Polyester splittable composite fiber, woven / knitted fabric, and method for producing the same

A composite fiber using recycled polyester resin A and B, with controlled diethylene glycol and carboxyl terminal group concentrations, addresses the issue of non-polyester resin contamination, ensuring high productivity and mechanical properties comparable to virgin polyester, suitable for fabrics.

JP7577271B2Active Publication Date: 2024-11-05UNITIKA LTD +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020083725
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-12
Publication Date
2024-11-05
Estimated Expiration
2040-05-12

AI Technical Summary

Technical Problem

Existing methods for recycling polyester waste fail to sufficiently remove non-polyester resin contaminants, leading to inferior mechanical properties and reduced productivity in fiber production, and are costly and inefficient in operation.

Method used

A composite fiber is developed using recycled polyester resin A, which is poorly alkali-eluting, and resin B, which is easily alkali-eluting, with specific diethylene glycol and carboxyl terminal group concentrations, allowing for alkali weight loss treatment to split resin A into multiple pieces, ensuring high productivity and mechanical properties comparable to virgin polyester.

Benefits of technology

The composite fiber achieves high-quality mechanical properties and productivity, enabling the production of fabrics with uniform fiber shapes and sizes, suitable for various applications, while minimizing non-polyester resin contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577271000003
    Figure 0007577271000003
  • Figure 0007577271000001
    Figure 0007577271000001
  • Figure 0007577271000002
    Figure 0007577271000002
Patent Text Reader

Abstract

To provide a polyester-based divided composite fiber, in at least part of which a recycled polyester resin is used which contains a recycled polyester material at high ratio, and which has a mechanical characteristic value equal to that when only a virgin polyester resin is used.SOLUTION: A polyester-based divided composite fiber has: a polyester resin A which is a hardly alkaline-soluble component; and a polyester resin B which is an easily alkaline-soluble component. The polyester resin A is divided into a plurality of pieces by the polyester resin B in a cross-sectional shape of a fiber. The polyester resin A is a recycled polyester resin that comprises a component derived from a recycled polyester material. In the recycled polyester resin, when a total amount of the whole glycol component is 100 mol%, a content of diethylene glycol is 4 mol% or less, and a density of carboxyl end group is 30 equivalent / t or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester-based splittable conjugate fiber, which is a conjugate fiber partially using a recycled polyester resin containing a recycled polyester raw material derived from used polyester products or unused polyester generated in the process of manufacturing polyester products, and in which an easily alkali-soluble component is split into a plurality of alkali-soluble components. The present invention further relates to a woven or knitted fabric containing a fiber made of the recycled polyester resin. [Background technology]

[0002] Polyethylene terephthalate (PET) has a high melting point, is resistant to chemicals, and is relatively low cost, so it is widely used in fibers, films, plastic bottles, and other molded products. These polyester products inevitably generate waste during the manufacturing and processing stages, and are often disposed of after use. However, when incinerated, high heat is generated, causing significant damage to the incinerator and shortening its lifespan. On the other hand, when not incinerated, it does not decompose and will remain semi-permanently.

[0003] In recent years, it has become a problem that plastics are a major cause of marine pollution, with a worldwide movement to reduce the use of plastics and switch to biodegradable plastics. Plastics are a major cause of marine pollution, and in recent years, plastics have been found to be harmful to marine ecosystems. Plastics are a major cause of marine pollution, and in recent years, plastics have been found to be harmful to marine ecosystems. In light of these environmental issues, various methods of recycling are being used to reuse resources. For polyester products such as PET, in addition to recycling polyester waste generated during the manufacturing process, methods are being considered for collecting products that were once on the market and then discarded and reusing them as raw materials. In particular, in recent years, textile products that have been given the Eco Mark, which is certified as having achieved a certain recycling rate, have become widespread.

[0004] Various methods have been proposed for recycling polyester raw materials, such as polyester waste generated in the manufacturing process or recovered used polyester products. For example, there have been proposed a method of adding methanol to PET scraps to decompose them into dimethylene terephthalate (hereinafter sometimes referred to as "DMT") and ethylene glycol (hereinafter sometimes referred to as "EG") (Patent Document 1), a method of adding EG to PET scraps to depolymerize them, and then adding methanol to recover DMT (Patent Document 2), and a method of depolymerizing PET scraps with EG to form oligomers, which are then used in a polycondensation reaction (Patent Document 3).

[0005] Incidentally, impurities that can become a problem when recycling PET bottles and other products that have already been made include various additives added to the polyester resin, as well as items attached to the bottle itself, such as a) caps (aluminum, polypropylene, polyethylene), b) inner stoppers, c) liners (polypropylene, polyethylene), d) labels (paper, resins such as polystyrene, ink), e) adhesives, and f) printing ink. Generally, as a pretreatment step for the recycling process, the collected PET bottles are put through a vibrating sieve to remove sand, metal, etc. The PET bottles are then washed, and the colored bottles are separated before being roughly crushed. Labels, etc. are then removed by wind separation. Furthermore, aluminum pieces from the caps, etc. are removed and the PET bottle pieces are finely crushed. Components such as adhesives, proteins, and mold are removed by high-temperature alkaline washing, and different components such as polypropylene and polyethylene are separated by differences in specific gravity. However, even after going through these steps, it is difficult to completely separate and remove non-polyester resins, particularly polypropylene, polyethylene, polystyrene, etc., from PET resin. For example, even if the production of recycled polyester resin is attempted by the recycling methods described in Patent Documents 1 to 4, the removal of foreign matter derived from non-polyester resins cannot be sufficiently performed, and the amount of foreign matter mixed in cannot be sufficiently reduced, making it difficult to obtain a product with the same quality as virgin polyester resin. If the amount of foreign matter mixed in is not sufficiently reduced in this way, the pressure rise rate of the filtration filter in the spinning process or film-forming process is fast, long-term continuous operation is not possible, and processing operability becomes very poor. Moreover, the methods described in Patent Documents 1 to 3 require a large amount of cost for the installation, operation, maintenance, etc. of the recovery device, and there is room for improvement in terms of practicality.

[0006] The invention described in Patent Document 4 describes a method in which polyester waste is depolymerized with ethylene glycol, filtered through a filter with an average mesh size of 10 to 50 μm, and then repolymerized. It is also shown that the obtained recycled polyester resin has a low amount of foreign matter mixed in and is excellent in operability during processing. However, even with this method, the above-mentioned foreign matter derived from the non-polyester resin cannot be sufficiently removed, and the amount of the foreign matter mixed in cannot be sufficiently reduced. As described above, a recycled polyester resin that can sufficiently remove not only various inorganic substances but also foreign matter derived from non-polyester resins, and that can produce various products similar to those produced from virgin polyester resins and that can produce high-quality products has not yet been obtained.

