Conductor-polyimide laminate
The conductor-polyimide laminate addresses transparency and thermal expansion issues in FPCs by using a multi-layer polyimide structure with specific residues, enhancing heat resistance and adhesion for transparent electronic applications.
Patent Information
- Application Number
- JP2020214104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Existing polyimide materials used in flexible printed circuits (FPCs) face challenges in achieving transparency, heat resistance, and dimensional stability due to issues like charge transfer complexes, yellowish color, and mismatched thermal expansion coefficients, which affect the integrity and functionality of transparent FPCs in applications such as transparent antennas and window-integrated devices.
A conductor-polyimide laminate is developed with specific polyimide layers containing diamine and tetracarboxylic anhydride residues, optimized for transparency, heat resistance, and thermal expansion control, featuring a multi-layer structure with thermoplastic and non-thermoplastic polyimide layers to enhance adhesiveness and flexibility, and incorporating fluorine-containing residues to reduce interlayer interactions.
The laminate achieves high transparency, excellent heat resistance, and controlled thermal expansion, ensuring reliable adhesion and dimensional stability, making it suitable for transparent FPCs and laminated barrier layers in electronic components.
Smart Images

Figure 0007577533000001 
Figure 0007577533000002 
Figure 0007577533000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductor-polyimide laminate having an insulating resin layer that is excellent in heat resistance, adhesiveness, and flexibility, and is highly transparent. [Background technology]
[0002] Polyimide is a heat-resistant resin obtained by ring-closing polyamic acid, which is synthesized by condensation reaction of tetracarboxylic anhydride and diamine as raw materials, and has excellent resistance to thermal decomposition due to rigidity of molecular chain, resonance stabilization, and strong chemical bonds, and has high durability against chemical changes such as oxidation or hydrolysis, and has excellent flexibility, mechanical properties, and electrical properties. Polyimide is widely used in the insulating resin layer of flexible printed circuit boards (FPC; Flexible Printed Circuits) that are generally used in electronic devices.
[0003] The insulating resin layer in commercially available copper-clad laminates generally used in FPCs is made of a wholly aromatic polyimide resin, which exhibits a yellowish-brown color due to the formation of charge-transfer complexes within and between molecules, making it difficult to apply this to transparent FPCs, which require colorless transparency.
[0004] In order to make polyimide colorless and transparent, it has been proposed to suppress the formation of intramolecular and intermolecular charge transfer complexes by using alicyclic diamines or alicyclic acid anhydrides as diamine components. For example, Patent Document 1 proposes a colorless and transparent semi-alicyclic polyimide formed from an alicyclic diamine and an aromatic acid dianhydride, and Patent Document 2 proposes a colorless and transparent full alicyclic polyimide made from an alicyclic diamine and an alicyclic acid anhydride. However, the glass transition temperatures of the obtained polyimides are all about 280°C or lower, and the heat resistance is insufficient, making it difficult to apply them to the main components as insulating layers of FPCs. In addition, since colorless and transparent polyimides suppress the formation of charge transfer complexes, there is also the problem that it is difficult to satisfy the low thermal expansion required for FPCs.
[0005] Patent Document 3 proposes a metal clad laminate that is transparent and has sufficient adhesive strength with a smooth metal layer. However, the polyimide that adheres to the metal layer is still colored, and there is room for improvement in terms of transparency.
[0006] The metal-clad laminates used in FPCs are composed of a thin metal foil and an insulating resin layer containing a polyimide layer. If there is a large difference in the coefficient of thermal expansion (CTE) between the metal foil and the insulating resin layer, the board will warp or curl, causing problems such as changes in dimensions when mounting electronic components, making it impossible to mount them accurately. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 7-10993 [Patent Document 2] JP 2008-163210 A [Patent Document 3] JP 2010-155360 A Summary of the Invention [Problem to be solved by the invention]
[0008] In addition to the background technologies mentioned above, in recent years, a transparent FPC with both the conductor layer and the insulating resin layer guaranteed to be transparent is used as a transparent antenna, and this is formed on the surface of window glass to turn the window into a base station, and a technology for embedding an antenna in a display for mobile applications has been developed. In these new applications, in addition to forming a transparent conductor layer, a method of forming thin wiring that is difficult to see with the naked eye is known, but in both methods, a transparent barrier layer is required to protect the wiring. In addition, a design in which a functional layer such as a transparent conductive layer and a transparent FPC are laminated is also considered. Therefore, when trying to form such a new device using a transparent FPC, it is necessary to develop a design that expresses transparency while taking into consideration the formation of the device.
[0009] Furthermore, in applications requiring such a transparent barrier layer or in applications in which it is laminated with various functional layers, there was concern that light reflection could occur between layers, reducing transparency, depending on the combination of the transparent insulating layer in the transparent FPC and the layer to be laminated therewith. Taking such concerns into account, there was room for further study of the transparency of the device as a whole.
[0010] The object of the present invention is to provide a laminate of a conductor layer and a polyimide layer (insulating resin layer), which has excellent heat resistance, dimensional stability represented by a coefficient of thermal expansion, flexibility, adhesion, and also high transparency, making it suitable for use as a wiring board, and which can also be used in new applications such as a transparent FPC by laminating it with a transparent barrier layer or various functional layers. [Means for solving the problem]
[0011] As a result of extensive investigations into solving the above problems, the inventors discovered that the above problems could be solved by using a specific resin structure in the polyimide layer in contact with the conductor layer, and thus completed the present invention.
[0012] That is, the present invention is as follows. [1] A conductor-polyimide laminate comprising an insulating resin layer and a conductor layer laminated on at least one surface of the insulating resin layer, the insulating resin layer includes a plurality of polyimide layers and has a yellowness index of 20 or less, and at least one polyimide layer (P1) is directly laminated on the conductor layer; A conductor-polyimide laminate, characterized in that the polyimide layer (P1) satisfies the following conditions a) and b): a) The diamine residues derived from the diamine compound represented by the following general formula (A1) constitute 10 mol % or more of the total diamine residues. b) The content of tetracarboxylic acid anhydride residues derived from a tetracarboxylic acid anhydride compound represented by the following general formula (B1) is 10 mol % or more relative to the total tetracarboxylic acid anhydride residues. [ka] [In formula (A1), R is independently a halogen atom, an alkyl group or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or a phenyl group or a phenoxy group which may be substituted with a monovalent hydrocarbon group or an alkoxy group having 1 to 6 carbon atoms; Z is independently a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, and -SO2-, and at least one Z is -SO2-; n1 is an integer of 0 to 3, and n2 is an integer of 0 to 4.] [ka] [2] The conductor-polyimide laminate according to [1], characterized in that the thermal expansion coefficient of the entire insulating resin layer is within the range of 10 ppm / K or more and 30 ppm / K or less. [3] The conductor-polyimide laminate according to [1] or [2], wherein the insulating resin layer as a whole has a total light transmittance of 80% or more. [4] The conductor-polyimide laminate according to any one of [1] to [3], wherein the insulating resin layer as a whole has a 1% weight loss temperature of 450° C. or higher. [5] The conductor-polyimide laminate according to any one of [1] to [4], characterized in that the thickness of the polyimide layer directly laminated to the conductor layer is 1% or more and less than 50% of the total thickness of the insulating resin layer. [6] The conductor-polyimide laminate according to any one of [1] to [5], wherein the insulating resin layer has a total thickness of 3 μm or more and 20 μm or less. [7] The conductor-polyimide laminate according to any one of [1] to [6], wherein the 180° peel strength between the insulating resin layer and the conductor layer is 0.3 kN / m or more. [8] The conductor-polyimide laminate according to any one of [1] to [7], characterized in that a polyimide layer (P2) which is not directly laminated to a conductor layer among the polyimide layers consisting of the multiple layers contains 20 mol % or more of diamine residues derived from a diamine compound represented by the following general formula (A2) relative to the total diamine residues: [ka] [In formula (A2), R 2 each independently represents a fluorine atom or an alkyl or alkoxy group having 1 to 3 carbon atoms which may be substituted by a fluorine atom, and p and q each independently represent an integer of 0 to 4. [9] The conductor-polyimide laminate according to any one of [1] to [8], wherein the polyimide layer (P1) has a refractive index of more than 1.54 and not more than 1.75. Effect of the Invention
[0013] The conductor-polyimide laminate of the present invention has excellent heat resistance, dimensional stability, adhesiveness, flexibility and high transparency, and is therefore suitable for use as an insulating material for producing electronic components such as FPCs, particularly for transparent FPCs that require colorless transparency and are accompanied by the mounting of semiconductor elements. It can also be used in new applications of transparent FPCs, such as laminating with a transparent barrier layer or a functional layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described.
