PRODUCT WITH PROTECTIVE COATING AND METHOD OF MANUFACTURING SAME - Patent application
A dual-layer protective coating formed by in-situ polymerization of fluorine-free and fluorine-containing precursors addresses slow film formation and single-layer limitations, enhancing waterproof and corrosion resistance in electronic products.
Patent Information
- Application Number
- JP2023060017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-02
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-10-25
AI Technical Summary
Existing protective coatings for electronic products suffer from slow film formation rates and low efficiency, as well as limitations due to single-layer materials with pores, leading to inadequate waterproof performance and resistance to salt spray corrosion.
A method involving the application of a first and second precursor dispersion, where the first is fluorine-free and the second contains a fluorine-containing monomer, which are applied to form a fluorine-free inner layer and a fluorine-containing outer layer through in-situ polymerization, enhancing adhesion and hydrophobicity to improve film formation efficiency and protective properties.
The method results in a dense protective coating with improved waterproof performance, resistance to salt spray corrosion, and UV aging resistance, while maintaining flexibility and adhesion, with the ability to compensate for surface roughness and enhance self-cleaning properties.
Smart Images

Figure 0007577151000003 
Figure 0007577151000004 
Figure 0007577151000005
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE This application relates to the technical field of polymeric protective coatings formed on articles, and in particular to articles with protective coatings and methods for making same. [Background technology]
[0002] As consumers increasingly demand reliability in electronic products, there has been an increasing amount of research into protective coatings for electronic components in electronic products. For example, electronic components such as printed circuit boards in electronic products are usually provided with protective coatings to improve their waterproof performance and resistance to salt spray corrosion.
[0003] Generally, parylene protective coatings can be formed on electronic devices by vapor deposition using paraxylene as a raw material. However, the rate of film formation is slow and the efficiency is low. Summary of the Invention [Problem to be solved by the invention]
[0004] To solve the problem that protective coatings for electronic products can only use a single layer material with micropores, and to solve the slow film formation rate and low efficiency, embodiments of the present application disclose a product with a protective coating and a method for manufacturing the same.
[0005] In order to solve the above technical problems, the present application is implemented as follows.
[0006] The present application provides a method for producing an article with a protective coating, the method comprising: preparing a first precursor dispersion comprising a first active organic precursor, the first active organic precursor being a fluorine-free monomer; preparing a second precursor dispersion comprising a second active organic precursor, the second active organic precursor being a fluorine-containing monomer; applying the first precursor dispersion to an article body, drying the applied first precursor dispersion to form a first dry layer; applying a second precursor dispersion to cover the first dry layer, drying the applied second precursor dispersion to form a second dry layer; and polymerizing the first active organic precursor and the second active organic precursor to obtain an article with a protective coating.
[0007] According to the manufacturing method of the present application, the first precursor dispersion and the second precursor dispersion are directly applied to the product body used as the substrate, so that the application efficiency of the first precursor dispersion and the second precursor dispersion can be significantly improved. Therefore, the film formation efficiency can be significantly improved. In certain embodiments, the first precursor dispersion and the second precursor dispersion can be applied by spraying, dot coating, brushing, dipping, or spray spraying according to the manufacturing parameters of different products.
[0008] According to another aspect of the present application, a product with a protective coating using the above manufacturing method comprises a product body and a polymeric protective coating formed on the surface of the product body. The polymeric protective coating is formed by in situ polymerization, and the polymeric protective coating comprises an inner polymer layer in contact with the product body and an outer polymer layer covering the outer surface of the inner polymer layer. The outer polymer layer is a fluorine-containing polymer layer formed by in situ polymerization, and the inner polymer layer is a fluorine-free polymer layer formed by in situ polymerization.
[0009] In some embodiments of the present application, the polymeric protective coating comprises an inner polymer layer in contact with the product body and an outer polymer layer covering the outer surface of the inner polymer layer. The outer polymer layer is a fluorine-containing polymer layer, and the inner polymer layer is a fluorine-free polymer layer. Thus, the waterproof performance and the ability of UV-resistant aging and self-cleaning function of the polymeric protective coating or the product body are improved by taking full advantage of the hydrophobicity, non-sticky to the touch and resistant to UV radiation in the fluorine-containing used as the outer polymer layer. In addition, since the inner polymer layer and the outer polymer layer formed by in situ polymerization form the polymeric protective coating together, the inner polymer layer and the outer polymer layer can offset each other in structure to form a high-density protective coating. Furthermore, the waterproof performance and resistance to salt spray corrosion of the polymeric protective coating and the product body are improved. [Brief description of the drawings]
[0010] The figures described in this specification are used to provide further understanding of the present application and constitute a part of the present application. In the following, the exemplary embodiments and descriptions of the present application are used to illustrate the present application, and are not intended to limit the present application. [Figure 1] 1 is a schematic diagram of the structure of a product with a protective coating in the present application; [Diagram 2] 1 is a SEM image of a cross section of an example protective coating. [Diagram 3] 1 is a flow chart of a first embodiment of a method for manufacturing a product with a protective coating in the present application. [Figure 4] 4 is a flow chart of a second embodiment of a method for producing a product with a protective coating in the present application. [Diagram 5] 4 is a flow chart of a third embodiment of a method for producing a product with a protective coating in the present application. [Figure 6]11 is a flow chart of a fourth embodiment of a method for producing a product with a protective coating in the present application. [Figure 7] 11 is a flowchart of a fifth embodiment of a method for manufacturing a product with a protective coating in the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In order to make the objectives, technical solutions and advantages of the present application clearer, the technical solutions of the present application will be clearly and completely described in conjunction with specific embodiments and figures of the present application. Obviously, the described embodiments are only some of the embodiments of the present application, rather than all the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work fall within the protection scope of the present disclosure.
