toner
The integration of an organosilicon polymer within toner particles, positioned to trap wax, addresses the dual challenges of low-temperature fixability and heat-resistant storage stability, ensuring effective image quality and stability.
Patent Information
- Application Number
- JP2020142510
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-29
- Filing Date
- 2020-08-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-08-26
AI Technical Summary
Existing toners face challenges in achieving both low-temperature fixability and heat-resistant storage stability due to issues such as wax seepage, decreased fluidity, and image defects, which are not adequately addressed by current methods involving plasticizers, silica encapsulation, or core-shell structures.
Incorporating an organosilicon polymer into toner particles, ensuring it is present in an area of 80% or less from the center of gravity to the outline of the cross-section, with a solubility parameter difference of 0.70 (cal/cm3)1/2 or less from the wax, effectively trapping the wax within the particles.
This approach enhances both low-temperature fixability and heat-resistant storage stability while preventing wax seepage and image defects, maintaining image density and preventing contamination.
Smart Images

Figure 0007577483000006 
Figure 0007577483000001 
Figure 0007577483000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for visualizing an electrostatic image in an image forming method such as electrophotography, electrostatic printing, and magnetic recording. [Background technology]
[0002] In recent years, energy saving has been considered a major technical issue in copiers, printers, and fax machines, and a significant reduction in the amount of heat required for image fixing devices is desired. Therefore, there is a growing need for toners that can fix images with less energy, that is, toners with so-called "low temperature fixability." A common method for improving the low-temperature fixability of a toner is to lower the glass transition temperature (Tg) of the binder resin used in order to soften it. However, simply lowering the Tg of the binder resin can cause offset to the fixing member due to insufficient releasability during fixing, or cause a decrease in heat resistance during storage of the toner.
[0003] As a method for sufficiently softening the toner during fixing without lowering the Tg, a plasticizer is added. Patent Document 1 discloses a method for lowering the toner viscosity during fixing by using a softener with excellent plasticity. However, in order to sufficiently soften the toner during fixing, it is necessary to use a plasticizer that has a large plasticizing ability for the binder resin. When such a plasticizer is used, the plasticizer is likely to seep onto the surface of the toner particles during storage, causing image problems due to blocking and reduced fluidity. In response to the above demands, Patent Document 2 discloses that by incorporating silica fine particles in the toner, wax that has low affinity with the binder resin is adsorbed to silica aggregates and uniformly dispersed in the binder resin, thereby suppressing the exudation of wax to the surface of the toner base particles. As a result, the fluidity of the toner base particles is improved, and adhesion and accumulation within the manufacturing equipment are prevented.
[0004] In addition, to address the issue of reduced toner strength due to improved low-temperature fixability, Patent Document 3 proposes incorporating pearl necklace-type silica to increase strength in order to prevent material contamination caused by using a low-melting crystalline resin. This achieves both low-temperature fixability and prevention of material contamination due to reduced toner strength. In addition, in Patent Document 4, toner is produced in an aqueous medium by using a vinyl polar resin in combination with ester wax to address the problems of reduced development durability and poor storage stability in high-temperature environments caused by the plasticization of the toner due to the use of ester wax. This allows the ester wax, binder resin, and vinyl polar resin to exist from the inner layer of the toner toward the surface layer of the toner, forming a core-shell structure in which the ester wax and binder resin are partially compatible with each other. The vinyl-based polar resin having a more highly polar carboxyl group is present in the vicinity of the toner surface layer with a concentration gradient, which can prevent the ester wax compatible with the binder resin from being present in the vicinity of the toner surface layer. This makes it difficult for the toner surface layer to be plasticized. This can prevent the deterioration of development durability and storage stability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2013 / 047296 [Patent Document 2] JP 2007-334118 A [Patent Document 3] JP 2009-42386 A [Patent Document 4] JP 2012-078628 A Summary of the Invention [Problem to be solved by the invention]
[0006] As in the toner described in Patent Document 1, a softener with excellent plasticity easily migrates to the surface of toner particles, causing the plasticizer to be exposed to the surface of toner particles during storage, resulting in a decrease in image density due to a decrease in fluidity. As with the toner described in Patent Document 2, simply incorporating silica fine particles into the toner makes it difficult for the highly hydrophobic wax to be adsorbed due to the high hydrophilicity of silica, and some challenges remain in achieving both low-temperature fixation and heat-resistant storage stability. As in the toner described in Patent Document 3, simply incorporating pearl necklace type silica improves the filming by improving the strength of the entire toner, but it is not possible to retain the wax that moves through the binder and seeps out to the surface inside the toner, and therefore is insufficient in terms of improving heat resistance storage stability. Although the heat-resistant storage stability is improved by covering the toner surface with a polar resin, as in the toner described in Patent Document 4, there is a tendency for the release properties from the media to be disadvantageous due to the exudation of wax during fixing. In addition, there are restrictions on the surface layer design, and the degree of freedom in toner design tends to be low compared to the diversification of the main body design of laser beam printers.
[0007] The present invention provides a toner which solves the above-mentioned problems. That is, the present invention provides a toner having excellent heat resistance and storage stability, which achieves both low-temperature fixability and heat resistance and is free from image defects such as a decrease in image density due to contamination of components caused by the seepage of wax onto the toner particle surface, even when a wax having excellent plasticity is used as a binder resin. [Means for solving the problem]
[0008] A toner including toner particles containing a binder resin and a wax, The toner particles contain an organosilicon polymer represented by the following formula (1): In a cross section of the toner particle observed by a transmission electron microscope, said organosilicon polymer is present in an area that is 80% or less of distance A from the center of gravity of said cross section of said toner particle to the contour of said cross section, The absolute value of the difference between the SP value of the organosilicon polymer and the SP value of the wax is 0.70 (cal / cm 3 ) 1 / 2A toner characterized in that: R 1 -SiO 3 / 2 (1) (In formula (1), R 1 is an alkyl group having 1 to 4 carbon atoms. Effect of the Invention
[0009] According to the present invention, even when a wax having excellent plasticity is used as a binder resin, it is possible to provide a toner having excellent heat-resistant storage stability, which achieves both low-temperature fixability and heat-resistant storage stability and is free from image defects such as a decrease in image density due to contamination of components caused by the exudation of the wax onto the toner particle surface. [Brief description of the drawings]
[0010] [Figure 1] Schematic diagram showing the state of organosilicon polymers in toner particles DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below. The expressions "XX or more and YY or less" or "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. In the following description, when numerical ranges are described stepwise, the upper and lower limits of each numerical range can be combined in any way.
[0012] The toner comprises toner particles having a binder resin and a wax, and the toner particles contain an organosilicon polymer represented by formula (1). In a cross section of a toner particle observed under a transmission electron microscope, the organosilicon polymer is present in an area that is 80% or less of the distance A from the center of gravity of the cross section of the toner particle to the outline of the cross section, and the absolute value of the difference between the SP value of the organosilicon polymer and the SP value of the wax is 0.70 (cal / cm 3 ) 1 / 2 The following is the result.
[0013] In order to achieve low-temperature fixability, it is preferable to use a wax such as an ester wax that is highly compatible with the binder resin and has excellent plasticity. However, such a wax is likely to cause a decrease in the heat-resistant storage stability of the toner under high temperature and high humidity conditions. However, constructing a strong shell structure or increasing the Tg of the binder resin tends to hinder low-temperature fixation. In other words, the above-mentioned heat-resistant storage stability and low-temperature fixability are considered to be in a complementary relationship. Therefore, it has been difficult to achieve both with conventional techniques.
[0014] In order to solve the above problems, the present inventors focused on incorporating an organosilicon polymer as a filler into the toner. Specifically, they conducted extensive research focusing on the relationship between the solubility parameters (SP values) of the wax and the organosilicon polymer. As a result, they found that by setting the absolute value of the difference in solubility parameters between the wax and the organosilicon polymer to a certain value or less and further controlling the location of the organosilicon polymer, it is possible to achieve low-temperature fixability while greatly improving the heat-resistant storage stability of the toner. That is, by satisfying the above-mentioned requirements, it is possible to achieve both low-temperature fixability and heat-resistant storage stability, and to suppress image defects such as a decrease in image density due to contamination of members caused by the exudation of wax onto the toner particle surfaces.
