Method for producing the compound or its salt

Novel compounds serve as OSDAs for AFX type zeolite synthesis, addressing safety and efficiency issues in existing methods, enabling high-purity zeolite production and effective nitrogen oxide purification.

JP7577653B2Active Publication Date: 2024-11-05OSAKA UNIVERSITY +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021522161
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-27
Filing Date
2020-05-08
Publication Date
2024-11-05
Estimated Expiration
2040-05-08

AI Technical Summary

Technical Problem

Existing methods for producing AFX type zeolite face challenges in achieving high purity and efficient synthesis due to the use of flammable and explosive precursors, and the need for safe and easy mass production of structure-directing agents (OSDAs) that can form desired zeolite structures.

Method used

Development of novel compounds represented by formula (1) or their salts, which serve as OSDAs, synthesized using safer methods, allowing for the production of AFX type zeolite with improved purity and efficiency, and the use of these compounds in zeolite synthesis to create a honeycomb stacked catalyst for efficient nitrogen oxide purification.

Benefits of technology

The novel compounds enable safe and easy synthesis of AFX type zeolite, facilitating high-purity zeolite production and the development of a catalyst that effectively purifies nitrogen oxides, enhancing industrial applicability and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577653000043
    Figure 0007577653000043
  • Figure 0007577653000044
    Figure 0007577653000044
  • Figure 0007577653000045
    Figure 0007577653000045
Patent Text Reader

Abstract

The present invention provides a compound represented by general formula (1), a salt thereof or the like. (In formula (1), each of R1-R4 independently represents an alkyl group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a compound and a method for producing the same, an AFX type zeolite and a method for producing the same, and a honeycomb laminated catalyst.

[0002] AFX zeolite is useful as a material for selective catalytic reduction (SCR) for purifying nitrogen oxides in automobile exhaust gas (Non-Patent Document 1). In the synthesis of AFX zeolite, a structure directing agent is used to form a framework structure. The structure directing agent is also called OSDA (Organic Structure Directing Agent), and for example, N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium is known. N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium is a useful compound that is used as an OSDA not only in AFX zeolite but also in the preparation of MCM-68 zeolite (see, for example, Patent Documents 1 and 2, Non-Patent Document 2).

[0003] Furthermore, Patent Document 3 discloses that N,N'-diethyl-N,N'-dipropylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium and N,N'-diethyl-N,N'-diisopropylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium can be used as OSDAs for MCM-70 zeolite.

[0004] Patent Document 4 discloses an AFX zeolite having mesopores, and it is said that the zeolite has excellent diffusion of substances and improved catalytic properties because the pore state is controlled. The AFX zeolite of Patent Document 4 is produced by a method of crystallizing a composition that includes a silica source, an alumina source, a sodium source, and seed crystals, and in which the molar ratio of quaternary ammonium cations to silica is less than 0.01, without using an OSDA. Patent Document 4 discloses that the AFX zeolite has mesopores, but AFX zeolite having macropores is not known. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] US Patent Publication No. 6,049,018 [Patent Document 2] JP 2016-169139 A [Patent Document 3] US Patent Publication No. 6,656,268 [Patent Document 4] JP 2017-128457 A [Non-patent literature]

[0006] [Non-Patent Document 1] SV Priya et al., Bull. Chem. Soc. Jpn, 91 (2018) 355. [Non-Patent Document 2] N. Nakazawa et al., Adv. Porous Mater., 4 (2016) 219. Summary of the Invention [Problem to be solved by the invention]

[0007] Patent Document 2 discloses the use of N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium as an OSDA. However, when considering the use of OSDA as a structure-directing agent, it is required that the OSDA has the performance to obtain zeolites of a desired framework structure more efficiently and with relatively high purity. In addition, from the viewpoint of expanding industrial applications, it is desirable to have a high process margin during synthesis, and therefore there is a demand for OSDAs that can be used in various forms such as compounds and their salts. One aspect of the present invention has been made in view of the above circumstances, and an object of the present invention is to provide a novel compound that is useful as an OSDA, and a method for producing the same.

[0008] Patent Document 2 discloses a method for producing the target N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium by N-ethylating N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium as a precursor. In this case, in the synthesis of the precursor, N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarbonyldiimide must be used as a reducing agent that requires careful handling, such as lithium aluminum hydride (LiAlH4), which is known to be flammable and explosive, making it difficult to mass-produce the target compound. Since it was difficult to obtain OSDA in such a safe manner, it is practically difficult to mass-produce AFX zeolite. Another aspect of the present invention has been made in consideration of the above circumstances, and an objective of the present invention is to provide a novel compound that is useful as an OSDA and can be synthesized safely and easily, and a method for producing the same.

[0009] Another aspect of the present invention has been made in consideration of the above circumstances, and has an object to provide a novel AFX zeolite and a manufacturing method for efficiently manufacturing this AFX zeolite. Also, a different aspect of the present invention has been made in consideration of the above circumstances, and has an object to provide a honeycomb laminated catalyst using the novel AFX zeolite.

[0010] In addition to the objectives stated here, the present invention can also be positioned as another objective of achieving effects that are derived from the various components shown in the description of the embodiments of the invention described below, and that cannot be obtained by conventional techniques. [Means for solving the problem]

[0011] Means for Solving the Problems The present inventors conducted extensive research to provide compounds useful for producing OSDA, and as a result discovered that certain compounds are useful as OSDA, thereby completing the present invention.

[0012] As a result of extensive investigations by the present inventors into the provision of compounds useful for the production of OSDA, they discovered that certain compounds can be synthesized safely and easily and are useful as OSDAs, thus completing the present invention.

[0013] As a result of intensive research by the inventors into providing a compound useful for producing OSDA, they discovered that AFX zeolite can be produced efficiently by using a specific compound useful as an OSDA, and thus completed the present invention.

[0014] That is, the present invention provides various aspects as shown below. [1] A compound represented by formula (1) or a salt thereof. [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group.

[0015] [2] A structure-directing agent for zeolite synthesis, comprising the compound according to [1] above and / or a salt thereof.

[0016] [3] Providing a compound represented by formula (2); A method for producing a compound represented by formula (1) or a salt thereof, comprising at least a step of N-alkylating a compound represented by formula (2) using an alkylating agent. [ka] (In the above formulas (1) and (2), R 1 ~R 4 are each independently an alkyl group.

[0017] [4] The composition other than water is as follows: M a / b Q c S 48-d Al d O 96 (wherein M represents a metal cation, a represents 1 to 10, b represents a valence of M, Q represents a cation derived from the compound according to claim 1 and / or a salt thereof, c represents 0.5 to 2, and d represents 4 to 12.) AFX type zeolite.

[0018] [5] X-ray diffraction data included the following 2θ values ​​(°): 7.50±0.15, 8.71±0.15, 11.60±0.15, 13.01±0.15, 15.67±0.15, 17.46±0.15, 17.72±0.15, 19.93±0.15, 20.42±0.15, 21.84±0.15, 23.47±0.15, 26.19±0.15, 27.79±0.15, 30.67±0.15, 31.65±0.15, and 33.56±0.15. The AFX zeolite described in [4] above.

[0019] [6] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more. AFX type zeolite.

[0020] [7] X-ray diffraction data included the following 2θ values ​​(°): 7.46±0.15, 8.69±0.15, 11.64±0.15, 12.93±0.15, 15.60±0.15, 17.43±0.15, 17.90±0.15, 19.81±0.15, 20.32±0.15, 21.77±0.15, 23.67±0.15, 26.03±0.15, 28.05±0.15, 30.49±0.15, 31.50±0.15, and 33.71±0.15. The AFX zeolite described in [6] above.

[0021] [8] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more, A transition metal is supported. AFX type zeolite.

[0022] [9] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. At least A method for producing the AFX zeolite according to any one of [4] to [8].

[0023]

[10] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. After the hydrothermal treatment step, the method includes at least a step of further calcining the obtained AFX zeolite. A method for producing the AFX zeolite according to any one of [6] to [8].

[0024]

[11] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. A step of further calcining the obtained AFX zeolite after the hydrothermal treatment step. A step of supporting a transition metal after the calcination step. Contains at least A method for producing the AFX zeolite described in [8].

[0025]

[12] A step (Step I) of preparing a compound represented by formula (A); a step (step II) of reacting the compound represented by formula (A) with a hydrogen source using a catalyst to obtain a compound represented by formula (2); A step of N-alkylating the compound represented by the formula (2) using an alkylating agent (step III); A method for producing a compound represented by formula (1) or a salt thereof, comprising at least the steps of: [ka] (In the above formula (A), formula (1), and formula (2), R 1 ~R 4 are each independently an alkyl group.

[0026]

[13] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. A method for producing AFX zeolite, comprising at least the steps of:

[0027]

[14] reacting N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarboxydiimide with a hydrogen source using a Pt-V / Z catalyst to obtain N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine; and The method includes a step of N-alkylating the N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine with an alkylating agent to obtain the organic structure directing agent (OSDA) containing the compound represented by formula (1) and / or a salt thereof. A method for producing the AFX zeolite described in

[13] above.

[0028]

[15] AFX type zeolite with macropores.

[0029]

[16] A honeycomb laminated catalyst in which the AFX zeolite according to the above [8] or

[15] is applied to a honeycomb carrier.

[0030] In addition, one aspect of the present invention provides various specific embodiments as shown below. Hereinafter, the embodiments [A1] to [A18] are also referred to as a first group of specific embodiments.

[0031] [A1] A compound represented by formula (1) or a salt thereof. [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group.

[0032] [A2] R in the above formula (1) 1 ~R 4 are the same alkyl group The compound according to [A1] or a salt thereof.

[0033] [A3] R in the above formula (1) 1 ~R 4 are ethyl groups. The compound according to [A1] or [A2] or a salt thereof.

[0034] [A4] A structure-directing agent for zeolite synthesis, comprising the compound according to any one of [A1] to [A3] and / or a salt thereof.

[0035] [A5] Providing a compound represented by formula (2); A method for producing a compound represented by formula (1) or a salt thereof, comprising at least a step of N-alkylating a compound represented by formula (2) using an alkylating agent. [ka] (In the above formulas (1) and (2), R 1 ~R 4 are each independently an alkyl group.

[0036] [A6] The alkylating agent is represented by R'-X. (R' is an alkyl group, and X is one or more leaving groups selected from the group consisting of halogen atoms and sulfonyl groups which may have a substituent.) The manufacturing method described in [A5].

[0037] [A7] The alkylating reagent is an alkyl halide. The manufacturing method described in [A6].

[0038] [A8] the alkylating reagent is an ethyl halide; R in the above formulas (1) and (2) 1 and R 2 is an ethyl group, R in the above formula (1) 3 and R 4 is an ethyl group The manufacturing method described in [A5].