[0012] Please refer to FIG. 1, which is a schematic diagram of the structure of the product with protective coating of the present application. The product with protective coating 10 includes a product body 11 and a polymer protective coating 12 formed on the surface of the product body 11 by in situ polymerization. In other words, the polymer protective coating 12 covers the entire product body 11. The polymer protective coating 12 includes an inner polymer layer 121 in contact with the product body 11 and an outer polymer layer 122 covering the outer surface of the inner polymer layer 121. The outer polymer layer 122 is a fluorine-containing polymer layer, and the inner polymer layer 121 is a fluorine-free polymer layer. Note that the polymer protective coating 12 covering the entire product body 11 can be understood as follows. That is, the polymer protective coating 12 is formed on the outer and / or inner surface of the product body 11, and the polymer protective coating 12 can be formed on the entire surface of the product body 11, or can be selectively formed on a part of the surface of the product body 11. Here, the fluorine-containing polymer layer is a perfluorocarbon organosiloxane polymer layer, and the fluorine-free polymer layer includes one or more of an alkoxysilane polymer layer, an epoxy resin polymer layer, a polyurethane polymer layer, and an acrylate polymer layer. The alkoxysilane polymer layer is amphiphilic, its organic end is similarly compatible with the outer layer, and its silane end can adhere well to the product body 11 (e.g., the product body is made of metal), so as to improve the slight roughness of the product body 11 (i.e., to compensate for the surface pores) while having good hydrophobicity. Thus, the polymer protective coating 12 can have excellent waterproof performance and resistance to salt spray corrosion by using the combination of materials disclosed herein. The fluorine-containing polymer layer has good waterproof performance, is not sticky to the touch, and has resistance to ultraviolet light. Thus, by applying (applying) a fluorine-containing polymer layer as the outer polymer layer, the waterproof performance of the product 10 with the protective coating can be greatly improved, and the ability of ultraviolet aging and self-cleaning can also be improved. The quality of the product 10 with the protective coating layer can be improved.In addition, the surface roughness of the product body 11 can be compensated for by the inner polymer layer 121, so that the outer polymer layer 122 can form a dense membrane without micropores. The polymer protective coating 12 forms a dense membrane layer as a whole, so that its protective performance is improved. In other words, the inner polymer layer 121 and the outer polymer layer 122 compensate each other in terms of structure, so that the polymer protective coating 12 is denser, and the protective coating is improved in terms of waterproof performance and resistance to salt spray corrosion of the product 10. In short, the polymer protective coating 12 of the present application can have good adhesion with the product body 11, waterproof performance, and resistance to salt spray corrosion.
[0013] As shown in Figure 2, it is a SEM image of the cross section of one example of the protective coating. The inner polymer layer 121 and the outer polymer layer 122 are chemically crosslinked. The inner polymer layer 121 and the outer polymer layer 122 have good interlayer bonding strength between them, and even form a single membrane structure without delamination. The polymer protective coating 12 is denser, so that the waterproof performance and resistance to salt spray corrosion of the product with the protective coating 10 are further guaranteed.
[0014] The product body 11 may generally be a printed circuit board such as a printed circuit board of a mobile phone (e.g., a smartphone or a pager), a sound and audio device (e.g., a radio or a personal audio device), a headset (e.g., a wireless earphone, a Bluetooth earphone, an anti-noise earphone), a video device (e.g., a TV, a DVD player, a portable DVD player, a video recorder, a virtual reality device, an augmented reality device, an extended reality device), a communication device (e.g., a digital and other set-top box, a computer and related components, a game control panel, or an antenna), a clock (e.g., an electronic clock or a smart clock), a data storage device, a lighting device, and a power bank, etc. Certainly, other electronic components may also be used as the product body 11 herein.
[0015] Although FIG. 1 only shows the polymeric protective coating 12 having a two-layer structure, i.e., an inner polymer layer 121 and an outer polymer layer 122, it should be understood that the polymeric protective coating 12 can also have a multi-layer structure having more than two layers in practice. For example, the polymeric protective coating 12 can have two, three, or more inner polymer layers 121 (i.e., multiple inner polymer sublayers) and one outer polymer layer 122. The polymeric protective coating 12 can also have two, three, or more inner polymer layers 121 (i.e., multiple inner polymer sublayers) and two, three, or more outer polymer layers 122 (i.e., multiple outer polymer sublayers). The polymeric protective coating 12 can also have one inner polymer layer 121 and two, three, or more outer polymer layers 122 (i.e., multiple outer polymer sublayers). The multiple inner polymer layers 121 can better compensate for the surface roughness of the product body 11, thereby making the polymeric protective coating 12 denser. The surface roughness of the product body 11 can also be compensated for by the multi-layer outer polymer layer 122, so that the waterproof performance, UV-resistant aging resistance and self-cleaning ability of the product 10 with the protective coating can be further improved. As a result, polymer protective coatings 12 with different structures can be used according to different products. Furthermore, users can combine the inner polymer sub-layer 121 and / or the outer polymer sub-layer 122 with different properties to achieve the best synergistic protective effect according to requirements.