[0015] Solubility parameter (SP value) is a parameter that indicates the affinity between substances with similar values. SP value can be calculated from the type and molar ratio of the constituent monomers using the commonly used Fedors method [Poly. Eng. Sci., 14(2)147(1974)]. The unit of SP value is (cal / cm 3 ) 1 / 2 However, 1 (cal / cm 3 ) 1 / 2 =2.046×10 3 (J / m 3 ) 1 / 2 by (J / m 3 ) 1 / 2 can be converted to units of
[0016] The present inventors believe that the reason why the above effects are obtained by using a toner that satisfies the above conditions is as follows. The toner particles are characterized by the fact that the organosilicon polymer is encapsulated in the toner particles, and that the organosilicon polymer encapsulated in the toner particles has an SP value close to that of the wax. Because the organosilicon polymer and the wax have a high affinity, the wax is attracted to the organosilicon polymer during storage and is retained in the toner particles. Therefore, even under high temperature and high humidity conditions, the wax is not exposed to the surface of the toner particles, and the associated problems such as blocking can be suppressed. Incidentally, the inclusion of an organosilicon polymer in a toner particle is defined as the presence of the organosilicon polymer in a region that is 80% or less of distance A from the center of gravity of the cross section of the toner particle to the outline of the cross section, as shown in Figure 1. If it is 80% or less, the distance between the organosilicon polymer and the toner particle surface is sufficiently long to prevent the wax retained in the organosilicon polymer from coming out to the toner particle surface. In order to have the organosilicon polymer exist in a region that is 80% or less of the distance A from the center of gravity, the location of the organosilicon polymer can be controlled as desired by mixing the organosilicon polymer with the polymerizable monomer and pigment, and adjusting the dispersion time, dispersion strength, amount of organosilicon polymer, etc. when obtaining the polymerizable monomer composition.
[0017] The toner contains an organosilicon polymer, the partial structure of which can be freely controlled by controlling the type and amount of organosilicon compound used in polymer formation, as well as the reaction temperature, reaction time, reaction solvent and pH of the hydrolysis, addition polymerization and condensation polymerization in the formation of the organosilicon polymer. In particular, when the structure represented by formula (1) is present in large quantities, a three-dimensional polymer is formed, and the hydrophobicity of the organosilicon polymer increases, so that the SP value of the organosilicon polymer approaches that of the wax, and the attractive effect of the wax becomes prominent. Furthermore, because organosilicon polymers have a higher affinity with binder resins than common inorganic fillers such as silica, even a small amount of the polymer can adequately suppress the bleeding of wax, which prevents the low-temperature fixing ability from being impaired by the inhibition of fixing caused by the addition of a large amount of filler, and suppresses image problems such as a decrease in image density due to contamination of components caused by the bleeding of wax onto the toner particle surface.
[0018] The organosilicon polymer has a structure represented by the following formula (1). R 1 -SiO 3 / 2 (1) In formula (1), R 1 R is an alkyl group having 1 to 4 carbon atoms (preferably 1 to 3, more preferably 1 or 2). 1 is more preferably a methyl group. The content of the structure represented by formula (1) in the organosilicon polymer is preferably 50% to 100% by mass, more preferably 80% to 100% by mass, even more preferably 90% to 100% by mass, still more preferably 95% to 100% by mass, and especially preferably 98% to 100% by mass. SP value of organosilicon polymer (cal / cm 3 ) 1 / 2 is preferably 8.00 or more and 9.70 or less, and more preferably 8.50 or more and 9.00 or less. The organosilicon polymer preferably exists in the toner particles in the form of particles, and the number average major axis of the organosilicon polymer particles is preferably about 10 nm to 200 nm.
[0019] To further improve heat resistance, the absolute value of the difference between the SP value of the organosilicon polymer and the SP value of the wax must be 0.40 (cal / cm 3 ) 1 / 2 The lower limit is preferably 0.00 (cal / cm 3 ) 1 / 2When the absolute SP values of the organosilicon polymer and the wax are close to each other, the attractive effect of the organosilicon polymer and the wax becomes more pronounced.
[0020] The method for producing the toner will be described below. The method for producing the toner is not particularly limited, but a suspension polymerization method and a solution suspension method are preferably used. The suspension polymerization method includes a granulation step of forming particles of a polymerizable monomer composition containing a polymerizable monomer capable of forming a binder resin, an organosilicon polymer and a wax, and, if necessary, additives such as a colorant, in the aqueous medium, and a polymerization step of polymerizing the polymerizable monomer contained in the particles of the polymerizable monomer composition after the granulation step to form toner particles. The solution suspension method includes a granulation step in which a mixed solution obtained by mixing a toner particle composition containing a binder resin, a wax, and, if necessary, additives such as a colorant with an organic solvent capable of dissolving the binder resin is dispersed in the aqueous medium to form particles of the mixed solution, and a solvent removal step in which, after the granulation step, the organic solvent present in the particles of the mixed solution is removed to form toner particles.
[0021] The toner production by the suspension polymerization method will be described in detail below, but is not limited thereto. (Preparation of Polymerizable Monomer Composition) Polymerizable monomers capable of forming a binder resin, organosilicon polymers and waxes, and optionally A polymerizable monomer composition containing additives such as a colorant is prepared according to the above. The colorant may be dispersed in a part of the polymerizable monomer in advance and then mixed with the remaining polymerizable monomer. Alternatively, all components may be mixed at the same time to prepare the polymerizable monomer composition.
[0022] (granulation process) The polymerizable monomer composition is added to an aqueous medium containing a surfactant or poorly water-soluble inorganic fine particles, and dispersed to form particles of the polymerizable monomer composition in the aqueous medium, thereby obtaining a dispersion containing the particles of the polymerizable monomer composition.
[0023] (Preparation of aqueous medium) The composition of the aqueous medium is not particularly limited, and any known aqueous medium containing water as the main component may be used. The aqueous medium may contain a dispersion stabilizer in order to improve the dispersion stability of the particles of the polymerizable monomer composition. Examples of the dispersion stabilizer include, but are not limited to, the poorly water-soluble inorganic fine particles shown below.
[0024] Carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; Metal phosphates such as aluminum phosphate, magnesium phosphate, calcium phosphate, barium phosphate, and zinc phosphate; Sulfates such as barium sulfate, calcium sulfate; Metal hydroxides of calcium hydroxide, aluminum hydroxide, magnesium hydroxide, ferric hydroxide; etc. These may be used alone or in combination of two or more. These particles exist in the aqueous medium as fine particles and thus function as a dispersion stabilizer.
[0025] (Polymerization process) After the above-mentioned granulation step, the polymerizable monomer contained in the particles of the obtained polymerizable monomer composition is polymerized to form toner particles. In the polymerization step, a polymerization initiator may be added. In the polymerization step, a reaction vessel having a general temperature-controllable stirring means may be used. The polymerization temperature is usually 40° C. or higher, and preferably 50 to 90° C. The polymerization temperature may be constant throughout, but may be elevated in the latter half of the polymerization process in order to obtain a desired molecular weight distribution. The stirring blade used in the stirring means may be of any type as long as it can suspend the particles of the polymerizable monomer composition without causing them to stagnate and can maintain a uniform temperature inside the tank.
[0026] Examples of the stirring blade or stirring means include common stirring blades such as a paddle blade, an inclined paddle blade, a triple swept blade, a propeller blade, a disk turbine blade, a helical ribbon blade and an anchor blade. In addition, "Fullzone" (manufactured by Kobelco Environmental Solutions Co., Ltd.), "Twinstar" (manufactured by Kobelco Environmental Solutions Co., Ltd.), "Maxblend" (manufactured by Sumitomo Heavy Industries, Ltd.), "Supermix" (manufactured by Satake Chemical Machinery Co., Ltd.), and "Hi-F Mixer" (manufactured by Soken Chemical Industries Co., Ltd.) may also be used.
[0027] (Distillation process) After the polymerization step, if necessary, in order to remove volatile impurities such as unreacted polymerizable monomers and by-products, a part of the aqueous medium may be distilled off after the completion of the polymerization. The distillation step can be carried out under normal pressure or reduced pressure.
[0028] (Washing process, solid-liquid separation process and drying process) For the purpose of removing the dispersion stabilizer adhering to the surfaces of the obtained toner particles, an acid or an alkali may be added to the dispersion to carry out a treatment for removing the dispersion stabilizer. Thereafter, the toner particles are separated from the liquid phase by a general solid-liquid separation method, but the toner particles may be washed again with water to completely remove the acid or alkali and the dispersion stabilizer components dissolved therein. This washing process may be repeated several times, and after sufficient washing, the toner particles may be obtained by solid-liquid separation again. The obtained toner particles may be dried by a known drying means.
[0029] (Classification process) The obtained toner particles have a sufficiently sharp particle size distribution, but if an even sharper particle size is required, classification can be performed using an air classifier or the like to separate and remove toner particles that deviate from the desired particle size distribution.
[0030] (External addition process) The obtained toner particles may be used as they are, or an additive may be added externally to the toner particles to produce a toner. In the external addition step, additives (sometimes called external additives) for the purpose of imparting various properties to the toner may be used. From the viewpoint of durability when added to toner particles, the additive preferably has a particle size of 1 / 10 or less of the weight average particle size of the toner particles. The particle size of the additive means the number average particle size determined by observation with an electron microscope.
[0031] Next, the production of the toner by the solution suspension method will be described, but the present invention is not limited to this. (Preparation of mixed solution) A toner particle composition containing a binder resin, an organosilicon polymer, and a wax, and optionally additives such as a colorant, is mixed with an organic solvent capable of dissolving the binder resin to prepare a mixed solution. The preparation method may be such that the binder resin and wax are gradually added to an organic solvent capable of dissolving the binder resin while stirring, and dissolved or dispersed. However, when a pigment is used as a colorant, or when wax, charge control agent, or the like that is difficult to dissolve in an organic solvent is added, it is advisable to reduce the particle size before adding to the organic solvent. For dispersion, a known dispersing machine such as a bead mill or a disk mill can be used.
