the fluidity of the unhardened cement composition may be reduced. The proportion of belite (2CaO·SiO2; abbreviated as C2S) in the powder containing ground cement clinker, calculated by the Bogue formula, is 12 to 40 mass%, preferably 12 to 38 mass%, more preferably 12.5 to 30 mass%, even more preferably 12.5 to 25 mass%, even more preferably 13 to 20 mass%, and particularly preferably 13 to 19 mass%. If the proportion is less than 12 mass%, the long-term strength development of the cement containing the ground cement clinker powder may decrease. If the proportion exceeds 40 mass%, the early strength development of the cement containing the ground cement clinker powder decreases.
[0010] The proportion of the aluminate phase (3CaO·Al2O3; abbreviated as C3A) in the powder containing ground cement clinker, calculated by the Bogue formula, is 12 to 18 mass%, preferably 12.5 to 16 mass%, more preferably 13 to 15 mass%, and particularly preferably 13 to 14 mass%. If the proportion is less than 12 mass%, the early strength development of the cement containing the powder containing ground cement clinker decreases. If the proportion exceeds 18 mass%, the heat of hydration of the cement composition becomes excessive. The proportion of ferrite phase (4CaO·Al2O3·Fe2O3; abbreviated as C4AF) in the powder containing ground cement clinker, calculated by the Bogue formula, is 0.5 to 12 mass%, preferably 1 to 10 mass%, more preferably 2 to 8 mass%, further preferably 3 to 7 mass%, and particularly preferably 4 to 6 mass%. It is difficult to produce a powder containing ground cement clinker with the above proportion of less than 0.5 mass%. If the above proportion exceeds 12 mass%, the fluidity of the unhardened cement composition may decrease.
[0011] In this specification, the contents of C3S (alite), C2S (belite), C3A (aluminate phase), and C4AF (ferrite phase) in the powder containing pulverized cement clinker are calculated using the following Bogue formulas (1) to (4) based on the proportion of f.CaO (mass%) in the total amount (100 mass%) of the powder containing pulverized cement clinker, and the chemical components of the raw materials of the powder containing pulverized cement clinker and the cement clinker (burned product). (1) C3S(mass%)=(4.07×CaO(mass%))-(7.60×SiO2(mass%))-(6.72×Al2O3(mass%))-(1.43×Fe2O3(mass%)) (In the formula (1), the value of "CaO (mass%)" is the value obtained by subtracting the percentage of f.CaO from the percentage of total CaO in the powder containing pulverized cement clinker (CaO (mass%) = total CaO - f.CaO).) (2) C2S(mass%)=(2.87×SiO2(mass%))-(0.754×C3S(mass%)) (3) C3A(mass%)=(2.65×Al2O3(mass%))-(1.69×Fe2O3(mass%)) (4) C4AF(mass%)=3.04×Fe2O3(mass%)
[0012] The proportion of free lime (f.CaO) in the powder containing ground cement clinker is 0.7 to 3.0 mass%, more preferably 0.8 to 2.5 mass%, even more preferably 0.9 to 2.2 mass%, even more preferably 1.2 to 2.1 mass%, even more preferably 1.6 to 2.0 mass%, and particularly preferably 1.7 to 1.9 mass%. If the proportion is less than 0.7 mass%, the early strength development of the cement containing the powder containing ground cement clinker decreases. If the proportion exceeds 3.0 mass%, the early strength development of the cement composition at low temperatures decreases.
[0013] The proportion of potassium in the powder containing pulverized cement clinker is, in terms of oxide (KO), preferably 0.40 to 0.80 mass%, more preferably 0.42 to 0.70 mass%, further preferably 0.44 to 0.60 mass%, and particularly preferably 0.45 to 0.55 mass%, from the viewpoints of improving the early strength development of the cement containing the powder containing pulverized cement clinker and the fluidity of the unhardened cement composition.