[0016] In one embodiment, the inner polymer layer 121 (i.e., the fluorine-free polymer layer) is an alkoxysilane polymer layer, and the outer polymer layer 122 (i.e., the fluorine-containing polymer layer) is a perfluorocarbon silicone oxyane polymer layer. The alkoxysilane polymer has good film-forming properties, good adhesion to the product body 11, and hydrophobicity, and is therefore particularly suitable as the inner polymer layer 121. The perfluorocarbon organosiloxane polymer has excellent hydrophobicity, is not sticky to the touch, and has resistance to ultraviolet radiation, and is therefore particularly suitable as the outer polymer layer 122. Therefore, the polymer protective coating 12 will have excellent waterproof performance and resistance to salt spray corrosion. Furthermore, the polymer protective coating 12 includes a fluorescent agent. The fluorescent agent is an externally added fluorescent agent or an internally added fluorescent agent. Here, the externally added fluorescent agent includes one or more of a stilbene type fluorescent agent, a coumarin type fluorescent agent, a pyrazoline type fluorescent agent, a benzoxazole type fluorescent agent, and a dimethylimide type fluorescent agent. Here, the internally added fluorescent agent connects to the outer polymer layer and / or the inner polymer layer via one or more of epoxy resin group, unsaturated triple bond, unsaturated double bond, silicone, -COONH, -OH, -COOH, -NH2, and -SH. In particular, the inner polymer layer 121 or the outer polymer layer 122 includes a fluorescent agent, or both the outer polymer layer 122 and the inner polymer layer 121 include a fluorescent agent. Here, the fluorescent agent of the outer polymer layer 122 may be the same as or different from the fluorescent agent of the inner polymer layer 121. In some embodiments of the present application, the fluorescent agent of the outer polymer layer 122 is the same as the fluorescent agent of the inner polymer layer 121, so that the polymer protective coating 12 has obvious indication effect. Therefore, the state of the polymer protective coating 12 can be better examined at any time, and then the polymer protective coating 12 can be repaired in time. In some embodiments of the present application, the fluorescent agent of the outer polymer layer 122 is different from the fluorescent agent of the inner polymer layer 121. For example, the fluorescent agent in the outer polymer layer 122 and the fluorescent agent in the inner polymer layer may fluoresce different colors under ultraviolet light.In this way, the state of each of the outer polymer layer 122 and the inner polymer layer 121 can be clearly observed. Thus, maintenance of each layer can be performed. Furthermore, in some embodiments, the inner polymer layer 121 and / or the outer polymer layer 122 includes multiple layers, and each of the inner polymer layer 121 and / or each of the outer polymer layer 122 includes a fluorescent agent, or only a part of the inner polymer layer 121 and / or the outer polymer layer 122 includes a fluorescent agent. In some embodiments of the present application, each of the inner polymer layer 121 and / or each of the polymer layers 122 includes a fluorescent agent, and the fluorescent agent in each sublayer of the inner polymer layer 121 and / or the fluorescent agent in each sublayer of the outer polymer layer 122 are the same or different. For example, if the fluorescent agent in each sublayer of the inner polymer layer 121 is the same as the fluorescent agent in each sublayer of the outer polymer layer 122, each sublayer of the inner polymer layer 121 and each sublayer of the outer polymer layer 122 can show the same fluorescent color. Therefore, the inner polymer layer 121 and the outer polymer layer 122 have obvious display effect, so that the status of the inner polymer layer 121 and the outer polymer layer 122 can be better examined at any time. If the fluorescent agent of each sublayer of the inner polymer layer 121 is different from the fluorescent agent of each sublayer of the outer polymer layer 122, each sublayer of the inner polymer layer 121 and each sublayer of the outer polymer layer 122 can show different fluorescent colors. Therefore, the respective status of each sublayer can be clearly observed, so that the maintenance of each layer can be performed.
[0017] In this embodiment and in some embodiments, the inner polymer layer 121 includes an adhesive resin. The adhesive resin is selected from the group consisting of silicone resin, epoxy resin, acrylic resin, polyurethane resin, and polyester resin. The adhesive resin can adhere well to the product body 11. Thus, the adhesion of the protective coating to the product body 11 is further improved, and the risk of the coating peeling off from the product body 11 is reduced. As shown in FIG. 1, the thickness of the outer polymer layer 122 is equal to or greater than the thickness of the inner polymer layer 121. For example, the thickness ratio of the outer polymer layer 122 to the inner polymer layer 121 can be 1:(0.1-1). In particular, the thickness ratio can be 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, etc. The thickness of the protective coating is not so thick as to affect the heat dissipation of the electronic components. Flexible protective coatings are generally required for flexible PCBs (printed circuit boards) and folding positions. Therefore, an inner polymer layer 121 with a thinner inner thickness can be selected. In one example, the overall thickness of the protective coating can be reduced. In another example, slight roughness of the product body 11 can be sufficiently improved. Thus, a dense outer polymer layer 122 can be formed on the inner polymer layer 121. Thereby, a dense polymer protective coating 12 can be formed thanks to good compensation between the inner polymer layer 121 and the outer polymer layer 122. The thickness of the outer polymer layer 122 is 0.5-10 μm, and the thickness of the inner polymer layer 121 is 0.1-2 μm. In this embodiment and some embodiments, the thickness of the outer polymer layer 122 is 1-5 μm, and the thickness of the inner polymer layer 121 is 0.5-1 μm. The combination of an outer polymer layer 122 having a thickness of 1-5 μm and an inner polymer layer 121 having a thickness of 0.5-1 μm can form a dense polymer protective coating 12 without significantly increasing the thickness of the polymer protective coating 12.Therefore, the formed flexible coating is flexible, and the formed flexible coating provides excellent protection for certain components that require higher light transmission. Furthermore, the heat dissipation performance of the product 10 with the protective coating is improved.