[0032] (granulation process) The resulting mixed solution is dispersed in an aqueous medium to form particles of the mixed solution. The mixed solution is poured into an aqueous medium containing a surfactant or poorly water-soluble inorganic fine particles, and dispersed to form particles of the mixed solution in the aqueous medium, thereby obtaining a dispersion containing particles of the mixed solution. In the case where the toner particle composition contains a modified resin having an isocyanate group, an active hydrogen group-containing compound may be added, and the active hydrogen group-containing compound may be reacted with a modified resin having a site capable of reacting with the active hydrogen group-containing compound in an aqueous medium to produce a binder resin.
[0033] The surfactants include the following: Anionic surfactants such as alkylbenzene sulfonates, alpha-olefin sulfonates, and phosphate esters; Amine salts such as alkylamine salts, aminoalcohol fatty acid derivatives, polyamine fatty acid derivatives, imidazoline, etc., alkyltrimethylammonium salts, dialkyldimethylammonium salts, etc. cationic surfactants of the quaternary ammonium salt type, such as ammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, and benzethonium chloride; Nonionic surfactants such as fatty acid amide derivatives and polyhydric alcohol derivatives; Amphoteric surfactants such as alanine, dodecyldi(aminoethyl)glycine, di(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine. As the dispersion stabilizer, those exemplified in the preparation of the aqueous medium described above may be used.
[0034] (Solvent removal process) After the above-mentioned granulation step, the organic solvent present in the particles of the resulting mixed solution is removed. For example, a method can be employed in which the temperature of the entire system is gradually increased while stirring to completely evaporate and remove the organic solvent in the particles. Alternatively, the pressure of the dispersion containing the particles in the mixed solution can be reduced while stirring to evaporate and remove the organic solvent.
[0035] The materials used for the toner will be described. Specific examples of the polymerizable monomer capable of forming the binder resin are as follows. Styrene; styrene derivatives such as α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, p-phenylstyrene; acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, dibutyl phosphate ethyl acrylate, and 2-benzoyloxyethyl acrylate; Methacrylic polymerizable monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, diethyl phosphate ethyl methacrylate, and dibutyl phosphate ethyl methacrylate.
[0036] The polymerizable monomers can be used alone or in combination of two or more kinds. Among these, it is preferable to use styrene or a styrene derivative alone or in combination, or to use them in combination with other polymerizable monomers, from the viewpoint of the development characteristics and durability of the toner. In particular, it is preferable that the binder resin contains a styrene-acrylic resin, and it is more preferable that the binder resin is a styrene-acrylic resin. In this case, the compatibility with wax, especially ester wax, is high, and the low-temperature fixing property is improved, so that the effect of the present invention is more remarkable. The styrene-acrylic resin preferably has a styrene-acrylic copolymer moiety. For example, the styrene-acrylic resin may be a hybrid resin having a styrene-acrylic copolymer moiety and a polyester moiety. The content of the styrene-acrylic copolymer moiety in the styrene-acrylic resin is preferably 50% by mass to 100% by mass, more preferably 80% by mass to 100% by mass, and further preferably 90% by mass to 100% by mass. It is preferable that the styrene-acrylic copolymer portion contains at least one selected from the group consisting of a styrene-acrylic acid alkyl ester copolymer and a styrene-methacrylic acid alkyl ester copolymer. The alkyl group of the alkyl ester preferably has 2 or more and 8 or less (more preferably 3 or more and 8 or less). When the carbon number is 2 or more, the decrease in Tg is suppressed and the heat resistance stability is improved, and when the carbon number is 8 or less, the Tg is not too high and the fixing property is good.
[0037] The toner particles may contain a colorant. Examples of the colorant include known colorants used in toners, such as organic pigments and oil-based dyes. Specific examples are shown below, but the present invention is not limited to these. Pigments used as cyan colorants include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Specifically, the following can be mentioned: CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3 and CI Pigment Blue 15:4. Pigments used in magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specifically, the following can be mentioned: CI Pigment Violet 19, CI Pigment Red 31, CI Pigment Red 122, CI Pigment Red 150 and CI Pigment Red 269.
[0038] Examples of pigments used in yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds and allylamide compounds. Specifically, the following can be mentioned: CI Pigment Yellow 74, CI Pigment Yellow 93, CI Pigment Yellow 120, CI Pigment Yellow 151, CI Pigment Yellow 155, CI Pigment Yellow 180 and CI Pigment Yellow 185. Examples of black colorants include carbon black, magnetic materials, and those toned to black using the above-mentioned yellow, magenta, and cyan colorants. The content of the colorant is preferably 1 part by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the binder resin or the polymerizable monomer capable of forming the binder resin.
[0039] As the wax, the following known waxes can be used. Polymethylene waxes such as paraffin waxes, polyolefin waxes, microcrystalline waxes and Fischer-Tropsch waxes; Petroleum waxes such as amide wax and petrolatum and their derivatives; montan wax and its derivatives, natural waxes such as carnauba wax and candelilla wax and their derivatives, hydrogenated castor oil and its derivatives; Examples of the wax include vegetable waxes, animal waxes, higher fatty acids, long-chain alcohols, ester waxes, ketone waxes, and derivatives thereof such as graft compounds or block compounds. These can be used alone or in combination of two or more. The wax preferably contains an ester wax, and more preferably is an ester wax.
[0040] At least one of the waxes has a melting point (the temperature corresponding to the maximum endothermic peak of the endothermic curve in the temperature range of 20 to 200°C, measured with a differential scanning calorimeter) of preferably 30°C or more and 120°C or less, more preferably 50°C or more and 100°C or less. Further, the wax is preferably solid at room temperature, and in particular, a solid wax having a melting point of 50° C. to 100° C. is preferred from the viewpoints of blocking resistance, durability for multiple sheets, low-temperature fixing property and offset resistance of the toner.
[0041] In addition, the SP value of the wax (cal / cm 3 ) 1 / 2 is preferably 8.30 or more and 9.00 or less, and more preferably 8.50 or more and 9.00 or less. When the wax has an SP value of 8.30 or more, the wax has a high affinity with the organosilicon polymer, so that the wax is prevented from bleeding out and the heat resistance stability is improved. In addition, the wax is easily compatible with the binder resin, which is advantageous for improving low-temperature fixability. When the wax has an SP value of 9.00 or less, the wax is not too hydrophilic, so that the wax is unlikely to be exposed on the surface of the toner particles during toner production and storage. This improves the heat resistance stability. The content of the wax (preferably ester wax) in the toner particles is preferably from 6.00% by mass to 16.00% by mass, and more preferably from 6.68% by mass to 15.19% by mass. When the wax content is equal to or greater than the lower limit, the resin plasticizing ability is high, and the effect of the present invention is remarkable. On the other hand, when the wax content is equal to or less than the upper limit, the heat resistance stability is good. In addition, the offset resistance is also good, and the toner is less likely to melt onto the drum or the developing sleeve.
[0042] Ester wax, which is a condensation product of an alcohol component and a carboxylic acid component, has high polarity and is highly compatible with binder resins. Therefore, it easily plasticizes the toner and contributes greatly to improving low-temperature fixability. In addition, it has high affinity with organosilicon polymers, so the effects of the present invention are significantly manifested. In particular, the ester wax preferably contains an ester compound of a diol and an aliphatic monocarboxylic acid. Specifically, it is preferably an ester compound of a diol having 2 to 6 carbon atoms and an aliphatic monocarboxylic acid having 14 to 22 carbon atoms, as represented by the following formula (2).
[0043] [ka]
[0044] In the above formula (2), R 1 represents a linear alkylene group having 2 to 6 carbon atoms (preferably 2 to 3 carbon atoms), R 2 and R 3 each independently represents a linear alkyl group having 10 or more and 21 or less (preferably 13 or more and 18 or less) carbon atoms. Examples of the diol having 2 to 6 carbon atoms include ethylene glycol, diethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol. Examples of the aliphatic monocarboxylic acid having 14 to 22 carbon atoms include aliphatic monocarboxylic acids such as myristic acid, palmitic acid, stearic acid, and behenic acid. When the ester wax has the above-mentioned structure, it has high compatibility with the binder resin, and the effects of the present invention are significantly exhibited.
[0045] In addition, when it is necessary to extract the wax from the toner in order to obtain the above-mentioned physical properties, the extraction method is not particularly limited, and for example, the following method can be used. For example, a predetermined amount of toner is subjected to Soxhlet extraction with toluene, and the solvent is removed from the obtained toluene-soluble portion to obtain a chloroform-insoluble portion, which is then subjected to identification analysis by IR method or the like. Regarding quantification and physical properties, measurements may be performed using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments). The glass transition temperature is the point where the line midway between the baselines before and after the specific heat change occurs during measurement intersects with the differential heat curve. The peak temperature (melting point) of the maximum endothermic peak of the wax can also be obtained from the DSC curve obtained during the temperature rise.
