Positive electrode active material for lithium secondary battery, method for producing same, and lithium secondary battery including same

A cobalt-coated lithium nickel-based composite oxide for lithium secondary batteries addresses structural instability and surface reactions, enhancing performance and longevity.

JP7577167B2Active Publication Date: 2024-11-01SAMSUNG SDI CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023120731
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-14
Filing Date
2023-07-25
Publication Date
2024-11-01
Estimated Expiration
2043-07-25

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face issues with structural collapse, cracking, reduced capacitance, and increased resistance due to repeated charging and discharging, leading to poor long-term life and high-temperature performance.

Method used

A positive electrode active material comprising lithium nickel-based composite oxides with a cobalt coating on secondary and single particles, where the cobalt content is adjusted to 1.45 to 1.60 times that of nickel and cobalt on the surface, is used to enhance stability and reduce surface reactions.

Benefits of technology

The material achieves high capacity and energy density while improving high-temperature long-term life characteristics and reducing gas generation, with enhanced initial charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577167000004
    Figure 0007577167000004
  • Figure 0007577167000005
    Figure 0007577167000005
  • Figure 0007577167000006
    Figure 0007577167000006
Patent Text Reader

Abstract

To provide a positive electrode active material for a lithium secondary battery, a manufacturing method for the same, and a lithium secondary battery including the same.SOLUTION: A positive electrode active material for a lithium secondary battery includes: a first positive electrode active material including a lithium nickel composite oxide, a secondary particle in which a plurality of primary particles are aggregated, and a cobalt coated part existing on a surface of the secondary particle; and a second positive electrode active material including a lithium nickel composite oxide, a single particle, and a cobalt coated part existing on a surface of the single particle. The content (at%) of cobalt to the total amount of nickel and cobalt in the cobalt-coated part in the first positive electrode active material is 1.45 to 1.60 times the content (at%) of cobalt to the total amount of nickel and cobalt in the cobalt-coated part in the second positive electrode active material. A manufacturing method for this positive electrode active material and a lithium secondary battery including the same are also provided.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a method for producing the same, and a lithium secondary battery including the same. [Background technology]

[0002] Lithium secondary batteries, which have high energy density yet are easy to carry, are mainly used as the driving power source for mobile information terminals such as mobile phones, laptops, and smartphones. Recently, active research has been conducted on using high-energy-density lithium secondary batteries as driving power sources or power storage sources for hybrid and electric vehicles.

[0003] In order to realize a lithium secondary battery suitable for such applications, various positive electrode active materials have been investigated. Among them, lithium nickel oxide, lithium nickel manganese cobalt composite oxide, lithium nickel cobalt aluminum composite oxide, lithium cobalt oxide, etc. are mainly used as positive electrode active materials. However, such positive electrode active materials have problems in that the structure collapses or cracks occur due to repeated charging and discharging, thereby reducing the long-term life of the lithium secondary battery, and the resistance increases, making it impossible to exhibit satisfactory capacity characteristics. Therefore, there is a need to develop a new positive electrode active material that can achieve high capacity and high energy density while ensuring long-term life characteristics. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a positive electrode active material for lithium secondary batteries, which realizes high capacity and high energy density while enhancing the stability of the positive electrode active material and reducing surface side reactions, thereby improving high-temperature long-term life characteristics and initial charge / discharge efficiency, and reducing the amount of gas generated during high-temperature storage; a method for producing the same; and a lithium secondary battery including the same. [Means for solving the problem]

[0005] In one embodiment, the present invention provides a positive electrode active material for a lithium secondary battery, comprising: a first positive electrode active material including a lithium-nickel-based composite oxide and including secondary particles formed by agglomeration of a plurality of primary particles and a cobalt coating portion located on a surface of the secondary particles; and a second positive electrode active material including a lithium-nickel-based composite oxide and including a single particle and a cobalt coating portion located on a surface of the single particle, wherein the content of cobalt (at %) relative to the total amount of nickel and cobalt in the cobalt coating portion of the first positive electrode active material is 1.45 to 1.60 times the content of cobalt (at %) relative to the total amount of nickel and cobalt in the cobalt coating portion of the second positive electrode active material.

[0006] In another embodiment, there is provided a method for manufacturing a positive electrode active material for a lithium secondary battery, the method including: performing a first step of introducing a second lithium-nickel-based composite oxide in the form of single particles and a cobalt raw material into a solvent; and sequentially performing a second step of introducing a first lithium-nickel-based composite oxide in the form of secondary particles formed by agglomeration of a plurality of primary particles and a cobalt raw material into the first step; obtaining a first positive electrode active material having a cobalt coating portion formed on a surface of the secondary particles; and a second positive electrode active material having a cobalt coating portion formed on a surface of the single particles, wherein a ratio of a time (min) required for the first step to a time (min) required for the second step is 65:35 to 75:25.

[0007] In yet another embodiment, a lithium secondary battery is provided that includes a positive electrode containing the positive electrode active material, a negative electrode, and an electrolyte. Effect of the Invention

[0008] The positive electrode active material for a lithium secondary battery manufactured according to an embodiment may realize high capacity and high energy density of a lithium secondary battery, while enhancing stability, reducing surface side reactions, suppressing gas generation during high temperature storage, improving initial charge / discharge efficiency, and improving high temperature long life characteristics. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic diagram showing a lithium secondary battery according to an embodiment. [Diagram 2] 1 is a SEM image of the final positive electrode active material prepared in Comparative Example 1. [Diagram 3] 1 is a SEM image showing a surface of a first positive active material in the form of secondary particles among the final positive active materials of Comparative Example 1. [Figure 4] 1 is a SEM image of the final positive electrode active material prepared in Example 1. [Diagram 5] 4 is a SEM image showing a surface of a first positive active material in the form of secondary particles among the final positive active materials in Example 1. [Figure 6] 6 shows an SEM image of a fracture surface of the first positive electrode active material of Comparative Example 1. The lower left part of FIG. 6 shows an image in which the cobalt element is highlighted by SEM-EDS analysis of the area indicated by a square. [Figure 7] 7 is a SEM image of a fracture surface of the first positive electrode active material of Example 1, and the lower left part of FIG. 7 is an image in which the cobalt element is highlighted by SEM-EDS analysis of the area indicated by a square. [Figure 8] 1 is an image in which the cobalt element is highlighted by SEM-EDS analysis of a fracture surface of the second positive electrode active material of Comparative Example 1. [Figure 9] 1 is an image in which cobalt element is highlighted by SEM-EDS analysis on a fracture surface of a second positive electrode active material of Example 1. [Figure 10] 1 is a graph showing high-temperature life characteristics of the lithium secondary batteries of Example 1 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings, in which: FIG. 1 is a block diagram of a semiconductor device according to an embodiment of the present invention;

[0011] The terms used herein are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless otherwise clearly indicated in the context.

[0012] As used herein, "combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like of compositions.