[0018] The following further describes the method for producing the product 10 with a protective coating. With reference to FIG. 1 and FIG. 3, FIG. 3 is a flow chart of the first embodiment of the method for producing the product with a protective coating of the present application. As shown in step S10, a first precursor dispersion is prepared. That is, an alkoxysilane, a silicone resin, a stilbene-type fluorescent agent, an alkyl titanium catalyst, and an isocyanate curing agent are dispersed in a hydrofluoroether solvent to obtain a first precursor dispersion. In the first precursor dispersion, the content of the alkoxysilane is 24.3% by weight, the content of the adhesive resin is 1.4% by weight, the content of the fluorescent agent is 0.08% by weight, the content of the catalyst is 0.05% by weight, the content of the isocyanate curing agent is 4.2% by weight, and the rest is the hydrofluoroether solvent and unavoidable impurities. As shown in step S12, a second precursor dispersion is prepared. That is, a perfluorocarbon organosiloxane, a stilbene-type fluorescent agent, an alkyl titanium catalyst, and an isocyanate curing agent are dispersed in a hydrofluoroether solvent to obtain a second precursor dispersion. In the second precursor dispersion, the content of the perfluorocarbon organosiloxane is 22.8% by weight, the content of the catalyst is 0.8% by weight, the content of the fluorescent agent is 0.1% by weight, the content of the isocyanate curing agent is 3.2% by weight, and the rest is the hydrofluoroether solvent and unavoidable impurities. The adhesive resin is a silicone resin, but the present application is not limited thereto. In other embodiments, the adhesive resin can be selected from the group consisting of a silicone resin, an epoxy resin, an acrylic resin, a polyurethane resin, and a polyester resin. That is, the adhesive resin can be one or more of a silicone resin, an epoxy resin, an acrylic resin, a polyurethane resin, and a polyester resin. In one embodiment, the catalyst is an alkyl titanium catalyst, but the present application is not limited thereto. In other embodiments, the catalyst is selected from the group consisting of alkyl titanium catalysts, alkyl aluminum catalysts, and alkyl tin catalysts, i.e., the catalyst can be one or more of alkyl titanium catalysts, alkyl aluminum catalysts, and alkyl tin catalysts.Before the step of applying (spraying) the first precursor dispersion onto the product body 11, the method further includes a step of performing a pretreatment on the surface of the product body 11 to clean and / or activate the surface. More specifically, the pretreatment includes one or more of plasma treatment, discharge treatment, sandblasting treatment, polishing treatment, flame treatment, and primer treatment, so that the first precursor dispersion can better adhere to the product body 11.
[0019] As shown in step S14, the first precursor dispersion is applied to the product body 11 (such as a printed circuit board) and then dried at room temperature for 1 to 10 minutes. Here, the room temperature applies between 20 and 25°C. In this embodiment, the applied first precursor dispersion is dried at 20°C for 1 minute to remove the hydrofluoroether solvent. Thereby, a first dry layer is formed. The solvent in the first precursor dispersion can be completely evaporated under the drying conditions, which can prevent the first active organic precursor from being polymerized earlier than expected. The first dry layer is applied to the inner polymer layer 121. As shown in step S16, the second precursor dispersion is applied to the first dry layer to cover the first dry layer. The applied second precursor dispersion is dried at room temperature for 1 to 10 minutes. In this embodiment, the applied second precursor dispersion is dried at 20°C for 1 minute. Then, the applied second precursor dispersion is dried at 70 to 90°C for 1 to 10 minutes. In this embodiment, the applied second precursor dispersion is dried at 80° C. for 2 minutes to remove the hydrofluoroether solvent. This forms a second dry layer covering the first dry layer. A pre-drying process at room temperature is carried out to evaporate the solvent, so that a thicker second dry layer is preliminarily formed. A drying process at 80° C. for 2 minutes is carried out to quickly evaporate the solvent, which can prevent the second active organic precursor from polymerizing earlier than expected. The second dry layer is applied to the outer polymer layer 122. Note that the applied amount of the second precursor dispersion is greater than that of the first precursor dispersion, so that the thickness of the second dry layer is greater than that of the first dry layer. Finally, as shown in step S18, the first active organic precursor and the second active organic precursor are polymerized to obtain the product 10 with a protective coating. In detail, the sample 111, i.e., the product 10 with a protective coating, is obtained by polymerizing the second dry layer and the first dry layer on the product body 11 at 23° C. and 50% humidity for 24 hours. It should be noted that in the above embodiment, the thicker second dry layer can be formed by a two-stage drying process, thereby preventing the second active organic precursor from polymerizing faster than expected.Since the polymerization conditions of the polymerization step are easily performed, the first active organic precursor and the second active organic precursor are significantly polymerized. Therefore, the inner polymer layer 121 and the outer polymer layer 122 can be polymerized respectively, and chemical cross-linking occurs at the interface of the two layers. Therefore, the inner polymer layer 121 can be integrated with the outer polymer layer 122, ensuring that the protective coating is dense. As a result, the waterproof performance and resistance to salt spray corrosion of the polymer protective coating 12 or the product body 11 are further ensured. The first dry layer is transformed into the inner polymer layer 121, and the second dry layer is transformed into the outer polymer layer 122. Furthermore, in the above description, the inner polymer layer 121 and the outer polymer layer 122 are formed by in-situ polymerization of the first dry layer and the second dry layer on the product body 11. Here, the initial conditions for forming the polymer protective coating 12 can be moisture curing, heat curing, UV curing, or electron beam curing, but the present application is not limited thereto.