[0015] <Laminate> The laminate of the present embodiment includes an insulating resin layer and a conductor layer laminated on at least one surface of the insulating resin layer. The laminate of the present embodiment may have the conductor layer on one side of the insulating resin layer, or may have the conductor layers on both sides of the insulating resin layer. The insulating resin layer and the conductor layer constituting the laminate and the method of forming the laminate will be further described below.
[0016] <Insulating resin layer> The insulating resin layer in the laminate of the present embodiment includes a plurality of polyimide layers. By having a plurality of polyimide layers, the insulating resin layer can be excellent in physical properties such as heat resistance, adhesiveness, flexibility, and transparency. Note that the insulating resin layer may include layers other than the polyimide layer, and may include transparent resin layers such as perfluoroalkoxyalkane (PFA), liquid crystal polymer (LCP), and polyethylene terephthalate (PET) depending on the application, but is not limited to these. The multiple polyimide layers may have a two-layer structure of a polyimide layer (P1) that is directly laminated on the conductor layer and a polyimide layer (P2) that is not directly laminated on the conductor layer. It is preferably a three-layer structure, and more preferably, the third polyimide layer (P3) is laminated in the order of (P1) / (P2) / (P3). The polyimide layer (P1) that is directly laminated on the conductor layer and the third polyimide layer (P3) may have the same composition. For example, when multiple polyimide layers are formed by a casting method, a two-layer structure in which the polyimide layer (P1) that is directly laminated on the conductor layer from the cast surface side and the polyimide layer (P2) that is not directly laminated on the conductor layer are laminated in this order may be used, or a three-layer structure in which the polyimide layer (P1) that is directly laminated on the conductor layer from the cast surface side and the polyimide layer (P2) that is not directly laminated on the conductor layer and the third polyimide layer (P3) are laminated in this order may be used. The "cast surface" referred to here refers to the surface on the support side when forming the polyimide layer. The support may be a conductor layer of a laminate, glass, etc., or a support used when forming a gel film, etc. In the multiple polyimide layers, the surface opposite to the cast surface is described as the "laminate surface," but unless otherwise specified, a conductor layer may or may not be laminated on the laminate surface.
[0017] The polyimide constituting the polyimide layer (P1) and the polyimide layer (P3) is preferably a thermoplastic polyimide, which improves the adhesiveness as an insulating resin layer and is suitable for use as an adhesive layer for a conductor layer.
[0018] A preferred embodiment of the insulating resin layer has a thermoplastic polyimide layer (P1) and a non-thermoplastic polyimide layer (P2) made of a non-thermoplastic polyimide, and at least one of the non-thermoplastic polyimide layers (P2) has a polyimide layer (P1) that becomes a thermoplastic polyimide layer. That is, the polyimide layer (P1) is preferably provided on one or both sides of the non-thermoplastic polyimide layer.
[0019] The non-thermoplastic polyimide layer constitutes a polyimide layer with low thermal expansion, and the thermoplastic polyimide layer constitutes a polyimide layer with high thermal expansion. Here, the low thermal expansion polyimide layer refers to a polyimide layer having a coefficient of thermal expansion (CTE) preferably in the range of 1 ppm / K to 25 ppm / K, more preferably in the range of 3 ppm / K to 25 ppm / K. The high thermal expansion polyimide layer refers to a polyimide layer having a CTE preferably in the range of 35 ppm / K or more, more preferably in the range of 35 ppm / K to 80 ppm / K, and even more preferably in the range of 35 ppm / K to 70 ppm / K. The polyimide layer can be made to have a desired CTE by appropriately changing the combination of raw materials used, the thickness, and the drying and curing conditions. Here, the non-thermoplastic polyimide generally refers to a polyimide that does not soften or exhibit adhesiveness even when heated. In this embodiment, the storage modulus at 30° C. measured using a dynamic mechanical analyzer (DMA) is 1.0×10 9 Pa or more, and the storage modulus at 350°C is 1.0×10 8 The term "thermoplastic polyimide" refers to a polyimide having a storage modulus of 1.0×10 Pa or more at 30° C. as measured by DMA. In addition, the term "thermoplastic polyimide" generally refers to a polyimide having a clearly identifiable glass transition temperature (Tg). In this embodiment, the term "thermoplastic polyimide" refers to a polyimide having a storage modulus of 1.0×10 Pa or more at 30° C. as measured by 9 Pa, and the storage modulus at 350°C is 1.0×10 8 This refers to polyimides with a modulus of less than Pa.
[0020] <Diamine Residue Used in Polyimide Layer P1> The polyimide layer P1 in contact with the conductor layer has diamine residues derived from a diamine compound and tetracarboxylic anhydride residues derived from a tetracarboxylic anhydride compound, and contains 10 mol % or more of diamine residues derived from a diamine compound represented by the following general formula (A1) (sometimes simply referred to as "A1 residues". The same applies to the subsequent compounds) relative to the total diamine residues. [ka]
[0021] In the above formula (A1), R is independently a halogen atom, an alkyl group or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or a phenyl group or a phenoxy group which may be substituted with a monovalent hydrocarbon group or an alkoxy group having 1 to 6 carbon atoms, and Z is independently a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, and -SO2-, and at least one Z is -SO2-. n1 is an integer of 0 to 3, and n2 is an integer of 0 to 4. Here, "independently" means that a plurality of substituents R, a divalent group Z, and further an integer n1 may be the same or different. The same applies to other chemical formulas and substituents, etc., which follow. In the above formula (A1), the hydrogen atoms in the two amino groups at the ends may be substituted, for example, -NR3R4 (wherein R3 and R4 are independently any substituent such as an alkyl group). The same applies to other diamine compounds which follow.
[0022] The diamine residue derived from the diamine compound represented by the above formula (A1) contains at least two benzene rings, which are bonded by a flexible bond such as an ether bond, and at least one of the bond sites Z contains -SO2-. Therefore, the refractive index can be increased due to the electron-rich nature of the -SO2- site, and the bent structure exhibits adhesion to the conductor layer. Furthermore, since the diamine residue contains multiple benzene rings, the proportion of imide groups in the polymer can be suppressed, and the effect of exhibiting transparency can be expected. From this perspective, the diamine residue used in the polyimide layer P1 contains 10 mol % or more of A1 residues relative to the total of all diamine residues, 100 mol %. It is preferable to contain it within the range of 30 to 100 mol %, more preferably within the range of 50 to 100 mol %, and even more preferably within the range of 75 to 100 mol %. If it is less than 10 mol %, the refractive index cannot be sufficiently ensured, and when laminated with a functional layer, there is a risk of the light transmittance decreasing due to interlayer reflection.
[0023] Preferred specific examples of the A1 residue include diamine residues derived from diamine compounds such as bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS) and 4,4'-diaminodiphenylsulfone (DDS). Among these, the diamine residue derived from bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS) is particularly preferred.
[0024] As long as the effect of the present invention is not impaired, the polyimide layer P1 in contact with the conductor layer may contain, as a diamine residue other than those mentioned above, a diamine residue derived from a diamine component generally used in the synthesis of polyimides. Examples of other diamine residues include 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-divinyl-4,4'-diaminobiphenyl (VAB), 4,4'-diaminobiphenyl, p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), 3,4'-diaminobenzophenone, (3,3'-bisamino)diphenylamine, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 3-[4 Examples of structural units include those derived from -(4-aminophenoxy)phenoxy]benzenamine, 3-[3-(4-aminophenoxy)phenoxy]benzenamine, 1,3-bis(3-aminophenoxy)benzene (APB), bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]ketone (BAPK), bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, etc. Among these, 1,3-bis(3-aminophenoxy)benzene (APB) and 1,3-bis(4-aminophenoxy)benzene (TPE-R) are preferred.