[0039] [A9] The composition other than water is as follows: M a / b Q c S 48-d Al dO 96 (In the formula, M represents a metal cation, a represents 1 to 10, b represents a valence of M, Q represents a cation derived from the compound according to any one of [1] to [3] and / or a salt thereof, c represents 0.5 to 2, and d represents 4 to 12.) AFX type zeolite.

[0040] [A10] X-ray diffraction data included the following 2θ values ​​(°): 7.50±0.15, 8.71±0.15, 11.60±0.15, 13.01±0.15, 15.67±0.15, 17.46±0.15, 17.72±0.15, 19.93±0.15, 20.42±0.15, 21.84±0.15, 23.47±0.15, 26.19±0.15, 27.79±0.15, 30.67±0.15, 31.65±0.15, and 33.56±0.15. The AFX zeolite according to [A9].

[0041] [A11] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more. AFX type zeolite.

[0042] [A12] X-ray diffraction data included the following 2θ values ​​(°): 7.46±0.15, 8.69±0.15, 11.64±0.15, 12.93±0.15, 15.60±0.15, 17.43±0.15, 17.90±0.15, 19.81±0.15, 20.32±0.15, 21.77±0.15, 23.67±0.15, 26.03±0.15, 28.05±0.15, 30.49±0.15, 31.50±0.15, and 33.71±0.15. The AFX zeolite according to [A11].

[0043] [A13] The average particle size is 1.0 μm or more and 3.0 μm or less. The AFX zeolite according to [A11] or [A12].

[0044] [A14] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more, A transition metal is supported. AFX type zeolite.

[0045] [A15] [A14] A zeolite having an AFX type and a honeycomb carrier. Honeycomb stacked catalyst.

[0046] [A16] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. At least A method for producing the AFX zeolite according to any one of [A9] to [A14].

[0047] [A17] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. After the hydrothermal treatment step, the method includes at least a step of further calcining the obtained AFX zeolite. A method for producing the AFX zeolite according to any one of [A11] to [A14].

[0048] [A18] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. A step of further calcining the obtained AFX zeolite after the hydrothermal treatment step. A step of supporting a transition metal after the calcination step. Contains at least A method for producing the AFX zeolite described in [A14].

[0049] In addition, one aspect of the present invention provides various specific embodiments as shown below. Hereinafter, the embodiments [B1] to [B8] are also referred to as a second group of specific embodiments.

[0050] [B1] A step (Step I) of preparing a compound represented by formula (A); a step (step II) of reacting the compound represented by formula (A) with a hydrogen source using a catalyst to obtain a compound represented by formula (2); A step of N-alkylating the compound represented by the formula (2) using an alkylating agent (step III); A method for producing a compound represented by formula (1) or a salt thereof, comprising at least the steps of: [ka] (In the above formula (A), formula (1), and formula (2), R 1 ~R 4 are each independently an alkyl group.

[0051] [B2] The hydrogen source is molecular hydrogen. The manufacturing method described in [B1].

[0052] [B3] The step II is carried out under a wet process. The manufacturing method according to [B1] or [B2].

[0053] [B4] The catalyst is a heterogeneous catalyst. The method according to any one of [B1] to [B3].

[0054] [B5] The alkylating agent is represented by R'-X. (R' is an alkyl group, and X is one or more leaving groups selected from the group consisting of halogen atoms and sulfonyl groups which may have a substituent.) The method for producing a product according to any one of [B1] to [B4].

[0055] [B6] The alkylating reagent is an alkyl halide. The manufacturing method described in [B5].

[0056] [B7] The alkylating reagent is an ethyl halide. The manufacturing method described in [B6].

[0057] [B8] R in the above formula (A), formula (1) and formula (2) 1 and R 2 is an ethyl group, R in the above formula (1) 3 and R 4 is an ethyl group The method according to any one of [B1] to [B7].

[0058] In addition, one aspect of the present invention provides various specific embodiments as shown below. Hereinafter, the embodiments [C1] to [C13] are also referred to as a third group of specific embodiments.

[0059] [C1] a source of silica and alumina; An organic structure directing agent (OSDA) comprising a compound represented by the following formula (1) and / or a salt thereof: [ka] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group; Alkali metal hydroxides, and water preparing a mixture comprising at least A step of hydrothermally treating the mixture to synthesize AFX zeolite. A method for producing AFX zeolite, comprising at least the steps of:

[0060] [C2] R in the above formula (1) 1 ~R 4 are the same alkyl group A method for producing the AFX zeolite described in [C1].

[0061] [C3] R in the above formula (1) 1 ~R 4 are ethyl groups. A method for producing the AFX zeolite according to [C1] or [C2].

[0062] [C4] The silica-alumina ratio (SiO2 / Al2O3) in the mixture is 5 to 30. A method for producing the AFX zeolite according to any one of [C1] to [C3].

[0063] [C5] The composition of the AFX zeolite other than water is as follows: M a / b Q c S 48-d Al d O 96 (In the formula, M represents a metal cation, a represents 1 to 10, b represents the valence of M, Q represents a cation derived from the compound represented by (1) and / or a salt thereof, c represents 0.5 to 2, and d represents 4 to 12.) A method for producing the AFX zeolite according to any one of [C1] to [C4].

[0064] [C6] The X-ray diffraction data of the AFX zeolite includes the following 2θ values ​​(°): 7.50±0.15, 8.71±0.15, 11.60±0.15, 13.01±0.15, 15.67±0.15, 17.46±0.15, 17.72±0.15, 19.93±0.15, 20.42±0.15, 21.84±0.15, 23.47±0.15, 26.19±0.15, 27.79±0.15, 30.67±0.15, 31.65±0.15, and 33.56±0.15. A method for producing the AFX zeolite according to any one of [C1] to [C5].

[0065] [C7] In the step of preparing the mixture, the mixture further containing a silica source (excluding those corresponding to the silica and alumina sources) is prepared. A method for producing the AFX zeolite according to any one of [C1] to [C6].

[0066] [C8] In the step of preparing the mixture, the mixture further containing an alumina source (excluding those corresponding to the silica and alumina sources) is prepared. A method for producing the AFX zeolite according to any one of [C1] to [C7].

[0067] [C9] In the step of preparing the mixture, the mixture further includes aluminosilicate seed crystals. A method for producing the AFX zeolite according to any one of [C1] to [C8].

[0068] [C10] After the hydrothermal treatment step, the obtained AFX zeolite is further calcined. A method for producing the AFX zeolite according to any one of [C1] to [C9].

[0069] [C11] The composition of the AFX zeolite after calcination other than water is as follows: M a / b H 2c S 48-d Al d O 96 (wherein M represents a metal cation, a represents 1 to 10, b represents the valence of M, Q represents the compound represented by (1) and / or a salt thereof, c represents 0.5 to 2, and d represents 4 to 12.) A method for producing the AFX zeolite according to [C10].

[0070] [C12] The obtained AFX zeolite was subjected to NH 4+ Type and / or H + The method further comprises the step of ion exchanging the mold. A method for producing the AFX zeolite according to any one of [C1] to [C11].

[0071] [C13] reacting N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarboxydiimide with a hydrogen source using a Pt-V / Z catalyst to obtain N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine; and The method includes a step of N-alkylating the N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine with an alkylating agent to obtain the organic structure directing agent (OSDA) containing the compound represented by formula (1) and / or a salt thereof. A method for producing the AFX zeolite according to any one of [C1] to [C12].

[0072] In addition, one aspect of the present invention provides various specific embodiments as shown below. Hereinafter, the embodiment [D1] is also referred to as a fourth group of specific embodiments.

[0073] [D1] AFX type zeolite with macropores.

[0074] [D2] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more. The AFX zeolite according to [D1].

[0075] [D3] X-ray diffraction data included the following 2θ values ​​(°): 7.46±0.15, 8.69±0.15, 11.64±0.15, 12.93±0.15, 15.60±0.15, 17.43±0.15, 17.90±0.15, 19.81±0.15, 20.32±0.15, 21.77±0.15, 23.67±0.15, 26.03±0.15, 28.05±0.15, 30.49±0.15, 31.50±0.15, and 33.71±0.15. The AFX zeolite according to [D1] or [D2].

[0076] [D4] The average particle size is 1.0 μm or more and 3.0 μm or less. The AFX zeolite according to any one of [D1] to [D3].

[0077] [D5] SAR (SiO2 / Al2O3 ratio) is 10 or more and 30 or less, In the XRD chart obtained by powder X-ray diffraction analysis, the strongest line is at 2θ=21.77°±0.15°, The average particle size is 0.6 μm or more, A transition metal is supported. The AFX zeolite according to [D1].

[0078] [D6] [D1] to [D5], and a honeycomb carrier. Honeycomb stacked catalyst.

[0079] [D7] The AFX zeolite according to any one of [D1] to [D5] is applied to a honeycomb carrier. Honeycomb stacked catalyst. Effect of the Invention

[0080] The compound according to one embodiment of the present invention is useful as a raw material compound (OSDA) for porous crystalline materials such as zeolites. According to the method for producing a compound of one embodiment of the present invention, it is possible to safely and easily provide a compound that is useful as a raw material for porous crystal materials such as zeolites (OSDA). According to the zeolite production method of one embodiment of the present invention, it is possible to efficiently produce AFX zeolite. A honeycomb laminated catalyst in which the AFX zeolite of one embodiment of the present invention is applied to a honeycomb carrier enables highly efficient purification of nitrogen oxides using a reducing component. [Brief description of the drawings]

[0081] [Figure 1] This is a diagram showing the 1H NMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Example A1. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Diagram 2] A figure showing the CNMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Example A1. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Diagram 3] This is a diagram showing the solid-state NMR spectrum data (A) of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium, the 13C NMR spectrum data (C) of the DO solution, and the solid-state NMR spectrum data (B) of the AFX zeolite obtained using N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium. Note that the * in (C) in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 4] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Example A2. [Diagram 5] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Example A3. [Figure 6] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Comparative Example A1. [Figure 7] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Example A4. [Figure 8] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Example A5. [Figure 9] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Example A6. [Figure 10] FIG. 2 is a diagram showing an XRD chart of the AFX zeolite of Comparative Example A2. [Figure 11]FIG. 2 shows the change in the total XRD peak integrated intensity before and after measurement of the hydrothermal durability of the AFX zeolites of Examples A4, A5, and A6, and Comparative Example A2. [Figure 12] FIG. 2 is a SEM image of the AFX zeolite of Example A4. [Figure 13] FIG. 2 is a SEM image of the AFX zeolite of Example A5. [Figure 14] FIG. 2 is a SEM image of the AFX zeolite of Example A6. [Figure 15] FIG. 2 is a SEM image of the AFX zeolite of Comparative Example A2. [Figure 16] FIG. 2 is a diagram showing an XRD chart of the Cu-supported AFX zeolite of Example A7. [Figure 17] FIG. 2 is a SEM image of the Cu-supported AFX zeolite of Example A7. [Figure 18] FIG. 2 is a diagram showing an SEM image of the Cu-supported CHA-type zeolite of Comparative Example A3. [Figure 19] FIG. 2 is a diagram showing an SEM image of the Cu-supported CHA-type zeolite of Comparative Example A4. [Figure 20] This is a diagram showing the 1H NMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Example B1. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 21] This is a diagram showing the CNMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Example B1. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 22] FIG. 2 is a diagram showing XRD data of the AFX zeolite of Reference Example B1. [Figure 23]This is a diagram showing the 1H NMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Reference Example B2. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 24] This is a diagram showing the CNMR spectrum data of the DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained in Reference Example B2. * in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Diagram 25] FIG. 2 is a diagram showing XRD data of the AFX zeolite of Reference Example B3. [Figure 26] This is a diagram showing the 1H NMR spectrum data of a DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained by Production Example C3. * in the diagram indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 27] This is a diagram showing the CNMR spectrum data of a DO solution of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide obtained by Production Example C3. * in the diagram indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). [Figure 28] FIG. 2 shows XRD data of the AFX zeolite of Example C1. [Figure 29] FIG. 2 shows XRD data of the zeolite obtained according to Comparative Example C1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0082] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. The following embodiments are examples (representative examples) of the present invention, and the present invention is not limited to these. In other words, the present invention can be implemented by making any changes without departing from the scope of the invention. In this specification, when a numerical value or a physical property value is expressed using "~" before and after the symbol, the values ​​before and after the symbol are included. For example, the expression of a numerical range of "1 to 100" includes both the lower limit "1" and the upper limit "100". The same applies to the expression of other numerical ranges.