[0013] It should be understood that the terms "including," "comprising," or "having" are intended to specify the presence of embodied features, numerals, steps, components, or combinations thereof, and do not preclude the presence or additional possibility of one or more other features, numerals, steps, components, or combinations thereof.

[0014] In the drawings, the thickness of layers and regions is exaggerated to clearly show them, and similar parts are designated by the same reference numerals throughout the specification. When a part such as a layer, film, region, or plate is said to be "on" another part, this includes not only the case where the part is "directly on" the other part, but also the case where there is another part between them. Conversely, when a part is said to be "directly on" the other part, it means that there is no other part between them.

[0015] Further, the term "layer" as used herein includes not only a shape formed on the entire surface when observed in a plan view, but also a shape formed on a portion of the surface.

[0016] The average particle size can be measured by a method widely known to those skilled in the art, for example, by using a particle size analyzer or by using a transmission electron microscope or a scanning electron microscope. Alternatively, the average particle size can be calculated by using a dynamic light scattering method to count the number of particles for each particle size range through data analysis. Unless otherwise defined, the average particle size can refer to the diameter of the particles that make up 50% of the cumulative volume in the particle size distribution (D50).

[0017] As used herein, "or" is not to be construed in the exclusive sense, e.g., "A or B" is to be construed as including A, B, A+B, etc.

[0018] The term "metal" is understood to include general metals, transition metals, and metalloids (semimetals).

[0019] positive electrode active material In one embodiment, a positive electrode active material for a lithium secondary battery is provided, comprising: a first positive electrode active material including a lithium nickel-based composite oxide and including secondary particles formed by agglomeration of a plurality of primary particles and a cobalt coating portion located on a surface of the secondary particles; and a second positive electrode active material including a lithium nickel-based composite oxide and including a single particle and a cobalt coating portion located on a surface of the single particle. The cobalt content (at%) of the cobalt coating portion of the first positive electrode active material relative to the total amount of nickel and cobalt is 1.45 to 1.60 times the cobalt content (at%) of the cobalt coating portion of the second positive electrode active material relative to the total amount of nickel and cobalt.

[0020] In order to increase the energy density and improve the initial efficiency and long-term life characteristics, a technology has been proposed in which a positive electrode active material in the form of secondary particles is mixed with a positive electrode active material in the form of single particles. In addition, a technology of coating a positive electrode active material with a material such as cobalt is used to increase the structural stability of the positive electrode active material and suppress side reactions on the surface. When synthesizing a positive electrode active material with a high nickel content to achieve high capacity, a cation mixing phenomenon occurs and unreacted lithium compounds remain on the surface, so a water washing process is generally performed after synthesis, and a technology of coating a compound such as cobalt at the same time as the water washing process is used. However, when coating the secondary particles and single particles at the same time, a larger amount of coating material reacts and coats the single particles, which have a relatively high specific surface area, resulting in a coating imbalance between the secondary particles and the single particles. As a result, secondary particles cannot obtain a sufficient coating effect, and structural collapse and side reactions occur on the surface, accelerating deterioration. The uneven presence of coating particles on the surface induces gas generation, and excessive coating on single particles acts as resistance, adversely affecting battery performance.

[0021] In one embodiment, the coating on the secondary particles is strengthened while suppressing excessive coating on the single particles, i.e., the relationship between the coating contents of the two types of particles is appropriately adjusted to improve the performance of the lithium secondary battery, such as high-temperature long-term life characteristics. In one embodiment, when the cobalt coating content of the first positive electrode active material in the form of secondary particles is 1.45 to 1.60 times the cobalt coating content of the second positive electrode active material in the form of single particles, high capacity and high energy density can be realized, and at the same time, high-temperature long-term life characteristics can be improved, the amount of gas generation during high-temperature storage can be suppressed, and initial charge / discharge efficiency can be improved.

[0022] The cobalt content (at%) relative to the total amount of nickel and cobalt in the cobalt-coated portion of the first positive electrode active material may be 1.45 to 1.60 times, for example, 1.45 to 1.55 times, or 1.50 to 1.60 times, of the cobalt content (at%) relative to the total amount of nickel and cobalt in the cobalt-coated portion of the second positive electrode active material.

[0023] First positive electrode active material The first positive electrode active material has a polycrystal form and includes secondary particles formed by agglomerating at least two or more primary particles.

[0024] According to an embodiment, the first positive electrode active material includes a cobalt coating portion located on a surface of the secondary particle. The cobalt coating portion may be located on the entire surface or at least a portion of the surface of the secondary particle. The first positive electrode active material is coated with cobalt, which effectively prevents the structure from collapsing due to repeated charging and discharging, and improves room temperature and high temperature life characteristics.

[0025] The cobalt coating portion includes a cobalt-containing compound. The cobalt-containing compound may be, for example, cobalt oxide, cobalt hydroxide, cobalt carbonate, a composite thereof, or a mixture thereof. The cobalt-containing compound may further include other metals or nonmetallic elements in addition to cobalt. For example, the cobalt-containing compound may further include lithium, manganese, and / or nickel. For example, the cobalt-containing compound may be lithium cobalt oxide.

[0026] The content of cobalt relative to the total amount of nickel and cobalt in the cobalt coating portion of the first positive electrode active material may be 55 at% to 70 at%, for example, 55 at% to 68 at%, 55 at% to 65 at%, 55 at% to 63 at%, 57 at% to 70 at%, 59 at% to 70 at%, 60 at% to 70 at%, 60 at% to 65 at%, or 61 at% to 63 at%. When the cobalt coating content of the first positive electrode active material satisfies the above range and is 1.45 to 1.60 times the cobalt coating content of the second positive electrode active material, coating non-uniformity between particles is eliminated and a uniform coating is formed on the surface of the first positive electrode active material, suppressing gas generation, and improving initial charge / discharge efficiency and long-term life characteristics.

[0027] According to an embodiment, the first positive electrode active material may further include a grain boundary cobalt coating portion located on the surface of the primary particle inside the secondary particle. The grain boundary cobalt coating portion is present inside the secondary particle, not on the surface, and may be coated along the interface of the primary particle inside the secondary particle, and therefore may be expressed as being coated on the grain boundary. Here, the inside of the secondary particle means the entire inside except for the surface, and may mean, for example, a region from a depth of about 10 nm to the entire inside of the outer surface, or from a depth of 10 nm to a depth of about 2 μm. According to an embodiment, the first positive electrode active material may further include a grain boundary cobalt coating portion, thereby enhancing structural stability, inducing a uniform and even coating on the surface, and appropriately controlling the coating content on the surface, thereby improving initial charge / discharge efficiency and life characteristics without increasing resistance.