[0020] As mentioned above, FIG. 2 is an SEM image of the sample 111. FIG. 2 shows that the inner polymer layer 121 and the outer polymer layer 122 are tightly bonded to each other, thus forming a dense polymer protective coating 12. Specifically, there are no other layers between the inner polymer layer 121 and the outer polymer layer 122, and each layer has a single membrane structure that is uniformly polymerized. There are no pinholes or defects in the structure. The thickness of the inner polymer layer 121 and the thickness of the outer polymer layer 122 of the sample 111 are tested. The static water contact angle (WCA) of the polymer protective coating 12 is tested (environmental parameters of the test: 25°C / 50%). The adhesion test is carried out according to the GBT9286-1998 standard. The resistance to salt spray corrosion test is carried out in 5% (by mass) NaCl solution (pH value: 6.5-7.2) at 35°C±1°C according to the national standard of GB6458-86 salt spray test. The bending resistance test is carried out. The light transmittance test is carried out according to GB-T2410-2008 standard.
[0021] For salt spray corrosion resistance, the level of resistance to salt spray corrosion of an example is defined as level 0 if the example has 0% rust area. The level of resistance to salt spray corrosion of an example sample is defined as level 1 if less than 1% of the example area is rust area. The level of resistance to salt spray corrosion of an example is defined as level 2 if less than 5% of the example area is rust area. The level of resistance to salt spray corrosion of an example is defined as level 3 if less than 10% of the example area is rust area. The level of resistance to salt spray corrosion of an example is defined as level 4 if less than 20% of the example area is rust area. The level of resistance to salt spray corrosion of an example is defined as level 5 if more than 20% of the example area is rust area.
[0022] The bending resistance test is carried out according to the following method: Apply the polymer protective coating on the polyimide (PI) film in order, bend the polyimide film 180 degrees after fully curing, and determine the result. Level 0: No wrinkles or slight wrinkles. Level 1: Many cracks appear, but the coating is not peeled off. Level 2: Many cracks appear and the coating is peeled off. Level 3: The coating is damaged and peeled off.
[0023] The above experiments and tests are repeated with different materials. The compositions of the different embodiments are shown in Table 1, and the test results are shown in Table 2.
[0024] Note that when sample 333 is prepared, two types of first precursor dispersions (shown in Table 1) are used to form inner polymer layer 121, and one type of second precursor dispersion (shown in Table 1) is used to form inner polymer layer 121. Thus, inner polymer layer 121 has two sublayers, and outer polymer layer 122 is a single layer.
[0025] When sample 444 is prepared, one first precursor dispersion (shown in Table 1) is used to form inner polymer layer 121, and two second precursor dispersions (shown in Table 1) are used to form inner polymer layer 121. Thus, inner polymer layer 121 is a single layer, and outer polymer layer 122 has two sublayers.
[0026] When sample 555 is prepared, two first precursor dispersions (shown in Table 1) are used to form the inner polymer layer 121, and two second precursor dispersions (shown in Table 1) are used to form the inner polymer layer 121. Thus, the inner polymer layer 121 has two sublayers, and the outer polymer layer 122 also has two sublayers.
[0027] Comparative Example 1 Using conventional methods, a protective coating is prepared on the printed circuit board as product body 11, thus forming test piece 666.
[0028] The thickness of the protective coating of sample 666 is tested. The static water contact angle (WCA) of the protective coating is tested (environmental parameters of the test: 25℃ / 50%). The adhesion test is carried out according to the GBT9286-1998 standard. The resistance test to salt spray corrosion is carried out in 5% (by mass) NaCl solution (pH value: 6.5-7.2) at 35±1℃ according to the national standard of GB6458-86 salt spray test. The bending resistance test is carried out. The light transmittance test is carried out according to the GB-T2410-2008 standard, and the test results are shown in Table 2.
[0029] [Table 1]
[0030] [Table 2]
[0031] Table 2 shows that although the difference between the thickness of the polymer protective coating 12 of Sample 111 and Sample 122 and the thickness of the polymer protective coating 12 of Sample 666 is small, the resistance to salt spray corrosion of Sample 111 and Sample 222 is better than that of Sample 666. In addition, the static water contact angle (WCA) of Sample 111, Sample 222, Sample 333, Sample 444 and Sample 555 is higher than that of Sample 666, so that Sample 111, Sample 222, Sample 333, Sample 444 and Sample 555 can be realized to have higher waterproof performance. The product 10 with the protective coating manufactured according to the method of the present application can be realized to have good waterproof performance and resistance to salt spray corrosion. Meanwhile, the polymer protective coating 12 of the present application can have excellent waterproof performance and resistance to salt spray corrosion with a transmittance of at least 89%.
[0032] According to the manufacturing method of the present application, the first precursor dispersion and the second precursor dispersion are directly applied to the product body 11 used as the substrate, which can significantly improve the efficiency of applying the first precursor dispersion and the second precursor dispersion, and therefore the film formation speed is greatly improved.
