Sodium battery high-voltage positive electrode material as well as preparation method and application thereof
By performing two-site doping and oxide coating treatment in Ni-Fe-Mn matrix material, the specific capacity and stability of sodium-electrode material at high voltage are solved, and specific capacity improvement and cyclic stability are achieved. The significant improvement in performance meets the needs of sodium ion batteries.
Patent Information
- Application Number
- CN202411122098.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-08
AI Technical Summary
The existing sodium electropositive electrode materials have low specific capacity and poor structural stability at high voltages, resulting in poor cycle life and difficult to meet the needs of commercial applications.
The Ni-Fe-Mn matrix material is used for double-site doping, and elements such as Li, K, Ca are added to support the Na layer, and elements such as Zn, Ti, Al are combined to enter the transition metal layer to improve the specific capacity and structural stability of the material. The electrolyte is also isolated by an oxide coating to prevent the material from reacting with the electrolyte.
It significantly improves the specific capacity and cycle stability of sodium electropositive electrode materials at high voltages, extends the service life of the materials, and meets the needs of commercial applications.
Smart Images

Figure CN118919692A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium battery positive electrode materials, and in particular to a sodium battery high-voltage positive electrode material and a preparation method and application thereof. Background Art
[0002] With the rapid development of the new energy industry, the global demand for lithium resources has grown rapidly. However, due to the limited lithium resources in the earth's crust, it is impossible to meet the increasingly mature battery industry chain in the long term. Therefore, we have to find a new type of battery material as a substitute for lithium batteries. The battery principle of sodium-ion batteries is similar to that of lithium-ion batteries. Both are "rocking chair batteries", but the reserves of sodium are extremely abundant, low in price, and relatively safe. Therefore, it has received widespread attention. At present, sodium-ion batteries have been used in household energy storage, large-scale energy storage, power and other fields.
[0003] Compared with lithium batteries, the biggest change in sodium-ion batteries is the positive electrode material, which is also a key factor in determining battery performance such as energy density, safety, and cycle life. There are currently three main types of positive electrode materials for sodium-ion batteries: layered oxides, Prussian blue compounds, and polyanion compounds. Among them, layered oxides have the advantage of high specific capacity, and are the most mature, with a production process similar to that of lithium batteries, and equipment that is compatible with lithium batteries, which can be quickly mass-produced. However, the capacity of the positive electrode material for sodium-ion batteries under conventional voltages is currently close to its limit, and a further substantial increase in capacity requires increasing the operating voltage to release more sodium ions. However, during the charge and discharge process, due to the Na + The deintercalation of NaO leads to complex phase transitions in layered oxide materials. In particular, the drastic PO phase transition under high voltage can cause a drastic change in the volume of the material, resulting in Na + The diffusion kinetics deteriorate. The residual stress generated by repeated volume changes causes cracks to form in the layered material, which in turn leads to poor cycle stability and is difficult to meet the needs of commercial applications. In addition, the current specific capacity of layered oxide positive electrode materials at high voltages is still low. Therefore, how to use effective methods to suppress the phase change of layered oxide positive electrode materials for sodium ion batteries at high voltages while simultaneously increasing the specific capacity of layered oxide positive electrode materials is crucial to promoting the industrialization of sodium ion batteries. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of existing sodium battery positive electrode materials, such as low specific capacity and weak structural stability under high voltage, thereby providing a sodium battery high-voltage positive electrode material and its preparation method and application that solve the above problems.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A sodium battery high voltage positive electrode material comprises a core body and a coating layer, wherein the chemical formula of the core body is Na x A a Ni b Fe c Mn d B e ; wherein A is at least one of Li, K, and Ca, B is at least one of Zn, Ti, Zr, and Al, 0.9≤x≤1.1, 0.005≤a≤0.05, 0.2≤b≤0.5, 0.2≤c≤0.5, 0.2≤d≤0.5, 0.01≤e≤0.1, and a+b+c+d+e=1.