[0028] The average particle size of the first positive electrode active material, that is, the average particle size of the secondary particles, may be 5 μm to 25 μm. For example, it may be 7 μm to 25 μm, 10 μm to 25 μm, 15 μm to 25 μm, or 10 μm to 20 μm. The average particle size of the secondary particles of the first positive electrode active material may be larger than the average particle size of the second positive electrode active material of single particles described later. The positive electrode active material according to an embodiment may be in a form in which the first positive electrode active material, which is polycrystalline and large particles, is mixed with the second positive electrode active material, which is single particles and small particles, and therefore the mixture density may be improved, and high capacity and high energy density may be realized. Here, the average particle size of the first positive electrode active material may be determined by measuring the particle size of about 30 active materials in the form of secondary particles in an electron microscope photograph of the positive electrode active material, and taking the diameter (D50) of the particle having a cumulative volume of 50% by volume in the particle size distribution as the average particle size.

[0029] The first positive electrode active material is a nickel-based positive electrode active material and includes a lithium-nickel-based composite oxide. As an example, the first positive electrode active material may be a high-nickel-based positive electrode active material containing a high content of nickel. In this case, the content of nickel in the lithium-nickel-based composite oxide may be 80 mol% or more based on the total amount of elements excluding lithium and oxygen, for example, 85 mol% or more, 90 mol% or more, 91 mol% or more, 99.9 mol% or less, or 99 mol% or less. Such a high-nickel-based first positive electrode active material can achieve high capacity and high performance.

[0030] Second positive electrode active material The second positive electrode active material is in the form of a single particle, which means that the second positive electrode active material is present alone without a grain boundary within the particle and is composed of one particle, and may mean a single particle, a monolith structure, a single body structure, or a non-aggregated particle in which the particles are not aggregated with each other in terms of morphology, and may be a single crystal, for example. The positive electrode active material according to an embodiment includes the second positive electrode active material in the form of such a single particle, and thereby can exhibit improved life characteristics while realizing high capacity and high energy density.

[0031] According to an embodiment, the second positive electrode active material includes a cobalt coating portion located on a surface of a single particle. The second positive electrode active material is coated with cobalt to effectively prevent structural collapse due to repeated charging and discharging, thereby improving room temperature and high temperature life characteristics.

[0032] The cobalt coating portion includes a cobalt-containing compound. The cobalt-containing compound may be, for example, cobalt oxide, cobalt hydroxide, cobalt carbonate, a composite thereof, or a mixture thereof. The cobalt-containing compound may further include other metals or nonmetallic elements in addition to cobalt. For example, the cobalt-containing compound may further include lithium, manganese, and / or nickel. For example, the cobalt-containing compound may be lithium cobalt oxide.

[0033] In the cobalt-coated portion of the second positive electrode active material, the content of cobalt relative to the total amount of nickel and cobalt may be 39 at% to 45 at%, for example, 39 at% to 44 at%, 39 at% to 43 at%, 39 at% to 42 at%, 40 at% to 45 at%, or 41 at% to 45 at%. When the cobalt-coated content of the second positive electrode active material satisfies the above range and the ratio of the cobalt-coated content of the first positive electrode active material thereto satisfies 1.45 to 1.60, uneven coating between particles is eliminated, excessive coating on the second positive electrode active material is suppressed, and uniform coating is induced, reducing resistance, and improving initial charge / discharge efficiency and long-term life characteristics.

[0034] Meanwhile, in one embodiment, a method for measuring the cobalt content relative to the total amount of nickel and cobalt on the surface of the positive active material may be performed by performing scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDS) on the surface of the positive active material, determining the nickel and cobalt contents through quantitative analysis, and then calculating the ratio of the cobalt content to the total. As a method for measuring the cobalt content, inductively coupled plasma-mass spectrometry (ICP-MS) or inductively coupled plasma optical emission spectroscopy (ICP-OES) may be used in addition to SEM-EDS.

[0035] The average particle size of the second positive electrode active material, i.e., the average particle size of the single particle, may be 0.1 μm to 10 μm, for example, 0.1 μm to 7 μm, 0.5 μm to 6 μm, or 1 μm to 5 μm. The particle size of the second positive electrode active material may be smaller than that of the first positive electrode active material, so that the density of the positive electrode active material can be further increased. Here, the average particle size of the second positive electrode active material may be determined by measuring the particle size of about 30 single particle-form active materials randomly selected from an electron microscope photograph of the positive electrode active material, and taking the diameter (D50) of the particle having a cumulative volume of 50% by volume in the particle size distribution as the average particle size.

[0036] The second positive electrode active material is a nickel-based active material and includes a lithium-nickel-based composite oxide. As an example, the second positive electrode active material may be a high-nickel-based positive electrode active material containing a high content of nickel. In this case, the content of nickel in the lithium-nickel-based composite oxide may be 80 mol% or more based on the total amount of elements excluding lithium and oxygen, for example, 85 mol% or more, 90 mol% or more, 91 mol% or more, 99.9 mol% or less, or 99 mol% or less. Such a high-nickel-based second positive electrode active material can achieve high capacity and high performance.

[0037] Specifically, the first positive electrode active material and the second positive electrode active material may each independently include a lithium nickel-based composite oxide represented by the following Chemical Formula 1.

[0038] [Chemical formula 1] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1

[0039] In the formula 1, 0.9≦a1≦1.8, 0.8≦x1≦1, 0≦y1≦0.2, 0≦z1≦0.2, 0.9≦x1+y1+z1≦1.1, and 0≦b1≦0.1; M 1 and M. 2 are each independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

[0040] In the formula 1, 0.85≦x1≦1, 0≦y1≦0.15, and 0≦z1≦0.15, or 0.9≦x1≦1, 0≦y1≦0.1, and 0≦z1≦0.1.

[0041] For example, the first positive electrode active material and the second positive electrode active material may each independently contain a lithium nickel-based composite oxide represented by the following Chemical Formula 2. The compound represented by Chemical Formula 2 can be said to be a lithium nickel cobalt-based composite oxide.

[0042] [Chemical formula 2] Li a2 Ni x2 Co y2 M 3 z2 O 2-b2 X b2

[0043] In the above formula 2, 0.9≦a2≦1.8, 0.8≦x2<1, 0 <y2≦0.2、0≦z2≦0.2、0.9≦x2+y2+z2≦1.1、および0≦b2≦0.1であり、M 3 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

[0044] In the formula 2, 0.85≦x2≦0.99, 0.01≦y2≦0.15, and 0.01≦z2≦0.15, or 0.9≦x2≦0.99, 0.01≦y2≦0.1, and 0.01≦z2≦0.1.

[0045] For example, the first positive electrode active material and the second positive electrode active material may each independently include a lithium nickel-based composite oxide represented by the following Chemical Formula 3. The compound of Chemical Formula 3 may be lithium nickel-cobalt-aluminum oxide or lithium nickel-cobalt-manganese oxide.

[0046] [Chemical formula 3] Li a3 Ni x3 Co y3 M 4 z3 M 5 w3 O 2-b3 X b3

[0047] In the formula 3, 0.9≦a3≦1.8, 0.8≦x3≦0.98, 0.01≦y3≦0.19, 0.01≦z3≦0.19, 0≦w3≦0.19, 0.9≦x3+y3+z3+w3≦1.1, and 0≦b3≦0.1; 4 is one or more elements selected from the group consisting of Al and Mn, 5is one or more elements selected from the group consisting of B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

[0048] In Formula 3, 0.85≦x3≦0.98, 0.01≦y3≦0.14, 0.01≦z3≦0.14, and 0≦w3≦0.14, or 0.9≦x3≦0.98, 0.01≦y3≦0.09, 0.01≦z3≦0.09, and 0≦w3≦0.09.