[0014] The crystallite size of the ferrite phase (C4AF) measured by X-ray diffraction is preferably 30 to 90 nm, more preferably 40 to 85 nm, even more preferably 45 to 80 nm, even more preferably 48 to 70 nm, and particularly preferably 50 to 60 nm. If the crystallite size is less than 30 nm, the early strength development of the cement containing the ground cement clinker powder decreases. It is difficult to produce a powder containing ground cement clinker with a crystallite size exceeding 90 nm.
[0015] The hydraulic hardness (HM) of the powder containing ground cement clinker is 2.10 to 2.40, preferably 2.15 to 2.38, more preferably 2.20 to 2.36, and particularly preferably 2.28 to 2.35. If the hydraulic hardness (HM) is less than 2.10, the early strength development of the cement containing the powder containing ground cement clinker is reduced. If the hydraulic hardness (HM) is more than 2.40, the fluidity of the unhardened cement composition is reduced. The silicate ratio (SM) of the powder containing ground cement clinker is 1.80 to 4.60, preferably 2.40 to 3.20, more preferably 2.70 to 3.00, further preferably 2.80 to 2.90, and particularly preferably 2.84 to 2.88. If the silicate ratio (SM) is less than 1.80, the early strength development of the cement containing the powder containing ground cement clinker is reduced. If the silicate ratio (SM) is more than 4.60, the fluidity of the unhardened cement composition is reduced.
[0016] The iron content (IM) of the powder containing ground cement clinker is 2.3 to 25.0, preferably 2.8 to 15.0, more preferably 3.0 to 10.0, even more preferably 3.2 to 6.0, even more preferably 3.4 to 5.0, and particularly preferably 3.6 to 4.0. If the iron content (IM) is less than 2.3, the early strength development of the cement containing the powder containing ground cement clinker is reduced. If the iron content (IM) is more than 25.0, the fluidity of the unhardened cement composition is reduced.
[0017] The hydraulic ratio, silica ratio, and iron ratio can each be calculated using the following formulas. Hydraulic rate=CaO / (SiO2+Al2O3+Fe2O3) Silicate ratio = SiO2 / (Al2O3+Fe2O3) Iron rate=Al2O3 / Fe2O3 (The chemical formula in the above formula represents the content (mass%) of the compound represented by the above chemical formula in the powder containing pulverized cement clinker.)
[0018] The powder containing pulverized cement clinker may consist of pulverized cement clinker alone, or may be a mixture of pulverized cement clinker and quicklime powder for the purpose of adjusting the proportion of free lime (f.CaO) in the powder containing pulverized cement clinker to within the range of 0.7 to 3.0 mass%. The powder containing pulverized cement clinker may be a mixture of pulverized cement clinker and a potassium salt (e.g., K2SO4) for the purpose of adjusting the proportion of potassium in the powder containing pulverized cement clinker to a desired numerical range (e.g., 0.40 to 0.80 mass% in terms of oxide (KO)). As the raw material for the pulverized cement clinker, there can be used typical raw materials used in the production of cement clinker, such as calcium-containing raw materials (CaO sources) such as limestone, quicklime, and slaked lime, silicon-containing raw materials (SiO sources) such as silica stone and clay, aluminum-containing raw materials (AlO sources) such as clay, and iron-containing raw materials (FeO sources) such as iron slag and iron cake. The above raw materials are mixed so as to obtain the desired hydraulic ratio, silicate ratio, iron ratio, etc., and then calcined at preferably 1,350 to 1,550°C (more preferably 1,400 to 1,500°C) to obtain cement clinker. The obtained cement clinker (lump) is then pulverized using a conventional pulverizing device such as a ball mill to obtain pulverized cement clinker.