[0007] In particular, when polyester resin is used for melt spinning to obtain fibers, the amount of foreign matter mixed in has a significant effect on productivity. The more complex the shape of the fiber is or the finer the fiber is, the more the foreign matter affects it, making production difficult and resulting in poor mechanical properties of the obtained fiber. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Special Publication No. 42-8855 [Patent Document 2] Japanese Patent Publication No. 48-62732 [Patent Document 3] Japanese Patent Application Laid-Open No. 60-248646 [Patent Document 4] JP 2005-171138 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to solve the above problems and provide a polyester-based splittable conjugate fiber that uses, at least in part, a recycled polyester resin containing a high proportion of recycled polyester raw material derived from used polyester products and unused polyester generated in the process of manufacturing polyester products, and that has mechanical property values ​​similar to those of a fiber using only virgin polyester resin and can be obtained with good productivity. [Means for solving the problem]

[0010] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention relates to the following (1) to (3). (1) A polyester resin A is a component that is hardly dissolved by alkali, and a polyester resin B is a component that is easily dissolved by alkali, and in the cross-sectional shape of the fiber, the polyester resin A is divided into a plurality of pieces by the polyester resin B. , single yarn fineness is 5.0 dtex or less A composite fiber, wherein the polyester resin A contains a component derived from at least one recycled polyester raw material selected from a) used polyester products and b) polyester waste generated in a process for producing a polyester resin or a polyester product. 40% by mass or more The recycled polyester resin (polyester resin A) has a diethylene glycol content of 4 mol% or less and a carboxyl end group concentration of 30 equivalents / t or less when the total amount of all glycol components is taken as 100 mol%. and the average pressure rise rate is 0.6 MPa / h or less (wherein the average pressure rise rate is a value calculated by the following procedure: a pressure rise tester including an extruder and a pressure sensor is used, a stainless steel filter (nominal mesh size: 1400 mesh, weave: twill weave, vertical mesh: 165 mesh, horizontal mesh: 1400 mesh, vertical wire diameter: 0.07 mm, horizontal wire diameter: 0.04 mm, filtration grain size: 12 μm) is set at the tip of the extruder, polyester resin is melted at 300° C. in the extruder, and the melt is extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion is defined as the "initial pressure value (MPa)" and the pressure value at the point when extrusion is continued for 12 hours is defined as the "final pressure value (MPa)". The average pressure rise rate is calculated based on these pressure values ​​using the following formula A: Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12···A) Characterized by For woven and knitted fabrics Polyester split composite fiber. (2) a) components derived from at least one recycled polyester raw material, such as used polyester products and b) polyester scraps generated in the process of manufacturing polyester resin or polyester products; 40% by mass or more A woven or knitted fabric containing a fiber made of a recycled polyester resin (polyester resin A) containing 1,2,4-trimethylsiloxyphenyl ether, 1,2,3 ... The average pressure rise rate is 0.6 MPa / h or less (wherein the average pressure rise rate is a value calculated by the following procedure: a pressure rise tester including an extruder and a pressure sensor is used, a stainless steel filter (nominal mesh size: 1400 mesh, weave: twill weave, vertical mesh: 165 mesh, horizontal mesh: 1400 mesh, vertical wire diameter: 0.07 mm, horizontal wire diameter: 0.04 mm, filtration grain size: 12 μm) is set at the tip of the extruder, polyester resin is melted at 300° C. in the extruder, and the melt is extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion is defined as the "initial pressure value (MPa)" and the pressure value at the point when extrusion is continued for 12 hours is defined as the "final pressure value (MPa)." Based on these pressure values, the average pressure rise rate is calculated by the following formula A: Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12···A), and wherein the single yarn fineness of the fiber made of polyester resin A is 1.0 dtex or less. (3) A method for producing the woven or knitted fabric according to (2), comprising the steps of: For woven and knitted fabrics A method for producing a woven or knitted fabric, comprising the steps of: obtaining a grey fabric by weaving or knitting a polyester-based splittable composite fiber; and subjecting the grey fabric to an alkali weight reduction treatment to elute the polyester resin B, thereby splitting the polyester resin A portion. Effect of the Invention

[0011] In the polyester splittable conjugate fiber of the present invention (hereinafter sometimes referred to as the conjugate fiber of the present invention), the recycled polyester resin used as the polyester resin A, which is a component hardly soluble in alkali, contains little foreign matter and has a carboxyl end group concentration and a diethylene glycol content that satisfy specific ranges, so that in the process of obtaining fibers by melt spinning, long-term continuous operation is possible even for fibers with complex cross-sectional shapes, and products can be obtained with good productivity. Furthermore, the conjugate fiber of the present invention has mechanical property values ​​similar to those of fibers using virgin polyester resin, and can be suitably used in various fields and applications such as various clothing and industrial fields. The woven or knitted fabric of the present invention contains fine fibers made of the recycled polyester resin, and therefore has mechanical properties similar to those of fabrics made using virgin polyester resin, and is also excellent in flexibility and density. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a cross section of a conjugate fiber (single fiber) of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. The conjugate fiber of the present invention contains polyester resin A, which is a component that is hardly soluble in alkali, and polyester resin B, which is a component that is easily soluble in alkali.

[0014] The polyester resin A, which is the poorly alkali-soluble component of the present invention, is a recycled polyester resin containing a component derived from at least one recycled polyester raw material, i.e., a) used polyester product and b) unused polyester generated in the process of manufacturing a polyester product. Examples of used polyester products in the above category a) include polyester molded products (including fibers) that were once on the market and then collected after use, etc. Representative examples of such products include containers such as PET bottles and packaging materials. The unadopted polyester generated in the manufacturing process of polyester products mentioned in b) above is polyester that has not been commercialized. Examples of such unadopted polyester include off-standard resin pellets, materials that are no longer needed during molding, pieces cut during molding, scraps generated during molding or processing, cut-up pieces of transitional products generated when changing brands, and cut-up pieces of prototypes or defective products. The above a) and b) are not limited in terms of their form, and may be pelletized by further processing such as crushing and cutting as necessary, or may be melted and pelletized. The recycled polyester raw materials a) and b) above may be either crystalline or amorphous. Therefore, for example, pellets of amorphous polyester waste that have not been heat-treated, crystalline pellets that have been heat-treated, or a mixture of crystalline pellets and amorphous pellets can be used. In the present invention, it is preferable to use crystalline recycled polyester raw materials, particularly for the purpose of preventing fusion between pellets during charging into the can or depolymerization reaction. Therefore, the materials a) or b) above that have been crystallized by heat treatment (crystallized pellets, etc.) can be suitably used.

[0015] The polyester resin A of the present invention preferably contains 40% by mass or more of the recycled polyester raw material, and more preferably 50% by mass or more. If the content of the recycled polyester raw material is less than 40% by mass, the objective of considering environmental issues cannot be achieved. The upper limit of the content of the recycled polyester raw material is not particularly limited, but according to the manufacturing method of the polyester resin A described later, it is possible to easily obtain a polyester resin A having a content of the recycled polyester raw material of up to 40 to 80% by mass.

[0016] The polyester resin A of the present invention has the characteristic values ​​of a diethylene glycol content of 4 mol % or less and a carboxyl terminal group concentration of 30 equivalents / t or less, when the total amount of all glycol components is 100 mol %.

[0017] In the polyester resin A of the present invention, when the total amount of all glycol components is 100 mol%, the diethylene glycol content is 4 mol% or less, and preferably 3.5 mol% or less. In particular, in the polyester resin A obtained by the production method described later, ethylene glycol is used as one of the raw materials, and diethylene glycol may be generated as a by-product at that time. The polyester resin A has a small amount of diethylene glycol as a by-product, and has excellent crystallinity due to the diethylene glycol content being 4 mol% or less. Therefore, melt spinning can be performed with good operability like virgin polyester, and it is possible to obtain a composite fiber with a complex cross-sectional shape in which the polyester resin A is divided into multiple pieces by the polyester resin B as shown in FIG. 1 described later. In addition, it is possible to obtain a composite fiber with excellent mechanical properties such as strength and elongation. The lower limit of the diethylene glycol content can be, for example, about 0.5 mol%, but is not limited thereto.