[0007] Preferably, the coating layer is an oxide coating layer containing at least one element of zirconium, boron, aluminum, calcium and magnesium.
[0008] The present invention also provides a method for preparing the above-mentioned sodium battery high-voltage positive electrode material, comprising: weighing a nickel source, an iron source, a manganese source, a sodium source, and a doping element source respectively according to a stoichiometric ratio, mixing them, and performing a pre-baking treatment, and a baking treatment to obtain a sintered product;
[0009] The sodium battery high voltage positive electrode material is obtained by mixing a sintered product with a coating agent and performing a sintering treatment.
[0010] Preferably, the nickel source is at least one of NiO, NiSO4, NiCl2, Ni(NO3)2, and Ni(CH3COO)2;
[0011] And / or, the iron source is at least one of Fe2O3, Fe2(SO4)3, FeCl2, Fe(NO3)3, and Fe(CH3COO)3;
[0012] And / or, the manganese source is at least one of MnO2, MnO, MnSO4, MnCl2, Mn(NO3)2, and Mn(CH3COO)2;
[0013] And / or, the sodium source is at least one of Na2CO3 and NaOH.
[0014] Preferably, the temperature of the pre-calcination treatment is 500-850°C;
[0015] And / or, the pre-calcination treatment is carried out for a heat preservation time of 3-6 hours.
[0016] Preferably, the calcination temperature is 800-1200°C;
[0017] And / or, the heat preservation time of the roasting treatment is 5-15h;
[0018] And / or, the heating rate of the pre-calcination treatment and the calcination treatment is 1-5°C / min;
[0019] And / or, the atmosphere of the pre-calcination treatment and the calcination treatment is air and / or oxygen.
[0020] Preferably, the calcination process is followed by natural cooling, pulverization and sieving.
[0021] Preferably, the mass of the coating agent is 0.5-3wt% of the mass of the sintered product.
[0022] Preferably, the sintering temperature is 250-900°C;
[0023] And / or, the heat preservation time of the sintering treatment is 3-8h;
[0024] And / or, the heating rate of the sintering treatment is 1-5°C / min;
[0025] And / or, the sintering atmosphere is air and / or oxygen;
[0026] And / or, after the sintering treatment, natural cooling and iron removal are further performed, wherein the iron removal by screening is only to remove magnetic substances outside the structure.
[0027] The present invention also provides the use of the above-mentioned sodium battery high-voltage positive electrode material or the sodium battery high-voltage positive electrode material prepared by the above-mentioned method for preparing the sodium battery high-voltage positive electrode material in lithium-ion batteries.
[0028] The technical solution of the present invention has the following advantages:
[0029] A sodium battery high voltage positive electrode material comprises a core body and a coating layer, wherein the chemical formula of the core body is Na x A a Ni b Fe c Mn d B e; Wherein, A is at least one of Li, K, and Ca, B is at least one of Zn, Ti, Zr, and Al, 0.9≤x≤1.1, 0.005≤a≤0.05, 0.2≤b≤0.5, 0.2≤c≤0.5, 0.2≤d≤0.5, 0.01≤e≤0.1, and a+b+c+d+e=1. The specific capacity of the layered oxide positive electrode material of the sodium ion battery is still low at high voltage, and it is easy to undergo complex phase changes at high voltage, thereby causing the material structure to be destroyed, resulting in poor cycle performance. The present invention is modified on the basis of the Ni-Fe-Mn matrix material, and double-site doping is performed using A elements (Li, K, Ca) and B elements (Zn, Ti, Zr, Al), and combined with a composite strategy of surface coating, while improving the specific capacity of the positive electrode material, the structural stability of the Ni-Fe-Mn matrix positive electrode material is improved, and the cycle performance is improved. In dual-site doping, element A can enter the Na layer of the layered oxide, and element B can enter the transition metal layer. + It plays a supporting role in the process of embedding and de-embedding, reduces the repulsion between the oxygen layers, and reduces the slippage of the transition metal layer; and the B element does not change in valence during the charge and discharge process, thereby effectively