[0019] The cement of the present invention is a cement containing the above-mentioned cement clinker pulverized powder and gypsum, and has a sulfur content of 3.0 to 3.5 mass% calculated as SO3 and a Blaine specific surface area of 4,800 to 6,000 cm 2 / g. Examples of gypsum include anhydrous gypsum, dihydrate gypsum, and hemihydrate gypsum, which may be used alone or in combination of two or more. The proportion of sulfur in the cement is 3.0-3.5 mass%, preferably 3.1-3.4 mass%, more preferably 3.2-3.4 mass%, calculated as SO3. If the proportion is less than 3.0 mass%, the usable time before hardening of the cement composition (the time during which good fluidity can be maintained) becomes shorter, and the workability decreases. If the proportion exceeds 3.5 mass%, the strength development of the cement decreases. The content of potassium in the cement, calculated as oxide (KO), is preferably 0.10 to 0.60 mass%, more preferably 0.20 to 0.55 mass%, further preferably 0.25 to 0.50 mass%, and particularly preferably 0.30 to 0.45 mass%, from the viewpoints of improving the early strength development of the cement and the fluidity of the unhardened cement composition.
[0020] The Blaine specific surface area of cement is 4,800 to 6,000 cm 2 / g, more preferably 4,900 to 5,800 cm 2 / g, and particularly preferably 5,000 to 5,600 cm 2 / g. The above Blaine specific surface area is 4,800 cm 2 If the Blaine specific surface area is less than 6,000 cm / g, the strength development of the cement decreases. 2 If it exceeds 1 / g, the fluidity of the cement decreases.
[0021] By using the powder containing ground cement clinker of the present invention as a raw material for cement, when a hardened body of a cement composition containing the ground cement clinker powder and gypsum is produced in a low temperature (e.g., 10°C) environment, the strength of the hardened body at an early age (e.g., 1 to 7 days) can be increased, and the degree of decrease in strength at an early age can be reduced compared to when the hardened body is produced in a room temperature environment. Such an effect can be obtained even when the cement composition does not contain a cement hardening accelerator. An example of a method for producing a hardened product of a cement composition (mortar, concrete or cement paste) containing the above cement includes a method including a kneading step of kneading the above cement with other materials (water, etc.) at a temperature of 10°C or lower (preferably -10 to 10°C, more preferably 0 to 10°C) to obtain an unhardened cement composition, and a curing step of curing the unhardened cement composition to obtain a hardened product of the cement composition. The other materials are not particularly limited, and examples thereof include fine aggregate, coarse aggregate, water, various admixtures such as air-entraining agents, water-reducing agents, air-entraining water-reducing agents, high-performance water-reducing agents, and high-performance air-entraining water-reducing agents, as well as various admixtures such as fly ash, silica fume, and ground granulated blast furnace slag. The kneading method in the kneading step and the curing method in the curing step are not particularly limited, and general kneading methods and curing methods for cement compositions can be used. EXAMPLES
[0022] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Examples 1 to 3] A cement clinker raw material was prepared using a general cement clinker raw material in an environment of 20° C. The prepared raw material was fired at 1,450° C. in a rotary kiln to obtain a cement clinker in the form of a lump. The obtained cement clinker in the form of a lump was pulverized in a ball mill to obtain a powder containing pulverized cement clinker. The proportions of alite, belite, aluminate phase (C3A), ferrite phase (C4AF), and free lime (f·CaO), as well as the hydraulic ratio, silicate ratio, and iron ratio, and the chemical composition of the obtained powder containing ground cement clinker are shown in Tables 1 and 2. In addition, the crystallite size of the ferrite phase (C4AF) of the powder containing ground cement clinker was measured by an X-ray diffraction method using an X-ray diffractometer (e.g., Bruker Japan, product name "D8 ADVANCE"). Specifically, it was calculated from the half-width (FMHM) of the diffraction line profile of the (0,2,0) plane of the ferrite phase near 2θ=12.2 (CuKα line) using Scherrer's formula (5). L = K λ / (β cosθ) (5) (In formula (5), L is the crystallite size (nm), K is a constant (0.94), λ is the wavelength of the X-ray (nm), β is the half-width, and θ is the flag angle (°) of the diffracted X-ray.) In addition, the percentage of free lime (f·CaO) was measured using the Cement Association standard test method "JCAS I-01-1997 (quantitative method for free calcium oxide)." The results are shown in Table 1.