[0018] The polyester resin A of the present invention has a carboxyl end group concentration of 30 equivalents / t or less, preferably 25 equivalents / t or less, and most preferably 20 equivalents / t or less. By making the carboxyl end group concentration 30 equivalents / t or less, the resin has excellent thermal stability, and therefore can be melt spun with good operability like virgin polyester. Therefore, it is possible to obtain a composite fiber with a complex cross-sectional shape in which the polyester resin A is divided into multiple pieces by the polyester resin B, as shown in FIG. 1 described later. It is also possible to obtain a composite fiber with excellent mechanical properties such as strength and elongation. The lower limit of the carboxyl end group concentration can be, for example, about 5 equivalents / t, but is not limited to this.

[0019] When the content of diethylene glycol in the polyester resin A of the present invention exceeds 4 mol % or the concentration of carboxyl terminal groups exceeds 30 equivalents / t, the crystallinity and thermal stability of the polyester resin A are inferior, so that it is not possible to efficiently obtain a composite fiber having a complex cross-sectional shape in which the polyester resin A is divided into a plurality of pieces by the polyester resin B through melt spinning. In other words, it is not possible to obtain a polyester resin A having a cross-sectional shape in which the individual pieces have the same shape and size as shown in FIG. 1. For this reason, the fiber made of the polyester resin A obtained by subjecting the polyester resin B to an alkali weight reduction treatment from such a composite fiber will have variations in shape and size.

[0020] The polyester resin A of the present invention preferably has an average pressure rise rate of 0.6 MPa / h or less, as measured by the following method. Among them, it is preferably 0.5 MPa / h or less, and more preferably 0.4 MPa / h or less. The average pressure rise rate in the present invention is an index of the amount of foreign matter derived from various inorganic substances or foreign matter derived from non-polyester resins, and the smaller the average pressure rise rate, the smaller the amount of foreign matter. By having an average pressure rise rate of 0.6 MPa / h or less, melt spinning can be performed with good productivity like virgin polyester, and it is also possible to produce fibers with excellent mechanical properties such as strength and elongation. The lower limit of the average pressure rise rate can be, for example, about 0.01 MPa / h, but is not limited thereto. The average pressure rise rate is measured using a pressure rise tester including an extruder and a pressure sensor. A stainless steel filter (nominal mesh size: 1400 mesh, weave: twill weave, vertical mesh: 165 mesh, horizontal mesh: 1400 mesh, vertical wire diameter: 0.07 mm, horizontal wire diameter: 0.04 mm, filtration grain size: 12 μm) is set at the tip of the extruder, polyester resin is melted at 300° C. in the extruder, and the melt is extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion is defined as the "initial pressure value (MPa)" and the pressure value at the time of continuous extrusion for 12 hours thereafter is defined as the "final pressure value (MPa)." The average pressure rise rate is calculated based on these pressure values ​​using the following formula A. Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12) A)

[0021] The polyester resin A of the present invention is not particularly limited in type, but it is preferable to use polyethylene terephthalate (PET) mainly composed of ethylene terephthalate units. The content of PET in the polyester resin A of the present invention is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90 to 100% by mass. In particular, in the manufacturing method of polyester resin A described later, PET, which is usually a polycondensation product of ethylene glycol and terephthalic acid, can be obtained, but when components other than ethylene glycol and terephthalic acid are present in the recycled polyester raw material, polyester resins other than PET may be produced by the polycondensation reaction. For this reason, in addition to the main component PET, the polyester resin A may contain the following components copolymerized as acid components or glycol components. Two or more of these components may be included.

[0022] Examples of the acid component include isophthalic acid, phthalic acid, phthalic anhydride, naphthalenedicarboxylic acid, adipic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, dodecanedioic acid, dimer acid, trimellitic anhydride, trimellitic acid, pyromellitic acid, 1,4-cyclohexanedicarboxylic acid, sebacic acid, dimer acid, etc. Examples of the glycol component include neopentyl glycol, 1,4-butanediol, 1,2-propylene glycol, 1,5-pentanediol, 1,3-propanediol, 1,6-hexamethylenediol, diethylene glycol, 1,4-cyclohexanedimethanol, dimer diol, butylethylpropanediol, (2-methyl-1,3-propanediol, trimethylolpropane, glycerin, pentaerythritol, ethylene oxide adducts of bisphenol A or bisphenol S, etc.

[0023] The polyester resin B, which is an alkali-soluble component of the present invention, is preferably polyethylene terephthalate (PET) mainly composed of ethylene terephthalate units, in view of alkali solubility, splittability, spinnability, etc. In order to increase the dissolution rate by alkali weight reduction treatment, it is preferable that the polyester resin B is copolymerized with an aromatic dicarboxylic acid component having a sulfonate group in the dicarboxylic acid component. As the aromatic dicarboxylic acid component containing a sulfonate group, 5-sodium sulfoisophthalic acid is suitable. The copolymerization amount is appropriately selected depending on the difference in alkali dissolution rate between the polyester resin A and the polyester resin B, etc., but is preferably 0.1 to 10.0 mol%, and it is preferable to make the copolymerization amount as small as possible in terms of spinning operability and cost.

[0024] Furthermore, it is preferable that the polyester is copolymerized with a polyalkylene glycol having an average molecular weight of 1000 to 10000. The polyalkylene glycol dissolves quickly in an alkali in the polyester, cutting the molecular chain of the polyester and generating voids on the surface to increase the surface area, thereby accelerating the dissolution rate. The copolymerization amount of the polyalkylene glycol in the polyester is preferably 1 to 20 mass%.

[0025] Modifiers (for example, matting agents, stabilizers, flame retardants, or colorants) may be added to the polyester resin A and polyester resin B as long as the effects of the present invention are not impaired. In addition, various functional components (for example, cationic dye-dyeable components or heat-shrinkable components) may be copolymerized or mixed and contained.

[0026] In the cross-sectional shape of the composite fiber of the present invention, polyester resin A, which is a component poorly soluble in alkali, is divided into a plurality of pieces by polyester resin B, which is a component easily soluble in alkali. The composite fiber of the present invention is split and split by dissolving all or a part of the polyester resin B when subjected to an alkali weight reduction treatment.

[0027] Next, the arrangement of polyester resin A and polyester resin B in the conjugated fiber of the present invention will be described. In the cross section of the constituting single fiber of the present invention cut perpendicularly to the longitudinal direction, polyester resin A is divided into a plurality of pieces by polyester resin B. Figures 1(a) to (d) are schematic diagrams showing embodiments of the cross-sectional shape of a single fiber of such conjugated fiber, in which 1 is polyester resin A, 2 is polyester resin B, and 3 is a hollow portion. FIG. 1(a) shows a fiber having a hollow portion 3 near the center, with 20 flat segments made of polyester resin A radially arranged around the hollow portion. FIG. 1(b) shows eight roughly triangular segments made of polyester resin A arranged radially. FIG. 1(c) shows 19 circular segments made of polyester resin A arranged in an array. FIG. 1(d) shows ten flat segments made of polyester resin A arranged radially.