[0033] In this embodiment and some other embodiments, before the step of drying the applied first precursor dispersion to form the first dry layer, the method further includes a step of masking the product body 11. After the step of drying the applied first precursor dispersion to form the first dry layer, the method further includes a step of demasking the product body 11. These steps can be adjusted based on the conditions of the manufacturing method, and the present application is not limited thereto. The present application can have various modifications and variations. A polymer protective coating 12 can be formed on the product body 11 with sensitive components (microphones, sensors, etc.) through the above masking / demasking steps.
[0034] In the embodiments of the present application, the dispersion can be formed on the surface of the product body 11 by spraying to form the polymer protective coating 12 described herein. In particular, the liquid is atomized and applied to the surface of the product. The atomized spray is beneficial for forming a larger area of coating. For example, a large area of product can be completely and quickly protected via a high-precision spray valve, a large-area atomizing spray valve, or a water curtain spray valve. It should be noted that when the coating is formed by spraying, the dispersion must have suitable adhesive properties. For example, the viscosity of the dispersion must be less than 2000 cps. In some embodiments of the present application, the viscosity of the dispersion can be less than 1000 cps. The present application is not limited to the viscosity of the dispersion.
[0035] According to the disclosure of the present application, selective protection for partial locations can be performed, and more specifically, targeted protection for specific locations of a product can be performed. For example, in one embodiment of the present application, the coating described herein can be formed by brushing. The edges of the coating are easily movable with respect to brushing, so that the polymer protective coating 12 can be formed well under control, so that the polymer protective coating 12 can form a neat boundary on the product body 11. On the other hand, when the surface structure of the product body 11 is more complicated, for example, when the product body 11 has an uneven structure, it is difficult to form a uniform polymer protective coating 12 by spraying the surface. In these embodiments, the uniform polymer protective coating 12 can be effectively formed on the uneven surface of the product body 11 by brushing the concave and convex parts of the product body 11, respectively. It should be noted that when the polymer protective coating 12 is formed by brushing, proper adhesion of the dispersion is required. For example, the viscosity of the dispersion should be less than 1000 cps. In some embodiments of the present application, the viscosity of the dispersion can be less than 500 cps. Here, the present application is not limited to the viscosity of the dispersion.
[0036] In an embodiment of the present application, the polymer protective coating 12 described herein can be formed by dot coating, so as to form the polymer protective coating 12 on a more complex and / or finer structure. In addition, the product body 11 with the formed polymer protective coating 12 can be improved by dot coating. For example, the slits of the polymer protective coating 12 can be reinforced. Furthermore, when the polymer protective coating 12 is formed by dot coating, there are more options for the viscosity of the dispersion. For example, the viscosity of the dispersion can be 1000 cps or less, or the viscosity of the dispersion can be 1000 cps to 2000 cps. The viscosity of the dispersion can also be greater than 2000 cps.
[0037] The present disclosure is not limited to the above methods of forming the coating by spraying, brushing, or dot coating. In other embodiments, the dispersion can also be formed on the surface of the product body 11 by dipping, atomized spraying, etc.
[0038] The coating can be formed by spraying, brushing, dot coating, and other combinations thereof according to different cases, that is, the corresponding polymer protective coating 12 can be formed according to the characteristics of different product bodies 11. For illustrative purposes, various embodiments are given below.
[0039] For example, the manufacturing method can be used to protect the entire surface of a large-area product body 11 by using a high-precision spray valve or a large-area atomizing spray valve or a water curtain spray valve. Please refer to FIG. 1 and FIG. 4. FIG. 4 is a flow chart of a second embodiment of the manufacturing method of a product with a protective coating of the present application. In the following description, the polymer protective coating 12 is formed on two surfaces of the product body 11. Therefore, the two surfaces need to be treated, and the polymer protective coating 12 is formed thereon, respectively. In detail, before the step of applying the first precursor dispersion and the second precursor dispersion, a pretreatment is performed on the two surfaces of the product body to clean and / or activate the surfaces. More specifically, the pretreatment includes one or more of plasma treatment, discharge treatment, sandblasting treatment, polishing treatment, flame treatment, and primer treatment. In this embodiment, plasma treatment is taken as an example. As shown in step S20, the first precursor dispersion is sprayed on the product body 11 (such as a printed circuit board), and the first precursor dispersion is sprayed again after rotating the product body 11, i.e., the first precursor dispersion is completely sprayed to cover two surfaces of the product body 11. Then, as shown in step S22, the applied first precursor is dried at a temperature of 70-90°C for 1-10 minutes after spraying. In one embodiment, the applied first precursor is dried at a temperature of 80°C for 3 minutes to form a first dry layer, i.e., the inner polymer layer 121. As shown in step S24, the second precursor dispersion is brushed on the first dry layer, and the second precursor dispersion is sprayed again after rotating the product body 11. That is, the second precursor dispersion is completely brushed to cover the first dry layer. Next, as shown in step S26, the applied second precursor dispersion is dried after brushing at a temperature of 70-90° C. for 1-10 minutes. In one embodiment, the applied second precursor dispersion is dried at a temperature of 80° C. for 3 minutes to form the second dried layer, i.e., the outer polymer layer 122.Finally, as shown in step S28, the applied first precursor dispersion and the applied second precursor dispersion are polymerized to obtain the product 10 with a protective coating. The first precursor dispersion formed on the surface of the product body 11 by spraying and the second precursor dispersion formed on the surface of the product body 11 by brushing are suitable for large and flat areas, have excellent liquid leveling, and provide a uniform coating. Note that, since brushing is more destructive to the polymer protective coating 12, the first precursor dispersion needs to be dried to form a first dry layer or reach a surface dry state before brushing the second precursor dispersion. (i.e., the surface can be felt to be dry when touched).