[0049] As an example, the first positive electrode active material and the second positive electrode active material may each independently include a lithium nickel-based composite oxide represented by the following Formula 4. The compound of Formula 4 may be said to be a cobalt-free lithium nickel-manganese-based oxide.

[0050] [Chemical formula 4] Li a4 Ni x4 Mn y4 M 6 z4 O 2-b4 X b4

[0051] In the above formula 4, 0.9≦a4≦1.8, 0.8≦x4<1, 0 <y4≦0.2、0≦z4≦0.2、0.9≦x4+y4+z4≦1.1、および0≦b4≦0.1であり、M 6 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

[0052] In the positive electrode active material according to an embodiment, the first positive electrode active material may be included in an amount of 50% by weight to 90% by weight, and the second positive electrode active material may be included in an amount of 10% by weight to 50% by weight, based on the total amount of the first positive electrode active material and the second positive electrode active material. The first positive electrode active material may be included in an amount of, for example, 60% by weight to 90% by weight, or 70% by weight to 90% by weight, and the second positive electrode active material may be included in an amount of 10% by weight to 40% by weight, or 10% by weight to 30% by weight. When the content ratio of the first positive electrode active material to the second positive electrode active material is as described above, the positive electrode active material including the first positive electrode active material and the second positive electrode active material may realize a high capacity, have an improved mixture density, and exhibit a high energy density.

[0053] Method for producing positive electrode active material In one embodiment, a method for manufacturing a positive electrode active material for a lithium secondary battery is provided, comprising: a first step of introducing a second lithium nickel-based composite oxide and a cobalt raw material in the form of a single particle into a solvent; a second step of introducing a first lithium nickel-based composite oxide and a cobalt raw material in the form of a secondary particle formed by agglomeration of a plurality of primary particles into the first step; and obtaining a first positive electrode active material having a cobalt coating portion formed on the surface of the secondary particle and a second positive electrode active material having a cobalt coating portion formed on the surface of the single particle. Here, the ratio of the time (min; min) required for the first step to the time (min; min) required for the second step is 65:35 to 75:25. According to this method, excessive coating on the single particle is suppressed and the coating on the secondary particle is strengthened, that is, the relationship between the coating contents of the two types of particles is appropriately controlled, and thus the performance of the lithium secondary battery, such as high-temperature long-term life characteristics, initial charge / discharge efficiency, and high-temperature storage performance, can be improved. For example, according to the preparation method, a positive electrode active material can be prepared in which the cobalt content (at%) relative to the total amount of nickel and cobalt in the cobalt-coated portion of the first positive electrode active material is 1.45 to 1.60 times the cobalt content (at%) relative to the total amount of nickel and cobalt in the cobalt-coated portion of the second positive electrode active material, as described above, and the above-mentioned positive electrode active material can be obtained.

[0054] Specifically, a solvent is put into a mixer, and then the second lithium-nickel-based composite oxide in the form of single particles and the cobalt raw material are put therein and mixed to perform the first process. The first process is performed for a certain period of time to obtain a first mixture, and the first lithium-nickel-based composite oxide in the form of secondary particles and the cobalt raw material are put into the first mixture and mixed in the second process. In other words, instead of simultaneously washing the single particles and the secondary particles while coating them, the first process of washing the single particles while coating them and the second process of washing the secondary particles while coating them are performed in sequence, thereby allowing the two types of particles to be uniformly coated.

[0055] Here, by appropriately adjusting the ratio of the time required for the first process to the time required for the second process, non-uniform coating of the single particles and secondary particles can be eliminated, and each can be coated at an appropriate ratio to suppress resistance and gas generation, thereby improving long-term life characteristics and initial charge / discharge efficiency. If the ratio of the time required for the first process (min) to the total time required for the first and second processes (min) is less than 0.65, the amount of coating on the surface of the second positive electrode active material in the form of single particles is excessively reduced, which reduces the structural stability of the second positive electrode active material, ultimately resulting in a deterioration in long-term life characteristics. Also, if the ratio of the time required for the first process (min) to the total time required for the first and second processes (min) is more than 0.75, the amount of coating on the second positive electrode active material is excessive, which increases the surface resistance, ultimately resulting in a shortened life.

[0056] In the first step, for example, the cobalt raw material may be added first, and then the second lithium-nickel-based composite oxide may be added sequentially, and in the second step, the cobalt raw material may be added first, and then the first lithium-nickel-based composite oxide may be added sequentially.

[0057] The first lithium nickel-based composite oxide and the second lithium nickel-based composite oxide may be a compound represented by the above-mentioned Chemical Formula 1, for example, a compound represented by Chemical Formula 2, Chemical Formula 3, or Chemical Formula 4.

[0058] The cobalt source may be, for example, cobalt hydroxide, cobalt carbonate, cobalt sulfate, cobalt oxide, cobalt nitrate, and the like.

[0059] In the first step, the cobalt raw material can be added so that the cobalt content relative to all elements excluding lithium and oxygen in the second lithium-nickel composite oxide is 0.01 to 7 molar parts, for example, 0.01 to 5 molar parts, or 0.1 to 3 molar parts, etc. In this case, a cobalt coating portion with an appropriate content can be formed.

[0060] Similarly, in the second step, the cobalt raw material can be added so that the cobalt content relative to all elements excluding lithium and oxygen in the first lithium-nickel composite oxide is 0.01 to 7 molar parts, for example, 0.01 to 5 molar parts, or 0.1 to 3 molar parts, etc. In this case, a cobalt coating portion with an appropriate content can be formed.

[0061] When the first lithium-nickel-based composite oxide is added in the second step, the first lithium-nickel-based composite oxide and the second lithium-nickel-based composite oxide may be added in a weight ratio of 9:1 to 5:5, for example, 8:2 to 6:4. When mixed in such a ratio, the energy density can be maximized.

[0062] In the first and second steps, a precipitant, a pH adjuster, etc. may be further added as necessary.

[0063] In one embodiment, the method for preparing a positive electrode active material may further include a process of performing the second process for a certain period of time to obtain a second mixture, filtering the second mixture to remove the solvent, and then drying the mixture. In this case, the drying may be performed for 5 to 15 hours at a temperature range of 100°C to 300°C. The dried product may be heat-treated. The heat treatment may be performed in an oxidizing gas atmosphere such as oxygen or air, and may be performed at 650°C to 900°C or 650°C to 800°C. The heat treatment time may vary depending on the heat treatment temperature, and may be performed for 5 to 30 hours or 10 to 24 hours, for example.