[0046] The organosilicon polymer is preferably a condensation polymer of a compound containing an organosilicon compound having a structure represented by the following formula (Z). [ka]
[0047] In formula (Z), R1 represents an alkyl group having 1 to 4 carbon atoms. R1 is R in formula (1) after polymerization. 1 The same applies to preferred groups. R2, R3 and R4 each independently represent a halogen atom, a hydroxy group, an acetoxy group, or an alkoxy group (preferably having 1 to 4 carbon atoms, more preferably having 1 to 3 carbon atoms) (hereinafter also referred to as a reactive group). These reactive groups undergo hydrolysis, addition polymerization, and condensation polymerization to form a crosslinked structure. R2, R3, and R4 are preferably alkoxy groups, more preferably methoxy groups or ethoxy groups, because the hydrolysis is mild at room temperature. In addition, the hydrolysis, addition polymerization, and condensation polymerization of R2, R3, and R4 can be controlled by the reaction temperature, reaction time, reaction solvent, and pH. To obtain an organosilicon polymer, one or more types of organosilicon compounds having one non-reactive group (R1) and three reactive groups (R2, R3, and R4) in one molecule (hereinafter also referred to as trifunctional silanes), as represented by formula (Z), may be used in combination.
[0048] Examples of the compound represented by the above formula (Z) include the following. Trifunctional methylsilanes such as methyltrimethoxysilane, methyltriethoxysilane, methyldiethoxymethoxysilane, methylethoxydimethoxysilane, methyltrichlorosilane, methylmethoxydichlorosilane, methylethoxydichlorosilane, methyldimethoxychlorosilane, methylmethoxyethoxychlorosilane, methyldiethoxychlorosilane, methyltriacetoxysilane, methyldiacetoxymethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydimethoxysilane, methylacetoxymethoxyethoxysilane, methylacetoxydiethoxysilane, methyltrihydroxysilane, methylmethoxydihydroxysilane, methylethoxydihydroxysilane, methyldimethoxyhydroxysilane, methylethoxymethoxyhydroxysilane, and methyldiethoxyhydroxysilane. Ethyltrimethoxysilane, Ethyltriethoxysilane, Ethyltrichlorosilane, Ethyltriacetoxysilane, Ethyltrihydroxysilane, Propyltrimethoxysilane, Propyltriethoxysilane, Propyltrichlorosilane, Propyltriacetoxysilane, Propyltrihydroxysilane, Butyltrimethoxysilane, Butyltriethoxysilane, Butyltrichlorosilane, Butyltriacetoxysilane, Butyltrihydroxysilane Silane, trifunctional silanes such as
[0049] In the present invention, an organosilicon polymer obtained by combining the following with an organosilicon compound having a structure represented by formula (Z) may be used to the extent that the effect of the present invention is not impaired. An organosilicon compound having four reactive groups in one molecule (tetrafunctional silane), an organosilicon compound having three reactive groups in one molecule (trifunctional silane), an organosilicon compound having two reactive groups in one molecule (bifunctional silane), or an organosilicon compound having one reactive group (monofunctional silane). For example, the following may be mentioned. Dimethyldiethoxysilane, tetraethoxysilane, hexamethyldisilazane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane; Trifunctional vinyl silanes such as vinyl triisocyanate silane, vinyl trimethoxy silane, vinyl triethoxy silane, vinyl diethoxy methoxy silane, vinyl ethoxy dimethoxy silane, vinyl ethoxy dihydroxy silane, vinyl dimethoxy hydroxy silane, vinyl ethoxy methoxy hydroxy silane, vinyl diethoxy hydroxy silane; Hexyltrimethoxysilane, hexyltriethoxysilane, hexyltrichlorosilane, hexyltriacetoxysilane, hexyltrihydroxysilane; Trifunctional phenylsilanes such as phenyltrimethoxysilane, phenyltriethoxysilane, phenyltrichlorosilane, phenyltriacetoxysilane, and phenyltrihydroxysilane.
[0050] The content of the organosilicon polymer in the toner particles is preferably from 0.040% to 0.800% by weight, and more preferably from 0.060% to 0.600% by weight. When the content is 0.040% by mass or more, the attraction effect of the wax due to the addition of the organosilicon compound is stronger, and the effect of improving heat-resistant storage stability is large. Also, when the content is 0.800% by mass or less, there is no inhibition of heat transfer during fixing due to the organosilicon polymer, and no decrease in the plasticizing ability of the binder resin due to an excessively strong attraction effect of the wax, and this is effective in improving low-temperature stability. Furthermore, granulation disorder due to the addition of a large amount of filler particles is unlikely to occur, and a toner with a sharp particle size distribution can be produced.
[0051] A charge control agent may be blended (internal addition) or mixed (external addition) into the toner particles in order to control the charge amount of the toner particles to a desired value. As the charge control agent, a known one can be used. For example, the following can be mentioned as a substance that controls the toner particles to have a negative chargeability. Organometallic compounds and chelating compounds are effective, such as monoazo dye metal compounds, acetylacetone metal compounds; aromatic hydroxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, their anhydrides, or their esters; and phenol derivatives such as bisphenol. Further examples include the following: urea derivatives, metal-containing salicylic acid compounds, calixarenes, silicon compounds, sulfonic acid group-containing resins such as styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, and styrene-acrylic-sulfonic acid copolymers, and non-metallic carboxylic acid compounds.
[0052] On the other hand, examples of toner particles that are controlled to have a positive charge include the following. Nigrosine and its modified products with fatty acid metal salts; quaternary ammonium salts such as tributylbenzylammonium 1-hydroxy-4-naphthosulfonate and tetrabutylammonium tetrafluoroborate; onium salts such as phosphonium salts and their derivatives. lake pigments, triphenylmethane dyes and their lake pigments (lake pigments such as phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, or ferrocyanide as lake agents), metal salts of higher fatty acids; diorganotin oxides such as dibutyltin oxide, dioctyltin oxide, and dicyclohexyltin oxide; diorganotin borates such as dibutyltin borate, dioctyltin borate, and dicyclohexyltin borate. The charge control agents can be used alone or in combination of two or more kinds. The content of the charge control agent is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.5 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the polymerizable monomer capable of forming the binder resin or the binder resin.
[0053] In the polymerization step, a polymerization initiator may be used. Examples of the polymerization initiator include an azo-based polymerization initiator and an organic peroxide-based initiator. Examples of the azo-based polymerization initiator include the following. 2,2'-Azobis-(2,4-dimethylvaleronitrile), 2,2'-Azobisisobutyronitrile, 1,1'-Azobis(cyclohexane-1-carbonitrile), 2,2'-Azobis-4-methoxy-2,4-dimethylvaleronitrile, Azobismethylbutyronitrile.
[0054] Examples of organic peroxide initiators include the following: Benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, tert-butyl peroxypivalate. Redox initiators that combine an oxidizing substance and a reducing substance can also be used. Examples of oxidizing substances include hydrogen peroxide, inorganic peroxides such as persulfates (sodium salts, potassium salts, ammonium salts, etc.), and oxidizing metal salts such as tetravalent cerium salts.
[0055] The reducing substances include reducing metal salts (divalent iron salts, monovalent copper salts, trivalent chromium salts), ammonia, lower amines (amines having 1 to 6 carbon atoms such as methylamine and ethylamine), amino compounds such as hydroxylamine, reducing sulfur compounds such as sodium thiosulfate, sodium hydrosulfite, sodium hydrogensulfite, sodium sulfite, and sodium formaldehyde sulfoxylate, lower alcohols (having 1 to 6 carbon atoms), ascorbic acid or a salt thereof, and lower aldehydes (having 1 to 6 carbon atoms). The polymerization initiator is selected with reference to its 10-hour half-life temperature, and may be used alone or in combination. The amount of the polymerization initiator added is generally about 0.5 parts by mass or more and 20 parts by mass or less based on 100 parts by mass of the polymerizable monomer.
[0056] Various crosslinking agents can also be used, including the following: Divinylbenzene, 4,4'-divinylbiphenyl, hexanediol diacrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, glycidyl (meth)acrylate, trimethylolpropane tri(meth)acrylate.
[0057] The binder resin in the dissolution suspension method is not particularly limited and can be appropriately selected from known resins. Also, a resin obtained by polymerizing the above-mentioned polymerizable monomers can be used. Specifically, styrenes such as styrene and chlorostyrene; monoolefins such as ethylene, propylene, butylene, and isoprene; vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate, and vinyl butyrate; methyl acrylate, ethyl acrylate, butyl acrylate, dodecyl acrylate, octyl acrylate, phenyl acrylate, ... Examples of the vinyl ketone include homopolymers or copolymers of α-methylene aliphatic monocarboxylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, and dodecyl methacrylate; vinyl ethers such as vinyl methyl ether, vinyl ethyl ether, and vinyl butyl ether; and vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone, and vinyl isopropenyl ketone.