[0025] <Acid anhydride residue used in polyimide layer P1> The polyimide layer P1 in contact with the conductor layer contains 10 mol % or more of tetracarboxylic acid anhydride residues derived from a tetracarboxylic acid anhydride compound represented by the following general formula (B1) relative to the total tetracarboxylic acid anhydride residues (which may be simply referred to as "acid anhydride residues", etc.). [ka]
[0026] The tetracarboxylic anhydride residue derived from the tetracarboxylic anhydride represented by the above formula (B1) has a structure in which two phenyl groups are bonded by an ether bond, and therefore when an imide structure is formed with a diamine, the electron-accepting property of the acid anhydride residue is suppressed, and charge transfer interaction is suppressed, and transparency can be expected. Furthermore, since the ether bond can impart moderate flexibility to the polymer chain, adhesiveness with the conductor layer can also be expected to be exhibited. From this viewpoint, the acid anhydride residue used in the polyimide layer P1 preferably contains 10 mol % or more of B1 residues relative to the total of 100 mol % of all acid anhydride residues, more preferably 30 to 100 mol %, and even more preferably 50 to 100 mol %. It is further preferable to contain 75 to 100 mol %. If it is less than 10 mol %, the yellowness index (YI) may deteriorate.
[0027] Preferred specific examples of the B1 residue include 4,4'-oxydiphthalic anhydride (ODPA) and 3,4'-oxydiphthalic anhydride, with 3,4'-oxydiphthalic anhydride being more preferred.
[0028] As long as the effect of the present invention is not impaired, the polyimide layer P1 in contact with the conductor layer may contain, as an acid anhydride residue other than the above, an acid anhydride residue derived from an acid anhydride component generally used in the synthesis of polyimides. As such an acid anhydride residue, an aromatic tetracarboxylic acid residue is preferred. In addition, an alicyclic tetracarboxylic acid residue may be contained, and examples of the acid anhydride residue that may be preferably mentioned include an acid anhydride residue derived from an alicyclic tetracarboxylic acid dianhydride such as 1,2,3,4-cyclobutane tetracarboxylic dianhydride, fluorenylidene bisphthalic anhydride, 1,2,4,5-cyclohexane tetracarboxylic dianhydride, and cyclopentanone bisspironorbornane tetracarboxylic dianhydride.
[0029] Other acid anhydride residues include, for example, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, naphthalene-1,2,5,6-tetracarboxylic dianhydride, naphthalene-1,2,4,5-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, naphthalene-1,2,6,7-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene, and the like. 1,2,5,6-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,2',3,3'-biphenyl Tetracarboxylic acid dianhydrides, 2,3,3',4'-biphenyltetracarboxylic acid dianhydride, 3,3'',4,4''-p-terphenyltetracarboxylic acid dianhydride, 2,2'',3,3''-p-terphenyltetracarboxylic acid dianhydride, 2,3,3'',4''-p-terphenyltetracarboxylic acid dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride phenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, perylene-2,3,8,9-tetracarboxylic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, perylene-4,5,10,11-tetracarboxylic dianhydride, perylene-5,6,11,12-tetracarboxylic dianhydride, phenanthrene-1,2,7,8-tetracarboxylic dianhydride, phenanthrene-1, 2,6,7-tetracarboxylic dianhydride, phenanthrene-1,2,9,10-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, (trifluoromethyl)pyromellitic dianhydride, di(trifluoromethyl)pyromellitic dianhydride, di(heptafluoropropyl)pyromellitic dianhydride, pentafluoroethylpyromellitic dianhydride, bis{3,5-di(trifluoromethyl)phenoxy}pyromellitic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'- Tetracarboxybiphenyl dianhydride, 2,2',5,5'-tetrakis(trifluoromethyl)-3,3',4,4'-tetracarboxybiphenyl dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'-tetracarboxydiphenyl ether dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'-tetracarboxybenzophenone dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}benzene dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}trifluoromethylbenzene dianhydride, bis(dicarboxyphenoxy)trifluoromethylbenzene dianhydride, bis(dicarboxyphenoxy)bis(trifluoromethyl)benzene dianhydride, bis(dicarboxyphenoxy)tetrakis(trifluoromethyl)benzene dianhydride, 2,2-bis{(4-(3,Examples of the acid anhydride residues derived from 4-dicarboxyphenoxy)phenyl}hexafluoropropane dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}biphenyl dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}bis(trifluoromethyl)biphenyl dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}diphenyl ether dianhydride, bis(dicarboxyphenoxy)bis(trifluoromethyl)biphenyl dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, fluorenylidene bisphthalic anhydride, and 1,2,4,5-cyclohexane tetracarboxylic dianhydride are listed. Among these, the acid anhydride residues derived from 3,3',4,4'-biphenyl tetracarboxylic dianhydride are preferred because they can impart strength and flexibility to the polyimide film.
[0030] <Refractive index> In addition, the refractive index of the polyimide layer (P1) directly laminated on the conductor layer is preferably in the range of more than 1.54 and not more than 1.75. More preferably, it is in the range of 1.60 to 1.75, and even more preferably, it is in the range of 1.65 to 1.75. By adjusting the refractive index to the above range, even in applications where a transparent barrier layer or a functional layer is provided, the refractive index of a general polyimide can be applied to the polyimide layer (P2) that is not directly laminated while suppressing interlayer reflection with those layers, so that the degree of freedom in design can be increased. As an example, when the laminate of the present invention is to be applied to applications such as glass antennas and embedding antennas in displays, a laminate structure with a barrier layer that protects wiring and a transparent conductive layer such as an ITO film may be used. For example, in the case of an ITO film, the refractive index is large compared to about 1.7 to 2.3 depending on the wavelength, and it is assumed that the difference in refractive index from the refractive index of a general polyimide (about 1.5) may be large. Therefore, by setting the refractive index of at least the polyimide layer P1 in the above range, it is possible to suppress the decrease in light transmittance during device formation due to reflection caused by the difference in refractive index between layers. There is no particular limitation on the method of controlling the refractive index, and examples include a method of increasing the refractive index to be higher than that of general polyimides by including an inorganic filler with a high refractive index or controlling the resin structure. A method of increasing the refractive index by including the A1 residue in the resin structure and increasing the content ratio of the A1 residue is preferable. A method of increasing the refractive index by including the B1 residue at the same time and increasing the total content ratio of the A1 residue and the B1 residue is more preferable.
[0031] <Diamine used in polyimide layer P2> The polyimide layer P2, which is not directly laminated on the conductor layer, preferably contains a fluorine-containing diamine residue. The fluorine-containing diamine residue has a bulky fluorine atom-containing group, which reduces interactions such as π-π stacking between polymer chains and makes charge transfer (CT) between the aromatic tetracarboxylic acid residue and the aromatic diamine residue less likely to occur, which is thought to make the polyimide closer to colorless transparency.
[0032] Among the fluorine-containing diamine residues, it is more preferable to contain a diamine residue derived from a diamine compound represented by general formula (A2). [ka]
[0033] In the above formula (A2), R 2 each independently represents a fluorine atom or an alkyl or alkoxy group having 1 to 3 carbon atoms which may be substituted by a fluorine atom; p and q each independently represent an integer of 0 to 4.
[0034] The diamine represented by the above formula (A2) has excellent heat resistance because it is mainly composed of an aromatic skeleton, and has excellent transparency due to its fluorine-containing structure. Furthermore, it is expected to have the effect of lowering the coefficient of thermal expansion (CTE) by orienting the molecules. 2From the viewpoint of the heat resistance, is preferably a fluorine atom or a fluorine atom-substituted methyl group. From this viewpoint, the diamine residues used in the polyimide layer P2 preferably contain 20 mol % or more of A2 residues relative to the total of all diamine residues (100 mol %), more preferably in the range of 50 to 100 mol %, and even more preferably in the range of 75 to 100 mol %. By keeping the A2 residues in the above range, it is possible to prevent an increase in the CTE of the entire polyimide layer and suppress the occurrence of warpage.
[0035] Specific examples include structural units derived from the following formulas (A2-1) to (A2-4).