[0083] (compound) The compound of this embodiment is a compound represented by the following formula (1) or a salt thereof. In this specification, the term "compound or a salt thereof" is also simply referred to as "compound", including the above salt. The compound of this embodiment is useful as an OSDA. In addition, the compound of this embodiment is particularly advantageous industrially because a compound that can be synthesized simply and safely can be used as a starting material without using a reducing agent reagent such as LiAlH4, which is difficult to handle and difficult to control the reaction. In addition, when the compound of this embodiment is used in the production of AFX zeolite, AFX zeolite can be obtained in a single phase. In this specification, the compound represented by the following formula (1) is also referred to as N,N,N',N'-tetraalkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium. [ka]

[0084] In the above formula (1), R 1 ~R 4 are each independently an alkyl group. 1 ~R 4 are preferably the same alkyl group. Suitable examples of the alkyl group include linear or branched alkyl groups having 1 to 4 carbon atoms, and specific examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a tert-butyl group. Among these alkyl groups, an alkyl group having 1 to 3 carbon atoms is preferable, and an alkyl group having 1 to 2 carbon atoms is more preferable. Specifically, the alkyl group is preferably a methyl group, an ethyl group, an n-propyl group, or an isopropyl group, more preferably a methyl group or an ethyl group, and further preferably an ethyl group.

[0085] Specific examples of the compound represented by formula (1) include the following compounds. [ka]

[0086] [ka]

[0087] [ka]

[0088] The compound of this embodiment also includes salt forms as described above. The counter anion that forms a salt with the ammonium cation of the compound of this embodiment is not particularly limited, and may be an inorganic anion or an organic anion. Examples of counter anions when forming the salt of this embodiment include hydroxide ion, nitrate ion, sulfate ion, carbonate ion, bicarbonate ion, halide ion (fluorine, chlorine, bromine, iodine), formate ion, acetate ion, citrate ion, tartrate ion, oxalate ion, fumarate ion, and anions of saturated or unsaturated chain fatty acids having 3 to 20 carbon atoms. Among these, hydroxide ion and halide ion are preferred. That is, the salt of the compound of this embodiment is preferably a hydroxide or a halide. The salt of the compound of this embodiment may be a mixture of two or more different salts.

[0089] (Manufacturing method) The compound represented by formula (1) of this embodiment can be produced by a known synthesis route, and the production method is not particularly limited. An example of a preferred production method includes a production method including a step of N-alkylating a compound represented by the following formula (2) using an alkylating agent. Here, the compound represented by the following formula (2) is also called N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine. A particularly preferred production method of this embodiment can be represented by the following scheme. [ka]

[0090] R in the above scheme 1 ~R 4 are each independently an alkyl group. 1 and R 2 is R in formula (1). 1 and R 2 The preferred substituents are the same as those in the formula (1). 1 and R 2 The same groups as those shown below can be mentioned.

[0091] The alkylating reagent is not particularly limited as long as it alkylates the nitrogen of the compound represented by formula (2), and examples thereof include alkylating reagents represented by R'-X. R' is an alkyl group, and X is a leaving group. Suitable examples of the leaving group include halogen atoms such as chlorine atom, bromine atom, and iodine atom; and sulfonyl groups such as methylsulfonyl, trifluoromethylsulfonyl, and p-toluenesulfonyl. The alkylating reagent is preferably an alkyl halide, more preferably a methyl halide or an ethyl halide.

[0092] In the prior art, N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium hydroxide is used in the synthesis of AFX zeolite (see JP 2016-169139 A (Patent Document 2)). In the synthesis of the hydroxide, N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium iodide obtained as a solid powder is ion-exchanged with a hydroxide-type anion exchange resin, and concentrated to obtain a hydroxide solution. On the other hand, the compound (salt) of this embodiment can be used as it is in the synthesis of zeolite, that is, the salt obtained by alkylation as described above, that is, the salt in which X is a counter anion. Therefore, in this case, the time and effort for preparing hydroxide can be saved, and zeolite can be produced efficiently. In addition, for example, when using as hydroxide, it is sufficient to ion-exchange with hydroxide-type anion exchange resin and concentrate as in the conventional method.

[0093] The amount of the alkylating reagent used may be appropriately determined in consideration of the synthesis efficiency, purity, and the like, and is not particularly limited. The amount is usually 2 equivalents or more, preferably 2 to 50 equivalents, and more preferably 2 to 10 equivalents, relative to the amount of the compound represented by formula (2).

[0094] The reaction in this embodiment may be carried out in the presence of a solvent, i.e., under a wet process. The solvent is not particularly limited as long as it can dissolve the compound represented by formula (2), and may be appropriately selected depending on the reaction temperature, reactants, etc. Examples of the solvent include water, aromatic hydrocarbon solvents such as benzene and toluene, amide solvents such as acetonitrile, N,N-dimethylacetamide and N,N-dimethylformamide, ether solvents such as tetrahydrofuran (hereinafter also referred to as THF), diethyl ether and 1,2-dimethoxyethane, alcohol solvents such as methanol, ethanol and isopropanol, halogen solvents such as dichloromethane, dichloroethane and chloroform, etc. These solvents can be used alone or in any combination and ratio of two or more. Among these solvents, alcohol-based solvents are preferred.

[0095] The use of a solvent and its amount may be appropriately determined in consideration of other reaction conditions and is not particularly limited. However, the concentration of the compound represented by formula (2) in the reaction mixture is preferably 0.001 to 10 mol / L, more preferably 0.01 to 5 mol / L, and even more preferably 0.01 to 3 mol / L.

[0096] The reaction temperature is not particularly limited, but may be appropriately adjusted depending on the type of solvent, etc. The reaction temperature is usually in the range of 20 to 200° C., preferably 50 to 150° C., and more preferably 50 to 120° C. The reaction may be carried out at a temperature at which the solvent refluxes. The reaction time may be appropriately adjusted by monitoring the progress of the reaction using GC-MS or the like, and is usually 1 minute to 100 hours, preferably 0.5 hours to 70 hours, and more preferably 1 hour to 60 hours.

[0097] When a solvent is used in the reaction, the mixture after the completion of the reaction may be used as a raw material as it is after concentrating the obtained reaction solution as necessary, or the reaction mixture may be appropriately post-treated to obtain the compound represented by the above formula (1). Specific methods of post-treatment include known purification methods such as washing with water, filtration, drying, extraction, distillation, and chromatography. Two or more of these purification methods may be combined. In addition, as a post-treatment, a counter anion may be adjusted using an ion exchange resin or the like to obtain a salt. Specifically, after the step of N-alkylating the compound represented by the formula (2) using an alkylating agent, the obtained compound is dissolved in an appropriate solvent and brought into contact with an ion exchange resin to obtain a desired salt.

[0098] The compound represented by formula (2) can be produced by a known synthesis route, and the production method is not particularly limited. For example, the compound represented by formula (2) can be produced by hydrogenating N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine, which can be synthesized according to Patent Document 2, as shown in the following scheme. [ka]

[0099] R in the above scheme 1 and R 2 are each independently an alkyl group. R in N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine 1 and R 2 is R in formula (1). 1 and R 2 The preferred substituents are the same as those in the formula (1). 1 and R 2 The same groups as those shown below can be mentioned.

[0100] Specifically, the compound represented by formula (2) is produced by reacting N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine with a hydrogen source in the presence or absence of a catalyst.

[0101] The hydrogen source used in the above production method can be appropriately selected from those capable of hydrogenating N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine. Specific examples include, but are not limited to, molecular hydrogen such as hydrogen gas; hydrogen donors such as ammonium formate, sodium formate, and hydrazine; and the like. Among these hydrogen sources, molecular hydrogen is preferred. In addition, when molecular hydrogen is used in the above production method, the hydrogen pressure in the reactor is usually 0.1 to 10 MPa, preferably 0.1 to 5 MPa, and more preferably 0.1 to 1.0 MPa.

[0102] The reaction in this embodiment may be carried out in the presence of a solvent, i.e., under a wet process. Examples of the solvent include water; aromatic hydrocarbon solvents such as benzene and toluene; amide solvents such as acetonitrile, N,N-dimethylacetamide, and N,N-dimethylformamide; ether solvents such as THF, diethyl ether, and 1,2-dimethoxyethane; alcohol solvents such as methanol, ethanol, and isopropanol; and halogen solvents such as dichloromethane, dichloroethane, and chloroform. These solvents may be used alone or in any combination and ratio of two or more. Among these solvents, alcohol solvents are preferred.

[0103] The use of a solvent and the amount of the solvent to be used may be appropriately determined in consideration of other reaction conditions and are not particularly limited. However, the concentration of N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine in the reaction mixture is preferably 0.001 to 10 mol / L, more preferably 0.01 to 5 mol / L, and even more preferably 0.01 to 3 mol / L.

[0104] The reaction temperature is not particularly limited, but may be appropriately adjusted depending on the type of solvent, etc. The reaction temperature is usually in the range of 20 to 200° C., preferably 20 to 150° C., and more preferably 30 to 120° C. The reaction may be carried out at a temperature at which the solvent refluxes. The reaction time may be appropriately adjusted by monitoring the progress of the reaction using GC-MS or the like, and is usually from 1 minute to 1000 hours, preferably from 0.5 hour to 300 hours, more preferably from 1 hour to 200 hours.