[0058] Examples of the polymer of styrene or its substitution product include polystyrene, poly-p-chlorostyrene, and polyvinyltoluene. Examples of styrene copolymers include styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers.
[0059] Representative binder resins include polystyrene resins, polyester resins, styrene-acrylic acid alkyl ester copolymers, styrene-methacrylic acid alkyl ester copolymers, styrene-acrylonitrile copolymers, styrene-butadiene copolymers, styrene-maleic anhydride copolymers, polyethylene resins, polypropylene resins, etc. These may be used alone or in combination of two or more. As in the case of suspension polymerization, the binder resin is preferably a styrene-acrylic resin, as described above.
[0060] The organic solvent is not particularly limited as long as it can dissolve the binder resin, but it is preferable that the organic solvent is volatile and has a boiling point of less than 100° C., since this makes it easier to remove the solvent later. Examples of the organic solvent include the following. These may be used alone or in combination of two or more. Toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc.
[0061] When the resin to be dissolved or dispersed in the organic solvent is a resin having a polyester skeleton, from the viewpoint of the solubility of the resin, an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone is preferred. From the viewpoint of solvent removability, methyl acetate, ethyl acetate, and methyl ethyl ketone are more preferable.
[0062] In the dissolution suspension method, a modified resin (hereinafter sometimes referred to as a "prepolymer") may be used. The modified resin is not particularly limited as long as it has at least a site capable of reacting with the active hydrogen group-containing compound, and can be appropriately selected from known resins. Specific examples include polyol resins, polyacrylic resins, polyester resins, epoxy resins, and derivative resins thereof. These may be used alone or in combination of two or more. Among these, polyester resins are preferred in terms of high fluidity and transparency when melted. There are no particular limitations on the sites in the prepolymer that can react with the active hydrogen group-containing compound. The substituent may be appropriately selected from known substituents, etc. Specific examples include an isocyanate group, an epoxy group, a carboxy group, and an acid chloride group. These may be contained alone or in combination of two or more. Among these, an isocyanate group is preferred.
[0063] The active hydrogen group-containing compound acts as an elongation agent, a crosslinking agent, etc. when a modified resin capable of reacting with the active hydrogen group-containing compound undergoes an elongation reaction, a crosslinking reaction, etc. in an aqueous medium. The active hydrogen group-containing compound is not particularly limited as long as it has an active hydrogen group, and can be appropriately selected according to the purpose.Specific examples include, when the polymer capable of reacting with the active hydrogen group-containing compound is an isocyanate group-containing polyester prepolymer, amines are suitable because they can be made into a high molecular weight by reaction such as elongation reaction or crosslinking reaction with the isocyanate group-containing polyester prepolymer.
[0064] The active hydrogen group is not particularly limited and can be appropriately selected according to the purpose. Specific examples include hydroxyl group (alcoholic hydroxyl group or phenolic hydroxyl group), amino group, carboxyl group, mercapto group, etc. These may be used alone or in combination of two or more. Among these, alcoholic hydroxyl group is preferred.
[0065] Toner may contain external additives for the purpose of improving various powder properties. Examples of the external additives include the following: Metal oxides such as aluminum oxide, titanium oxide, strontium titanate, cerium oxide, magnesium oxide, chromium oxide, tin oxide, zinc oxide; nitrides such as silicon nitride; carbides such as silicon carbide; inorganic metal salts such as calcium sulfate, barium sulfate, calcium carbonate; fatty acid metal salts such as zinc stearate, calcium stearate; carbon black, silica. The content of the external additive is preferably 0.01 parts by mass or more and 10 parts by mass or less, more preferably 0.05 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the toner particles. The external additives may be used alone or in combination. In addition, it is more preferable that these external additives are hydrophobized.
[0066] The toner particles may be magnetic toner particles containing a magnetic material. The magnetic material contained in the toner particles can also serve as a colorant. Iron oxides such as magnetite, hematite, ferrite; metals such as iron, cobalt, nickel or alloys of these metals with metals such as aluminium, cobalt, copper, lead, magnesium, tin, zinc, antimony, beryllium, bismuth, cadmium, calcium, manganese, selenium, titanium, tungsten, vanadium and mixtures thereof. The content of the magnetic material is preferably 20 parts by mass or more and 200 parts by mass or less, and more preferably 40 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of the polymerizable monomer capable of forming the binder resin or the binder resin.
[0067] When a magnetic material is used, it is preferable to subject the surface of the magnetic material to a hydrophobic treatment in order to improve the dispersibility of the magnetic material in the toner particles. For the hydrophobic treatment, coupling agents such as silane coupling agents and titanium coupling agents may be used. Of these, silane coupling agents are preferred. Examples of the silane coupling agent include the following. Vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, methyltrimethoxysilane, methyltriethoxysilane, isobutyltrimethoxysilane, dimethyldimethoxysilane, di Methyldiethoxysilane, trimethylmethoxysilane, hydroxypropyltrimethoxysilane, phenyltrimethoxysilane, n-hexadecyltrimethoxysilane, n-octadecyltrimethoxysilane.
[0068] The measurement methods for each physical property will be described below. <Method of measuring the volume-based median diameter (Dv50), number-based median diameter (Dn50) and particle size distribution of toner particles> The volume-based median diameter (Dv50) and number-based median diameter (Dn50) of the toner particles are calculated as follows. The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000. The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.). Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.
[0069] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 mL of the electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted about three times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, drip the solution into the round-bottom beaker (1) placed in the sample stand. The electrolytic solution (5) in which the toner particles are dispersed is dropped to adjust the measurement concentration to about 5%. Then, the measurement is continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software provided with the device, and the volume-based median diameter (Dv50) and number-based median diameter (Dn50) are calculated. The particle size distribution is indicated by the ratio of Dv50 to Dn50 (Dv50 / Dn50), which is closer to 1.00, so that the particle size distribution is sharper.
[0070] <How to calculate solubility parameter (SP value)> The SP value is calculated using Fedors' formula (4). The values of Δei and Δvi here refer to the evaporation energies and molar volumes (25°C) of atoms and atomic groups in Table 3-9 of "Basic Science of Coatings" pp. 54-57, 1986 (Maki Shoten). δi=[Ev / V] 1 / 2 = [Δei / Δvi] 1 / 2 Formula (4) Ev: Evaporation energy V: Molar volume Δei: Evaporation energy of the atom or atomic group of the i component Δvi: Molar volume of the atom or atomic group of the i component For example, hexanediol is composed of the atomic groups (-OH) x 2 + (-CH2) x 6, and its calculated SP value can be calculated using the following formula. δi = [Δei / Δvi] 1 / 2 =[{(5220)×2+(1180)×6} / {(13)×2+(16.1)×6}] 1 / 2 The SP value (δi) is 11.95. The unit of SP value is (cal / cm 3 ) 1 / 2 It is.
[0071] (Measurement of SP value of wax and organosilicon polymer from toner) The SP value of the wax can be calculated by the above-mentioned method using the results of separating the wax from the toner and analyzing it for identification. Furthermore, using the results of confirming the structure of the organosilicon polymer by NMR, as described below, the SP value of the organosilicon polymer can be calculated by this method.
[0072] <Method for determining the location of organosilicon polymers by observing the cross-section of toner particles using a scanning transmission electron microscope (STEM)> The cross section of a toner particle is observed by the following method. A specific method for observing the cross section of a toner particle is to thoroughly disperse the toner in a room temperature curing epoxy resin, and then cure it for two days in an atmosphere at 40°C. A thin sample is cut out from the obtained cured product using a microtome equipped with a diamond blade. This sample is magnified at a magnification of 10,000 to 100,000 times with a scanning transmission electron microscope (JEM2800, manufactured by JEOL Ltd.) (STEM), and the cross section of the toner particle is observed. The difference in atomic weight between the resin used in the toner and the organic silicon compound is utilized, and the larger the atomic weight, the brighter the contrast is, and this is utilized for confirmation. In addition, the ruthenium tetroxide staining method and the osmium tetroxide staining method may be used to provide contrast between materials. To confirm the exact location of the organosilicon polymer, a bright-field image of the cross section of the toner particle is obtained using a Tecnai TF20XT electron microscope manufactured by FEI at an acceleration voltage of 200 kV. Next, an EF mapping image of the Si-K edge (99 eV) is obtained using a Gatan EELS detector GIF Tridiem by the Three Window method, and it is confirmed that the organosilicon polymer is present in an area of 80% or less of the distance A from the center of gravity of the cross section of the toner particle to the outline of the cross section. To distinguish between organosilicon polymers and silica, an EF mapping image of oxygen is also obtained, and the difference in brightness is used to distinguish between them.