[0036] [ka]
[0037] Among the above formulas (A2-1) to (A2-4), formula (A2-1) which is a structural unit derived from 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB) is more preferred.
[0038] The polyimide layer P2 may contain, as a diamine residue other than those mentioned above, a diamine residue derived from a diamine component generally used in the synthesis of polyimides. Examples of such diamine components include 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenylsulfide, 3,3'-diaminodiphenylsulfone, 3,3-diaminodiphenylether, 3,4'-diaminodiphenylether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenylsulfide, 3,4'-diaminobenzophenone, (3,3'-bisamino)diphenyl Amines, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene (APB), 1,3-bis(4-aminophenoxy)benzene (TPE-R), 3-[4-(4-aminophenoxy)phenoxy]benzenamine, 3-[3-(4-aminophenoxy)phenoxy]benzenamine, 4,4'-[2-methyl-(1,3-phenylene)bisoxy]bisaniline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy]bisaniline, 4 ,4'-[5-methyl-(1,3-phenylene)bisoxy]bisaniline, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, bis[4,4'-(3-aminophenoxy)]benzanilide, 4-[3-[4-(4-aminophenoxy)pheno Examples of such bis[4-(4-aminophenoxy)]aniline, 4,4'-[oxybis(3,1-phenyleneoxy)]bisaniline, bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]ketone (BAPK), bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, 2,2-bis(4-aminophenoxyphenyl)propane (BAPP), and 4,4'-diaminodiphenyl ether.Among these, 1,3-bis(3-aminophenoxy)benzene (APB) and 1,3-bis(4-aminophenoxy)benzene (TPE-R) are preferable.
[0039] <Acid anhydride used in polyimide layer P2> The polyimide layer P2 preferably contains 10 mol % or more of the acid anhydride residues derived from the acid anhydride compound represented by the general formula (B2) based on the total acid anhydride residues.
[0040] [ka]
[0041] In the above formula (B2), X represents a divalent group selected from a single bond, -O-, or -C(CF3)2-.
[0042] The aromatic tetracarboxylic anhydride represented by the above formula (B2) has an X group that contributes to bending, and therefore imparts flexibility to the polyimide, improves the tensile strength of the insulating resin layer, and reduces interactions such as π-π stacking between polymer chains, making charge transfer (CT) between the aromatic tetracarboxylic acid residue and the aromatic diamine residue less likely to occur, which is thought to enable the resulting polyimide to approach colorless transparency.
[0043] Examples of aromatic tetracarboxylic anhydrides represented by the above formula (B2) include 4,4'-oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), and 2,2-bis(3,4-dicarboxyphenyl)-hexafluoropropane dianhydride (6FDA). These aromatic tetracarboxylic anhydrides are preferred because they can impart strength and flexibility to the polyimide film, have excellent heat resistance and transparency, and can control the CTE within an appropriate range. Among these, ODPA and 6FDA are particularly preferred.
[0044] The polyimide layer P2 preferably contains a fluorine-containing acid anhydride residue, which has a bulky fluorine atom-containing group and therefore reduces interactions such as π-π stacking between polymer chains and makes charge transfer (CT) between aromatic tetracarboxylic acid residues and aromatic diamine residues less likely to occur, which is believed to make the polyimide closer to colorless and transparent.
[0045] In addition, in order to control the CTE of the polyimide layer within the above range, the polyimide layer P2 preferably contains a tetravalent acid anhydride residue (hereinafter, sometimes referred to as "PMDA residue") derived from pyromellitic dianhydride (PMDA) represented by the following formula (B3). The PMDA residue is preferably contained in an amount of 50 molar parts or more, more preferably in the range of 60 to 100 molar parts, relative to a total of 100 molar parts of all acid anhydride residues. When the PMDA residue is in the above range, it is possible to prevent the CTE of the polyimide layer from becoming too high and suppress a decrease in dimensional stability.
[0046] [ka]
[0047] The polyimide layer P2 may contain, as an acid anhydride residue other than the above, an acid anhydride residue derived from an acid anhydride component generally used in the synthesis of polyimides. As such an acid anhydride residue, an aromatic tetracarboxylic acid residue is preferable. In addition, the polyimide layer P2 may contain an alicyclic tetracarboxylic acid residue, and preferable examples thereof include an acid anhydride residue derived from an alicyclic tetracarboxylic acid dianhydride such as 1,2,3,4-cyclobutane tetracarboxylic acid dianhydride, fluorenylidene bisphthalic anhydride, 1,2,4,5-cyclohexane tetracarboxylic acid dianhydride, and cyclopentanone bisspironorbornane tetracarboxylic acid dianhydride.
[0048] Other acid anhydride residues include, for example, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, naphthalene-1,2,5,6-tetracarboxylic dianhydride, naphthalene-1,2,4,5-tetracarboxylic dianhydride, naphthalene-1,4,5,8-tetracarboxylic dianhydride, naphthalene-1,2,6,7-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene, and the like. 1,2,5,6-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 2,2',3,3'-biphenyl Tetracarboxylic acid dianhydrides, 2,3,3',4'-biphenyltetracarboxylic acid dianhydride, 3,3'',4,4''-p-terphenyltetracarboxylic acid dianhydride, 2,2'',3,3''-p-terphenyltetracarboxylic acid dianhydride, 2,3,3'',4''-p-terphenyltetracarboxylic acid dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride phenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, perylene-2,3,8,9-tetracarboxylic dianhydride, perylene-3,4,9,10-tetracarboxylic dianhydride, perylene-4,5,10,11-tetracarboxylic dianhydride, perylene-5,6,11,12-tetracarboxylic dianhydride, phenanthrene-1,2,7,8-tetracarboxylic dianhydride, phenanthrene-1, 2,6,7-tetracarboxylic dianhydride, phenanthrene-1,2,9,10-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, (trifluoromethyl)pyromellitic dianhydride, di(trifluoromethyl)pyromellitic dianhydride, di(heptafluoropropyl)pyromellitic dianhydride, pentafluoroethylpyromellitic dianhydride, bis{3,5-di(trifluoromethyl)phenoxy}pyromellitic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'- Tetracarboxybiphenyl dianhydride, 2,2',5,5'-tetrakis(trifluoromethyl)-3,3',4,4'-tetracarboxybiphenyl dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'-tetracarboxydiphenyl ether dianhydride, 5,5'-bis(trifluoromethyl)-3,3',4,4'-tetracarboxybenzophenone dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}benzene dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}trifluoromethylbenzene dianhydride, bis(dicarboxyphenoxy)trifluoromethylbenzene dianhydride, bis(dicarboxyphenoxy)bis(trifluoromethyl)benzene dianhydride, bis(dicarboxyphenoxy)tetrakis(trifluoromethyl)benzene dianhydride, 2,2-bis{(4-(3,Examples of the acid anhydride residues derived from 4-dicarboxyphenoxy)phenyl}hexafluoropropane dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}biphenyl dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}bis(trifluoromethyl)biphenyl dianhydride, bis{(trifluoromethyl)dicarboxyphenoxy}diphenyl ether dianhydride, bis(dicarboxyphenoxy)bis(trifluoromethyl)biphenyl dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, fluorenylidene bisphthalic anhydride, and 1,2,4,5-cyclohexane tetracarboxylic dianhydride are listed. Among these, the acid anhydride residues derived from 3,3',4,4'-biphenyl tetracarboxylic dianhydride are preferred because they can impart strength and flexibility to the polyimide film and the coefficient of thermal expansion (CTE) of the polyimide film does not increase too much and can be controlled within an appropriate range.
[0049] <Polyimide layer P3> The polyimide layer P3 is not particularly limited, and may have the same composition as the polyimide layer P1. When a composition different from that of the polyimide layer P1 is applied, it is preferable that the polyimide layer P3 contains 50 mol % or more of a diamine residue derived from an aromatic diamine compound represented by general formula (A3). [ka]
[0050] In the above formula (A3), Z independently represents a divalent group selected from -O-, -S-, -CH2-, -CH(CH3)-, -C(CH3)2-, or -SO2-, and is preferably -O-. n2 represents an integer of 0 to 4, and is preferably 0 or 1. R represents a substituent, and independently represents a halogen atom, an alkyl group or alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or a phenyl group or phenoxy group which may be substituted with a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms. n1 independently represents an integer of 0 to 3, and is preferably 0 or 1.