[0028] In the conjugated fiber of the present invention, in order to easily peel off each segment during the alkali weight reduction treatment and subsequent steps and to achieve a high degree of splitting, it is preferable that the multiple segments of polyester resin A exist in an independent state without contacting each other due to polyester resin B, as shown in FIG. 1.

[0029] The number of segments of polyester resin A in the conjugated fiber of the present invention is not particularly limited, but in consideration of spinnability, ease of spinneret preparation, etc., and also in consideration of the productivity of ultrafine fibers, it is preferably 2 to 60 segments, and more preferably 4 to 30 segments. The shape of the segments is not particularly limited, and as shown in Figure 1, they can be flat, approximately triangular, round, etc., and according to the conjugated fiber of the present invention, the ultrafine fibers made of polyester resin A finally obtained can have various shapes.

[0030] In other words, the composite fiber of the present invention is split by alkali weight reduction treatment, and when alkali weight reduction treatment is performed, polyester resin B is eluted and ultrafine fibers in which each segment of polyester resin A is independent can be obtained.

[0031] The volumetric composite ratio of polyester resin A to polyester resin B is preferably 60 / 40 to 95 / 5, and more preferably 75 / 25 to 85 / 15, taking into consideration the single yarn fineness of the composite fiber, the number of divisions, the single yarn fineness of the ultrafine fiber after the division process, etc. Within such a range, the polyester resin A can be easily divided by the alkali weight reduction treatment, and the amount of polyester resin B eluted by the alkali solution is small, which is economical. In addition, the looseness of the structure of the fabric obtained after the alkali weight reduction treatment is small, and the occurrence of structure misalignment can be suppressed, so that a high-density fabric with excellent texture can be obtained.

[0032] The ultrafine fibers made of polyester resin A obtained after such splitting and slitting must have a single-filament fineness of 1.0 dtex or less, preferably 0.5 dtex or less, and more preferably 0.2 dtex or less. If the ultrafine fibers are 0.5 dtex or less, the resulting fiber structure will be more flexible and dense, and will be suitable for polishing and cleaning performance. In addition, in consideration of spinnability, ease of spinneret preparation, etc., the single-filament fineness is preferably 0.01 dtex or more.

[0033] The composite fiber of the present invention may be either a highly oriented undrawn yarn (POY) or a drawn yarn (FDY). The single fiber fineness of the conjugated fiber of the present invention is not particularly limited, but considering the number of segments of the polyester resin A as described above and the single fiber fineness of the ultrafine fibers obtained after splitting, it is preferably 1 to 5.0 dtex. The conjugate fiber of the present invention may be either a multifilament or a monofilament, but is preferably a multifilament, and preferably has a total fineness of 40 to 130 dtex.

[0034] The composite fiber of the present invention uses a recycled polyester resin satisfying the above-mentioned characteristic values ​​as polyester resin A, and therefore can have the same performance as virgin polyester resin. For this reason, the strength of the composite fiber of the present invention is preferably 2.0 cN / dtex or more, more preferably 2.4 cN / dtex or more, in the case of POY. In the case of FDY, it is preferably 3.0 cN / dtex or more, more preferably 3.5 cN / dtex or more. In addition, the elongation of the composite fiber of the present invention is preferably 90 to 140% in the case of POY, more preferably 100 to 130%. In the case of FDY, it is preferably 25 to 55%, more preferably 30 to 50%. By satisfying the above strength and elongation, woven fabrics and knitted fabrics can be obtained with good operability without yarn breakage during weaving and knitting.

[0035] Next, the woven or knitted fabric of the present invention is a woven or knitted fabric which contains, at least in part, fibers made of the polyester resin A described above. The content of the fiber made of polyester resin A in the woven or knitted fabric of the present invention is preferably 25% by mass or more, more preferably 35% by mass or more. As a fiber that can be used as a fiber other than the fiber made of polyester resin A, polyester fibers are preferable, and those having the same fineness as the composite fiber of the present invention or those having a fine fineness can be used. Also, those having high shrinkage can be used.

[0036] The woven or knitted fabric of the present invention can be obtained by subjecting a woven or knitted fabric obtained by weaving or knitting a part of the conjugated fiber of the present invention to an alkali weight reduction treatment to elute the polyester resin B in the conjugated fiber of the present invention and splitting the polyester resin A. The details of the production method will be described later.

[0037] The woven or knitted fabric of the present invention is not particularly limited in weave, etc. Examples of the woven fabric include woven, twill, satin, dobby, and double weave. The knitted fabric of the present invention is also not particularly limited in weave, and examples of the knitted fabric include circular knits such as plain stitch, smooth, milling, and pique, and warp knits such as single tricot and half tricot.

[0038] Next, a method for producing polyester resin A, which is a recycled polyester resin, will be described. In the method for producing polyester resin A of the present invention, it is important to carry out the steps shown in (1) to (5) in that order. (1) Add a slurry of ethylene glycol and terephthalic acid to obtain ethylene terephthalate oligomers. (2) Ethylene glycol is added to the oligomer obtained in (1). (3) The recycled polyester raw material is added to the oligomer obtained in (2) to which ethylene glycol has been added under normal pressure while stirring so that the molar ratio of total glycol components / total acid components becomes 1.08 to 1.35, and depolymerization is performed under heat treatment conditions of 245 to 280°C. (4) The depolymerized polymer obtained in (3) is passed through a metal filter having a filtration grain size of 10 to 25 μm to filter out foreign matter. (5) A polymerization catalyst is added to the depolymerized product obtained in (4) after filtering out foreign matter, and a polycondensation reaction is carried out at a temperature of 260° C. or higher and under reduced pressure of 1.0 hPa or less.

[0039] First, in the step (1), a slurry of ethylene glycol and terephthalic acid is added as a preliminary step to depolymerize the recycled polyester raw material [a) used polyester products and b) at least one of unused polyesters generated in the process of manufacturing polyester products] to obtain an esterification reaction product (ethylene terephthalate oligomer). The amount of ethylene terephthalate oligomer is preferably 0.20 to 0.80 mass% and more preferably 0.30 to 0.70 mass% in 100 mass% of the finally obtained recycled polyester resin. If the amount of ethylene terephthalate oligomer is less than the above amount, the recycled polyester raw material is likely to block with itself when the recycled polyester raw material is added in step (3), which is undesirable because it places an excessive load on the mixer. On the other hand, if the amount of ethylene terephthalate oligomer is more than the above range, no particular problem occurs in the depolymerization reaction, but the recycling rate of the finally obtained recycled polyester resin is undesirably low.

[0040] In the step (2), ethylene glycol is added to the ethylene terephthalate oligomer obtained in the step (1). In order to sufficiently advance the depolymerization reaction in the step (3), the amount of ethylene glycol added is preferably 5 to 15 mass% relative to 100 mass% of the ethylene terephthalate oligomer, and more preferably 10 to 15 mass%. If the amount of ethylene glycol added exceeds 15 mass%, the ethylene terephthalate oligomer tends to solidify in the reactor, which may make it impossible to continue the subsequent reaction, and this is not preferable. When ethylene glycol is added to the ethylene terephthalate oligomer, it is preferable to uniformize the temperature of the contents while rotating the stirrer before adding the ethylene glycol, in order to prevent the oligomer from solidifying.