[0105] After the reaction is completed, when a solvent is used in the above reaction, the obtained reaction solution may be concentrated as necessary, and the residue may be used as a raw material as it is, or the reaction mixture may be appropriately post-treated to obtain the compound represented by the above formula (2). Specific examples of the post-treatment method include known purification methods such as washing with water, filtration, drying, extraction, distillation, and chromatography. These purification methods may be combined and used in two or more kinds.

[0106] (Structure-directing agent for zeolite synthesis) The compound and its salt of the present embodiment can be used as a structure-directing agent (OSDA; Organic Structure Directing Agents) in the production of zeolite. That is, one of the present embodiments is a structure-directing agent for zeolite synthesis containing the compound represented by the formula (1) and / or its salt.

[0107] <AFX-type zeolite and its production method> The method for producing an AFX-type zeolite of the present embodiment includes at least a step of preparing a mixture containing a silica and alumina source, an organic structure-directing agent (OSDA) containing the compound represented by the following (1) and / or its salt, an alkali metal hydroxide, and water, and a step of hydrothermally treating the mixture to synthesize an AFX-type zeolite.

Chemical formula

[0108] In the manufacturing method of this embodiment, the compound represented by (1) above and / or its salt is used as the organic structure directing agent (OSDA). The compound represented by (1) above and its salt are highly available. In addition, when the compound represented by (1) above and / or its salt is used as the organic structure directing agent (OSDA), AFX zeolite can be obtained in a single phase without being mixed with other phases. As described above, the manufacturing method of this embodiment can efficiently produce AFX zeolite. The AFX zeolite of this embodiment is an aluminosilicate given the three-letter code "AFX" by the International Zeolite Association Structure Commission (IZA-SC).

[0109] (Silica and Alumina Source) As the silica and alumina source used as the raw material, any known one can be used without any particular limitation as long as it contains at least an aluminosilicate (Si-Al element source) with a silica-alumina ratio (SiO2 / Al2O3, hereinafter sometimes referred to as "SAR") of 2 or more and less than 50. The type is not particularly limited. Here, the aluminosilicate has a structure in which a part of the silicon atoms in the silicate is replaced with an aluminum atom. The crystal form of the silica-alumina source is not particularly limited, but may be amorphous or may have a zeolite structure such as FAU. The silica-alumina ratio is preferably 5 or more and less than 40, more preferably 10 or more and 30 or less. In this specification, the silica-alumina ratio means a value obtained from fluorescent X-ray analysis. Specifically, a sample obtained by pressurizing about 5 g of a sample at 20 t was measured using Axios (Spectolys), and the SAR was calculated from the results of the mass% of Al2O3 and SiO2 obtained.

[0110] As the silica and alumina source used in this embodiment, the above-mentioned Si-Al element source can be used alone, but it may be used in combination with a Si element source (excluding those corresponding to the Si-Al element source) or an Al element source (excluding those corresponding to the Si-Al element source), or a mixture of a Si element source and an Al element source can be used as the silica and alumina source. For example, as the silica and alumina source, the Si-Al element source may be used in combination with a Si element source (excluding those corresponding to the Si-Al element source) and / or an Al element source (excluding those corresponding to the Si-Al element source). Among these, it is preferable to use the Si-Al element source alone.

[0111] Examples of the Si element source include, but are not limited to, precipitated silica, colloidal silica, fumed silica, silica gel, sodium silicate (sodium metasilicate, sodium orthosilicate, sodium silicate No. 1, No. 2, No. 3, No. 4, etc.), alkoxysilanes such as tetraethoxysilane (TEOS) and trimethylethoxysilane (TMEOS), etc. However, in this specification, aluminosilicates with an SAR of 2 or more and less than 20 correspond to the above-mentioned Si-Al element source and are not included in this Si element source.

[0112] The Si element source may be used alone or in any combination and ratio of two or more kinds.

[0113] Examples of Al element sources include, but are not limited to, aluminum hydroxide, sodium aluminate, aluminum oxide hydroxide, aluminum oxide, etc. However, in this specification, aluminosilicates having an SAR of 2 or more and less than 50 correspond to the above-mentioned Si-Al element source and are not included in this Al element source.

[0114] The Al element source may be used alone or in any combination and ratio of two or more kinds.

[0115] In the AFX zeolite of this embodiment, the SAR is preferably 2 or more and less than 50, more preferably 5 or more and less than 40, and even more preferably 10 or more and less than 30. As described above, the SAR of AFX zeolite can be adjusted to the above range by using an aluminosilicate (Si-Al element source) with a SAR in the range of 2 or more and less than 50 in the production of AFX zeolite.

[0116] (alkali metal hydroxides) Examples of the alkali metal source include alkali metal hydroxides such as LiOH, NaOH, KOH, CsOH, and RbOH, aluminates of these alkali metals, and the above-mentioned Si-Al element source and alkali components contained in the Si element source. Among these, NaOH and KOH are preferably used. In addition, the alkali metal in the mixture can also function as an inorganic structure directing agent, so that an aluminosilicate with excellent crystallinity tends to be easily obtained.

[0117] The alkali metal sources can be used alone or in any combination and ratio of two or more kinds.

[0118] (water) The water to be used may be tap water, RO water, deionized water, distilled water, industrial water, pure water, ultrapure water, etc., depending on the desired performance. In addition, the method of adding water to the mixture may be to add it separately from each of the above-mentioned components, or to mix it with each component in advance and add it as an aqueous solution or dispersion of each component.

[0119] In the step of preparing the mixture, a mixture (slurry) containing the above-mentioned silica and alumina sources, an organic structure directing agent (OSDA) containing a compound represented by formula (1) and / or a salt thereof, an alkali metal hydroxide, and water is prepared. At this time, wet mixing can be performed using a known mixer or stirrer, such as a ball mill, a bead mill, a media stirring mill, a homogenizer, etc., as necessary. When stirring, it is usually preferable to perform the stirring at a rotation speed of about 30 to 2000 rpm, more preferably 50 to 1000 rpm.

[0120] The content of water in the mixture can be appropriately set in consideration of reactivity, handling, etc., and is not particularly limited, but the water-silica ratio (H2O / SiO2 molar ratio) of the mixture is usually 5 to 100, preferably 6 to 50, more preferably 7 to 40. When the water-silica ratio is within the above-mentioned preferred range, stirring during preparation of the mixture or during crystallization by hydrothermal synthesis becomes easy, and the handling is improved, and the generation of by-products and impurity crystals is suppressed, so that a high yield tends to be obtained. The method of blending water into the mixture may be blended separately from each of the above-mentioned components, or may be mixed with each component in advance and blended as an aqueous solution or dispersion of each component.

[0121] The silica-alumina ratio (SiO2 / Al2O3) in the mixture can also be appropriately set and is not particularly limited, but is usually from 5 to 50, preferably from 7 to less than 45, and more preferably from 10 to 30. When the silica-alumina ratio is within the above preferred range, dense crystals are easily obtained while having sufficient cationic sites effective for catalytic reactions, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be easily obtained.

[0122] On the other hand, the hydroxide ion / silica ratio (OH - The hydroxide ion / silica ratio can also be appropriately set and is not particularly limited, but is usually 0.10 to 0.90, preferably 0.15 to 0.50, and more preferably 0.20 to 0.40. When the hydroxide ion / silica ratio is within the above preferred range, crystallization tends to proceed easily, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be obtained.

[0123] The content of the alkali metal in the mixture can also be appropriately set, and is not particularly limited, but the molar ratio of the alkali metal (M) in terms of oxide, i.e., the alkali metal oxide / silica ratio (MO / SiO2 molar ratio), is usually 0.01 to 0.50, preferably 0.05 to 0.30. When the alkali metal oxide / silica ratio is within the above preferred range, crystallization due to mineralization is promoted, and the generation of by-products and impurity crystals is suppressed, tending to easily obtain a high yield.

[0124] On the other hand, the organic structure directing agent / silica ratio (organic structure directing agent / SiO2 molar ratio) in the mixture can also be appropriately set, and is not particularly limited, but is usually 0.05 to 0.40, preferably 0.07 to 0.30, and more preferably 0.09 to 0.25. When the organic structure directing agent / silica ratio is within the above preferred range, crystallization tends to proceed easily, and an aluminosilicate having excellent thermal durability in a high-temperature environment or after exposure to high temperatures tends to be easily obtained at low cost.

[0125] The above-mentioned mixture may contain a specific anion from the viewpoint of promoting crystallization and controlling the crystal grain size. For example, as in Patent Document 2, when a mixture is produced by OSDA consisting of only the hydroxide of the compound represented by formula (1) without adding a specific anion, AFX zeolite with a relatively small crystal grain size is obtained. On the other hand, when a halide ion is added to the mixture, AFX zeolite with a relatively large crystal grain size can be obtained. The halide ion may be any of fluoride, chloride, bromide, and iodide. In addition, the method for including the halide ion in the mixture is not particularly limited, and the halide ion may be added as a counter ion of OSDA, as a counter ion of an alkali metal, or as a free acid.

[0126] In addition, the above-mentioned mixture may further contain a seed crystal of an aluminosilicate having a desired skeletal structure from the viewpoint of promoting crystallization. By blending the seed crystal, the crystallization of the desired skeletal structure is promoted, and a high-quality aluminosilicate tends to be easily obtained. The seed crystal used here is not particularly limited as long as it has a desired skeletal structure. As the seed crystal, for example, a seed crystal of an aluminosilicate having at least one skeletal structure of CHA, AEI, ERI, and AFX can be used. The silica-alumina ratio of the seed crystal is arbitrary, but is preferably the same or similar to the silica-alumina ratio of the mixture. From this viewpoint, the silica-alumina ratio of the seed crystal is preferably 5 or more and 50 or less, more preferably 8 or more and less than 40, and even more preferably 10 or more and less than 30.

[0127] The seed crystals used here can be not only separately synthesized aluminosilicates, but also commercially available aluminosilicates. Naturally produced aluminosilicates can be used, and aluminosilicates synthesized according to the present invention can also be used as seed crystals. The cation type of the seed crystals is not particularly limited, and for example, sodium type, potassium type, ammonium type, proton type, etc. can be used.

[0128] The particle size of the seed crystal used here (D 50 ) is not particularly limited, but from the viewpoint of promoting crystallization of the desired crystal structure, it is desirable that it is relatively small, and is usually 0.5 nm to 5 μm, preferably 1 nm to 3 μm, and more preferably 2 nm to 1 μm. The amount of the seed crystals to be mixed can be appropriately set according to the desired crystallinity, and is not particularly limited, but is preferably 0.05 to 30 mass%, more preferably 0.1 to 20 mass%, and even more preferably 0.5 to 10 mass%, based on the mass of SiO2 in the mixture.

[0129] In the step of hydrothermally treating the mixture, the above-mentioned mixture is heated in a reaction vessel to carry out hydrothermal synthesis, thereby obtaining a crystallized aluminosilicate (AFX-type zeolite).