[0051] The aromatic diamine compound represented by the above formula (A3) has two or more benzene rings, and the presence of amino groups and divalent linking group Z directly bonded to at least two of the benzene rings increases the degree of freedom of the polyimide molecular chain, resulting in high flexibility. This is thought to contribute to improving the flexibility of the polyimide molecular chain and promote increased adhesion and toughness.
[0052] In addition, when a composition different from that of the polyimide layer P1 is applied to the polyimide layer P3, it is preferable that the polyimide layer P3 contains 50 mol % or more of acid anhydride residues derived from an aromatic tetracarboxylic acid anhydride represented by the general formula (B2) relative to the total acid anhydride residues, and that the polyimide contains 50 mol % or more of diamine residues derived from an aromatic diamine compound represented by the general formula (A3) relative to the total diamine residues contained in the polyimide.
[0053] Examples of the aromatic diamine compound represented by the above formula (A3) include 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,3-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenyl sulfide, 3,4'-diaminobenzophenone, (3,3' -bis(amino)diphenylamine, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene (APB), 1,3-bis(4-aminophenoxy)benzene (TPE-R), 3-[4-(4-aminophenoxy)phenoxy]benzenamine, 3-[3-(4-aminophenoxy)phenoxy]benzenamine, 4,4'-[2-methyl-(1,3-phenylene)bisoxy]bisaniline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy] Bisaniline, 4,4'-[5-methyl-(1,3-phenylene)bisoxy]bisaniline, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, bis[4,4'-(3-aminophenoxy)]benzanilide, 4-[3-[4-(4-aminophenoxy )phenoxy]phenoxy]aniline, 4,4'-[oxybis(3,1-phenyleneoxy)]bisaniline, bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]ketone (BAPK), bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, 2,2-bis(4-aminophenoxyphenyl)propane (BAPP), 4,4'-diaminodiphenyl ether, etc. Among these, 1,3-bis(3-aminophenoxy)benzene (APB) and 1,3-bis(4-aminophenoxy)benzene (TPE-R) are preferred.
[0054] Other diamine residues include, for example, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), bis[4-(aminophenoxy)phenyl]sulfone (BAPS), 4,6-dimethyl-m-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, 2,4-diaminomesitylene, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,5,3',5'-tetramethyl-4,4'-diaminodiphenylmethane, 2,4-toluenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 4,4'-diaminodiphenylethane, 3,3'-diaminodiphenylethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl) 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, benzidine, 3,3'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 4,4"-diamino-p-terphenyl, 3,3"-diamino-p-terphenyl, bis(p-aminocyclohexyl)methane, bis(p-β-amino-t-butylphenyl)ether ter, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-t-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylylenediamine, p-xylylenediamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4- Oxadiazole, piperazine, 4-(1H,1H,11H-eicosafluoroundecanoxy)-1,3-diaminobenzene, 4-(1H,1H-perfluoro-1-butanoxy)-1,3-diaminobenzene, 4-(1H,1H-perfluoro-1-heptanoxy)-1,3-diaminobenzene, 4-(1H,1H-perfluoro-1-octanoxy)-1,3-diaminobenzene, 4-pentafluorophenoxy-1,3-diaminobenzene, 4-(2,3,5,6-tetrafluorophenoxy)-1,3-diaminobenzene, 4-(4-furanoxyl)-1,3-diaminobenzene, 1,3-diaminobenzene, 4-(1H,1H,2H,2H-perfluoro-1-hexanoxy)-1,3-diaminobenzene, 4-(1H,1H,2H,2H-perfluoro-1-dodecanoxy)-1,3-diaminobenzene, (2,5)-diaminobenzotrifluoride, diaminotetra(trifluoromethyl)benzene, diamino(pentafluoroethyl)benzene, 2,5-diamino(perfluorohexyl)benzene, 2,5-diamino(perfluorobutyl)benzene, 2,2'-bis(trifluoromethyl)benzene -4,4'-diaminobiphenyl, 3,3'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, octafluorobenzidine, 4,4'-diaminodiphenyl ether, 2,2-bis(4-aminophenyl)hexafluoropropane, 1,3-bis(anilino)hexafluoropropane, 1,4-bis(anilino)octafluorobutane, 1,5-bis(anilino)decafluoropentane, 1,7-bis(anilino)tetradecafluoroheptane, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 3,3'-Bis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 3,3',5,5'-tetrakis(trifluoromethyl)-4,4'-diaminodiphenyl ether, 3,3'-bis(trifluoromethyl)-4,4'-diaminobenzophenone, 4,4'-diamino-p-terphenyl, 1,4-bis(p-aminophenyl)benzene, p-(4-amino-2-trifluoromethylphenoxy)benzene, bis(aminophenoxy)bis(trifluoro Bis(aminophenoxy)tetrakis(trifluoromethyl)benzene, 2,2-bis{4-(4-aminophenoxy)phenyl}hexafluoropropane, 2,2-bis{4-(3-aminophenoxy)phenyl}hexafluoropropane, 2,2-bis{4-(2-aminophenoxy)phenyl}hexafluoropropane, 2,2-bis{4-(4-aminophenoxy)-3,5-dimethylphenyl}hexafluoropropane, 2,2- Examples of the diamine residue derived from bis{4-(4-aminophenoxy)-3.5-ditrifluoromethylphenyl}hexafluoropropane, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-3-trifluoromethylphenoxy)biphenyl, 4,4'-bis(4-amino-2-trifluoromethylphenoxy)diphenyl sulfone, 4,4'-bis(3-amino-5-trifluoromethylphenoxy)diphenyl sulfone, 2,2-bis{4-(4-amino-3-trifluoromethylphenoxy)phenyl}hexafluoropropane, bis{(trifluoromethyl)aminophenoxy}biphenyl, bis[{(trifluoromethyl)aminophenoxy}phenyl]hexafluoropropane, bis{2-[(aminophenoxy)phenyl]hexafluoroisopropyl}benzene, and 4,4'-bis(4-aminophenoxy)octafluorobiphenyl are mentioned. Among these, from the viewpoint of producing a polyimide having high transparency and a low degree of coloration, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,Diamine residues derived from diamine compounds such as 4'-bis(2-(trifluoromethyl)-4-aminophenoxy)biphenyl, 2,2-bis(4-(2-(trifluoromethyl)-4-aminophenoxy)phenyl)hexafluoropropane, 4,4'-bis(3-(trifluoromethyl)-4-aminophenoxy)biphenyl, 4,4'-bis(3-(trifluoromethyl)-4-aminophenoxy)biphenyl, and p-bis(2-trifluoromethyl)-4-aminophenoxy]benzene are preferred.
[0055] By selecting the types of the acid anhydride residues and diamine residues and the molar ratios of two or more types of acid anhydride residues or diamine residues, it is possible to control the toughness, thermal expansion properties, adhesiveness, glass transition temperature (Tg), and the like.
[0056] <Polyimide synthesis method> Next, a method for synthesizing the polyimide constituting the polyimide layer will be described. The polyimide of the present embodiment can be produced by reacting the acid anhydride and diamine in a solvent to generate polyamic acid, followed by heating to close the ring. For example, the acid anhydride component and the diamine component are dissolved in an organic solvent in approximately equal moles, and the mixture is stirred at a temperature in the range of 0 to 100°C for 30 minutes to 24 hours to polymerize, thereby obtaining polyamic acid, which is a precursor of polyimide. In the reaction, the reaction components are dissolved so that the precursor generated is in the range of 5 to 30% by weight, preferably in the range of 10 to 20% by weight, in the organic solvent. Examples of organic solvents used in the polymerization reaction include N,N-dimethylformamide, N,N-dimethylacetamide (DMAC), N-methyl-2-pyrrolidone, 2-butanone, dimethyl sulfoxide, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diglyme, triglyme, and γ-butyrolactone. Two or more of these solvents can be used in combination, and further, aromatic hydrocarbons such as xylene and toluene can be used in combination. The amount of such an organic solvent used is not particularly limited, but it is preferable to adjust the amount used so that the concentration of the polyamic acid solution (polyimide precursor solution) obtained by the polymerization reaction is about 5 to 30% by weight.