reducing the Jahn-Teller distortion caused by the valence change of Ni, Fe, and Mn ions in the Ni-Fe-Mn matrix material of the present invention, eliminating harmful phase changes under high voltage, thereby improving the structural stability of the material. The coating layer can isolate the positive electrode material from contact with the electrolyte, avoiding the reaction between the positive electrode material and the electrolyte during the charge and discharge process, thereby improving the cycle stability of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a SEM image of the sodium battery high voltage positive electrode material prepared in Example 1 of the present invention;
[0032] Figure 2 This is the XRD diagram of the sodium battery high voltage positive electrode material prepared in Example 1 of the present invention;
[0033] Figure 3 It is a dQ / dV curve diagram of the sodium battery high voltage positive electrode material prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0034] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0035] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0036] Example 1
[0037] This embodiment provides a method for preparing a sodium battery high voltage positive electrode material, and the specific steps are as follows:
[0038] 1) First, follow K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 K2CO3, NiO, Fe2O3, MnO2, and TiO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved through a 350-mesh sieve to obtain NaK 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 One burning product;
[0039] 2) According to NaK 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 The mass ratio of the sintered product to the coating agent ZrO2 is 100:1. The product is weighed and mixed, placed in an air atmosphere and heated to 600°C at a heating rate of 2°C / min for sintering for 6 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material. The SEM image of the sodium battery high-voltage positive electrode material prepared in this embodiment is as follows: Figure 1 As shown, according to Figure 1It can be seen that it is a single crystal morphology; the XRD pattern of the sodium high voltage positive electrode material prepared in this embodiment is as follows Figure 2 As shown by Figure 2 It can be seen that the sodium battery positive electrode material prepared in this embodiment is a standard O3 phase, and no other impurities are introduced; the dQ / dV curve of the sodium battery high voltage positive electrode material prepared in this embodiment is as follows: Figure 3 As shown by Figure 3 It can be seen that the phase change platform of the sodium battery high-voltage positive electrode material prepared in this embodiment at 4.1V is lower, and the phase change voltage is increased. It can be seen that dual-site doping is beneficial to inhibiting the complex phase change of layered oxides during high-voltage charging and discharging, thereby helping to improve material stability and cycle stability.
[0040] Example 2
[0041] This embodiment provides a method for preparing a sodium battery high voltage positive electrode material, and the specific steps are as follows:
[0042] 1) First, follow K 0.04 Ni 0.35 Fe 0.2 Mn 0.35 Ti 0.06 K2CO3, NiO, Fe2O3, MnO2, and TiO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 The molar ratio of the metal element in the sodium is 0.95:1. Weigh Na2CO3, mix well, place in air atmosphere and heat to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heat to 950℃ at a heating rate of 2℃ / min for 12h, cool naturally, crush and pass through a 350-mesh sieve to obtain Na 0.95 K 0.04 Ni 0.35 Fe 0.2 Mn 0.35 Ti 0.06 One burning product;
[0043] 2) According to Na 0.95 K 0.04 Ni 0.35 Fe 0.2 Mn 0.35 Ti 0.06 The sintered product and the coating agent B2O3 are weighed and mixed in a mass ratio of 100:2, placed in an air atmosphere and heated to 300°C at a heating rate of 2°C / min for sintering for 5 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0044] Example 3
[0045] This embodiment provides a method for preparing a sodium battery high voltage positive electrode material, and the specific steps are as follows:
[0046] 1) First follow Li 0.03 Ni 0.2 Fe 0.27 Mn 0.4 Zn 0.1 Li2CO3, NiO, Fe2O3, MnO2, and ZnO were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and Li 0.03 Ni 0.2 Fe 0.27 Mn 0.4 Zn 0.1 The molar ratio of the metal element in the sodium is 1.05:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 850℃ at a heating rate of 1℃ / min for pre-baking for 4h, then heated to 950℃ at a heating rate of 1℃ / min for 8h, and then naturally cooled, crushed, and sieved through a 350-mesh sieve to obtain Na 1.05 Li 0.03 Ni 0.2 Fe 0.27 Mn 0.4 Zn 0.1 One burning product;
[0047] 2) According to Na 1.05 Li 0.03 Ni 0.2 Fe 0.27 Mn 0.4 Zn 0.1 The sintered product and the coating agent CaCO3 are weighed and mixed in a mass ratio of 100:1, placed in an air atmosphere and heated to 800°C at a heating rate of 5°C / min for sintering for 5 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0048] Example 4
[0049] This embodiment provides a method for preparing a sodium battery high voltage positive electrode material, and the specific steps are as follows:
[0050] 1) First, follow the Ca 0.01 Ni 0.35 Fe 0.27 Mn 0.35 Zr 0.02 CaCO3, NiO, Fe2O3, MnO2, and ZrO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and Ca 0.01 Ni 0.35 Fe0.27 Mn 0.35 Zr 0.02 The molar ratio of the metal element in the sodium is 0.9:1. Weigh Na2CO3, mix well, place in air atmosphere and heat to 500℃ at a heating rate of 5℃ / min for pre-baking for 6h, then heat to 800℃ at a heating rate of 2℃ / min for 15h, cool naturally, crush and pass through a 350-mesh sieve to obtain Na 0.9 Ca 0.01 Ni 0.35 Fe 0.27 Mn 0.35 Zr 0.02 One burning product;
[0051] 2) According to Na 0.9 Ca 0.01 Ni 0.35 Fe 0.27 Mn 0.35 Zr 0.02 The sintered product and the coating agent Al2O3 are weighed and mixed in a mass ratio of 100:0.5, placed in an air atmosphere and heated to 450°C at a heating rate of 1°C / min for sintering for 8 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0052] Example 5
[0053] This embodiment provides a method for preparing a sodium battery high voltage positive electrode material, and the specific steps are as follows:
[0054] 1) First, follow K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Al 0.05 K2CO3, NiO, Fe2O3, MnO2, Al2O3 were weighed out in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Al 0.05 The molar ratio of the metal elements in the sodium was 1.1:1. Na2CO3 was weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 3h, then heated to 1200℃ at a heating rate of 2℃ / min for 5h, and then naturally cooled, crushed, and passed through a 350-mesh sieve to obtain Na 1.1 K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Al 0.05 One burning product;
[0055] 2) According to Na 1.1 K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Al 0.05 The sintered product and the coating agent MgO are weighed and mixed in a mass ratio of 100:3, placed in an air atmosphere and heated to 900°C at a heating rate of 2°C / min for sintering for 3 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0056] Comparative Example 1
[0057] The difference between this comparative example and Example 1 is that K2CO3 and TiO2 are not added, and the specific steps are as follows:
[0058] 1) First, follow Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 NiO, Fe2O3, and MnO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved with a 350-mesh sieve to obtain NaNi 1 / 3Fe 1 / 3 Mn 1 / 3 One burning product;
[0059] 2) According to NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The sintered product and the coating agent ZrO2 are weighed and mixed in a mass ratio of 100:1, placed in an air atmosphere and heated to 600°C at a heating rate of 2°C / min for sintering for 6 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0060] Comparative Example 2
[0061] The difference between this comparative example and Example 1 is that K2CO3 is not added, and the specific steps are as follows:
[0062] 1) First, follow Ni 0.32 Fe 0.32 Mn 0.32 Ti 0.04NiO, Fe2O3, MnO2, and TiO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved with a 350-mesh sieve to obtain NaNi 0.32 Fe 0.32 Mn 0.32 Ti 0.04 One burning product;
[0063] 2) According to NaNi 0.32 Fe 0.32 Mn 0.32 Ti 0.04 The sintered product and the coating agent ZrO2 are weighed and mixed in a mass ratio of 100:1, placed in an air atmosphere and heated to 600°C at a heating rate of 2°C / min for sintering for 6 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that TiO2 is not added, and the specific steps are as follows:
[0066] 1) First, follow K 0.04 Ni 0.32 Fe 0.32 Mn 0.32 K2CO3, NiO, Fe2O3, and MnO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.04 Ni 0.32 Fe 0.32 Mn 0.32 The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved through a 350-mesh sieve to obtain NaK 0.04 Ni 0.32 Fe 0.32 Mn 0.32 One burning product;
[0067] 2) According to NaK 0.04 Ni0.32 Fe 0.32 Mn 0.32 The sintered product and the coating agent ZrO2 are weighed and mixed in a mass ratio of 100:1, placed in an air atmosphere and heated to 600°C at a heating rate of 2°C / min for sintering for 6 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0068] Comparative Example 4
[0069] The difference between this comparative example and Example 1 is that no coating treatment is performed, and the specific steps are as follows:
[0070] 1) First, follow K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 K2CO3, NiO, Fe2O3, MnO2, and TiO2 were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and K 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved through a 350-mesh sieve to obtain NaK 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Ti 0.05 A fired positive electrode material.
[0071] Comparative Example 5
[0072] The difference between this comparative example and Example 1 is that K element and Ti element doping are replaced by Mg element and Cu element doping. The specific steps are as follows:
[0073] 1) First, follow Mg 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Cu 0.05 MgO, NiO, Fe2O3, MnO2, and CuO were weighed in the stoichiometric ratio, and then the sodium element in the sodium source and the Mg 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Cu 0.05The molar ratio of the metal element in the sodium is 1.0:1. Na2CO3 is weighed, mixed evenly, placed in an air atmosphere and heated to 800℃ at a heating rate of 2℃ / min for pre-baking for 5h, then heated to 1000℃ at a heating rate of 2℃ / min for 10h, and then naturally cooled, crushed, and sieved through a 350-mesh sieve to obtain NaMg 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Cu 0.05 One burning product;
[0074] 2) According to NaMg 0.05 Ni 0.3 Fe 0.3 Mn 0.3 Cu 0.05 The sintered product and the coating agent ZrO2 are weighed and mixed in a mass ratio of 100:1, placed in an air atmosphere and heated to 600°C at a heating rate of 2°C / min for sintering for 6 hours, cooled to room temperature, and sieved to remove iron to obtain a sodium battery high-voltage positive electrode material.
[0075] Test Case
[0076] The materials prepared in the examples and comparative examples were used as positive electrode active materials and slurried with polyvinylidene fluoride and carbon black in a mass ratio of 95:2.5:2.5. The compacted density of the electrode was 3.2 g / cm 3 , make pole pieces, use metal lithium sheet as counter electrode, use glass fiber as diaphragm, use 1mol / L lithium hexafluorophosphate ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (the volume ratio of EC to DMC is 1:1) as electrolyte, assemble into CR2032 button cells in a glove box filled with argon, and finally put the battery into the blue electric test system for electrical performance testing. Among them, the charge / discharge specific capacity test: at room temperature, charge to 4.2V at a constant current of 0.1C charging rate, and then discharge to 2.0V at a discharge rate of 0.1C; cycle test: 50 cycles of charge and discharge test at a rate of 1C / 1C between 2.0-4.2V to characterize the capacity retention rate of the positive electrode material after 50 cycles; the statistical results of the button performance of the embodiment and the comparative example are shown in Table 1 below.
[0077] Table 1
[0078]
[0079]
[0080] According to the test results in Table 1, compared with Comparative Example 1 without dual-site doping, Comparative Examples 2-3 with only single-site doping, Comparative Example 4 without coating treatment, and Comparative Example 5 with other dual-element doping, the specific capacity and cycle stability of the sodium battery positive electrode materials prepared in Examples 1-5 of the present invention at high voltage are significantly improved.