[0064] When the obtained product is heat-treated, a lithium raw material may be further added and heat-treated. The lithium raw material may be, for example, Li 2 CO 3 , LiOH, hydrates thereof, or combinations thereof. The lithium raw material can be added so that the lithium content relative to elements other than lithium and oxygen in the first lithium-nickel-based composite oxide and the second lithium-nickel-based composite oxide as a whole is 0.1 to 10 molar parts, for example, 0.1 to 8 molar parts, or 1 to 6 molar parts. In the process of washing with the above-mentioned solvent, damage occurs on the surface of the lithium-nickel-based composite oxide particles, which can cause problems such as a decrease in capacity and rate characteristics and an increase in resistance during high-temperature storage. However, by adding the lithium raw material during the heat treatment, the surface damage can be repaired and the capacity and rate characteristics can be improved.

[0065] positive electrode The positive electrode for a lithium secondary battery may include a current collector and a positive electrode active material layer located on the current collector. The positive electrode active material layer includes a positive electrode active material, and may further include a binder and / or a conductive material.

[0066] The binder serves to favorably adhere the positive electrode active material particles to each other and to favorably adhere the positive electrode active material to a current collector. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, and the like.

[0067] The content of the binder in the positive electrode active material layer may be about 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.

[0068] The conductive material is used to impart conductivity to the electrodes, and any electronically conductive material that does not undergo chemical changes in the battery that is constructed therewith can be used. Examples of the conductive material that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metal-based materials in the form of metal powder or metal fibers containing copper, nickel, aluminum, silver, and the like; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures thereof.

[0069] The content of the conductive material in the positive electrode active material layer may be 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.

[0070] The positive electrode current collector may be, but is not limited to, an aluminum foil.

[0071] negative electrode The negative electrode for a lithium secondary battery includes a current collector and a negative electrode active material layer located on the current collector. The negative electrode active material layer contains a negative electrode active material and may further contain a binder and / or a conductive material.

[0072] The negative electrode active material includes a material capable of reversibly inserting / desorbing lithium ions, lithium metal, an alloy of lithium metal, a material dopable and dedopable with lithium, or a transition metal oxide.

[0073] Examples of the material capable of reversibly inserting / desorbing lithium ions include carbon-based negative electrode active materials, which can include, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, fired coke, and the like.

[0074] As the alloy of lithium metal, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.

[0075] As the material dopable and dedopable with lithium, an Si-based negative electrode active material or an Sn-based negative electrode active material can be used. As the Si-based negative electrode active material, silicon, a silicon-carbon composite, SiO x (0 < x < 2), an Si-Q alloy (wherein Q is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and a combination thereof and is not Si), and as the Sn-based negative electrode active material, Sn, SnO 2, Sn-R alloy (wherein R is an element selected from the group consisting of alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), and a combination of at least one of these with SiO 2 The elements Q and R can be selected from the group consisting of Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.

[0076] The silicon-carbon composite may be a silicon-carbon composite including, for example, a core including crystalline carbon and silicon particles, and an amorphous carbon coating layer located on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon precursor may be coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or polymer resin such as phenol resin, furan resin, or polyimide resin. At this time, the content of silicon may be 10% by weight to 50% by weight based on the total weight of the silicon-carbon composite. The content of the crystalline carbon may be 10% by weight to 70% by weight based on the total weight of the silicon-carbon composite, and the content of the amorphous carbon may be 20% by weight to 40% by weight based on the total weight of the silicon-carbon composite. The thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D50) of the silicon particles may be 10 nm to 20 μm. The silicon particles may have an average particle size (D50) of preferably 10 nm to 200 nm. The silicon particles may be present in an oxidized form, and in this case, the ratio of the atomic content of Si:O in the silicon particles, which indicates the degree of oxidation, may be 99:1 to 33:67. The silicon particles may be SiO x particles, in which case SiO xHere, x may range from more than 0 to less than 2. Unless otherwise defined herein, the average particle size (D50) refers to the diameter of particles whose cumulative volume is 50% by volume in the particle size distribution.

[0077] The Si-based or Sn-based negative electrode active material may be mixed with a carbon-based negative electrode active material, and the weight ratio of the Si-based or Sn-based negative electrode active material to the carbon-based negative electrode active material may be 1:99 to 90:10.

[0078] The content of the negative active material in the negative active material layer may be 95 wt % to 99 wt % based on the total weight of the negative active material layer.

[0079] In one embodiment, the negative electrode active material layer may further include a binder and may optionally further include a conductive material. The content of the binder in the negative electrode active material layer may be 1 wt% to 5 wt% based on the total weight of the negative electrode active material layer. When the conductive material is further included, the negative electrode active material layer may include 90 wt% to 98 wt% of the negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.

[0080] The binder serves to effectively adhere the negative active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0081] Examples of the non-water-soluble binder include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, ethylene propylene copolymers, polystyrene, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.

[0082] The water-soluble binder may be a rubber-based binder or a polymeric resin binder. The rubber-based binder may be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The polymeric resin binder may be selected from polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0083] When a water-soluble binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity may be further included. As the cellulose-based compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or alkali metal salts thereof may be mixed and used. As the alkali metal, Na, K, or Li may be used. The content of such a thickener may be 0.1 to 3 parts by weight per 100 parts by weight of the negative electrode active material.

[0084] The conductive material is used to impart conductivity to the electrode, and any electronically conductive material that does not undergo chemical changes in the battery that is constructed can be used. Examples of the conductive material that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metal-based materials in the form of metal powder or metal fibers, including copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials including mixtures thereof.

[0085] The negative electrode current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0086] Lithium secondary battery Another embodiment provides a lithium secondary battery including a positive electrode, a negative electrode, a separator positioned between the positive electrode and the negative electrode, and an electrolyte.

[0087] 1 is a schematic diagram showing a lithium secondary battery according to an embodiment. Referring to FIG 1, a lithium secondary battery 100 according to an embodiment includes a battery cell including a positive electrode 114, a negative electrode 112 facing the positive electrode 114, a separator 113 disposed between the positive electrode 114 and the negative electrode 112, and a lithium secondary battery electrolyte impregnated in the positive electrode 114, the negative electrode 112, and the separator 113, a battery container 120 including the battery cell, and a sealing member 140 sealing the battery container 120.

[0088] The electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0089] The non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move. As the non-aqueous organic solvent, carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvents can be used. As the carbonate-based solvent, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used. Examples of the ester solvent include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, etc. Examples of the ether solvent include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., and examples of the ketone solvent include cyclohexanone, etc. The alcohol solvent may be ethyl alcohol, isopropyl alcohol, or the like, and the aprotic solvent may be nitriles such as R-CN (wherein R is a C2-C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond, an aromatic ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, or the like.

[0090] The non-aqueous organic solvent may be used alone or in combination of two or more thereof. When two or more thereof are used in combination, the mixing ratio may be appropriately adjusted depending on the desired battery performance, which is widely understood by those skilled in the art.