[0057] In the synthesis of polyimide, the above-mentioned acid anhydrides and diamines may be used alone or in combination of two or more. By selecting the types of acid anhydrides and diamines, or the molar ratios of two or more acid anhydrides or diamines, the thermal expansion, adhesiveness, glass transition temperature, etc. can be controlled.
[0058] In addition, the polyimide of the present embodiment may use a terminal blocking agent. As the terminal blocking agent, monoamines or dicarboxylic acids are preferable. The amount of the terminal blocking agent to be introduced is preferably 0.0001 to 0.1 mol per 1 mol of the acid anhydride component, and particularly preferably 0.001 to 0.05 mol. As the monoamine terminal blocking agent, for example, methylamine, ethylamine, propylamine, butylamine, benzylamine, 4-methylbenzylamine, 4-ethylbenzylamine, 4-dodecylbenzylamine, 3-methylbenzylamine, aniline, 4-methylaniline, etc. are recommended. Of these, benzylamine and aniline are preferably used. As the dicarboxylic acid terminal blocking agent, dicarboxylic acids are preferable, and a part of them may be ring-closed. For example, phthalic acid, phthalic anhydride, 4-chlorophthalic acid, tetrafluorophthalic acid, cyclopentane-1,2-dicarboxylic acid, 4-cyclohexene-1,2-dicarboxylic acid, etc. are recommended. Of these, phthalic acid and phthalic anhydride are preferably used.
[0059] The synthesized polyamic acid is usually advantageously used as a reaction solvent solution, but can be concentrated, diluted, or replaced with another organic solvent if necessary. In addition, polyamic acid is advantageously used because it generally has excellent solvent solubility. The method of imidizing polyamic acid is not particularly limited, and for example, a heat treatment in which the polyamic acid is heated in the above-mentioned solvent at a temperature within a range of 80 to 400°C for 1 to 24 hours is preferably used.
[0060] The weight-average molecular weight of the polyamic acid is, for example, preferably in the range of 10,000 to 400,000, more preferably in the range of 50,000 to 350,000. If the weight-average molecular weight is less than 10,000, the strength of the film tends to decrease and it tends to become brittle. On the other hand, if the weight-average molecular weight exceeds 400,000, the viscosity increases excessively, and defects such as unevenness in the film thickness and streaks tend to occur during the coating process.
[0061] <Thickness and thickness ratio> The thickness of the insulating resin layer is preferably within the range of 3 to 20 μm. By controlling the thickness within such a range, high transparency and colorlessness can be improved. Furthermore, if the thickness of the insulating resin layer is less than the lower limit, problems such as the inability to ensure electrical insulation and difficulty in handling during the manufacturing process due to reduced handleability may occur. On the other hand, if the thickness of the insulating resin layer exceeds the upper limit, the dimensional change before and after etching becomes large, and the yellow to yellowish brown coloring becomes stronger, tending to reduce the visibility of the insulating resin layer. The thickness of the insulating resin layer is more preferably within the range of 5 to 12 μm.
[0062] In order to maintain the dimensional stability of the conductor-polyimide laminate of the present embodiment, the high transparency and colorlessness of the insulating resin layer, and improve adhesion to the conductor layer, the thickness of the polyimide layer (P1) in contact with the conductor layer is T1, and the thickness of the polyimide layer (P2) not directly laminated to the conductor layer is T2. The thickness of T1 is preferably in the range of 1 to 4 μm, and the thickness of T2 is preferably in the range of 4 to 19 μm. From another viewpoint, the thickness of T1 is preferably 1% or more and less than 50% of the thickness of the insulating resin layer, and more preferably 1% or more and 30% or less. The thickness of T2 is preferably 60% or more, more preferably 70% or more of the thickness of the insulating resin layer.
[0063] <Physical properties of insulating resin layer> In order to be applicable to the main components of FPC, the insulating resin layer has a heat resistance of a glass transition temperature (Tg) of 280° C. or higher, preferably 350° C. or higher, and more preferably 380° C. or higher.
[0064] The 1% thermal weight loss temperature (TD1) of the insulating resin layer is 450° C. or higher, preferably 470° C. or higher, and more preferably 490° C. or higher. By controlling it within this range, it has sufficient heat resistance even when applied to the main components of FPCs.
[0065] The coefficient of thermal expansion (CTE) of the insulating resin layer is preferably within the range of 10 to 30 ppm / K. By controlling it within such a range, deformation such as curling can be suppressed and high dimensional stability can be ensured. Here, CTE is the average value of the coefficient of thermal expansion in the MD and TD directions of the insulating resin layer.
[0066] For example, the insulating resin layer is preferably applied to transparent FPC applications with a total light transmittance of 80% or more. For example, it is preferable that this is satisfied when the insulating resin layer has a thickness of 10 μm. More preferably, the total light transmittance is 85% or more. By controlling the total light transmittance within this range, clouding due to reflection and scattering of light in the insulating resin layer is suppressed, resulting in excellent transparency. If the total light transmittance is less than 80%, the turbidity increases and the transparency of the insulating resin layer tends to decrease.
[0067] The yellowness index (YI) of the insulating resin layer is preferably 20 or less, more preferably 10 or less, and further preferably 7 or less. For example, it is preferable to satisfy this when the insulating resin layer has a thickness of 10 μm. By controlling the YI within this range, the insulating resin layer can be made almost colorless. On the other hand, if the YI is out of the above range, the yellow to yellowish brown coloration becomes stronger, and the visibility of the insulating resin layer tends to decrease.
[0068] The haze of the insulating resin layer is preferably 3% or less, and more preferably 2% or less. By controlling it to such a range, the visibility of the insulating resin layer can be improved. If the haze exceeds 3%, for example, light scattering is likely to occur. In addition, the haze depends on the surface profile of the insulating resin layer, and even a low-profile insulating resin layer can achieve both adhesive strength and transparency, and can be suitably used, for example, for circuit boards on which fine metal layers are laminated.
[0069] <Method of forming laminate> The method for forming the insulating resin layer in the laminate of the present embodiment is not particularly limited, but examples thereof include: [1] a method in which a polyamic acid solution is applied to a supporting substrate, dried, and then imidized to produce a polyimide resin film (hereinafter, cast method); [2] a method in which a polyamic acid solution is applied to a supporting substrate, dried, and then the polyamic acid gel film is peeled off from the supporting substrate and imidized to produce a polyimide resin film. In addition, when the insulating resin layer is composed of a plurality of polyimide layers, examples of the manufacturing method include: [3] a method in which a polyamic acid solution is applied to a supporting substrate and dried multiple times, and then imidized (hereinafter, sequential coating method); and [4] a method in which a laminated structure of polyamic acid is simultaneously applied to a supporting substrate by multilayer extrusion, dried, and then imidized (hereinafter, multilayer extrusion method). The method for applying a polyimide solution (or polyamic acid solution) to a substrate is not particularly limited, and it is possible to apply it using a coater such as a comma, die, knife, lip, or spin coater. In forming multiple polyimide layers, a method in which a polyimide solution (or a polyamic acid solution) is applied to a substrate and then dried is preferably used.
[0070] The polyimide layer of the present embodiment may contain an inorganic filler in the polyimide layer as necessary, as long as it does not impair the object of the present invention. Specific examples of the inorganic filler include silicon dioxide, aluminum oxide, magnesium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, etc. These may be used alone or in combination of two or more.
[0071] <Conductor layer> The material of the conductor layer in the laminate of the present embodiment is not particularly limited, and examples thereof include copper, stainless steel, iron, nickel, beryllium, aluminum, zinc, indium, silver, gold, tin, zirconium, tantalum, titanium, lead, magnesium, manganese, and alloys thereof. Among these, the metal elements of copper, iron, or nickel, or indium tin oxide (ITO) are preferred. In selecting these conductor layers, the conductor layer is selected so as to exhibit the properties required for the intended use, such as the conductivity of the conductor layer, the light transmittance of the polyimide layer, and the adhesion to the polyimide layer. There is no particular restriction on the shape of the conductor layer, but when used as a transparent antenna or a transparent shielding layer, it is preferable to process the conductor layer into a mesh type. In this case, when a non-transparent conductor layer such as copper is used as the conductor layer, it is preferable to make it into a thin wiring. When used as a raw material for processing the conductor layer into an arbitrary shape, a shape in which the conductor layer is laminated over the entire surface is preferred.