[0073] <How to determine the range in which organosilicon polymers exist> For the various measurements described below, commercially available image analysis software, WinROOF (Mitani Shoji Co., Ltd.), was used. Since the organosilicon polymer is thought to be uniformly dispersed three-dimensionally within the toner particles, even if the organosilicon polymer is contained inside the toner particles, the probability of it being observed in a cross section cut randomly from each particle is low. In view of the above, the range in which the organosilicon polymer exists is determined by the following method. A line segment is drawn from the center of gravity of the cross section of a toner particle to the outline of the cross section of the toner particle, passing through the organosilicon polymer. The length L of the line segment from the center of gravity to the organosilicon polymer is measured. Note that length L is measured at the position closest to the center of gravity on one organosilicon polymer particle. The ratio of length L to the length of the line segment (distance A) is X%. X% is measured for all organosilicon polymers observed on the cross section of one toner particle. 100 particles are observed, and the minimum value of all the measured X% is taken as Xmin. When Xmin is 80% or less, the measured sample is determined to be a toner particle in which the organosilicon polymer is present in an area that is 80% or less of distance A from the center of gravity of the cross section of the toner particle to the outline of the cross section. It is to be noted that Xmin is, for example, preferably about 1% to 70%, and more preferably about 10% to 60%. The arithmetic mean value of X is, for example, preferably about 10% to 70%, and more preferably about 20% to 60%.
[0074] <Method of confirming the structure represented by formula (1)> The structure represented by formula (1) in the organosilicon polymer contained in the toner particles is confirmed by the following method. R in Equation (1) 1 The presence or absence of an alkyl group represented by 13 The detailed structure of formula (1) is 1 H-NMR, 13 C-NMR and 29 The measurement was confirmed by Si-NMR. The equipment and measurement conditions used are as follows: "Measurement conditions" Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of a measurement sample (tetrahydrofuran (THF)-insoluble portion of toner particles for NMR measurement) is placed in a sample tube with a diameter of 4 mm. In this method, R in formula (1) 1 If a signal is confirmed, the structure of formula (1) is deemed to be "present."
[0075] " 13 C-NMR (solid state) measurement conditions Measurement nuclear frequency: 125.77MHz Reference substance: Glycine (external standard: 176.03ppm) Observation width: 37.88kHz Measurement method: CP / MAS Contact time: 1.75ms Repeat time: 4s Number of times accumulated: 2048 LB value: 50Hz
[0076] " 29 "Si-NMR (solid state) measurement method" "Measurement conditions" Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of a measurement sample (THF insoluble portion of toner particles for NMR measurement) is placed in a sample tube with a diameter of 4 mm. Measurement nuclear frequency: 99.36MHz Reference material: DSS (external standard: 1.534ppm) Observation width: 29.76kHz Measurement method: DD / MAS, CP / MAS 29 Si 90° Pulse width: 4.00μs@-1dB Contact time: 1.75ms~10ms Repeat time: 30s (DD / MASS), 10s (CP / MAS) Number of times accumulated: 2048 LB value: 50Hz
[0077] (Method of separating external additives) When an external additive is added to a toner particle and the toner particle is to be used as a sample, the external additive is removed by the following specific method. Add 160g of sucrose (Kishida Chemical) to 100mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Place 31g of the concentrated sucrose solution and 6mL of Contaminon N in a centrifuge tube to prepare a dispersion. Add 1g of toner to this dispersion and break up any clumps of toner with a spatula or similar. The centrifuge tubes were shaken in a shaker (Iwaki Sangyo Co., Ltd.'s "KM Shaker") The solution is shaken for 20 minutes at 350 reciprocations per minute. After shaking, the solution is transferred to a glass tube for a swing rotor (50 mL) and centrifuged at 3500 rpm for 30 minutes in a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.). After centrifugation, the toner particles are present in the top layer in the glass tube, and external additives are present in the aqueous solution layer below, so only the toner particles in the top layer are collected. If the external additives are not completely removed, centrifugation is repeated as necessary to separate the toner sufficiently, and then the toner liquid is dried and the toner particles are collected.
[0078] (Analysis of toner coated with organosilicon polymer) When analyzing toner particles having an organosilicon polymer present on the surface thereof, a portion can be sampled before the toner particle surface is coated with the organosilicon polymer, cooled, and then hydrochloric acid is added to adjust the pH to 1.4 or less to dissolve the dispersion stabilizer, followed by filtering, washing and drying, and then the resulting sample can be used for analysis.
[0079] <Method of measuring glass transition temperature Tg (℃)> The glass transition temperature (Tg) is measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction. Specifically, about 10 mg of a sample is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference. Measurements are performed in the measurement range of 30 to 200°C at a temperature rise rate of 10°C / min. During this temperature rise process, a change in specific heat is obtained in the temperature range of 40°C to 100°C. The glass transition temperature Tg (° C.) of the sample is determined as the intersection point between the line midway between the baselines before and after the specific heat change occurs and the differential heat curve.
[0080] <Measurement of the amount of organosilicon polymer in toner particles> The amount of organosilicon polymer in the toner particles can be measured by measuring the amount of silicon using fluorescent X-rays. The measurement of fluorescent X-rays for each element conforms to JIS K 0119-1969, and specifically, is as follows. The measurement equipment used was a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. The anode used is Rh, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 10 mm, and the measurement time is 10 seconds. In addition, when measuring light elements, a proportional counter (PC) is used, and when measuring heavy elements, a scintillation counter (SC) is used. The measurement sample was prepared by placing approximately 1 g of toner particles into a specially designed aluminum ring with a diameter of 10 mm, flattening it, and then pressing it at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (manufactured by Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of approximately 2 mm. Measurements are performed under the above conditions, and elements are identified based on the peak positions of the obtained X-rays, and their concentrations are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time. The method for quantifying the amount of silicon in toner particles is, for example, to add silica (SiO2) fine powder so that it is 0.5 parts by mass per 100 parts by mass of toner particles, and thoroughly mix using a coffee mill. Similarly, silica fine powder is mixed with the toner particles in amounts of 2.0 parts by mass and 5.0 parts by mass, respectively, and these are used as samples for the calibration curve. For each sample, a pellet of the calibration curve sample is prepared as described above using a tablet press, and the count rate (unit: cps) of the Si-Kα ray observed at a diffraction angle (2θ) = 109.08° when PET is used as the analyzing crystal is measured. In this case, the acceleration voltage and current value of the X-ray generator are 24 kV and 100 mA, respectively. A linear function calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the amount of SiO2 added in each calibration curve sample on the horizontal axis. Next, the toner particles to be analyzed are pelletized as described above using a tablet molding machine, and the count rate of the Si-Kα radiation is measured. The content of the organosilicon polymer in the toner is then calculated from the calibration curve.
[0081] <Method of measuring wax content, glass transition temperature (Tg), and melting point> The wax content, glass transition temperature (Tg), and melting point are measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments) in accordance with ASTM D3418-82. The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction. Specifically, 1 mg of a sample is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference. First, a toner is used as a sample, and the temperature is raised from 0° C. to 150° C. at a heating rate of 10° C. / min. The amount of heat absorbed by the endothermic peak derived from the wax observed at this time is defined as H1 (J / g). After holding at 150°C for 15 minutes, cool from 150°C to 0°C at a rate of 10°C / min. After holding at 0°C for another 10 minutes, heat from 0°C to 150°C at a rate of 10°C / min for the second time, and the endothermic heat of the endothermic peak derived from the wax observed at this time is taken as H2 (J / g). The endothermic amount is calculated from the area enclosed by a differential scanning calorimetric curve showing an endothermic peak obtained by heating in a temperature region where an endothermic peak appears and the baseline of the differential scanning calorimetric curve. The above measurement is also carried out on the wax alone in the same manner, and the peak temperature of the endothermic peak in the second temperature rise process is taken as the melting point of the wax (° C.), and the amount of endotherm is taken as Hw (J / g). The wax content (mass%) is calculated using the following formula. Wax content (mass%) = 100 × H1 / Hw The glass transition temperature (Tg) of the toner or resin is measured by using the above-mentioned measuring device and performing modulation measurement on 1 mg of sample at a temperature rise rate of 1°C / min and a temperature amplitude of ±0.318°C / min in the measurement range of 20°C to 140°C. During this temperature rise process, the specific heat change is obtained in the temperature range of 20°C to 140°C. The glass transition temperature is the temperature (°C) at which a line equidistant in the vertical direction from the extended line of each baseline intersects with the curve of the stepwise change in the glass transition before and after the specific heat change appears in the obtained specific heat change curve. EXAMPLES
[0082] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. Note that, unless otherwise specified, "parts" and "%" in the following formulations are all based on mass.
[0083] <Preparation of Organosilicon Polymer 1> (Preparation of apatite dispersion) After 916.4 parts of ion-exchanged water, 14.83 parts of sodium phosphate, and 6.4 parts of hydrochloric acid were placed in a container, the temperature was raised to 60°C to prepare a sodium phosphate aqueous solution. Meanwhile, 8.60g of calcium chloride was dissolved in 60.2 parts of ion-exchanged water to prepare a calcium chloride aqueous solution. The sodium phosphate aqueous solution was stirred at 12,000 rpm in a Clearmix (M Technique Co., Ltd.), the calcium chloride aqueous solution was added, and the mixture was held for 30 minutes to obtain an apatite dispersion.