[0040] With reference to FIG. 1 and FIG. 5, FIG. 5 is a flow chart of a third embodiment of the method for manufacturing a product with a protective coating of the present application. In the following description, the polymer protective coating 12 is formed on two surfaces of the product body 11. Thus, the two surfaces need to be treated and the polymer protective coating 12 is formed thereon, respectively. This embodiment is suitable for products with sturdy parts and / or slits in part of their surfaces. Thus, the inner polymer layer 121 is applied twice to cover the areas that are not completely covered after the first spraying process. That is, this embodiment is used to form a coating on a product body 11 with an uneven surface by dot coating or to compensate for slits generated from spraying (i.e., the surface is not completely covered by spraying). In detail, before the step of applying the first precursor dispersion and the second precursor dispersion, a pretreatment is performed on the two surfaces of the product body to clean and / or activate the surfaces. More specifically, the pretreatment includes one or more of plasma treatment, discharge treatment, sandblasting treatment, polishing treatment, flame treatment, and primer treatment. As an example in this embodiment, plasma treatment is taken. As shown in step S30, the first precursor dispersion is sprayed on the product body 11 (such as a printed circuit board), and the first precursor dispersion is sprayed again after turning over the product body 11, i.e., the first precursor dispersion is sprayed completely to cover two surfaces of the product body 11. Then, as shown in step S31, the applied first precursor is dried at a temperature of 70-90°C for 1-10 minutes after spraying. In one embodiment, the applied first precursor is dried at a temperature of 80°C for 3 minutes. Then, as shown in step S32, the first precursor dispersion is dot-coated on the area of the product body 11 that is not covered by spraying, and the first precursor dispersion is dot-coated again on the area of the product body that is not covered by spraying after turning over the product body. Then, as shown in step S33, the applied first precursor dispersion is dried at a temperature of 80°C for 3 minutes to form a first dried layer, i.e., the inner polymer layer 121.The uniformity and reliability of the polymer protective coating 12 can be increased in two steps of coating. After the coating problems of the partial areas with the sturdy parts and slits are solved, the second precursor dispersion is sprayed on the first dry layer, as shown in step S34, and the second precursor dispersion is sprayed on the first dry layer again after turning the product body 11 inside out. That is, the second precursor dispersion is sprayed completely to cover the first dry layer. Then, as shown in step S35, the applied second precursor dispersion is dried at a temperature of 70-90°C for 1-10 minutes after spraying. In one embodiment, the applied second precursor dispersion is dried at a temperature of 80°C for 3 minutes to form the second dry layer, i.e., the outer polymer layer 122. Finally, as shown in step S36, the first precursor dispersion and the second precursor dispersion are polymerized to obtain the product 10 with the protective coating.
[0041] Referring to FIG. 1 and FIG. 6, FIG. 6 is a flow chart of a fourth embodiment of the method for manufacturing a product with a protective coating of the present application. In the following description, the polymer protective coating 12 is formed on two surfaces of the product body 11. Therefore, the two surfaces need to be treated, and the polymer protective coating 12 is formed thereon, respectively. In detail, before the step of applying the first precursor dispersion and the second precursor dispersion, a pretreatment is performed on the two surfaces of the product body to clean and / or activate the surfaces. More specifically, the pretreatment includes one or more of plasma treatment, discharge treatment, sandblasting treatment, polishing treatment, flame treatment, and primer treatment. As shown in step S40, the first precursor dispersion is sprayed on the product body 11 (such as a printed circuit board), and the first precursor dispersion is sprayed again after turning over the product body 11. That is, the first precursor dispersion is sprayed completely to cover the two surfaces of the product body 11. Next, in step S42, the applied first precursor dispersion is dried at room temperature for 1-10 minutes, where the room temperature corresponds to 20-25°C. In this embodiment, the applied first precursor dispersion is dried at a temperature of 20°C for 2 minutes to form a first dry layer, i.e., the inner polymer layer 121. It should be noted that the drying conditions in this embodiment are suitable for these product bodies 11 with high requirements for residual surface stress and for these applications with high requirements for bonding strength between the upper layer and the lower layer. Therefore, the first precursor dispersion can be dried at room temperature to reduce the residual stress. Furthermore, as shown in step S44, the second precursor dispersion is brushed against the first dry layer, and the second precursor dispersion is sprayed again after rotating the product body 11. That is, the second precursor dispersion is sprayed completely to cover the first dry layer. Next, as shown in step S46, the applied second precursor dispersion is dried at a temperature of 70-90°C for 1-10 minutes after brushing. In this embodiment, the applied second precursor dispersion is dried at a temperature of 80° C. for 3 minutes to form the second dry layer, i.e., the outer polymer layer 122. Finally, as shown in step S48, the first precursor dispersion and the second precursor dispersion are polymerized to obtain the product 10 with a protective coating.In this step, the method also includes a plasma activation treatment, thus improving the surface energy of the fluorine-containing material to facilitate the bonding and use of subsequent materials.