[0041] In the step (3), the recycled polyester raw material is added to the oligomer obtained in the step (2) to which ethylene glycol has been added while stirring, so that the molar ratio of total glycol components / total acid components is 1.08 to 1.35, and depolymerization is carried out under heat treatment conditions of 245 to 280°C. In the manufacturing method of the present invention, this step is important. That is, in the conventional method using recycled polyester raw materials, depolymerization is performed using only recycled polyester raw materials, but in the present invention, depolymerization of recycled polyester raw materials is performed in the presence of ethylene terephthalate oligomer and ethylene glycol, and the recycled polyester raw materials are charged with all components of oligomer, ethylene glycol, and recycled polyester raw materials so that the molar ratio of total glycol components / total acid components is 1.08 to 1.35, and depolymerization is performed. The molar ratio of total glycol components / total acid components is preferably 1.10 to 1.33, more preferably 1.12 to 1.30. By carrying out the above-mentioned steps (1) to (3), not only various inorganic substances but also foreign substances derived from non-polyester resins are efficiently precipitated, so that these foreign substances can be filtered out without fail in the step (4).In addition, in the polycondensation reaction in the step (5), it becomes possible to obtain a recycled polyester resin having a diethylene glycol content and a carboxyl end group concentration that are not more than a specific amount as characteristic values ​​of the present invention, and having a small amount of foreign substances mixed in. In the production method of the present invention, it is preferable that the depolymerization reaction does not decompose the recycled polyester raw material into monomers, but into oligomers having a repeating unit of about 5 to 20. By controlling the depolymerization reaction in this way, not only various inorganic substances but also foreign substances derived from non-polyester resins are efficiently precipitated, so that more foreign substances can be removed. If the molar ratio of total glycol components / total acid components during the depolymerization reaction is outside the above range, the resulting recycled polyester resin will not satisfy at least one of the carboxyl end group concentration and diethylene glycol content specified in the present invention, and will have a high average pressure rise rate. This is because, when the molar ratio of total glycol components / total acid components during the depolymerization reaction is outside the above range, the precipitation of various inorganic substances and foreign substances derived from non-polyester resins is not efficiently carried out, and these foreign substances cannot be filtered out completely in step (4), and the foreign substances precipitate after the polycondensation reaction in step (5), resulting in a recycled polyester resin with a high average pressure rise rate.

[0042] The reactor used in the production method of the present invention may be a commonly used esterification reactor without any particular problem in terms of volume and shape of the stirring blades. However, in order to efficiently advance the depolymerization reaction, it is preferable that the reactor has a structure equipped with a distillation column that does not distill ethylene glycol outside the system. When the recycled polyester raw material is charged, it is preferable to do so under normal pressure while stirring, and it is more preferable to charge it in a state where it is purged with a small amount of inert gas (generally nitrogen gas is used).

[0043] The reaction temperature during depolymerization in the step (3) is preferably set at an internal temperature of the reactor in the range of 245 to 280°C, and more preferably set at an internal temperature in the range of 255 to 280°C. If the reaction temperature during depolymerization is less than 245°C, the reaction product solidifies, the operability deteriorates, and even if a recycled polyester resin is obtained, the diethylene glycol content and the carboxyl end group concentration become too high. If the reaction temperature exceeds 280°C, the diethylene glycol content and the carboxyl end group concentration of the obtained recycled polyester resin become too high. The depolymerization reaction time (the reaction time from the end of the addition of the recycled polyester raw material) is preferably within 4 hours, and more preferably within 2 hours from the viewpoints of suppressing the amount of diethylene glycol as a by-product and suppressing deterioration of the color tone of the polyester.

[0044] In the step (4), the depolymerized product obtained in the step (3) is passed through a metal filter having a filtration size of 10 to 25 μm to filter out foreign matter. As described above, by carrying out the depolymerization reaction under the conditions of the step (3), not only various inorganic substances but also foreign matter derived from non-polyester resins is efficiently precipitated, and therefore, by passing the depolymerized product through a metal filter having a filtration size of 10 to 25 μm, the precipitated foreign matter can be filtered out to obtain a depolymerized product with a small amount of foreign matter. If a metal filter with a filtering particle size of more than 25 μm is used, foreign matter in the polymer cannot be sufficiently removed, and the resulting recycled polyester resin contains a large amount of foreign matter. Therefore, when such a resin is used for spinning, the nozzle pack pressure increases and thread breakage occurs. On the other hand, if a metal filter with a filtering particle size of less than 10 μm is used, clogging due to foreign matter easily occurs, and the filter life is shortened, which is disadvantageous in terms of cost and also deteriorates operability.

[0045] As the metal filter that can be used in step (4) of the present invention, any ordinary filter can be used without any particular problems, and examples thereof include a screen changer type filter, a leaf disc filter, and a candle type sintered filter.

[0046] In the manufacturing method of the present invention, a polymerization catalyst is added to the depolymerized product obtained after filtering foreign matter through the above step (4), and a polycondensation reaction is carried out at a temperature of 260° C. or higher and a reduced pressure of 1.0 hPa or lower. As the polymerization catalyst, for example, one or more of germanium, antimony, titanium and cobalt compounds can be used, but a germanium or antimony compound is preferably used. Furthermore, when the transparency of the resulting recycled polyester resin is important, it is preferable to use a germanium compound. Examples of germanium or antimony compounds include oxides, inorganic acid salts, organic acid salts, halides, and sulfides thereof. These polycondensation catalysts are used in an amount of 5×10 per mole of the acid component of the polyester resin to be produced. -5 It is preferable to set the concentration to 6×10 moles / unit or more. -5It is more preferable that the amount is mol / unit or more. In addition, since the polymerization catalyst contained in the recycled polyester raw material may also act as a catalyst during the polycondensation reaction, it is preferable to take into consideration the amount and type of polymerization catalyst contained in the recycled polyester raw material when adding the polymerization catalyst in step (4).

[0047] During the polycondensation reaction, a fatty acid ester, a hindered phenol-based antioxidant, or a phosphorus compound may be added in addition to the above-mentioned polymerization catalyst. Specific examples of fatty acid esters include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate, dipentaerythritol hexastearate, etc. Among these, glycerin monostearate, pentaerythritol tetrastearate, and dipentaerythritol hexastearate are preferred.

[0048] Hindered phenol antioxidants include 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-butylidenebis-(3-methyl-6-t-butylphenol), triethyl Examples of suitable compounds include ethylene glycol-bis[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate] and 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1'-dimethylethyl}-2,4,8,10-tetraoxaspiro[5,5]undecane, but from the standpoint of effectiveness and cost, tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane is preferred.

[0049] Examples of phosphorus compounds that can be used include phosphorous acid, phosphoric acid, trimethyl phosphite, triphenyl phosphite, tridecyl phosphite, trimethyl phosphate, tridecyl phosphate, and triphenyl phosphate.

[0050] Then, in the polycondensation reaction tank, the polycondensation reaction is carried out at a temperature of 260° C. or higher and under reduced pressure of 1.0 hPa or lower. If the polycondensation reaction temperature is lower than 260° C. or the pressure during the polycondensation reaction exceeds 1.0 hPa, the polycondensation reaction time becomes long, resulting in poor productivity. The polycondensation reaction temperature is more preferably 270° C. or higher. However, if the polycondensation reaction temperature is too high, the polymer is colored due to thermal decomposition, the color tone is deteriorated, and the amount of terminal groups (COOH) is also increased due to thermal decomposition. Therefore, in the present invention, the upper limit of the polycondensation reaction temperature is preferably 285° C. or lower.