[0084] (Preparation of hydrolysis solution of organosilicon compound) 100 parts of methyltrimethoxysilane and 112 parts of ion-exchanged water whose pH had been adjusted to 4 with hydrochloric acid were placed in a container and mixed with a paddle impeller. Stirring was continued until phase separation was no longer visible to the naked eye, yielding a hydrolyzed liquid of an organosilicon compound.
[0085] (Polymerization / solid-liquid separation / drying process) 400 parts of the apatite dispersion was placed in a container, heated to 55°C in a water bath, and stirred at 200 rpm with a paddle stirring blade. Then, 22.1 parts of the hydrolyzed solution of the organosilicon compound was added to the apatite dispersion. After 10 minutes, 9.7 parts of a 7.94% by mass aqueous sodium carbonate solution was added over 15 minutes using a gear pump, and polymerization was carried out for 3 hours. The dispersion was then cooled, and 30 parts of 10% by weight hydrochloric acid was added with stirring, followed by stirring for 2.5 hours to obtain a dispersion containing organosilicon polymer 1. Organosilicon polymer 1 was separated from the dispersion by filtration, washed with water, and dried at a temperature of 40° C. for 48 hours to obtain organosilicon polymer 1.
[0086] <Preparation of Organosilicon Polymer 2> Organosilicon polymer 2 was obtained in the same manner as organosilicon polymer 1, except that the organosilicon compound was changed from 100 parts of methyltrimethoxysilane to a combination of 97 parts of methyltrimethoxysilane and 3 parts of phenyltrimethoxysilane.
[0087] <Preparation of Organosilicon Polymer 3> Organosilicon Polymer 3 was obtained in the same manner as Organosilicon Polymer 1, except that the organosilicon compound was changed from 100 parts of methyltrimethoxysilane to a combination of 94 parts of methyltrimethoxysilane and 6 parts of phenyltrimethoxysilane.
[0088] <Preparation of Organosilicon Polymer 4> Organosilicon Polymer 4 was obtained in the same manner as Organosilicon Polymer 1, except that the organosilicon compound was changed from 100 parts of methyltrimethoxysilane to a combination of 92 parts of methyltrimethoxysilane and 8 parts of phenyltrimethoxysilane.
[0089] <Production Example of Toner Particle 1> Styrene 72.0 parts n-Butyl acrylate 28.0 parts 1,6-Hexanediol diacrylate 0.6 parts Copper phthalocyanine pigment (Pigment Blue 15:3) 6.2 parts Aluminum salicylate compound 0.8 parts (Bontron E88; manufactured by Orient Chemical Industries Co., Ltd.) Polar resin 4.0 parts (A saturated polyester resin obtained by the condensation polymerization reaction of 2 moles of propylene oxide adduct of bisphenol A with terephthalic acid and isophthalic acid; weight average molecular weight is 13,000, acid value is 8 mgKOH / g, and glass transition temperature is 74°C) Wax (ethylene glycol distearate: melting point 76°C) 10 parts Organosilicon polymer 1 0.10 parts The above materials were mixed, 15 mm ceramic beads were added to the resulting mixture, and the mixture was dispersed for 2 hours using a wet attritor (manufactured by Nippon Coke & Co., Ltd.) to obtain a polymerizable monomer composition. Meanwhile, 6.3 parts of sodium phosphate (Na3PO4) was added to 414.0 parts of ion-exchanged water, and the mixture was heated to 60°C while stirring using a Clearmix (M Technique Co., Ltd.). After that, an aqueous calcium chloride solution in which 3.6 parts of calcium chloride (CaCl2) was dissolved in 25.5 parts of ion-exchanged water was added, and stirring was continued to prepare an aqueous medium containing a dispersion stabilizer made of tricalcium phosphate (Ca3(PO4)2). To the polymerizable monomer composition, 9.0 parts of t-butyl peroxypivalate as a polymerization initiator was added, and the mixture was charged into the above aqueous medium, followed by a granulation step for 10 minutes in the above Clearmix while maintaining the rotation speed at 15,000 rpm. The polymerization process was then carried out for 5 hours in a stirring tank equipped with a standard stirrer, while maintaining the temperature at 70°C with stirring, after which the temperature was raised to 85°C and maintained there for 1 hour, and then further raised to 100°C and maintained there for 2 hours. Thereafter, the mixture was cooled to obtain a toner particle dispersion 1. Hydrochloric acid was added to the toner particle dispersion liquid 1 to adjust the pH to 1.4 or less to dissolve the dispersion stabilizer, and the mixture was filtered, washed, and dried to obtain toner particles 1.
[0090] <Production Examples of Toner Particles 2-6, 8-24, and 26-28> Except for changing the materials used as shown in Table 1, the same procedure as in the production example of toner particle 1 was carried out to obtain toner particles 2 to 6, 8 to 24, and 26 to 28. In the toner 27, the SiO2 particles used were silica fine particles having a number average particle size of 40 nm for the primary particles.
[0091] <Production Example of Toner Particle 7> In a reaction vessel equipped with a reflux condenser, a stirrer, and a nitrogen inlet tube, the following materials were placed under a nitrogen atmosphere. Toluene 110 parts Polyester resin 110 parts (Saturated polyester resin solution obtained by polycondensation of 2 moles of ethylene oxide adduct of bisphenol A with terephthalic acid; resin Tg=54.5℃) The inside of the reaction vessel was stirred at 200 revolutions per minute, heated to 70° C. and stirred for 10 hours, whereby a binder resin solution 7 was obtained. Next, Binder resin solution 7 201.2 parts Polar resin 4.0 parts (Bisphenol A propylene oxide 2 mole adduct with terephthalic acid and isophthalic acid) Saturated polyester resin solution obtained by polycondensation reaction with ethyl acetate (resin Tg=74°C) Wax (ethylene glycol distearate: melting point 76°C) 10 parts Organosilicon polymer 1 0.10 parts Copper phthalocyanine pigment (Pigment Blue 15:3) 6.2 parts Aluminum salicylate compound 0.8 parts (Bontron E88; manufactured by Orient Chemical Industries Co., Ltd.) The above components were mixed and dispersed for 10 hours using a wet attritor (manufactured by Nippon Coke & Co., Ltd.) containing ceramic beads with a diameter of 15 mm, to obtain a resin composition solution 7. Meanwhile, 6.3 parts of sodium phosphate (Na3PO4) was added to 414.0 parts of ion-exchanged water, and the mixture was heated to 60°C while stirring using a Clearmix (manufactured by M Technique Co., Ltd.). Thereafter, an aqueous calcium chloride solution prepared by dissolving 3.6 parts of calcium chloride (CaCl2) in 25.5 parts of ion-exchanged water was added, and stirring was continued to prepare an aqueous medium containing a dispersion stabilizer made of tricalcium phosphate (Ca3(PO4)2). Resin composition solution 7 was added to the above aqueous medium, and a granulation step was carried out for 10 minutes while maintaining the rotation speed at 15,000 rpm in the above Clearmix, thereby obtaining resin composition dispersion 7. The temperature of the resin composition dispersion 7 was raised to 95° C., and the mixture was stirred for 120 minutes to remove the toluene from the resin composition dispersion 7. Thereafter, the mixture was cooled to obtain a toner particle dispersion 7. Hydrochloric acid was added to the toner particle dispersion liquid 7 to adjust the pH to 1.4 or less to dissolve the dispersion stabilizer, and the mixture was filtered, washed, and dried to obtain toner particles 7.
[0092] <Production Example of Toner Particle 25> Toner particles 25 were obtained in the same manner as in the production example of toner particles 1, except that the materials used were changed as shown in Table 1 and the reaction step and subsequent steps were carried out as follows. (Preparation of aqueous medium A) 35.0 parts of ion-exchanged water was weighed into a vessel equipped with a stirrer and a thermometer, and the pH was adjusted to 5.0 with 10% by mass of hydrochloric acid. The mixture was heated with stirring until the temperature reached 30°C. Thereafter, 3.0 parts of methyltrimethoxysilane was added and stirred for 1 hour, to obtain an aqueous medium A. (Reaction process / organosilicon polymer coated toner particle production process) The dispersion of the polymerizable monomer composition was transferred to another tank, kept at 55°C, and stirred with a paddle stirring blade. 20.4 parts of aqueous medium A was added to the dispersion of the polymerizable monomer composition, and the mixture was kept for 30 minutes while stirring. After that, the slurry was adjusted to pH 9.0 using an aqueous sodium hydroxide solution and kept for another 300 minutes, to obtain a dispersion of toner particles coated with an organosilicon polymer. Thereafter, the mixture was cooled to obtain a toner particle dispersion 25. Hydrochloric acid is added to the toner particle dispersion liquid 25 to adjust the pH to 1.4 or less to dissolve the dispersion stabilizer, and the mixture is filtered, washed, and dried to obtain toner particles 25.
[0093] (Examples 1 to 25 and Comparative Examples 1 to 3) To 100.0 parts of each of the obtained toner particles, 1.0 part of silica fine particles having a primary particle number average particle size of 40 nm was added and mixed using an FM mixer (manufactured by Nippon Coke & Co., Ltd.) to obtain toners 1 to 25 (toners of Examples 1 to 25). Similarly, silica fine particles were mixed to obtain toners 26 to 28 (toners of Comparative Examples 1 to 3). Table 1 shows the physical properties of the obtained toners.