[0130] The reaction vessel used in this hydrothermal synthesis can be any known sealed pressure vessel that can be used in hydrothermal synthesis, and the type is not particularly limited. For example, a sealed heat-resistant pressure vessel such as an autoclave equipped with a stirring device, a heat source, a pressure gauge, and a safety valve is preferably used. The crystallization of the aluminosilicate may be performed with the above-mentioned mixture (raw material composition) left to stand, but from the viewpoint of increasing the uniformity of the obtained aluminosilicate, the above-mentioned mixture (raw material composition) may be stirred and mixed. At this time, it is usually preferable to perform the crystallization at a rotation speed of about 30 to 2000 rpm, more preferably 50 to 1000 rpm. In addition, the stirring may be performed intermittently for the purpose of controlling the crystal grain size, etc.

[0131] The treatment temperature (reaction temperature) of the hydrothermal synthesis is not particularly limited, but from the viewpoints of the crystallinity of the obtained aluminosilicate and economic efficiency, it is usually 100°C or higher and 200°C or lower, preferably 120°C or higher and 190°C or lower, and more preferably 150°C or higher and 180°C or lower.

[0132] The treatment time (reaction time) of the hydrothermal synthesis is not particularly limited as long as it is long enough to allow crystallization. From the viewpoints of the crystallinity of the resulting aluminosilicate and economic efficiency, the treatment time is usually from 1 hour to 20 days, preferably from 4 hours to 15 days, and more preferably from 12 hours to 10 days.

[0133] The treatment pressure for the hydrothermal synthesis is not particularly limited, and the autogenous pressure generated when the mixture charged in the reaction vessel is heated to the above-mentioned temperature range is sufficient. At this time, an inert gas such as nitrogen or argon may be introduced into the vessel as necessary.

[0134] By carrying out such hydrothermal treatment, a crystallized aluminosilicate can be obtained. At this time, if necessary, a solid-liquid separation treatment, a water washing treatment, a drying treatment for removing moisture in air at a temperature of about 50 to 150°C, etc. may be carried out according to a conventional method.

[0135] The AFX zeolite obtained by the hydrothermal treatment step has a composition other than water of the AFX zeolite as follows: M a / b Q c S 48-d Al d O 96 (wherein M represents a metal cation, a represents 1 to 10, b represents the valence of M, Q represents a cation derived from the compound represented by (1) and / or a salt thereof, c represents 0.5 to 2, and d represents 4 to 12).

[0136] The AFX zeolite having the above composition is also referred to as AFX zeolite before calcination. The AFX zeolite having the above composition is one of the present embodiments. The X-ray diffraction data of this AFX zeolite preferably includes the following 2θ values ​​(°): 7.50±0.15, 8.71±0.15, 11.60±0.15, 13.01±0.15, 15.67±0.15, 17.46±0.15, 17.72±0.15, 19.93±0.15, 20.42±0.15, 21.84±0.15, 23.47±0.15, 26.19±0.15, 27.79±0.15, 30.67±0.15, 31.65±0.15, and 33.56±0.15.

[0137] In the above composition formula, M is usually a Na cation. The above composition represents the composition per unit cell of AFX zeolite.

[0138] The AFX zeolite thus obtained may contain a structure-directing agent, an alkali metal, etc., in the pores, etc. Therefore, it is preferable to carry out a removal step for removing these, as necessary. The organic structure-directing agent, the alkali metal, etc., can be removed according to a conventional method, and the method is not particularly limited. For example, liquid-phase treatment using an acidic aqueous solution, liquid-phase treatment using an aqueous solution containing ammonium ions, liquid-phase treatment using a chemical solution containing a decomposition component of the organic structure-directing agent, exchange treatment using a resin, etc., baking treatment, etc. can be carried out. These treatments can be carried out in any combination. Among these, the organic structure-directing agent, the alkali metal, etc. are preferably removed by baking treatment from the viewpoint of production efficiency, etc.

[0139] The treatment temperature (calcination temperature) in the calcination treatment can be appropriately set depending on the raw materials used, etc., and is not particularly limited, but from the viewpoint of maintaining crystallinity and reducing the remaining proportion of the structure-directing agent, alkali metal, etc., the treatment temperature is usually 300° C. or higher and 1000° C. or lower, preferably 400° C. or higher and 900° C. or lower, more preferably 430° C. or higher and 800° C. or lower, and further preferably 480° C. or higher and 750° C. or lower. The calcination treatment is preferably carried out in an oxygen-containing atmosphere, for example, in the air.

[0140] The treatment time (calcination time) in the calcination treatment can be appropriately set depending on the treatment temperature, economic efficiency, etc., and is not particularly limited, but is usually 0.5 hours or more and 72 hours or less, preferably 1 hour or more and 48 hours or less, and more preferably 3 hours or more and 40 hours or less.

[0141] The AFX zeolite after calcination has a composition other than water of the AFX zeolite as follows: M a / b H 2c S 48-d Al d O 96 (wherein M is a metal cation, a is 1 to 10, b is the valence of M, Q is the compound represented by (1) above and / or a salt thereof, c is 0.5 to 2, and d is 4 to 12.) The AFX zeolite having the above composition is one embodiment of the present invention.

[0142] Moreover, one of the AFX zeolites of this embodiment is an AFX zeolite having an SAR (SiO2 / Al2O3 ratio) of 10 or more and 30 or less, an XRD chart obtained by powder X-ray diffraction analysis having the strongest line at 2θ=21.77°±0.15°, and an average particle diameter of 0.6 μm or more. This AFX zeolite can be obtained, for example, by subjecting the above-mentioned pre-calcined AFX zeolite to the above-mentioned calcination treatment. The X-ray diffraction data of this AFX zeolite preferably includes the following 2θ values ​​(°): 7.46±0.15, 8.69±0.15, 11.64±0.15, 12.93±0.15, 15.60±0.15, 17.43±0.15, 17.90±0.15, 19.81±0.15, 20.32±0.15, 21.77±0.15, 23.67±0.15, 26.03±0.15, 28.05±0.15, 30.49±0.15, 31.50±0.15, 33.71±0.15.

[0143] The average particle size of the AFX zeolite of this embodiment is preferably from 0.01 μm to 20 μm, more preferably from 0.6 to 6.0 μm, even more preferably from 0.7 μm to 4.0 μm, and particularly preferably from 1.0 μm to 3.5 μm.

[0144] In the above composition formula, M is usually a Na cation. The above composition represents the composition per unit cell of AFX zeolite.

[0145] <Ion exchange> After crystallization, the aluminosilicate may have metal ions, such as alkali metal ions, on its ion exchange sites. Depending on the desired performance, an ion exchange step may be carried out. In this ion exchange step, ammonium ions (NH4 + ) and protons (H +) or other nonmetallic cations. For example, the aluminosilicate can be ion-exchanged into the ammonium type by performing a liquid-phase treatment with an aqueous solution containing ammonium ions, such as an aqueous ammonium nitrate solution or an aqueous ammonium chloride solution. Also, the aluminosilicate can be ion-exchanged into the proton type by performing a calcination treatment after ion-exchanging with ammonia. In the above-mentioned manufacturing method, from the viewpoint of omitting the calcination treatment and high-temperature drying treatment by using a neutralized treatment solution in the P-supporting treatment, the ammonium ion (NH4 + ) type. The aluminosilicate thus obtained can be further treated, if necessary, to reduce the amount of acid. The treatment to reduce the amount of acid can be carried out, for example, by silylation, steam treatment, dicarboxylic acid treatment, etc. These treatments to reduce the amount of acid and to change the composition can be carried out according to conventional methods.

[0146] <Transition metal support> A transition metal-supported zeolite can also be obtained by supporting a transition metal on the above-mentioned aluminosilicate (aluminosilicate not supporting a transition metal) as necessary. The supporting treatment of the transition metal may be carried out according to a conventional method. By supporting a transition metal in this way, it can function as a catalyst in various applications. Examples of the transition metal supported here include, but are not limited to, copper (Cu), iron (Fe), tungsten (W), etc.

[0147] The supporting treatment of the transition metal may be carried out according to a conventional method. For example, the above-mentioned aluminosilicate may be contacted with a simple substance or compound of the transition metal, or a transition metal ion. The supporting method of the transition metal may be a method in which the transition metal is held at least in the ion exchange sites or pores of the aluminosilicate. The transition metal may be supplied as an inorganic acid salt of the transition metal, for example, a sulfate, a nitrate, an acetate, a chloride, an oxide, a composite oxide, and a complex salt of the transition metal. Among these, in the case of the P supporting treatment, it is preferable to supply the transition metal as a strong acid inorganic salt such as a sulfate or a nitrate, since a neutralized treatment liquid is used in the treatment. Specific methods include, but are not limited to, an ion exchange method, an evaporation to dryness method, a precipitation supporting method, a physical mixing method, a framework replacement method, and an impregnation supporting method. After the supporting treatment of the transition metal, if necessary, a solid-liquid separation treatment, a water washing treatment, and a drying treatment for removing moisture at a temperature of about 50 to 150 ° C. in the air may be carried out according to a conventional method.

[0148] If necessary, platinum group elements (PGM: platinum group metals) such as platinum, palladium, rhodium, and iridium may be supported on the aluminosilicate. The method of supporting the precious metal elements and platinum group elements can be applied by known methods and is not particularly limited. For example, a solution of a salt containing the precious metal elements and platinum group elements is prepared, the aluminosilicate is impregnated with this salt-containing solution, and then calcined, whereby the precious metal elements and platinum group elements can be supported. The salt-containing solution is not particularly limited, but is preferably a nitrate solution, a dinitrodiamine nitrate solution, an aqueous chloride solution, or the like. The calcination treatment is also not particularly limited, but is preferably performed at 350°C to 1000°C for about 1 to 12 hours. Prior to the high-temperature calcination, it is preferable to perform reduced pressure drying using a vacuum dryer or the like, and a drying treatment at about 50°C to 180°C for about 1 to 48 hours.

[0149] Next, the transition metal-unsupported zeolite and transition metal-supported zeolite thus prepared will be described. The transition metal-unsupported zeolite and transition metal-supported zeolite are crystalline aluminosilicates classified by the AFX structure code in the IZA. AFX-type zeolite has a structure in which the main framework metal atoms are aluminum (Al) and silicon (Si), and a network of these and oxygen (O). The structure is characterized by X-ray diffraction data.

[0150] The particle diameters of the transition metal-unsupported zeolite and the transition metal-supported zeolite are not particularly limited because they may vary depending on synthesis conditions, etc., but from the viewpoints of surface area, handleability, etc., the average particle diameter (D 50 ) is preferably from 0.01 μm to 20 μm, more preferably from 0.6 to 6.0 μm, even more preferably from 0.7 μm to 4.0 μm, and particularly preferably from 1.0 μm to 3.5 μm.