[0081] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A sodium battery high voltage positive electrode material, characterized in that: It includes a core body and a coating layer, wherein the chemical formula of the core body is Na x A a Ni b Fe c Mn d B e ; wherein A is at least one of Li, K, and Ca, B is at least one of Zn, Ti, Zr, and Al, 0.9≤x≤1.1, 0.005≤a≤0.05, 0.2≤b≤0.5, 0.2≤c≤0.5, 0.2≤d≤0.5, 0.01≤e≤0.1, and a+b+c+d+e=1.
2. The sodium battery high voltage positive electrode material according to claim 1, characterized in that: The coating layer is an oxide coating layer containing at least one element of zirconium, boron, aluminum, calcium and magnesium.
3. The method for preparing the sodium battery high voltage positive electrode material according to claim 1 or 2, characterized in that: include: According to the stoichiometric ratio, nickel source, iron source, manganese source, sodium source and doping element source are weighed and mixed, and pre-baked and baked to obtain a baked product; The sodium battery high voltage positive electrode material is obtained by mixing a sintered product with a coating agent and performing a sintering treatment.
4. The method for preparing a sodium battery high voltage positive electrode material according to claim 3, characterized in that: The nickel source is at least one of NiO, NiSO4, NiCl2, Ni(NO3)2, and Ni(CH3COO)2; And / or, the iron source is at least one of Fe2O3, Fe2(SO4)3, FeCl2, Fe(NO3)3, and Fe(CH3COO)3; And / or, the manganese source is at least one of MnO2, MnO, MnSO4, MnCl2, Mn(NO3)2, and Mn(CH3COO)2; And / or, the sodium source is at least one of Na2CO3 and NaOH.
5. The method for preparing a sodium battery high voltage positive electrode material according to claim 3 or 4, characterized in that: The temperature of the pre-calcination treatment is 500-850°C; And / or, the pre-calcination treatment is carried out for a heat preservation time of 3-6 hours.
6. The method for preparing a sodium battery high voltage positive electrode material according to any one of claims 3 to 5, characterized in that: The temperature of the calcination treatment is 800-1200°C; And / or, the heat preservation time of the roasting treatment is 5-15h; And / or, the heating rate of the pre-calcination treatment and the calcination treatment is 1-5°C / min; And / or, the atmosphere of the pre-calcination treatment and the calcination treatment is air and / or oxygen.
7. The method for preparing a sodium battery high voltage positive electrode material according to any one of claims 3 to 6, characterized in that: After the calcination, the molten steel is naturally cooled, crushed and sieved.
8. The method for preparing a sodium battery high voltage positive electrode material according to any one of claims 3 to 7, characterized in that: The mass of the coating agent is 0.5-3wt% of the mass of the sintered product.
9. The method for preparing a sodium battery high voltage positive electrode material according to any one of claims 3 to 8, characterized in that: The sintering temperature is 250-900°C; And / or, the heat preservation time of the sintering treatment is 3-8h; And / or, the heating rate of the sintering treatment is 1-5°C / min; And / or, the sintering atmosphere is air and / or oxygen; And / or, the sintering process is followed by natural cooling and iron removal through screening.
10. Use of the sodium-based high-voltage positive electrode material according to claim 1 or 2 or the sodium-based high-voltage positive electrode material prepared by the preparation method of the sodium-based high-voltage positive electrode material according to any one of claims 3 to 9 in lithium-ion batteries.
Citation Information
Cited By
Layered positive electrode material, preparation method thereof and sodium ion battery
CN119742326A
Air-stable layer oxygen positive electrode material, preparation method thereof, positive plate and sodium ion battery
CN120878828A
High-entropy sodium battery positive electrode material as well as preparation method and application thereof
CN121054677A
High-entropy sodium battery cathode material, preparation method and application thereof
CN121054677B