[0091] In addition, in the case of the carbonate-based solvent, a cyclic carbonate and a chain carbonate can be mixed and used. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte can be excellent.

[0092] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent in addition to the carbonate-based solvent, and the carbonate-based solvent and the aromatic hydrocarbon-based organic solvent may be mixed in a volume ratio of about 1:1 to about 30:1.

[0093] The aromatic hydrocarbon solvent may be an aromatic hydrocarbon compound represented by the following formula I:

[0094] [ka]

[0095] In the above formula I, R 4 ~R 9 are the same or different and are selected from the group consisting of hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, and combinations thereof.

[0096] Specific examples of the aromatic hydrocarbon solvent include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorobenzene ... and combinations thereof.

[0097] The electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound of the following formula II as a life-improving additive in order to improve the battery life.

[0098] [ka]

[0099] In the above formula II, R 10 and R 11 are the same or different and are selected from the group consisting of hydrogen, a halogen group, a cyano group, a nitro group, and a fluorinated alkyl group having 1 to 5 carbon atoms, 10 and R 11At least one of R is selected from the group consisting of a halogen group, a cyano group, a nitro group, and a fluorinated alkyl group having 1 to 5 carbon atoms, with the proviso that 10 and R 11 is not hydrogen at the same time.

[0100] Representative examples of the ethylene carbonate-based compound include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, etc. When such a life-improving additive is further used, the amount of the additive used can be appropriately adjusted.

[0101] The lithium salt is a material that is dissolved in a non-aqueous organic solvent and acts as a source of lithium ions in a battery to enable basic operation of a lithium secondary battery and to promote the movement of lithium ions between a positive electrode and a negative electrode.

[0102] A typical example of a lithium salt is LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiN(SO 2 C 2 F 5 ) 2 , Li(CF 3 SO 2 ) 2 N, LiN(SO 3 C 2 F 5 ) 2 , Li(FSO 2 ) 2 N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC 4 F 9 SO 3 , LiClO 4 , LiAlO 2 , LiAlCl 4 , LiPO2 F 2 , LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 ) (wherein x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxalato) phosphate, LiCl, LiI, LiB(C 2 O 4 ) 2 (lithium bis(oxalato)borate; LiBOB), and lithium difluoro(oxalato)borate (LiDFOB).

[0103] The lithium salt is preferably used at a concentration within the range of 0.1 M to 2.0 M. When the lithium salt concentration is within this range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance and can effectively migrate lithium ions.

[0104] The separator 113 separates the positive electrode 114 and the negative electrode 112 and provides a path for lithium ions to move, and can be any separator that is generally used in lithium ion batteries. That is, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability can be used. For example, the separator 113 can include glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene, or a combination thereof, and can be in the form of a nonwoven fabric or a woven fabric. For example, polyolefin-based polymer separators such as polyethylene and polypropylene are mainly used in lithium ion batteries, and coated separators containing ceramic components or polymer materials to ensure heat resistance or mechanical strength can also be used, and can be selectively used in a single-layer or multi-layer structure.

[0105] Lithium secondary batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used, into cylindrical, square, coin, pouch, etc. types depending on the shape, and into bulk and thin film types depending on the size. The structure and manufacturing method of these batteries are widely known in the art, so a detailed description will be omitted.

[0106] The lithium secondary battery according to an embodiment has a high capacity and is excellent in storage stability at high temperatures, life characteristics, and high rate characteristics, and can be used in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and portable electronic devices.

[0107] Examples of the present invention and comparative examples are described below. The following examples are merely examples of the present invention, and the present invention is not limited to the following examples.

[0108] Example 1 1. Preparation of the first lithium nickel-based composite oxide in the form of secondary particles Nickel sulfate (NiSO) is used as a metal raw material. 4 6H 2 O), cobalt sulfate (CoSO 4 7H 2 O) and manganese sulfate (MnSO 4 H 2 A mixture solution was prepared by dissolving 1,2-dichlorophenyl ether (1,2,3,4-tetrafluoroethylene) in distilled water (solvent) in a molar ratio of 95:4:1. Ammonia water (NH 4 OH) and sodium hydroxide (NaOH) as a precipitant were prepared.

[0109] After feeding the ammonia water dilution solution into the continuous reactor, the metal raw material mixed solution is continuously fed, and sodium hydroxide is fed to maintain the pH inside the reactor. The reaction is carried out slowly for about 80 hours, and when the reaction is stabilized, the overflowing product is collected and washed and dried to obtain the final precursor. As a result, the primary particles are aggregated to produce the first nickel hydroxide (Ni 0.95 Co 0.04 Mn 0.01 (OH) 2 ) is obtained, washed and dried.

[0110] The first nickel-based hydroxide and LiOH were mixed so that the mole ratio of lithium to the total metal amount of the first nickel-based hydroxide was 1.04, and the mixture was subjected to a first heat treatment at about 750°C for 15 hours in an oxygen atmosphere to obtain a first nickel-based oxide (LiNi 0.95 Co 0.04 Mn 0.01 O 2 The first nickel-based oxide thus obtained has an average particle size of approximately 15 μm and is in the form of secondary particles formed by agglomeration of primary particles.

[0111] 2. Preparation of the second lithium nickel-based composite oxide in the form of single particles Prepare a mixed solution by dissolving nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 95:4:1 in distilled water. 4 A dilution solution of nickel hydroxide (NiOH) and a precipitant, sodium hydroxide (NaOH), are prepared. After that, the metal raw material mixed solution, ammonia water, and sodium hydroxide are each put into the reactor. Next, the reaction is carried out for about 20 hours while stirring. After that, the slurry solution in the reactor is filtered and washed with high-purity distilled water, and then dried for 24 hours to obtain a second nickel hydroxide (Ni 0.95 Co 0.04 Mn 0.01 (OH) 2 The resulting second nickel hydroxide powder has an average particle size of about 4.0 μm and a specific surface area measured by the BET measurement method of about 15 m. 2 / g.

[0112] The obtained second nickel-based hydroxide, LiOH satisfying Li / (Ni+Co+Mn)=1.05, and 1 mol part of Al, 0.2 mol parts of Zr, and 0.1 mol parts of Mg as dopants per 100 mol parts of total metals in the second nickel-based hydroxide are mixed together and placed in a sintering furnace, where a second heat treatment is performed at 820°C for 10 hours in an oxygen atmosphere. The obtained material is then pulverized for about 30 minutes to separate / disperse into a large number of second nickel-based oxides having a single particle form. The average particle size of the obtained second nickel-based oxide having a single particle form is about 3.7 μm.

[0113] 3. Cobalt coating and final cathode active material fabrication The first step is carried out by adding distilled water solvent and cobalt sulfate to a mixer, and then adding and mixing the prepared second lithium-nickel-based composite oxide. The cobalt sulfate is added so that the second lithium-nickel-based composite oxide has a cobalt content of 2.5 molar parts relative to the total elements excluding lithium and oxygen. After the second lithium-nickel-based composite oxide is added in the first step, sodium hydroxide acting as a precipitant and pH adjuster is added and mixed.