[0051] The intrinsic viscosity of the polyester resin A of the present invention obtained by the above polycondensation reaction is preferably 0.38 to 0.70 dl / g, taking into consideration melt spinning.

[0052] Next, a method for producing the composite fiber of the present invention will be described. The following is an embodiment of a manufacturing method in which the conjugate fiber of the present invention is an FDY, and melt spinning can be performed using a normal conjugate spinning device. In melt conjugate spinning of the FDY of the present invention, polyester resin B is spun from a spinneret so as to split polyester resin A. Specifically, polyester resin A and polyester resin B are prepared, and after being melted separately, they pass through separate pipes and flow into a spinneret pack. The polymers flowing into the pack are joined by the spinneret, and are combined into a split fiber type, orange type, sea island type, or other form by a known technique and discharged from the spinneret. In this case, it is appropriate to spin under conditions of a spinning temperature of 280 to 295°C and a spinning speed of 3000 to 3600 m / min. After spinning, the polymer discharged from the spinneret is cooled and solidified, and an oil agent is applied, and then the conjugate fiber of the present invention (FDY) is obtained by drawing and heat treating at a drawing temperature of 70 to 90°C, a draw ratio of 1 to 2 times, and a heat treatment temperature of 140 to 170°C.

[0053] Next, the method for producing the woven or knitted fabric of the present invention will be described. The woven or knitted fabric of the present invention can be obtained, for example, by subjecting a grey fabric obtained through processes such as weaving and knitting using the conjugate fiber of the present invention obtained by the above-mentioned production method to an alkali weight reduction treatment. The alkali weight loss treatment may be carried out by a conventionally known method. In the case of a splittable composite fiber as shown in Fig. 1(a), the amount of dissolution and removal by the alkali solution, i.e., the weight loss, is preferably about 15 to 30% by mass, more preferably about 20 to 25% by mass. If the weight loss rate is less than 15% by mass, the splittable composite fiber is not sufficiently split and split, and the woven or knitted fabric tends not to have a good feel. If the weight loss rate exceeds 30% by mass, the splittable fiber is satisfactorily split, but the ultrafine fibers are also slightly dissolved, and the strength of the resulting woven or knitted fabric tends to decrease. The conditions for the alkali dissolution treatment are generally those used in the weight reduction process of polyester fiber structures, and include, for example, a method using a 0.5% to 5.0% aqueous sodium hydroxide solution. More preferably, it is 1.0% to 3.0%, and particularly preferably, it is 1.0% to 2.0%. The treatment temperature is preferably 85°C to 100°C, and more preferably 90°C to 98°C. EXAMPLES

[0054] The present invention will now be described in more detail with reference to the following examples, in which the various property values ​​and the like are measured and evaluated as follows: (a) Intrinsic viscosity The solvent was an equal mass mixture of phenol and tetrachloroethane, and the measurement was performed at a concentration of 0.5 g / dl and a temperature of 20°C. (b) Composition of polyester resin The copolymer was dissolved in a mixed solvent of deuterated hexafluoroisopropanol and deuterated chloroform in a volume ratio of 1 / 20, and 1H-NMR was measured using a JEOL LA-400 NMR apparatus. The type and content of the copolymerized components were determined from the integrated intensity of the proton peaks of each component in the obtained chart. (c) Carboxyl end group concentration 0.1 g of the resulting recycled polyester resin was dissolved in 10 ml of benzyl alcohol, and 10 ml of chloroform was added to the solution, which was then titrated with a 1 / 10 N solution of potassium hydroxide in benzyl alcohol to determine the content. (d) Average boost rate measured by a boost test machine The measurement was performed by the method described above.

[0055] (e) Strength of splittable composite fibers According to JIS L-1013, the measurement was performed using an autograph DSS-500 manufactured by Shimadzu Corporation, with a gripping distance of 25 cm and a pulling speed of 30 cm. (f) Elongation of splittable composite fibers According to JIS L-1013, the measurement was performed using an autograph DSS-500 manufactured by Shimadzu Corporation, with a gripping distance of 25 cm and a pulling speed of 30 cm. (g) Single yarn fineness (dtex) of splittable composite fiber Measurement was performed according to JIS L-1013 8.3.1B method.

[0056] (h) Spinnability The state of yarn breakage during melt spinning to obtain POY was evaluated on the following three-level scale based on the number of yarn breakages per spindle during continuous melt spinning for 24 hours. ○ The number of thread breakages was 0. △: Yarn breakage occurred 1 or 2 times. ×: Yarn breakage occurred three or more times. (i) Stretchability The state of yarn breakage during drawing of POY was evaluated into three levels as follows based on the number of breaks (total number) when drawing was performed continuously for 10 hours using 100 spindles. ○ The number of cuts was 0 to 1. △: The number of cuts was 2 to 4. ×: The number of cuts was 5 or more. (j) Fabric nap (brushed feel, texture) The resulting woven fabric was evaluated for nap feel based on the following criteria. ◯: The nap is good. △: The hair standing feeling is normal. ×: The feeling of standing up is insufficient. (k) Softness of the fabric The softness of the obtained woven fabric was evaluated by touch according to the following criteria. ○: Feels soft to the touch. △: Feels normal to the touch. ×: Feels hard to the touch.

[0057] [Production of Recycled Polyester Resin] Recycled polyester resin A A slurry of terephthalic acid (TPA) and ethylene glycol (EG) (TPA / EG molar ratio = 1 / 1.6) was supplied to an esterification reactor and reacted at a temperature of 250°C and a pressure of 50 hPa to obtain ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95%. 45.0 parts by mass of ethylene terephthalate oligomer was charged into the esterification reactor, and then 10.0 parts by mass of ethylene glycol was added while the agitator of the esterification reactor was rotating. When the internal temperature of the esterification reactor (hereinafter referred to as the "ES can") stopped decreasing, 55.0 parts by mass of recycled polyester raw material (pellet-shaped polyester waste generated in the process of manufacturing polyester resin) was added in a fixed amount over about 2 hours via a rotary valve. At this time, the recycled polyester raw material was added so that the molar ratio of total glycol components / total acid components (hereinafter sometimes referred to as "G / A") was 1.20. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerization product was then pumped into a polycondensation reactor (hereinafter referred to as PC can) through a candle filter with a mesh size of 20 μm that was set between the esterification reactor and the polycondensation reactor, and 1.0 × 10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, EG slurry of titanium dioxide was added to make 0.20 mass%, and the PC can was decompressed and after 60 minutes, the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours to obtain recycled polyester resin A (intrinsic viscosity: 0.64).

[0058] Recycled polyester resin B In the same manner as in the case of recycled polyester resin A, ethylene terephthalate oligomer (number average polymerization degree: 5) with an esterification reaction rate of 95% was obtained. 30.0 parts by mass of ethylene terephthalate oligomer was charged into the ES can, and then 7.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 70.0 parts by mass of recycled polyester raw material (same as in Example 1) was added in a fixed amount over about 2 hours via a rotary valve. At this time, the recycled polyester raw material was charged so that the G / A was 1.10. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerized polymer was then pressure-fed into the PC can through a candle filter with a mesh size of 20 μm set between the ES can and the PC can, and antimony trioxide was added as a polymerization catalyst at a rate of 1.0×10-4 The mixture was added so as to obtain a ratio of mol / unit, and the PC can was decompressed for 60 minutes, after which the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 5 hours to obtain recycled polyester resin B (intrinsic viscosity: 0.65).