[0094] [Table 1] In Table 1, "parts" refers to the number of parts relative to 100 parts of binder resin. "Content (mass%)" refers to the content in the toner particles. "Tg" refers to the Tg of the binder resin. In the column of "No." for the organosilicon polymer, In the above, SiO2 indicates that SiO2 has been added. SP value difference is the difference between the SP value of the wax and the SP value of the organosilicon polymer. Particle size is the median diameter based on volume. (A) indicates the presence or absence of organosilicon polymer in an area that is 80% or less of distance A from the center of gravity of the cross section of a toner particle to the outline of said cross section.
[0095] The obtained toners were evaluated by the methods described below, and the results are shown in Table 2. <Evaluation of developability> (Image density after exposure to high temperature and humidity; rated as 1 in the table) 200 g of the toner was left to stand for 30 days in an environment of a temperature of 40° C. and a humidity of 95% RH, and this was used as the toner for evaluation. An LBP-7700C (manufactured by Canon) was used as the image forming apparatus, the toner was removed from the cyan cartridge, and the toner to be evaluated was filled in place of the cyan cartridge. The image was evaluated under normal temperature and humidity conditions (temperature: 23° C., humidity: 50% RH). Image density was measured as an index of the coloring power of the toner. A4 color laser copier paper (Canon, 80g / m 2 ) with a toner load of 0.3mg / cm 2 I adjusted it so that it was like this, and then output a solid image. The solid image was evaluated by measuring the density (average of five points: upper right, lower right, center, upper left, and lower left). The image density was measured using a "504 Spectrodensitometer" (manufactured by X-Rite Corporation) as a relative density to the white background part where the image density was 0.00. A grade of C or higher was judged to be good. (Evaluation Criteria) A: Density difference 1.45 or more B: Density difference 1.35 or more and less than 1.45 C: Density difference 1.20 or more and less than 1.35 D: Density difference 1.05 or more and less than 1.20 E: Density difference less than 1.05
[0096] (Low temperature fixability: rated 2 in the table) Color laser printer with the fuser unit removed (HP Color LaserJet The toner was removed from the cyan cartridge and replaced with the toner to be evaluated. Next, the receiving paper (HP Laser Jet90, manufactured by H company, 90 g / m 2 ) using the filled toner, an unfixed toner image of 2.0 cm length x 15.0 cm width (toner loading amount: 0.9 mg / cm 2) was formed at a position 1.0 cm from the upper end in the paper feed direction. Next, the removed fixing unit was modified so that the fixing temperature and process speed could be adjusted, and a fixing test of an unfixed image was carried out using this. First, in a normal temperature and humidity environment (23° C., 60% RH), the process speed was set to 250 mm / s, and the initial temperature was 110° C., and the set temperature was successively increased by 5° C. at each temperature, while fixing the unfixed image at each temperature. The evaluation criteria for low-temperature fixability are as follows. The low-temperature fixation start point is the lowest temperature at which the low-temperature offset phenomenon (the phenomenon in which part of the toner adheres to the fixing device) is not observed. C or higher was judged to be good. A: The low temperature side fixing start point is 140℃ or less B: Low temperature side fixing start point is 145℃ or more and 155℃ or less C: The low temperature side fixing start point is 160℃ or more and 170℃ or less D: The low-temperature side fixing start point is 175°C or higher and 185°C or lower E: The low temperature side fixing start point is 190℃ or higher
[0097] <Evaluation of heat resistance> (Evaluation of blocking resistance: rated 3 in the table) The blocking resistance of the toner was evaluated by the following method. Approximately 10 g of toner was placed in a 100 mL polypropylene cup, and left for 7 days in an environment with a temperature of 45° C. and a humidity of 95% RH, and then visually evaluated. A grade of C or higher was deemed to be good. (Evaluation Criteria) A: No aggregates were observed. B: A few aggregates are visible, but they crumble easily. C: Agglomerates are visible but easily disintegrate. D: Agglomerates are visible, but can be broken down by shaking. E: The aggregates can be grasped and do not easily crumble.
[0098] (Evaluation of toner wettability; rated 4 in the table) Since the degree of hydrophobicity of the toner particle surface increases when the wax bleeds out, the degree of hydrophobicity of the toner was measured using a methanol wettability test. In the evaluation of the blocking resistance, the methanol wettability was measured for the toner that had been left for 7 days in an environment of a temperature of 45° C. and a humidity of 95% RH, and for the toner that had not been left for 7 days, and the rate of change in hydrophobicity was calculated using the following formula. The greater the rate of change in hydrophobicity, the more the wax bleeds out in a high-temperature and high-humidity environment. Hydrophobicity change rate=(Hydrophobicity of toner after standing) / (Hydrophobicity of toner without standing) The degree of hydrophobicity of the toner was determined from a methanol drop amount-transmittance curve obtained by the following method. First, 60 mL of water was placed in a cylindrical glass container having a diameter of 5 cm and a thickness of 1.75 mm, and the water was dispersed for 5 minutes using an ultrasonic disperser to remove air bubbles and the like in the water. Next, the toner was sieved through a mesh with 150 μm openings, and 0.1 g of the toner that had passed through the mesh was precisely weighed and added to the container containing the water to prepare a sample liquid for measurement. The sample liquid for measurement was then placed in a powder wettability tester "WET-100P" (manufactured by Rhesca Co., Ltd.) and stirred for 5.0 s using a magnetic stirrer. -1 The mixture was stirred at a speed of (300 rpm). The rotor of the magnetic stirrer was a fluororesin-coated spindle-shaped rotor having a length of 25 mm and a maximum body diameter of 8 mm. Next, the transmittance was measured using light with a wavelength of 780 nm while continuously adding methanol to this measurement sample liquid through the above-mentioned device at a dropping rate of 0.8 mL / min, and a methanol dropping amount vs. transmittance curve was created. From the obtained methanol drop amount-transmittance curve, the methanol concentration at which the transmittance became 50% was determined as the degree of hydrophobicity.
[0099] [Table 2] [Explanation of symbols]
[0100] 1: organosilicon polymer, 2: boundary line representing an area of 80% or less of distance A from the center of gravity of the cross section of a toner particle to the contour of the cross section, 3: center of gravity of the cross section of a toner particle, 4: distance A from the center of gravity of the cross section of a toner particle to the contour of the cross section, 5: distance 80% of distance A from the center of gravity of the cross section of a toner particle
Claims
1. A toner including toner particles containing a binder resin and a wax, The toner particles contain an organosilicon polymer represented by the following formula (1): In a cross section of the toner particle observed by a transmission electron microscope, said organosilicon polymer is present in an area that is 80% or less of distance A from the center of gravity of said cross section of said toner particle to the contour of said cross section, The absolute value of the difference between the SP value of the organosilicon polymer and the SP value of the wax is 0.70 (cal / cm 3 ) 1/2 A toner characterized in that: R 1 -SiO 3 / 2 (1) In formula (1), R 1 is an alkyl group having 1 to 4 carbon atoms.
2. The SP value of the wax (cal / cm 3 ) 1/2 2. The toner according to claim 1, wherein the molecular weight distribution is 8.30 or more and 9.00 or less.
3. 3. The toner according to claim 1, wherein the wax contains an ester wax.
4. The toner according to claim 3 , wherein the ester wax is represented by the following formula (2): In formula (2), R 1 represents a linear alkylene group having 2 to 6 carbon atoms; R 2 and R 3 each independently represents a linear alkyl group having 10 to 21 carbon atoms.
5. 5. The toner according to claim 1, wherein the content of the wax in the toner particles is 6.00% by mass or more and 16.00% by mass or less.
6. 6. The toner according to claim 1, wherein the content of said organosilicon polymer in said toner particles is from 0.040% by weight to 0.800% by weight.
7. 7. The toner according to claim 1, wherein the binder resin comprises a styrene-acrylic resin.
8. The binder resin contains a styrene-acrylic resin, The styrene-acrylic resin has a styrene-acrylic copolymer moiety, the styrene-acrylic copolymer moiety includes at least one selected from the group consisting of a styrene-acrylic acid alkyl ester copolymer and a styrene-methacrylic acid alkyl ester copolymer; 8. The toner according to claim 1, wherein the alkyl acrylate and the alkyl methacrylate each have an alkyl group having 2 or more and 8 or less carbon atoms.
9. The SP value (cal / cm) of the organosilicon polymer 3 ) 1/2 The toner according to any one of claims 1 to 8, wherein the molecular weight distribution is 8.00 or more and 9.70 or less.
Citation Information
Patent Citations
Electrostatic charge image developing toner
JP2000305318A
Toner for electrostatic image development
JP2007334118A
Electrostatic charge image developing toner, electrostatic charge image developer and image forming apparatus
JP2009042386A
Toner containing polyhedral oligomeric silsesquioxanes
JP2010145994A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge and image forming apparatus
JP2011203511A