[0151] The silica-alumina ratio of the transition metal-unsupported zeolite or the transition metal-supported zeolite can be appropriately set and is not particularly limited, but from the viewpoint of thermal durability, catalytic activity, and the like in a high-temperature environment or after exposure to high temperatures, it is preferably from 7 to 30, more preferably from 8 to 25, and even more preferably from 10 to 20. By using an aluminosilicate with a silica-alumina ratio within the above-mentioned preferred numerical range, it tends to be easy to obtain a catalyst or catalyst carrier in which thermal durability and catalytic activity are highly balanced.

[0152] On the other hand, the content of the transition metal in the transition metal-supported small pore zeolite is not particularly limited, but is preferably 0.1 to 10 mass %, more preferably 0.5 to 8 mass %, based on the total amount.

[0153] The atomic ratio of the transition metal to aluminum (transition metal / aluminum) in the transition metal-supported small pore zeolite is not particularly limited, but is preferably 0.01 to 1.0, more preferably 0.05 to 0.7, and even more preferably 0.1 to 0.5.

[0154] As described above, the zeolite may support a transition metal. Thus, one of the zeolites of the present embodiment is an AFX zeolite having an SAR (SiO2 / Al2O3 ratio) of 10 or more and 30 or less, an XRD chart obtained by powder X-ray diffraction analysis showing the strongest line at 2θ=21.77°±0.15°, an average particle diameter of 0.6 μm or more, and a transition metal supported thereon.

[0155] The zeolite carrying the transition metal may be laminated on a honeycomb carrier to form a honeycomb laminated catalyst. The honeycomb laminated catalyst can be produced, for example, by wet-coating the AFX zeolite carrying the transition metal on a honeycomb carrier, drying at 100 to 150°C, and firing at 200 to 800°C. In this case, the amount of AFX zeolite applied is usually 10 to 1000g, preferably 50 to 300g, and more preferably 80 to 200g per 1L of the honeycomb carrier. One of the present embodiments is a honeycomb laminated catalyst including the AFX zeolite carrying the transition metal of the present embodiment and a honeycomb carrier.

[0156] <Method for producing the compound represented by formula (1) or a salt thereof> One of the manufacturing methods of this embodiment is as follows: A step (Step I) of preparing a compound represented by formula (A); a step (step II) of reacting the compound represented by formula (A) with a hydrogen source using a catalyst to obtain a compound represented by formula (2); A step of N-alkylating the compound represented by the formula (2) using an alkylating agent (step III); The present invention relates to a method for producing a compound represented by formula (1) or a salt thereof, the method comprising the steps of: [ka]

[0157] R in the above formula (A) and formula (2) 1 and R 2 are each independently an alkyl group.1 ~R 4 are each independently an alkyl group.

[0158] (Process I) Step I is a step of preparing a compound represented by formula (A). The compound represented by formula (A) may be obtained as a commercially available product, or may be appropriately synthesized by a known synthesis route. For example, the compound may be obtained by synthesis by reacting commercially available bicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarboxylic dianhydride with an alkylamine or a salt thereof.

[0159] (Process II) Step II is a step of reacting the compound represented by formula (A) with a hydrogen source using a catalyst to obtain a compound represented by formula (2), which can be represented by the following scheme: Here, the compound represented by formula (A) is also called N,N'-dialkylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarboxydiimide. [ka]

[0160] R in the above scheme 1 and R 2 are each independently an alkyl group. R in the compounds represented by formula (2) and formula (A) 1 and R 2 is R in formula (1). 1 and R 2 The preferred substituents are the same as those in the formula (1). 1 and R 2 The same groups as those shown below can be mentioned.

[0161] This production method does not require the use of a strong reducing agent that is difficult to handle, such as a reducing agent that poses a risk of ignition, and therefore can safely and easily produce the compound N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine represented by formula (2). Furthermore, this production method allows synthesis under relatively safe conditions, so the burden on equipment is small and large-scale production is possible, thereby improving the productivity and economy of the compound represented by formula (2).

[0162] The hydrogen source used in the production method of this embodiment can be appropriately selected from those capable of hydrogenating the compound represented by formula (A).Specific examples include, but are not limited to, molecular hydrogen such as hydrogen gas; hydrogen donors such as ammonium formate, sodium formate, and hydrazine; and the like.Of these hydrogen sources, molecular hydrogen is preferred.

[0163] The catalyst used in the production method of the present embodiment can be any catalyst that can be generally used for hydrogenation, and the type of catalyst is not particularly limited. The catalyst is preferably a heterogeneous catalyst. By using a heterogeneous catalyst, the operation such as post-treatment is simple, and the productivity and economy of the compound are improved even when produced in large batches. The catalyst is preferably a transition metal-containing catalyst. Examples of transition metals include palladium (Pd), platinum (Pt), rhodium (Rh), vanadium (V), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), ruthenium (Ru), rhenium (Re), osmium (Os), molybdenum (Mo), tungsten (W), etc. These metals may be used alone or in combination of two or more. The transition metal may be supported on a carrier. The carrier is not particularly limited as long as it is a carrier that is usually used as a catalyst carrier. For example, inorganic oxides, activated carbon, ion exchange resins, etc. are included. Specific examples of inorganic oxides include silica (SiO2), titania (TiO2), zirconia (ZrO2), alumina (Al2O3), magnesium oxide (MgO), tricalcium phosphate (HAP; hydroxyapatite), and composites of two or more of these inorganic oxides (e.g., zeolite, etc.).

[0164] The amount of the catalyst used is not particularly limited, but is usually 0.01 to 10 mol %, preferably 0.1 to 5 mol %, in terms of the amount of metal in the catalyst relative to the amount of the compound represented by formula (2).

[0165] The catalyst used in the above production method is preferably a catalyst in which Pt and V are supported on a carrier. By using a catalyst in which Pt and V are supported on a carrier, the compound represented by formula (2) can be reduced under milder conditions. In this specification, a catalyst in which Pt and V are supported on a support is also referred to as "Pt-V / Z," where Z represents the support.

[0166] The platinum constituting the Pt-V / Z is not particularly limited, but is preferably, for example, platinum particles. Here, the platinum particles are at least one type of particles of platinum metal or platinum oxide, and are preferably platinum metal particles. The platinum particles are not particularly limited as long as they contain at least platinum, and may contain small amounts of precious metals such as ruthenium, rhodium, and palladium. The platinum particles may be primary particles or secondary particles. The average particle size of the platinum particles is preferably 1 to 30 nm, more preferably 1 to 10 nm. The average particle size refers to the average value of the diameters of any number of particles observed under an electron microscope.

[0167] The vanadium constituting the Pt-V / Z is not particularly limited, but is preferably, for example, vanadium oxide. Examples of vanadium oxide include vanadate ions (VO4 3- , VO3 3- ), vanadium pentoxide, vanadium(II) oxide, vanadium(IV) oxide, etc. Among these vanadium oxides, V2O5 is preferred.

[0168] The composition ratio of Pt to V in the above Pt-V / Z is preferably 1:0.001-10, and more preferably 1:0.005-5, calculated as the number of moles of Pt as metal:V as metal.

[0169] The carrier Z in the Pt-V / Z is not particularly limited, but may have an adsorption capacity of 0.1 to 300 m in terms of BET value. 2 / g, and the average particle size may be 0.02 to 200 μm. The form of the carrier is not particularly limited, but examples thereof include powder, spherical particles, irregular granules, cylindrical pellets, extrusions, rings, and the like. Of the above-mentioned carriers, HAP is preferred as a component constituting the carrier.

[0170] The Pt-V / Z can be produced by mixing a mixed solution of a platinum compound and a vanadium compound with a carrier to obtain a mixture, and then drying the mixture. Examples of the platinum compound include platinum complex salts such as platinum acetylacetonate (Pt(acac)2), tetraammineplatinum(II) acetate, dinitrodiammineplatinum(II), hexaammineplatinum(II) carbonate, and bis(dibenzalacetone)platinum(0), as well as salts such as platinum chloride and potassium tetrachloroplatinate. Among these platinum compounds, Pt(acac)2 is preferred. Examples of the vanadium compound include vanadyl acetylacetonate (VO(acac)2), vanadium complex salts such as tetramethylammonium bis(tartrate)bis[oxovanadate(IV)]ate, ammonium vanadate(V), vanadium naphthenate, etc. Among these vanadium compounds, VO(acac)2 is preferred.

[0171] The mixed solution in the production of the Pt-V / Z is a solution in which a platinum compound and a vanadium compound are suspended or dissolved in a solvent. Examples of the solvent include water and organic solvents such as alcohol and acetone. These solvents may be used alone or in combination of two or more.

[0172] The mixture is mixed with a carrier. The method for mixing the mixture with the carrier is not particularly limited as long as each component is sufficiently dispersed. The amount of the carrier is preferably 0.1 to 100 g, more preferably 1 to 10 g, per 0.1 mmol of platinum in metal equivalent. After mixing with the carrier, it is preferable to stir for 0.5 to 12 hours. The mixture of the mixed solution and the carrier is dried after removing the solvent with a rotary evaporator or the like. The drying is preferably performed, for example, at 80 to 200° C. for 1 to 60 hours. After drying, the dried product is preferably pulverized as necessary and fired using a muffle furnace or the like.

[0173] Specifically, the production method of this embodiment includes a method in which a compound represented by formula (A) is prepared, mixed with a catalyst and a hydrogen source, and reacted. Here, the compound represented by formula (A), the catalyst, and the hydrogen source may be mixed in any order. From the viewpoint of workability, in the production method of the present embodiment, it is preferable to mix the compound represented by formula (A) and the catalyst, add a solvent as necessary, and then introduce the hydrogen source into the reactor. In the production method of the present embodiment, molecular sieves may be added to the reaction system in order to proceed with the reaction under low temperature and low pressure conditions. The amount of molecular sieves added is preferably 0.1 to 10 times, and more preferably 0.5 to 5 times, the mass of the compound represented by formula (A).

[0174] Step II in this embodiment may be carried out in the presence of a solvent, that is, in a wet process. The solvent is not particularly limited as long as it can dissolve the compound represented by formula (A), and may be appropriately selected depending on the reaction temperature, reactants, etc. Examples of the solvent include water, aromatic hydrocarbon solvents such as benzene and toluene, amide solvents such as acetonitrile, N,N-dimethylacetamide and N,N-dimethylformamide, ether solvents such as tetrahydrofuran (hereinafter also referred to as THF), diethyl ether and 1,2-dimethoxyethane, alcohol solvents such as methanol, ethanol and isopropanol, halogen solvents such as dichloromethane, dichloroethane and chloroform, etc. These solvents can be used alone or in any combination and ratio of two or more. Among these solvents, ether solvents are preferred, and 1,2-dimethoxyethane is more preferred.