[0059] Recycled polyester resin C An ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95% was obtained in the same manner as in Example 1. 45.0 parts by mass of the ethylene terephthalate oligomer was charged into an ES can, and then 7.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 55.0 parts by mass of recycled polyester raw material (PET bottles crushed or remelted and pelletized) was added at a fixed amount over about 2 hours via a rotary valve. At this time, the recycled polyester raw material was charged so that the G / A was 1.16. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerized polymer was then pressure-fed into the PC can through a candle filter with a mesh size of 20 μm set between the ES can and the PC can, and antimony trioxide was added as a polymerization catalyst at a rate of 1.0×10 -4 mol / unit, EG slurry of titanium dioxide was added to make 0.40 mass%, and the PC can was decompressed for 60 minutes, after which the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours to obtain recycled polyester resin C (intrinsic viscosity: 0.64).

[0060] Recycled polyester resin D In the same manner as in Example 1, an ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95% was obtained. 45.0 parts by mass of ethylene terephthalate oligomer was charged into the ES can, and then 10.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 55.0 parts by mass of recycled polyester was added in a fixed amount over about 2 hours via a rotary valve. At this time, the recycled polyester raw material (same as in Example 1) was added so that the G / A was 1.20. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerized polymer was pressure-fed into a PC can through a candle filter with a mesh size of 25 μm set between the ES can and the PC can, and then 1.0 × 10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, cobalt acetate 0.5×10 -4 mol / unit, EG slurry of titanium dioxide was added to make 0.05 mass%, and the PC can was decompressed for 60 minutes, after which the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 280°C for 3 hours to obtain recycled polyester resin D (intrinsic viscosity: 0.56).

[0061] Recycled polyester resin E In the same manner as in the case of recycled polyester resin A, ethylene terephthalate oligomer (number average polymerization degree: 5) with an esterification reaction rate of 95% was obtained. 30.0 parts by mass of ethylene terephthalate oligomer was charged into the ES can, and then 2.5 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 70.0 parts by mass of recycled polyester was added in a fixed amount over about 2 hours via a rotary valve. At this time, the recycled polyester raw material (same as in Example 1) was added so that the G / A was 1.06. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerized polymer was pressure-fed into a PC can through a candle filter with a mesh size of 20 μm set between the ES can and the PC can, and then 1.0 × 10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, cobalt acetate 0.5×10 -4 mol / unit, EG slurry of titanium dioxide was added to make 0.40 mass%, and the PC can was decompressed and after 60 minutes, the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours to obtain recycled polyester resin E (intrinsic viscosity: 0.64).

[0062] Recycled polyester resin F In the same manner as in the case of recycled polyester resin A, ethylene terephthalate oligomer (number average polymerization degree: 5) with an esterification reaction rate of 95% was obtained. 50.0 parts by mass of ethylene terephthalate oligomer was charged into an ES can, and then 19.0 parts by mass of ethylene glycol was added while the agitator of the ES can was rotating. When the internal temperature of the ES can stopped decreasing, 50.0 parts by mass of recycled polyester was added in a fixed amount over about 2 hours via a rotary valve. At this time, recycled polyester raw material (same as in Example 1) was added so that G / A was 1.36. Then, the depolymerization reaction was carried out for 1 hour under heat treatment conditions at 270°C. The obtained depolymerized polymer was pressure-fed into a PC can through a candle filter with a mesh size of 20 μm set between the ES can and the PC can, and then 1.0 × 10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, cobalt acetate 0.5×10 -4 mol / unit, EG slurry of titanium dioxide was added to make 0.40 mass%, and the PC can was decompressed for 60 minutes, after which the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 4 hours to obtain recycled polyester resin F (intrinsic viscosity: 0.64).

[0063] Virgin polyester resin A slurry of terephthalic acid (TPA) and ethylene glycol (EG) (TPA / EG molar ratio = 1 / 1.6) was supplied to an esterification reactor and reacted at a temperature of 250°C and a pressure of 50 hPa to obtain ethylene terephthalate oligomer (number average degree of polymerization: 5) with an esterification reaction rate of 95%. 100.0 parts by mass of ethylene terephthalate oligomer was charged into a PC can, and 1.0×10 antimony trioxide was added as a polymerization catalyst. -4 mol / unit, EG slurry of titanium dioxide was added to make 0.20 mass%, and the PC can was decompressed and after 60 minutes, the melt polymerization reaction was carried out at a final pressure of 0.5 hPa and a temperature of 275°C for 3 hours to obtain a virgin polyester resin (intrinsic viscosity 0.46).

[0064] The properties of the recycled polyester resins A to F and the virgin polyester resin are shown in Table 1.

[0065] [Table 1]

[0066] As is clear from Table 1, the recycled polyester resins A to D obtained by sequentially carrying out the above-mentioned steps (1) to (5) had carboxyl terminal group amounts and diethylene glycol contents within the ranges specified in the present invention, and also had low average pressure rise rates. On the other hand, in the case of recycled polyester resin E, since the G / A during the depolymerization reaction in the above-mentioned step (3) was low, the concentration of carboxyl terminal groups was high and the average pressure increase rate was also high. In the case of recycled polyester resin F, since the G / A during the depolymerization reaction in the above-mentioned step (3) was high, the diethylene glycol content was high and the average pressure increase rate was also high.

[0067] Example 1 Recycled polyester resin A was used as polyester resin A, and copolymerized PET with an intrinsic viscosity of 0.72, which was copolymerized with 2.5 mol% of 5-sodium sulfoisophthalic acid (SIP-Na) and 12.0 mass% of polyethylene glycol (PEG) with an average molecular weight of 8000, was used as polyester resin B. The composite mass ratio of polyester resin A / B was 81.2 / 18.8, and the spinning temperature was 288°C, the discharge rate was 36 g / min, and the spinning was performed using a composite spinning device equipped with a spinneret having 48 spinning holes designed so that polyester resin B divides polyester resin A into 8. The spun yarn was cooled, oiled, and wound up at a speed of 3100 m / min to obtain POY of 120 dtex / 48 filaments. Next, this POY was stretched 1.56 times using a heated roller at 84°C, and further heat-treated on a heat plate at 153°C to obtain a splittable composite fiber (FDY) of 75 dtex / 48 filaments. The resulting splittable composite fiber had a strength of 3.45 cN / dtex and an elongation of 37.9%, and the cross-sectional shape of each single fiber was as shown in Figure 1(b). The resulting splittable conjugate fiber was false-twisted at 175°C and 3000 twists / m using a commercially available false-twisting machine, and a plain weave fabric with a green density of 145 warp threads / 2.54cm and 95 weft threads / 2.54cm was woven using this textured yarn as the warp and weft. The resulting plain weave fabric was subjected to an alkali weight reduction treatment in the dyeing process under conditions of 20g / L caustic soda, a bath ratio of 1:30, and a temperature of 98°C, whereby polyester resin B was dissolved and removed from the splittable conjugate fiber in the fabric, and the fabric was split into ultrafine fibers made of polyester resin A. A conventional finishing process was then performed to obtain a woven fabric.