[0072] The thickness of the conductor layer is not particularly limited, but is preferably within the range of 0.1 to 20 μm, and more preferably within the range of 1 to 10 μm.
[0073] In the case of a metal clad laminate in which a metal layer is applied to a conductor layer, the laminate may be prepared, for example, by preparing a resin film containing the polyimide of this embodiment, sputtering a metal onto the resin film to form a seed layer, and then forming a metal layer by, for example, plating.
[0074] In addition, in the case of a metal clad laminate in which a metal layer is applied to a conductor layer, the laminate may be prepared by preparing a resin film containing the polyimide of this embodiment and laminating a metal foil thereon by a method such as thermocompression bonding.
[0075] In the case of a metal clad laminate in which a metal layer is applied to the conductor layer, the surface of the resin film may be subjected to a modification treatment such as a plasma treatment in order to increase the adhesion between the resin film and the metal layer.
[0076] Furthermore, in the case of a metal clad laminate in which a metal layer is applied to a conductor layer, the polyimide layer may be formed by casting a coating solution containing the polyamic acid of the present embodiment onto a metal layer, drying the coating film, and then heat-treating the coating solution to imidize the polyimide layer (casting method). The coating solution containing the polyamic acid of the present embodiment may be cast directly onto the metal layer, or may be cast after forming a coating film containing another polyamic acid.
[0077] In the casting method, the polyamic acid resin layer is imidized while being fixed to the metal foil, so that the expansion and contraction changes of the polyimide layer during the imidization process can be suppressed and the anisotropy in the transport direction (MD) and the width direction (TD) can be reduced, which is a preferred embodiment.
[0078] In the case of a metal clad laminate in which a metal layer is applied to a conductor layer, when a metal clad laminate having metal layers on both sides is manufactured, for example, it can be obtained by laminating a metal layer directly on the polyimide layer of the single-sided metal clad laminate obtained by the above method, or after forming an adhesive layer that does not inhibit the transparency of the insulating resin layer as necessary, by a means such as hot pressing. In addition, the heat pressing temperature when the metal layer is hot pressed is not particularly limited, but it is preferably equal to or higher than the glass transition temperature of the polyimide layer adjacent to the metal layer used. In addition, the heat pressing pressure is 1 to 500 kg / m, depending on the type of pressing equipment used. 2 It is desirable that the range is.
[0079] In the case of a metal clad laminate in which a metal layer is applied to a conductor layer, from the viewpoint of the light transmittance of the insulating resin layer, the ten-point mean roughness Rzjis of the surface of the metal layer is preferably 0.5 μm or less, more preferably in the range of 0.01 to 0.3 μm or less, and even more preferably in the range of 0.01 to 0.2 μm. In particular, by making the ten-point mean roughness Rzjis of the surface of the metal layer 0.2 μm or less, the haze value of the insulating resin layer can be reduced, which is a more preferred embodiment. Also, from the viewpoint of adhesion with the insulating resin layer, the insulating resin layer in contact with the metal layer is a cast surface. It is preferred
[0080] <Peel strength> The 180° peel strength between the insulating resin layer and the conductor layer in the laminate of this embodiment is preferably 0.3 kN / m or more, more preferably 0.5 kN / m. In this specification, the total light transmittance, CTE, and peel strength are measured under the conditions described in the examples, and unless otherwise specified, are measured at room temperature (23°C). EXAMPLES
[0081] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the scope of these examples. In the following examples, various measurements and evaluations are as follows, unless otherwise specified.
[0082] [Calculation of light transmittance and yellowness index (YI)] The yellowness index (YI) of the polyimide film (50 mm x 50 mm) was measured using a Shimadzu UV-3600 spectrophotometer. YI (yellowness) Calculation was performed based on the following formula (1) in accordance with JIS Z 8722. YI=100×(1.2879X-1.0592Z) / Y (1) X, Y and Z: Tristimulus values of the test piece The YI (T10) of the polyimide film having a thickness of 10 μm was calculated by substituting the value of YI calculated by the above formula (1) into the following formula (2). YI(T10)=YI / T×10 (2) T: Polyimide film thickness (μm)
[0083] [Measurement of coefficient of thermal expansion (CTE)] A polyimide film (3 mm x 15 mm) was heated from 30°C to 280°C at a heating rate of 10°C / min while applying a load of 5.0 g in a thermomechanical analysis (TMA) device, and then cooled. The thermal expansion coefficient was measured from the elongation (linear expansion) of the polyimide film from 250°C to 100°C as the temperature was lowered.
[0084] [Measurement of thermal decomposition temperature (Td1)] A polyimide film weighing 10 to 20 mg was heated from 30°C to 550°C at a constant rate in a nitrogen atmosphere using a Seiko thermogravimetric analyzer (TG) TG / DTA6200, and the weight change was measured. The weight at 200°C was set to zero, and the temperature at which the weight loss rate was 1% was defined as the thermal decomposition temperature (Td1).
[0085] [Calculation of total light transmittance (TT) and haze (turbidity)] The total light transmittance (TT) and haze (turbidity) of the polyimide film (50 mm x 50 mm) were measured in accordance with JIS K7136 using a haze meter NDH500 manufactured by Nippon Denshoku Industries Co., Ltd. For the insulating resin layer of the metal clad laminate, a polyimide film was prepared by etching one or both sides of the metal foil, and this was measured in the same manner.
[0086] [Viscosity measurement] The viscosity of the polyamic acid solution obtained in the synthesis example was measured at 25° C. using a cone-plate viscometer equipped with a thermostatic water bath (manufactured by Tokimec Co., Ltd.).
[0087] [Measurement of glass transition temperature (Tg)] A polyimide film (10 mm x 22.6 mm) was heated from 20°C to 500°C at a rate of 5°C / min using a dynamic thermomechanical analyzer, and the dynamic viscoelasticity was measured to determine the glass transition temperature (Tan δ maximum value: °C).
[0088] [Peel strength measurement] Using a tension tester, the resin side of a test sample having a 1 mm wide circuit pattern obtained from the laminate was fixed to an aluminum plate with double-sided tape, and the copper was peeled off in a 180° direction at a speed of 50 mm / min to determine the peel strength. For double-sided metal-clad laminates, the peel strength of the press side was also measured.
[0089] [Measurement of elastic modulus] The polyimide film was cut into a size of 12.7 mm x 150 mm, and a tensile test was performed at room temperature at 50 mm / min and 100 N in accordance with JIS K 7127 using a tensile tester (STROGRAPHVE1D manufactured by TOYO SEIKI) to measure the elastic modulus of the film.
[0090] [Refractive index measurement] A 2 μm-thick polyimide thin film was formed on glass, and the refractive index of 633 nm light was measured using a prism coupler Model 2010 / M manufactured by Metricon. The refractive index was measured three times, and the average value was calculated to determine the refractive index of the polyimide film.
[0091] The abbreviations used in the examples represent the following compounds. APB: 1,3-bis(3-aminophenoxy)benzene TFMB: 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl BAPS: Bis[4-(aminophenoxy)phenyl]sulfone PMDA: Pyromellitic dianhydride 6FDA: 2,2-bis(3,4-dicarboxyphenyl)-hexafluoropropane dianhydride BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride ODPA: 4,4'-oxydiphthalic dianhydride DMAc: N,N-dimethylacetamide
[0092] Synthesis Examples 1-8 To synthesize polyamic acid solutions A to H, the solvent DMAc was added to a 200 ml separable flask under a nitrogen stream so as to obtain the solid content concentration shown in Table 1, and the diamine components and acid anhydride components shown in Table 1 were dissolved by heating at 45°C for 2 hours while stirring. The solution was then stirred at room temperature for 2 days to carry out a polymerization reaction, and viscous polyamic acid solutions A to H were prepared.