[0175] The use of a solvent and its amount may be appropriately determined in consideration of other reaction conditions and is not particularly limited. The concentration of the compound represented by formula (A) in the reaction mixture is preferably 0.001 to 10 mol / L, more preferably 0.01 to 5 mol / L, and even more preferably 0.01 to 3 mol / L.

[0176] The amount of the catalyst used is preferably 0.1 to 50 times, more preferably 0.5 to 20 times, and even more preferably 1 to 10 times, the mass of the compound represented by formula (A).

[0177] The reaction temperature is not particularly limited, but is usually in the range of 20 to 200°C, preferably 50 to 150°C, and more preferably 50 to 120°C. The reaction time may be appropriately adjusted by monitoring the progress of the reaction using GC-MS or the like, and is usually 1 minute to 100 hours, preferably 0.5 hours to 70 hours, and more preferably 1 hour to 60 hours.

[0178] In the production method of this embodiment, when molecular hydrogen is used, the hydrogen pressure in the reactor is usually 0.1 to 10 MPa, preferably 1.0 to 10 MPa, and more preferably 2.0 to 8.0 MPa.

[0179] When a solvent is used in the reaction, the mixture after the reaction in step II may be used as a raw material, precursor, or intermediate as it is after concentrating the resulting reaction solution as necessary, or the reaction mixture may be appropriately post-treated to obtain the compound represented by formula (2). Specific methods for post-treatment include known purification methods such as washing with water, filtration, drying, extraction, distillation, and chromatography. Two or more of these purification methods may be combined.

[0180] (Process III) Step III is a step of N-alkylating the compound represented by formula (2) using an alkylating agent, and can be represented by the following scheme: Here, the compound represented by the following formula (2) is also called N,N'-dialkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine. [ka]

[0181] In the prior art, N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium hydroxide has been used in the synthesis of zeolites (see U.S. Patent Application Publication No. 6,049,018 (Patent Document 1) and JP-A-2016-169139 (Patent Document 2)). In the synthesis of the above hydroxide, N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium iodide obtained as a solid powder is ion-exchanged with a hydroxide-type anion exchange resin and concentrated to obtain a hydroxide solution. On the other hand, as described above, the compound (salt) of the present embodiment can be directly used in the synthesis of zeolites as a salt obtained by alkylation, that is, a salt in which X is a counter anion. Therefore, in this case, the labor of preparing the hydroxide can be saved, and the production of zeolites can be efficiently performed. Further, for example, when used as a hydroxide, it may be ion-exchanged with a hydroxide-type anion exchange resin and concentrated in the same manner as in the prior art.

[0182] <Method for Producing AFX-Type Zeolite> One embodiment of the present invention is a method for producing an AFX-type zeolite, the production method including at least a step of preparing a mixture containing a silica and alumina source, an organic structure-directing agent (OSDA) containing the compound represented by the following (1) and / or its salt, an alkali metal hydroxide, and water, and a step of hydrothermally treating the mixture to synthesize an AFX-type zeolite. [Chemical formula] (In the above formula (1), R 1 ~R 4 are each independently an alkyl group.)

[0183] By the method for producing an AFX-type zeolite of the present embodiment, the AFX-type zeolite of the present embodiment can be obtained.

[0184] <AFX-Type Zeolite Having Macropores> One of the present embodiments is an AFX zeolite having macropores. The macropores in this embodiment are defined according to the IUPAC definition. Specifically, the macropores refer to pores having a pore diameter of more than 50 nm. The fact that the AFX zeolite has macropores can be determined from an SEM image of the zeolite.

[0185] The AFX zeolite having macropores of this embodiment can be produced, for example, by using an organic structure directing agent (OSDA) containing a compound represented by formula (1) and / or a salt thereof. Specifically, the AFX zeolite having macropores of this embodiment can be produced by the above-mentioned method for producing AFX zeolite. That is, it can be produced by a production method including at least a step of preparing a mixture containing at least silica and alumina sources, an organic structure directing agent (OSDA) containing a compound represented by the following (1) and / or a salt thereof, an alkali metal hydroxide, and water, and a step of hydrothermally treating the mixture to synthesize AFX zeolite. EXAMPLES

[0186] The features of the present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. In addition, the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limits in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or the values ​​of the examples.

[0187] Examples and Comparative Examples relating to the specific embodiment of the first group are referred to as Example A and Comparative Example A, respectively. Preparation Examples, Examples and Reference Examples relating to the specific embodiment of the second group are referred to as Preparation B, Example B and Reference Example B, respectively. Preparation Examples, Examples and Comparative Examples relating to the specific embodiment of the third group are referred to as Preparation C, Example C and Comparative Example C, respectively. It should be noted that the examples relating to the specific embodiment of the fourth group are included in the examples relating to the specific embodiments of the first group or the third group.

[0188] [Example A1: Synthesis of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide] 370.0 g of N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine (molecular weight 246.39) synthesized according to Patent Document 2 was dissolved in 1,200 mL of isopropyl alcohol (IPA) modified alcohol, and 31.08 g of 5% palladium carbon catalyst (K-type water-containing product manufactured by N.E. Chemcat) was added in dry mass equivalent (equivalent to 1.0 mol% of the substrate as palladium), and the reaction was carried out for 190 hours at 50°C under normal pressure hydrogen. The conversion rate of the substrate was 99% or more by gas chromatography (GC). After filtering to remove the catalyst, 516.0 g of ethyl iodide (molecular weight 155.11, 2.2 equivalents) was added dropwise while stirring. After gently refluxing for 16 hours under a nitrogen atmosphere, the mixture was allowed to cool, filtered, washed with acetone, and dried to obtain 703.0 g (90% yield) of the desired product, N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide as a white powder. The resulting white powder 1 H-NMR and 13 The C-NMR spectrum is shown below. 1 H-NMR (400MHz, D2O) δ: 3.82 (dd, 4H), 3.49 (q4, 4H), 3.38 (q4, 4H), 3.33 (d, 4H), 2.69 (m, 4H), 1.80 (s, 2H), 1.64 (s, 4H), 1.36 (t, 6H), 1.31 (t, 6H). 13C-NMR(100Hz, D2O) δ: 65.00(×4), 58.51(×2), 54.41(×2), 40.11(×4), 28.33(×2), 14.86(×2), 11.01(×2), 10.17(×2) N,N,N',N'-Tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide in DO solution 1 The H-NMR spectrum data is shown in FIG. 13 The C-NMR spectrum data is shown in Figure 2.

[0189] The gas chromatography conditions were as follows: Instrument name: GCMS-QP2010 (Shimadzu Corporation) Column: SHIMADZU SH-Rtx-200MS Carrier gas: Helium Total flow rate: 98.9mL / min Column flow rate: 2.56mL / min Temperature: The column oven was heated from 40° C. to 300° C. at a rate of 10° C. / min. Then, the temperature was kept at 300° C. for 10 min.

[0190] The NMR measurement conditions were as follows: Device name: Ascend4000 (BRUKER) Measurement method: 1 H-NMR and 13 C-NMR was measured by dissolving the sample in deuterium oxide.

[0191] [Example A2: Synthesis of AFX-type zeolite] 28.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62), 116.0 g of 4.8 mass% sodium hydroxide solution, 37.5 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 47.0 g of water were stirred in a polyethylene beaker for 48 hours. The composition of the mixture was as follows:

[0192] [Table 1]

[0193] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 300 cc stainless steel sealed pressure vessel with a Teflon (registered trademark) inner cylinder and allowed to stand at 170°C for 40 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. Figure 3 shows the solid-state NMR spectrum data (B) of AFX zeolite obtained using N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium. In Figure 3, A is the solid-state NMR spectrum data of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium, and C is the solid-state NMR spectrum data of the DO solution. 13 CNMR spectrum data. The * in C in the figure indicates the peak of the internal standard (4,4-dimethyl-4-silapentane-1-sulfonic acid). FIG. 4 shows an XRD chart of the AFX zeolite obtained in Example A2.

[0194] The conditions for the powder X-ray diffraction measurement were as follows. Device name: X'Pert Pro (Spectris Corporation) Measurement method: The powder sample was filled into a grooved glass sample plate container and used for measurement. The X-ray source was CuKα radiation, the tube voltage was 45 kV, and the tube current was 40 mA.

[0195] [Example A3: Synthesis of AFX-type zeolite] 120.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62) was dissolved in 800 mL of water, and 800.0 g of Diaion SA10AOH (manufactured by Mitsubishi Chemical Corporation) was added and stirred at room temperature for 48 hours. After filtration and washing, the filtrate and washings were combined and concentrated to a mass of 379.9 g, obtaining 19.26 mass% N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium dihydroxide (molecular weight 340.55). 6.5 g of this solution was mixed with 6.2 g of 4.8% sodium hydroxide solution, 4.0 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 5.8 g of water in a polyethylene beaker and stirred for 72 hours. The composition of the mixture was as follows:

[0196] [Table 2]

[0197] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 50 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and allowed to stand at 170° C. for 96 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of water and dried at 105° C. to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. FIG. 5 shows an XRD chart of the AFX zeolite obtained in Example A3.

[0198] Table 3 shows the main peak positions, and Table 4 shows the relative intensities of each XRD peak of the AFX zeolite obtained by Examples A2 and A3, when the integrated intensity of the strongest peak (2θ = 20.42°) of the AFX zeolite obtained by Example A2 is set to 1.0.

[0199] [Table 3]

[0200] [Table 4]

[0201] The composition of the AFX zeolite obtained in Example A2, excluding water, was as follows. M a / b Q c S 48-d Al d O 96 (In the formula, M represents a metal cation, a represents 1 to 10, b represents the valence of M, Q represents an N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium cation, c represents 0.5 to 2, and d represents 4 to 12.) The composition of the AFX zeolite obtained in Example A2, excluding water, was specifically a=5.0, b=1.0, c=1.3, and d=7.6.

[0202] [Comparative Example A1: Synthesis of AFX-type zeolite] A product was obtained in the same manner as in Example A1, except that 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62) was replaced with 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium diiodide (molecular weight 556.61) synthesized according to the method of Patent Document 2. Powder X-ray diffraction analysis confirmed that beta zeolite was produced in addition to AFX zeolite. FIG. 6 shows an XRD chart of the AFX zeolite obtained in Comparative Example A1.

[0203] [Example A4: Production of AFX zeolite including a calcination step] The mixture was stirred in a polyethylene beaker for 48 hours with 3.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide, 12.7 g of 4.8% by mass sodium hydroxide solution, 4.2 g of FAU-type zeolite CBV712, and 2.7 g of water. The mixture had the following composition:

[0204] [Table 5]

[0205] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 50 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and left to stand at 170°C for 40 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the resulting solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Next, the temperature was raised to 600°C at a rate of 1°C / min and then calcined for 5 hours. When the obtained powder was subjected to powder X-ray diffraction analysis, it was confirmed that the product was a single phase of AFX zeolite. FIG. 7 shows an XRD chart of the AFX zeolite obtained in Example A4.