[0114] After the first step is carried out for 70 minutes, cobalt sulfate is added thereto, and then the first lithium-nickel-based composite oxide is added and mixed in the second step. The first lithium-nickel-based composite oxide is added so that the weight ratio of the first lithium-nickel-based composite oxide to the second lithium-nickel-based composite oxide added earlier is 7:3. The cobalt sulfate is added so that the cobalt content in the first lithium-nickel-based composite oxide is 2.5 molar parts relative to the total elements excluding lithium and oxygen. In the second step, after the first lithium-nickel-based composite oxide is added, sodium hydroxide is added and mixed together.

[0115] After the second process is performed for 30 minutes, the mixture is filtered and dried at 200°C for 10 hours. The resulting material is then mixed with lithium raw material and placed in a sintering furnace and heat-treated in an oxygen atmosphere at about 710°C for 15 hours. The lithium raw material is added so that the lithium content is 5 mol parts based on the total elements in the resulting material excluding lithium and oxygen. The sintering furnace is then cooled at room temperature to obtain a final positive electrode active material in which a first positive electrode active material in which a cobalt coating portion is formed on the surface of a first lithium-nickel-based composite oxide in the form of secondary particles and a second positive electrode active material in which a cobalt coating portion is formed on the surface of a second lithium-nickel-based composite oxide in the form of single particles are mixed.

[0116] 4. Fabrication of the Positive Electrode 95% by weight of the final positive electrode active material, 3% by weight of polyvinylidene fluoride binder, and 2% by weight of carbon nanotube conductive material are mixed in N-methylpyrrolidone solvent to prepare a positive electrode active material slurry. The positive electrode active material slurry is applied to an aluminum current collector, dried, and then rolled to prepare a positive electrode.

[0117] 5. Manufacturing of lithium secondary batteries The prepared positive electrode and lithium metal counter electrode were used, and a polyethylene polypropylene multilayer separator was placed between them. 1.0 M LiPF was then placed in a solvent of ethylene carbonate and diethyl carbonate in a volume ratio of 50:50. 6 An electrolyte containing lithium salt is injected to produce a coin half-cell.

[0118] Comparative Example 1 In "3. Cobalt coating and preparation of final positive active material" of Example 1, simultaneous coating is performed without separately performing the first and second steps. That is, the first lithium-nickel-based composite oxide, the second lithium-nickel-based composite oxide, and the cobalt raw material are added to a solvent and mixed for 100 minutes, and then filtered and dried to obtain the final positive active material. Here, the cobalt raw material is added so that the content of cobalt relative to the total elements excluding lithium and oxygen in the first lithium-nickel-based composite oxide and the second lithium-nickel-based composite oxide as a whole is 2.5 molar parts.

[0119] The other steps are the same as in Example 1 to produce a positive electrode active material, a positive electrode, and a lithium secondary battery.

[0120] Comparative Example 2 In "3. Preparation of cobalt coating and final positive electrode active material" of Example 1, except that the first step is performed for 80 minutes and the second step is performed for 20 minutes, a positive electrode active material, a positive electrode, and a lithium secondary battery are prepared in the same manner as in Example 1.

[0121] Comparative Example 3 In "3. Preparation of cobalt coating and final positive electrode active material" of Example 1, except that the first step is performed for 60 minutes and the second step is performed for 40 minutes, a positive electrode active material, a positive electrode, and a lithium secondary battery are prepared in the same manner as in Example 1.

[0122] Evaluation example 1: Analysis of the surface of the positive electrode active material FIG. 2 is a SEM image of the final positive active material prepared in Comparative Example 1, and FIG. 3 is a SEM image of the surface of a first positive active material in the form of secondary particles in the final positive active material prepared in Comparative Example 1.

[0123] FIG. 4 is a SEM image of the final positive active material prepared in Example 1, and FIG. 5 is a SEM image of the surface of a first positive active material in the form of secondary particles in the final positive active material prepared in Example 1.

[0124] Comparing FIGS. 2 and 3 of Comparative Example 1 with FIGS. 4 and 5 of Example 1, it can be seen that in Example 1, the surface of the first positive electrode active material is more uniformly and thinly coated.

[0125] Evaluation example 2: Analysis of fracture surface of positive electrode active material Fig. 6 is an SEM image of a fracture surface of the first positive electrode active material of Comparative Example 1, and the lower left part of Fig. 6 is an image in which the cobalt element is highlighted by SEM-EDS analysis of the part indicated by a square. Fig. 7 is an SEM image of a fracture surface of the first positive electrode active material of Example 1, and the lower left part of Fig. 7 is an image in which the cobalt element is highlighted by SEM-EDS analysis of the part indicated by a square.

[0126] 6 and 7, it can be seen that in Comparative Example 1, a thick coating material is formed only on the surfaces of the secondary particles of the first positive active material, whereas in Example 1, cobalt is coated not only on the surfaces of the secondary particles of the first positive active material but also on the grain boundaries of the surfaces of the internal primary particles.

[0127] FIG. 8 is an image in which the cobalt element is highlighted by SEM-EDS analysis of a fracture surface of the second positive electrode active material of Comparative Example 1, and FIG. 9 is an image in which the cobalt element is highlighted by SEM-EDS analysis of a fracture surface of the second positive electrode active material of Example 1.

[0128] 8 and 9, it can be seen that the cobalt coating was more uniformly and evenly formed on the surface of the single particles of the second positive electrode active material in Example 1 compared to Comparative Example 1.

[0129] Evaluation Example 3: Analysis of cobalt coating content of positive electrode active material Through the SEM-EDS analysis performed in Evaluation Example 2, the cobalt content (Co / (Ni+Co), at %) on the surface of each of the first and second positive active materials was measured, and the results are shown in Table 1 below. The data in Table 1 are values ​​in which the total cobalt coating content of the first and second positive active materials was corrected to be the same as that of Example 1 in order to remove noise.

[0130] [Table 1]

[0131] Evaluation example 4: Evaluation of high temperature battery life characteristics The lithium secondary batteries manufactured in Example 1 and Comparative Examples 1 to 3 were initially charged under constant current (0.2C) and constant voltage (4.25V, 0.05C cut-off) conditions, and after a 10-minute pause, were discharged to 3.0V under constant current (0.2C) conditions to perform initial charge and discharge. Then, the batteries were repeatedly charged and discharged 150 times at 0.5C / 0.5C at 45°C. The capacity retention rate, which is the ratio of the discharge capacity at each cycle to the initial discharge capacity, that is, the high-temperature life characteristics, was evaluated, and the results are shown in FIG. 10.

[0132] Referring to Table 1 and FIG. 10, in the case of Comparative Example 1 where simultaneous coating was performed, an excessive amount of cobalt coating was performed on the surface of the first positive active material having a large surface area, and the high temperature life characteristics in FIG. 10 were deteriorated compared to Example 1. This is understood to be because non-uniform coating occurred between the first positive active material and the second positive active material, which accelerated the deterioration of the first positive active material during long life, resulting in a decrease in performance.