[0042] The polymer protective coating 12 can be formed not only on the entire surface of the product body 11 but also on a part of the surface of the product body 11, so that it is suitable for the location of sensitive components that require masking, such as a microphone or a sensor. FIG. 7 is a flow chart of a fifth embodiment of the method for manufacturing a product with a protective coating of the present application. As shown in step S50, a masking element is used to mask the location of sensitive components (microphone, sensor, etc.) of the product body 11. Before the step of applying the first precursor dispersion and the second precursor dispersion, a pretreatment is performed on the two surfaces of the product body to clean and / or activate the surfaces. More specifically, the pretreatment includes one or more of plasma treatment, discharge treatment, sandblasting treatment, polishing treatment, flame treatment, and primer treatment. As shown in step S51, the first precursor dispersion is sprayed on the product body 11 (such as a printed circuit board), and the first precursor dispersion is sprayed again after turning the product body 11 over. That is, the first precursor dispersion is sprayed completely to cover the two surfaces of the product body 11 (except the positions of the masked sensitive components). Then, as shown in step S52, the applied first precursor dispersion is dried at room temperature for 1-10 minutes, where the room temperature corresponds to 20-25°C. In this embodiment, the applied first precursor dispersion is dried at a temperature of 20°C for 2 minutes to form a first dry layer, i.e., the inner polymer layer 121. As shown in step S53, the second precursor dispersion is brushed against the first dry layer, and the second precursor dispersion is sprayed again after rotating the product body 11. That is, the second precursor dispersion is sprayed all over to cover the first dry layer. Then, as shown in step S54, the applied second precursor dispersion is dried at a temperature of 70-90°C for 1-10 minutes after brushing. In this embodiment, the applied second precursor dispersion is dried at a temperature of 80° C. for 3 minutes to form a second dry layer, i.e., the outer polymer layer 122. In step S55, a laser cutting process is performed to cut and remove the unnecessary portions of the product body 11. In step S56, the masking elements disposed on the sensitive elements are removed.Finally, as shown in step S57, the first precursor dispersion and the second precursor dispersion are polymerized to obtain an article 10 with a protective coating.
[0043] According to the above description, the advantage of the present application is that the polymer protective coating includes an inner polymer layer that contacts the product body and an outer polymer layer that covers the outer surface of the inner polymer layer. The outer polymer layer is a fluoropolymer layer, and the inner polymer layer is a non-fluoropolymer layer. Therefore, the waterproof performance and the ability of UV aging resistance and self-cleaning function of the polymer protective coating or the product body are improved by making full use of hydrophobicity. The fluorine-containing material used as the outer polymer layer is non-sticky to the touch and resistant to UV radiation. In addition, since the inner polymer layer and the outer polymer layer formed by in-situ polymerization form the polymer protective coating together, the inner polymer layer and the outer polymer layer can offset each other in structure to form a high-density protective coating. Furthermore, the waterproof performance and salt spray corrosion resistance of the polymer protective coating and the product body are improved. Furthermore, in the present application, the first precursor dispersion and the second precursor dispersion can be applied by different combinations of spraying, dot coating, brushing, dipping, or atomized spraying according to the production parameters of different products, so that the efficiency of applying the first precursor dispersion and the second precursor dispersion can be improved, and the membrane formation speed is greatly improved.
[0044] The above description is merely an example of the present application and is not intended to limit the present application. This disclosure may have various modifications and variations for those skilled in the art. Any modifications, equivalent replacements, improvements, etc. made within the scope of the spirit and principles of this application shall be included in the scope of the claims of this disclosure.
Claims
[Claim 1] 1. A method of producing an article having a protective coating, comprising: preparing a first precursor dispersion, the first precursor dispersion comprising a first active organic precursor, the first active organic precursor being a fluorine-free monomer; preparing a second precursor dispersion, the second precursor dispersion comprising a second active organic precursor, the second active organic precursor being a fluorine-containing monomer; applying the first precursor dispersion to a product body, and drying the applied first precursor dispersion to form a first dry layer; applying the second precursor dispersion to the first dry layer to cover the first dry layer, and drying the applied second precursor dispersion to form a second dry layer; polymerizing the first active organic precursor and the second active organic precursor in situ to obtain an article having the protective coating; wherein the first precursor dispersion liquid contains 0.5 to 1.5 wt % of an adhesive resin, 0.01 to 0.1 wt % of a fluorescent agent, 0.1 to 5 wt % of an isocyanate curing agent, and 0.01 to 1 wt % of a catalyst; and the solvent is hydrofluoroether; The second precursor dispersion liquid contains 0.05 to 0.1 wt % of a fluorescent agent, 3.2 to 5 wt % of an isocyanate curing agent, and 0.4 to 0.8 wt % of a catalyst, and the solvent is a hydrofluoroether; the first active organic precursor is an alkoxysilane and the second active organic precursor is a perfluorocarbon organosiloxane; The method of claim 1, wherein the content of alkoxysilane in the first precursor dispersion is 9.7 to 24.3 wt % and the content of perfluorocarbon organosiloxane in the second precursor dispersion is 17.8 to 24.9 wt %.
Citation Information
Patent Citations
Composition for coating metals to protect against corrosion
JP2006525376A
Method for modifying surface of base material
JP2007501708A
Liquid repellent coating composition and coating with high alkali resistance
JP2007515498A
Perfluoropolyethersilanes and their use
JP2010502784A
Water-curable polysiloxane coating composition
JP2015527436A