[0023] Next, the powder containing the ground cement clinker and the gypsum powder were mixed to produce cement. The amount of gypsum powder was set so that the ratio of sulfur in the cement, converted into SO3, was the value shown in Table 3. The ratio of potassium in the cement (converted into K2O) and the Blaine specific surface area are also shown in Table 3. Using the obtained cement, mortar specimens were prepared in accordance with "JIS R 5201:2015 (Physical testing methods for cement)", and the compressive strength of the mortar specimens at ages of 1 day and 7 days was measured. In addition, mortar specimens were prepared in the same manner as described above for preparing the mortar specimens, except that the production of cement clinker, the production of cement, and the preparation of mortar specimens were carried out in an environment of 10°C instead of 20°C, and the compressive strength of the mortar specimens at ages of 1 day and 7 days was measured.
[0024] Furthermore, the ratio ((A) / (B)) of the mortar compressive strength (A) at 1 day of age of the mortar produced in an environment at 10°C to the mortar compressive strength (B) at 1 day of age of the mortar produced in an environment at 20°C was calculated. The results are shown in Table 3. A larger ratio indicates a smaller degree of decrease in early strength development when produced in an environment at 10°C compared to when produced in an environment at 20°C.
[0025] [Example 4] Mortar specimens were prepared in the same manner as in Example 2, except that the cement clinker obtained in Example 2 was pulverized using a ball mill, and then quicklime was added and mixed to obtain a powder containing pulverized cement clinker. The amount of quicklime was set so that the ratio of free lime (f·CaO) in the powder containing pulverized cement clinker would be the value shown in Table 1. The compressive strength and other properties of the mortar specimens obtained at ages of 1 day and 7 days were measured in the same manner as in Example 1. [Example 5] Mortar specimens were prepared in the same manner as in Example 1, except that the cement clinker raw material was prepared so as to obtain the values shown in Tables 1 and 2. The compressive strength and other properties of the obtained mortar specimens at ages of 1 day and 7 days were measured in the same manner as in Example 1. [Example 6] A mortar specimen was prepared in the same manner as in Example 5, except that the cement clinker obtained in Example 5 was pulverized using a ball mill, and then K2SO4 (reagent) was added and mixed to obtain a powder containing pulverized cement clinker. The amount of K2SO4 (reagent) was set so that the ratio of K2O and SO3 in the powder containing pulverized cement clinker would be the values shown in Table 2. The compressive strength of the mortar specimen obtained at ages of 1 day and 7 days was measured in the same manner as in Example 1.
[0026] [Example 7] Mortar specimens were prepared in the same manner as in Example 1, except that the cement clinker raw material was prepared so as to obtain the values shown in Tables 1 and 2. The compressive strength and other properties of the obtained mortar specimens at ages of 1 day and 7 days were measured in the same manner as in Example 1.
[0027] [Comparative Example 1] Mortar specimens were prepared in the same manner as in Example 1, except that the cement clinker raw material was prepared so as to obtain the values shown in Tables 1 and 2. The compressive strength and other properties of the obtained mortar specimens at ages of 1 day and 7 days were measured in the same manner as in Example 1. [Comparative Example 2] Mortar specimens were prepared in the same manner as in Comparative Example 1, except that the cement clinker obtained in Comparative Example 1 was pulverized using a ball mill, and then quicklime was added and mixed to obtain a powder containing pulverized cement clinker. The amount of quicklime was set so that the ratio of free lime (f·CaO) in the powder containing pulverized cement clinker would be the value shown in Table 1. The compressive strength and other properties of the mortar specimens obtained at ages of 1 day and 7 days were measured in the same manner as in Example 1.
[0028] [Comparative Example 3] Mortar specimens were prepared in the same manner as in Example 1, except that the cement clinker raw material was prepared so as to obtain the values shown in Tables 1 and 2. The compressive strength and other properties of the obtained mortar specimens at ages of 1 day and 7 days were measured in the same manner as in Example 1. The cement produced in Comparative Example 3 corresponds to high early strength Portland cement. The results are shown in Tables 1 to 3.