[0068] Example 2 A composite fiber of the present invention, 75 dtex / 48 filaments, was obtained in the same manner as in Example 1, except that recycled polyester resin B was used instead of polyester resin A. Further, a woven fabric was obtained by weaving and performing an alkali weight reduction treatment in the same manner as in Example 1.

[0069] Example 3 A composite fiber of the present invention, 75 dtex / 48 filaments, was obtained in the same manner as in Example 1, except that recycled polyester resin C was used instead of polyester resin A. Further, a woven fabric was obtained by weaving and performing an alkali weight reduction treatment in the same manner as in Example 1.

[0070] Example 4 A composite fiber of the present invention, 75 dtex / 48 filaments, was obtained in the same manner as in Example 1, except that recycled polyester resin D was used instead of polyester resin A. Further, a woven fabric was obtained by weaving and performing an alkali weight reduction treatment in the same manner as in Example 1.

[0071] Comparative Example 1 A polyester splittable composite fiber 75 dtex / 48 filament was obtained in the same manner as in Example 1, except that recycled polyester resin E was used instead of polyester resin A. Further, a woven fabric was obtained by weaving and performing an alkali weight reduction treatment in the same manner as in Example 1.

[0072] Comparative Example 2 A polyester splittable composite fiber 75 dtex / 48 filament was obtained in the same manner as in Example 1, except that recycled polyester resin F was used instead of polyester resin A. Further, a woven fabric was obtained by weaving and treating with an alkali in the same manner as in Example 1.

[0073] Reference example 1 A polyester splittable composite fiber of 78 dtex / 48 filaments was obtained in the same manner as in Example 1, except that a virgin polyester resin was used as the polyester resin A. Further, a woven fabric was obtained by weaving and carrying out an alkali weight reduction treatment in the same manner as in Example 1.

[0074] [Table 2] As is clear from Table 2, the polyester-based splittable conjugate fibers obtained in Examples 1 to 4 were able to be easily spun into conjugate fibers having a complex cross-sectional shape in which polyester resin A was split into multiple pieces by polyester resin B, as shown in FIG. 1(b). In addition, the yarn properties were comparable to those of fibers made from virgin polyester resin, and fibers with no practical problems were obtained. In addition, the texture of the woven fabrics obtained in Examples 1 to 4 after alkali weight reduction treatment was comparable to that of fibers made from virgin polyester resin in terms of both nap feel and softness, since the fibers made from polyester resin A obtained by alkali weight reduction treatment were uniform in shape and size. On the other hand, the polyester splittable conjugate fiber obtained in Comparative Example 1 had poor spinnability due to the high concentration of carboxyl end groups in the recycled polyester resin used, and the cross-sectional shape of the conjugate fiber could not be made to have a uniform cross-sectional shape and size as shown in FIG. 1(b) for polyester resin A. In addition, the yarn properties were low in strength and elongation. Furthermore, the texture of the woven fabric obtained after the alkali weight reduction treatment was poor in nap feel due to the variation in shape and size of the fibers made of polyester resin A obtained by the alkali weight reduction treatment. The polyester splittable conjugate fiber obtained in Comparative Example 2 had poor stretchability because the regenerated polyester fiber used contained a high diethylene glycol content, and the cross-sectional shape of the conjugate fiber could not be made to have a uniform cross-sectional shape and size of each of the polyester resins A as shown in Fig. 1(b). In addition, the texture of the woven fabric obtained after the alkali weight reduction treatment was inferior in softness because the shapes and sizes of the fibers made of the polyester resin A obtained by the alkali weight reduction treatment varied. [Explanation of symbols]

[0075] 1. Polyester resin A 2 Polyester resin B 3 Hollow part

Claims

1. A conjugated fiber having a polyester resin A which is a component hardly soluble in alkali and a polyester resin B which is a component easily soluble in alkali, in which the polyester resin A is divided into a plurality of pieces by the polyester resin B in the cross section of the fiber, and having a single yarn fineness of 5.0 dtex or less, wherein the polyester resin A is a recycled polyester resin containing 40 mass % or more of a component derived from at least one recycled polyester raw material, which is a) used polyester product and b) polyester waste generated in a process for producing a polyester resin or a polyester product, and the recycled polyester resin (polyester resin A) has a diethylene glycol content of 4 mol % or less, a carboxyl terminal group concentration of 30 equivalents / t or less, and an average pressure rise rate of 0.6 MPa / h or less when the total amount of all glycol components is taken as 100 mol % (in particular, The average pressure rise rate is a value calculated by the following procedure: a pressure rise tester including an extruder and a pressure sensor is used, a stainless steel filter (nominal mesh size: 1400 mesh, weave: twill weave, vertical mesh: 165 mesh, horizontal mesh: 1400 mesh, vertical line diameter: 0.07 mm, horizontal line diameter: 0.04 mm, filtration grain size: 12 μm) is set at the tip of the extruder, polyester resin is melted at 300° C. in the extruder, and the melt is extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion is defined as the "initial pressure value (MPa)", and the pressure value at the time of extrusion for 12 hours thereafter is defined as the "final pressure value (MPa)". The average pressure rise rate is calculated based on these pressure values ​​by the following calculation formula A: Average pressure rise rate (MPa / h)=(final pressure value-initial pressure value) / 12...A).

2. a) used polyester products; and b) a woven or knitted fabric containing fibers made of recycled polyester resin (polyester resin A) containing 40% by mass or more of a component derived from at least one recycled polyester raw material of polyester waste generated in a process for producing polyester resin or polyester products, wherein the polyester resin A has a diethylene glycol content of 4 mol% or less, a carboxyl end group concentration of 30 equivalents / t or less, and an average pressure rise rate of 0.6 MPa / h or less when the total amount of all glycol components is taken as 100 mol% (wherein the average pressure rise rate is a value calculated by the following procedure: a pressure rise tester including an extruder and a pressure sensor is used to test the extruder. A stainless steel filter (nominal mesh size: 1400 mesh, weave: twill weave, vertical mesh: 165 mesh, horizontal mesh: 1400 mesh, vertical line diameter: 0.07 mm, horizontal line diameter: 0.04 mm, filtration particle size: 12 μm) was set at the tip of an extruder, polyester resin was melted at 300° C. in an extruder, and the melt was extruded from the filter at a discharge rate of 29.0 g / min. The pressure value at the start of extrusion was defined as the "initial pressure value (MPa)" and the pressure value at the time of continuous extrusion for 12 hours thereafter was defined as the "final pressure value (MPa)." Based on these pressure values, the average pressure rise rate was calculated using the following calculation formula A: Average pressure rise rate (MPa / h) = (final pressure value - initial pressure value) / 12 ... A), and wherein the single yarn fineness of the fiber made of the polyester resin A is 1.0 dtex or less.

3. A method for producing a woven or knitted fabric according to claim 2, A step of obtaining a green fabric by weaving or knitting the polyester-based splittable conjugate fiber for woven or knitted fabrics according to claim 1; and subjecting the grey fabric to an alkali weight reduction treatment to elute the polyester resin B, thereby splitting and splitting the polyester resin A portion.

Citation Information

Patent Citations

  • JP1967008855Y1

  • JP1973062732A

  • Polyester fiber of high strength with high thermal dimensional stability as well as chemical stability

    JP1983098419A

  • Depolymerization of waste polyester