[0133] In Comparative Example 2, the first and second processes were performed sequentially, but the ratio of the time required for the first process to the total process was high. As a result, excessive coating was formed on the surface of the second positive electrode active material, which acted as resistance, and the coating on the surface of the first positive electrode active material was insufficient, resulting in high side reactions on the surface, which ultimately reduced the long-life characteristics.

[0134] In Comparative Example 3, the first and second processes were performed sequentially, but the ratio of the time required for the first process to the total process was low. It is understood that the coating content on the surface of the second positive electrode active material was reduced, resulting in a decrease in the surface stabilization effect, resulting in a decrease in long-life characteristics.

[0135] On the other hand, in the case of Example 1, it can be seen that the unevenness of the coating of the first and second positive electrode active materials is eliminated, the resistance due to the coating is reduced, and the effect of stabilizing the surface by the coating is maximized, resulting in improved high-temperature long-life characteristics.

[0136] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts defined in the claims also fall within the scope of the present invention. [Explanation of symbols]

[0137] 100: Lithium secondary battery 112: Negative electrode 113: Separator 114: Positive electrode 120:Battery container 140: Sealing member

Claims

1. a first positive electrode active material including a lithium nickel-based composite oxide, the first positive electrode active material including secondary particles formed by agglomerating a plurality of primary particles and a cobalt coating portion located on a surface of the secondary particles; A positive electrode active material for a lithium secondary battery, comprising: a second positive electrode active material including a lithium nickel-based composite oxide, the second positive electrode active material including a single particle and a cobalt coating portion located on a surface of the single particle, A positive electrode active material for a lithium secondary battery, wherein a content (at %) of cobalt relative to a total amount of nickel and cobalt in the cobalt-coated portion of the first positive electrode active material is 1.45 to 1.60 times a content (at %) of cobalt relative to a total amount of nickel and cobalt in the cobalt-coated portion of the second positive electrode active material.

2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the content of cobalt in the cobalt-coated portion of the second positive electrode active material is 39 at % to 42 at % based on the total amount of nickel and cobalt.

3. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the content of cobalt in the cobalt-coated portion of the first positive electrode active material is 61 at % to 63 at % based on the total amount of nickel and cobalt.

4. 2 . The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the first positive electrode active material further comprises a grain boundary cobalt coating portion located on a surface of a primary particle inside the secondary particle.

5. The average particle size of the first positive electrode active material is 5 μm to 25 μm, 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the average particle size of the second positive electrode active material is 0.1 μm to 10 μm.

6. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the first positive electrode active material is contained in an amount of 50% by weight to 90% by weight, and the second positive electrode active material is contained in an amount of 10% by weight to 50% by weight, based on the total amount of the first positive electrode active material and the second positive electrode active material.

7. The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the lithium nickel-based composite oxide of the first positive electrode active material and the lithium nickel-based composite oxide of the second positive electrode active material are each independently represented by the following chemical formula 1: [Chemical formula 1] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 (In the above Chemical Formula 1, 0.9≦a1≦1.2, 0.8≦x1≦1, 0≦y1≦0.2, 0≦z1≦0.2, 0.9≦x1+y1+z1≦1.1, and 0≦b1≦0.1; M 1 and M. 2 are each independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

8. A first step is carried out in which a second lithium-nickel-based composite oxide in a single particle form and a cobalt raw material are introduced into a solvent; A second process is then carried out in which the first lithium nickel-based composite oxide, which is in the form of secondary particles formed by agglomeration of a plurality of primary particles, and the cobalt raw material are added, obtaining a first positive electrode active material having a cobalt coating portion formed on a surface of the secondary particle and a second positive electrode active material having a cobalt coating portion formed on a surface of the single particle, A method for producing a positive electrode active material for a lithium secondary battery, wherein the ratio of the time (minutes) required for the first step to the time (minutes) required for the second step is 65:35 to 75:

25.

9. 9. The method for producing a positive electrode active material for a lithium secondary battery according to claim 8, wherein in the first step, the cobalt raw material is added so that the cobalt content of the cobalt raw material is 0.01 to 7 molar parts relative to all elements excluding lithium and oxygen in the second lithium-nickel-based composite oxide.

10. 9. The method for producing a positive electrode active material for a lithium secondary battery according to claim 8, wherein in the second step, the cobalt raw material is added so that the first lithium-nickel-based composite oxide has a cobalt content of 0.01 to 7 mol parts relative to all elements excluding lithium and oxygen.

11. The method for producing a positive electrode active material for a lithium secondary battery according to claim 8 , wherein the first lithium-nickel based composite oxide and the second lithium-nickel based composite oxide are each independently represented by the following chemical formula 1: [Chemical formula 1] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1 (In the above Chemical Formula 1, 0.9≦a1≦1.2, 0.8≦x1≦1, 0≦y1≦0.2, 0≦z1≦0.2, 0.9≦x1+y1+z1≦1.1, and 0≦b1≦0.1; M 1 and M. 2 are each independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.

12. 9. The method for producing a positive electrode active material for a lithium secondary battery according to claim 8, wherein a weight ratio of the first lithium-nickel based composite oxide to the second lithium-nickel based composite oxide is 9:1 to 5:

5.

13. 9. The method of claim 8, further comprising heat-treating the obtained material after the second process.

14. The method for producing a positive electrode active material for a lithium secondary battery according to claim 13, wherein the heat treatment is carried out at a temperature range of 650°C to 900°C.

15. The method of claim 13, further comprising adding a lithium raw material when the obtained material is heat-treated.

16. The method for producing a positive electrode active material for a lithium secondary battery according to claim 15, wherein the lithium raw material is added so that the content of lithium in the first lithium-nickel-based composite oxide and the second lithium-nickel-based composite oxide as a whole is 0.1 to 10 parts by mole based on elements excluding lithium and oxygen.

17. 9. The method of claim 8, wherein a cobalt content (at %) relative to a total amount of nickel and cobalt in the cobalt-coated portion of the first positive electrode active material is 1.45 to 1.60 times a cobalt content (at %) relative to a total amount of nickel and cobalt in the cobalt-coated portion of the second positive electrode active material.

18. 10. The method of claim 8, wherein the first positive active material further comprises a grain boundary cobalt coating portion located on a surface of a primary particle inside the secondary particle.

19. A lithium secondary battery comprising a positive electrode containing the positive electrode active material for lithium secondary batteries according to any one of claims 1 to 7, a negative electrode, and an electrolyte.

Citation Information

Patent Citations

  • Composite positive electrode active material, positive electrode containing the same, lithium battery and manufacturing method thereof

    JP2020068210A

  • Positive electrode active material for lithium secondary battery, method of manufacturing the same, and lithium secondary battery including the same

    JP2020072092A

  • Positive electrode active material for lithium secondary battery, manufacturing method for the same, and lithium secondary battery including positive electrode including the same

    JP2022082508A