[0029] [Table 1]
[0030] [Table 2]
[0031] [Table 3]
[0032] From Table 1, the compressive strength of the mortar of the hardened bodies of the cement compositions of Examples 1 to 7 (produced in an environment of 10°C using the powder containing ground cement clinker of the present invention and cement containing gypsum) (material age of 1 day: 8.8 to 10.6 N / mm 2 , material age 7 days: 35.6~38.2N / mm 2 ) is the compressive strength of the mortar of Comparative Examples 1 to 3 (material age 1 day: 4.2 to 6.2 N / mm 2 , material age 7 days: 32.8~35.2N / mm 2) is found to be larger than It can also be seen that the ratio (0.29 to 0.38) of the mortar compressive strength at one day of the mortar produced in an environment at 10°C in Examples 1 to 7 to the mortar compressive strength at one day of the mortar produced in an environment at 20°C is greater than the above ratio (0.16 to 0.25) in Comparative Examples 1 and 4 to 7. The above ratios (0.34 to 0.36) in Examples 5 to 6 are equivalent to those in Examples 1 to 3, but the compressive strength of the hardened mortar of the mortar compositions in Examples 5 to 6 (age 1 day: 8.9 to 9.2 N / mm 2 , 7 days old: 35.6~36.4N / mm 2 ) is the compressive strength of the hardened mortar of the mortar compositions of Examples 1 to 3 (age 1 day: 10.3 to 10.6 N / mm 2 , material age 7 days: 37.4~38.2N / mm 2 ) is smaller than
Claims
1. A powder containing ground cement clinker, which is a mixture of ground cement clinker and quicklime powder, Borg type (but Alite (C 3 The value of the percentage of CaO used in the calculation of the percentage of free lime (f.CaO) is calculated by subtracting the percentage of free lime (f.CaO) from the percentage of total CaO contained in the powder containing pulverized cement clinker. 3 S) is 56 to 65 mass%, belite (C 2 S) is 12 to 20 mass%, and aluminate phase (C 3 A) is 12 to 18 mass %, and the ferrite phase (C 4 The ratio of free lime (f.CaO) is 0.5 to 12 mass% and the ratio of free lime (f.CaO) is 0.8 to 3.0 mass%, A powder containing pulverized cement clinker, characterized in that the proportion of potassium is 0.40 to 0.80 mass % calculated as oxide (K 2 O).
2. The value calculated by the Bogue formula is alite (C 3 S) is 59 to 65 mass%, belite (C 2 S) is 12 to 20 mass%, and aluminate phase (C 3 A) is 12 to 18 mass %, and the ferrite phase (C 4 The cement clinker pulverized powder according to claim 1, wherein the proportion of free lime (f.CaO) is 2 to 12 mass% and the proportion of free lime (f.CaO) is 0.9 to 2.2 mass%.
3. Ferrite phase (C) measured by X-ray diffraction method 4 The powder containing ground cement clinker according to claim 1 or 2, wherein the crystallite size of AF) is 30 to 90 nm.
4. A cement comprising the powder containing ground cement clinker according to any one of claims 1 to 3 and gypsum, The proportion of sulfur is SO 3 The calculated molecular weight is 3.0 to 3.5 mass % and the Blaine specific surface area is 4,800 to 6,000 cm 2 / g.
5. A kneading step of kneading the cement according to claim 4 with other materials including water at a temperature of 10°C or less to obtain an unhardened cement composition; a curing step of curing the unhardened cement composition to obtain a hardened cement composition; A method for producing a hardened product of a cement composition comprising the above-mentioned.
Citation Information
Patent Citations
Hardening accelerator and cement composition
JP2003277111A
Cement composition and method for producing the same
JP2010228926A
Cement composition and method for producing cement composition
JP2012012285A
Cement production method
JP2016183060A
Cement composition
JP2017154904A