[0093] [Table 1]
[0094] [Example 1] A diluted solution of polyamic acid solution A (viscosity: 3000 cP) was uniformly applied onto copper foil 1 (electrolytic copper foil, manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name: CF-T9DA-SV-12, thickness: 12 μm, Rzjis: 0.01 μm) so that the thickness after curing would be 1.5 μm, and then the diluted solution was dried by heating at 125° C. to remove the solvent. Next, a diluted solution of polyamic acid solution G (viscosity; 20,000 cP) was uniformly applied thereon to a thickness of 7 μm after curing, and then heated and dried at 125° C. to remove the solvent. Furthermore, a diluted solution of polyamic acid solution H (viscosity; 3,000 cP) was uniformly applied thereon to a thickness of 1.5 μm after curing, and then heated and dried at 125° C. to remove the solvent. In this way, three polyamic acid layers were formed, and then a stepwise heat treatment was performed from 125° C. to 360° C. over 30 minutes to complete the imidization, forming a polyimide layer 1 with a thickness of 10 μm consisting of a polyimide layer A / polyimide layer G / polyimide layer H, and a metal clad laminate 1 was prepared. The peel strength of the metal clad laminate 1 was 0.5 kN / m.
[0095] The copper foil was etched away using an aqueous solution of ferric chloride to prepare polyimide film 1. The physical properties of polyimide film 1 were measured. The results of these measurements are shown in Table 2. Here, YI(T10) indicates the yellowness index converted to a polyimide film thickness of 10 μm.
[0096] Example 2 ,Reference Example 3, Working Example 4, Comparative Examples 1 and 2, Reference Example 1] Similarly to Example 1, in order to prepare metal clad laminates 2 to 4, 6, 7, and 10, polyimide layers 2 to 4, 6, 7, and 10 were formed using different types of polyamic acid as shown in Table 2, and metal clad laminates 2 to 4, 6, 7, and 10 were prepared.
[0097] The copper foils of the metal clad laminates 2 to 4, 6, 7, and 10 were removed by etching using an aqueous solution of ferric chloride to prepare polyimide films 2 to 4, 6, 7, and 10. The measurement results for each polyimide film are shown in Table 2.
[0098] [Example 5] A metal clad laminate 5 was prepared in the same manner as in Example 1, except that polyamic acid A was used instead of polyamic acid solution H in Example 1. The prepared metal laminate 5 was cut to 15 cm x 15 cm, and copper foil 1 cut to a size of 15 cm x 15 cm was superimposed on the insulating resin layer surface of this laminate, and pressed at 340 ° C. / 30 min with a press machine to prepare a double-sided metal clad laminate 5. The copper foil was partially copper foil etched to form a circuit pattern with a copper foil width of 1 mm. When the 180 ° peel strength was measured, the peel strength of the pressed side was 1.1 kN / m. In addition, double-sided copper foil etching was performed to prepare a transparent polyimide film 5. The measurement results of the polyimide film 5 are shown in Table 2.
[0099] Comparative Example 3 A diluted solution of polyamic acid solution A (viscosity: 3000 cP) was uniformly applied onto copper foil 1 (electrolytic copper foil, manufactured by Fukuda Metal Foil and Powder Co., Ltd., product name: CF-T9DA-SV-12, thickness: 12 μm, Rzjis: 0.01 μm) so that the thickness after curing was 10 μm, and then heated and dried at 125 ° C. to remove the solvent. In this way, a single-layer polyamic acid layer was formed, and then a stepwise heat treatment was performed from 125 ° C. to 360 ° C. for 8 hours to complete the imidization, and a polyimide layer 8 having a thickness of 10 μm consisting of the polyimide layer A was formed, and a metal clad laminate 8 was prepared.
[0100] The copper foil of the metal clad laminate 8 was etched away using an aqueous solution of ferric chloride to prepare a polyimide film 8. The measurement results of the polyimide film 8 are shown in Table 2.
[0101] Comparative Example 4 A metal clad laminate 9 was prepared in the same manner as in Comparative Example 3, except that polyamic acid F was used instead of polyamic acid solution A in Comparative Example 3. The copper foil of the metal clad laminate 9 was etched away using an aqueous ferric chloride solution to prepare a polyimide film 9. The measurement results of the polyimide film 9 are shown in Table 2.
[0102] [Table 2]
[0103] A comparison of Comparative Example 3 and Comparative Example 4 reveals that BAPS-ODPA has a lower yellowness than BAPS-BPDA. This difference is more pronounced when comparing Example 1 and Reference Example 1, in which the polyimide has a three-layer structure and the curing time is shortened to increase productivity. This shows that it is effective to include ODPA when forming a three-layer transparent polyimide layer. Also, it shows that when a transparent polyimide composition not including BAPS is applied to polyimide layer 1 as in Comparative Example 1 and Comparative Example 2, adhesion cannot be guaranteed.
Claims
1. A conductor-polyimide laminate comprising an insulating resin layer and a conductor layer laminated on at least one surface of the insulating resin layer, the insulating resin layer includes a plurality of polyimide layers and has a yellowness index of 20 or less, and at least one polyimide layer (P1) is directly laminated on the conductor layer; The polyimide layer (P1) has a refractive index in the range of 1.65 to 1.75, A conductor-polyimide laminate, characterized in that the polyimide layer (P1) satisfies the following conditions a) and b): a) The diamine residue derived from the diamine compound represented by the following general formula (A1) accounts for 75 to 100 mol % of all diamine residues: b) The content of tetracarboxylic anhydride residues derived from a tetracarboxylic anhydride compound represented by the following general formula (B1) is 75 to 100 mol % based on the total tetracarboxylic anhydride residues: [Formula 1] [In formula (A1), R independently represents a halogen atom, an alkyl group or an alkoxy group having 1 to 6 carbon atoms which may be substituted with a halogen atom, or a phenyl group or a phenoxy group which may be substituted with a monovalent hydrocarbon group or an alkoxy group having 1 to 6 carbon atoms; Z independently represents -O-, -S-, -CH 2 -, -CH(CH 3 )-, -C(CH 3 ) 2 -, -SO 2 -, and at least one Z is -SO 2 n1 is an integer of 0 to 3, and n2 is an integer of 0 to 4. [Case 2]
2. 2. The conductor-polyimide laminate according to claim 1, wherein the thermal expansion coefficient of the entire insulating resin layer is within a range of 10 ppm / K to 30 ppm / K.
3. 3. The conductor-polyimide laminate according to claim 1, wherein the insulating resin layer as a whole has a total light transmittance of 80% or more.
4. 4. The conductor-polyimide laminate according to claim 1, wherein the insulating resin layer as a whole has a 1% weight loss temperature of 450° C. or higher.
5. 5. The conductor-polyimide laminate according to claim 1, wherein the thickness of the polyimide layer directly laminated on the conductor layer is 1% or more and less than 50% of the total thickness of the insulating resin layer.
6. 6. The conductor-polyimide laminate according to claim 1, wherein the insulating resin layer has a total thickness of 3 μm or more and 20 μm or less.
7. 7. The conductor-polyimide laminate according to claim 1, wherein a 180° peel strength between the insulating resin layer and the conductor layer is 0.3 kN / m or more.
8. The conductor-polyimide laminate according to any one of claims 1 to 7, characterized in that a polyimide layer (P2) which is not directly laminated with a conductor layer among the polyimide layers consisting of the multiple layers contains 20 mol % or more of diamine residues derived from a diamine compound represented by the following general formula (A2) with respect to all diamine residues: [C3] [In formula (A2), R 2 each independently represents a fluorine atom or an alkyl or alkoxy group having 1 to 3 carbon atoms which may be substituted by a fluorine atom, and p and q each independently represent an integer of 0 to 4.
Citation Information
Patent Citations
Polyimide molding and its production
JP1991143924A
Heat-resistant resin, its production and varnish containing the same
JP1995010993A
New polyimide resin composition and its varnish
JP2008163210A
Laminate for wiring board, having transparent insulating resin layer
JP2010155360A
Polyimide precursor composition and polyimide film and flexible device made of the same, and method for producing polyimide film
JP2020109166A