[0206] [Example A5: Production of AFX zeolite including a calcination step] The amount of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide used was 310.0 g, the amount of 4.8 mass% sodium hydroxide solution used was 1310.0 g, the amount of FAU type zeolite CBV712 used was 425.0 g, and the amount of water used was 335.0 g, and the mixture was stirred in a polyethylene beaker for 48 hours. The composition of the mixture was as follows.

[0207] [Table 6]

[0208] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, 1450 g of this raw material composition (mixture) was placed in a 1 L stainless steel autoclave, stirred at 300 rpm, and held at 170°C for 60 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the resulting solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Next, the temperature was raised to 600°C at a rate of 1°C / min, and then calcined for 5 hours. The SAR (SiO2 / Al2O3 ratio) calculated as the solid content, measured by fluorescent X-ray analysis of the obtained powder, was 10.7. The conditions for the powder X-ray diffraction measurement were as follows. For the X-ray fluorescence analysis, an Axios (Spectris Inc., PANalytical Division) was used as the device. Five grams of the measurement sample was placed in a polyvinyl chloride ring, pressurized with a load of 20 tons, and then subjected to the measurement. The analysis software used was UniQuant5. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX-type zeolite. FIG. 8 shows an XRD chart of the AFX zeolite obtained in Example A5.

[0209] [Example A6: Production of AFX zeolite including a calcination step] 9.0 g of the 19.26 mass% N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium dihydroxide (molecular weight 340.55) solution obtained in Example A3 was stirred in a polyethylene beaker for 48 hours with 2.5 g of 4.8% sodium hydroxide solution, 4.1 g of FAU-type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), 1.0 g of sodium chloride, and 5.8 g of water. The composition of the mixture was as follows.

[0210] [Table 7]

[0211] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 50 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and left to stand at 155°C for 240 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the resulting solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Next, the temperature was raised to 600°C at a rate of 1°C / min and then calcined for 5 hours. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. FIG. 9 shows an XRD chart of the AFX zeolite obtained in Example A6.

[0212] [Comparative Example A2: Production of AFX zeolite including a calcination step] Instead of the N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium dihydroxide solution, 7.7 g of 17.4 mass% N,N,N',N'-tetraethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidinium dihydroxide (molecular weight 338.53) synthesized according to the method of Patent Document 2, 3.1 g of 4.8% sodium hydroxide solution, 3.0 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 3.5 g of water were stirred in a polyethylene beaker for 48 hours. The composition of the mixture was as follows.

[0213] [Table 8]

[0214] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was treated in the same manner as in Example A6 to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. FIG. 10 shows an XRD chart of the AFX zeolite obtained in Comparative Example A2.

[0215] <Measurement of hydrothermal durability> Weighed 2.0 g each of the AFX-type zeolite powders of Example A4, A5, and A6 and Comparative Example A2 into a crucible, placed them in an electric furnace (trade name: OXK-600X, manufactured by Koei Electric Furnace Co., Ltd.) connected to a gas humidifying device (trade name: RMG-1000, manufactured by J Science Lab Co., Ltd.), and held them at 750 °C for 40 hours under a supply of Air containing 10% water vapor at a flow rate of 70 L / min to measure the hydrothermal durability. Table 9 shows the change in the integrated intensity of each XRD peak before and after the measurement of hydrothermal durability for each sample. The numerical values of each peak intensity are relative values when the integrated intensity of the strongest peak (2θ = 21.77°) of the AFX-type zeolite before the hydrothermal durability measurement obtained in Example A4 is set to 1.0. Also, at the bottom of the table, the relative values of the total integrated intensity of each Example and Comparative Example are shown when the total integrated intensity in Example A4 before the hydrothermal durability measurement is set to 100%. Also, Figure 11 shows the change in the total integrated intensity of the XRD peaks before and after the measurement of hydrothermal durability for each sample. As shown in Figure 11, the slopes of the numerical changes before and after the measurement in Example A4, A5, and A6 are suppressed more than those in Comparative Example A2, indicating that they are excellent in hydrothermal durability.

[0216]

Table 9

[0217] <SEM image> SEM images of the AFX-type zeolites obtained in Example A4, Example A5, Example A6, and Comparative Example A2 are shown in Figures 12, 13, 14, and 15, respectively. The average particle diameters of the AFX-type zeolites in Example A4, Example A5, and Example A6 were approximately 3.84 μm, approximately 0.70 μm, and approximately 3.13 μm, respectively, and the coefficients of variation were 30.4%, 36.9%, and 24.9%, respectively. The median particle diameters were 3.60 μm, 0.67 μm, and 3.15 μm, respectively. On the other hand, the average particle diameter of the AFX-type zeolite in Comparative Example A2 was 0.3 μm, the coefficient of variation was 55.6%, and the median particle diameter was 0.45 μm. It was considered that the hydrothermal durability was improved due to the SAR being 10-30, the strongest line being at 2θ=21.77°±0.15°, and the average particle diameter being 0.6 μm or more. The average particle size was measured by taking a 6000x image using a scanning electron microscope (SEM, manufactured by Phenom-World) at an accelerating voltage of 10 kV, randomly selecting 100 particles from the image, and measuring the longest diameter of the particles. The average value of the longest diameter of each particle was taken as the average particle size, and the median value was taken as the median particle size. Furthermore, the AFX zeolites of Examples A4, A5, and A6 included particles having macropores. The presence of macropores in the AFX zeolite particles was confirmed from SEM images.

[0218] [Example A7: Production of AFX zeolite including a calcination step and an ion exchange step] 930 g of the raw material composition (mixture) obtained in Example A5 was placed in four stainless steel sealed pressure vessels with 300 ml Teflon inner cylinders and held at 170°C for 40 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the solid phase obtained was washed with a sufficient amount of water and dried at 105°C to obtain a product. The product was then heated to 600°C at a heating rate of 1°C / min and calcined for 5 hours. Ion exchange was repeated three times using an ammonium nitrate aqueous solution containing the same amount of ammonium nitrate and 10 times the amount of water, followed by washing with a sufficient amount of pure water and drying at 120°C to obtain NH4 + AFX-type zeolite was obtained.

[0219] (Cu supported) The obtained NH4 +120.0 g of AFX zeolite was impregnated with a mixture of 36.0 g of 50% copper nitrate trihydrate aqueous solution and 30.0 g of water, and then dried at 100 to 120 ° C. This was impregnated with a mixture of 7.0 g of morpholine and 35 g of water in an environment of 25 ° C., and dried again at 100 to 120 ° C. to obtain Cu-supported AFX zeolite of Example A7. The amount of Cu supported in terms of solid content measured by fluorescent X-ray analysis was 4.22 mass%, and the SAR (SiO2 / Al2O3 ratio) was 10.7. When the obtained powder was subjected to powder X-ray diffraction analysis, it was confirmed that the product was a single phase of AFX zeolite. Fig. 16 shows an XRD chart of the Cu-supported AFX zeolite of Example A7, and Fig. 17 shows an SEM image of the Cu-supported AFX zeolite of Example A7. The average particle size of the Cu-supported AFX zeolite of Example A7 was about 2 µm. From the SEM image, the AFX zeolite of Example A7 included particles having macropores.

[0220] (Manufacturing honeycomb laminated catalysts) The obtained Cu-supported AFX zeolite of Example A7 was wet-coated on a honeycomb carrier so that the loading ratio was 180 g per 1 L of honeycomb carrier, and then fired at 500° C. This resulted in the honeycomb laminated catalyst of Example A7, in which a catalyst layer containing Cu-supported AFX zeolite was provided on a honeycomb carrier.

[0221] [Comparative Example A3: Synthesis of CHA-type zeolite] 2,080g of water, 826g of amorphous synthetic aluminum silicate (manufactured by Kyowa Chemical Industry, synthetic aluminum silicate, trade name: Kyoward (registered trademark) 700PEL, SAR: 10.0), 320.0g of colloidal silica (manufactured by Nissan Chemical Industry, trade name: Snowtex (registered trademark) 40, SiO2 content: 39.7%), 133.0g of 48% sodium hydroxide (manufactured by Kanto Chemical Industry), and 23.0g of chabazite seed crystals (SAR10) were added to 930.0g of N,N,N-trimethyladamanta ammonium hydroxide 25% aqueous solution (hereinafter sometimes referred to as "TMAdaOH 25% aqueous solution"), and mixed thoroughly to obtain a raw material composition (mixture). The composition (molar ratio) of the raw material composition was as follows.

[0222] [Table 10]

[0223] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. This raw material composition (mixture) was placed in a 5,000cc stainless steel autoclave and sealed, and then heated to 160°C while stirring at 300 rpm, and held for 48 hours, and then held at 170°C for 24 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the obtained solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of pure CHA-type zeolite. Fluorescent X-ray analysis showed that the silica-alumina ratio (SiO2 / Al2O3) of the obtained CHA-type aluminosilicate of Comparative Example A3 was 11.3. From the obtained CHA type zeolite of Comparative Example A3, NH4 + The CHA type zeolite was obtained.

[0224] (Cu-loaded CHA zeolite) The obtained NH4 +120.0 g of CHA-type zeolite was impregnated with a mixture of 34.0 g of 50% copper nitrate trihydrate aqueous solution and 30.0 g of water, and then dried at 100 to 120 ° C. This was impregnated with a mixture of 12.0 g of morpholine and 48.0 g of water in an environment of 25 ° C., and dried again at 100 to 120 ° C. to obtain Cu-supported CHA-type zeolite. The amount of Cu supported in terms of solid content measured by fluorescent X-ray analysis was 3.9 mass%, and the SAR (SiO2 / Al2O3 ratio) was 11.3. Figure 18 shows an SEM image. The average particle size was about 0.2 μm.

[0225] (Manufacturing honeycomb laminated catalysts) A honeycomb laminated catalyst of Comparative Example A3 was obtained in the same manner as in Example A7, except that the obtained Cu-supported CHA-type zeolite of Comparative Example A3 was used.

[0226] [Comparative example A4] 2,800g of water, 45.0g of sodium aluminate (manufactured by Wako Pure Chemical Industries, Ltd.), 220.0g of precipitated silica (manufactured by Tosoh Silica Corporation, trade name: Nipsil (registered trademark) ER), 60.0g of J sodium silicate No. 3 (manufactured by Nippon Chemical Industry Co., Ltd., SiO2 content 29 mass%, Na2O content 9.5 mass%), and 20g of chabazite seed crystals (SAR13) were added to 330.0g of 25% TMAdaOH aqueous solution, and thoroughly mixed to obtain a raw material composition. The composition (molar ratio) of the raw material composition was as follows.

[0227] [Table 11]

[0228] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. This raw material composition was placed in a 5,000cc stainless steel autoclave and sealed, and then heated to 160°C while stirring at 300 rpm and held for 48 hours. The product after this hydrothermal treatment was separated into solid and liquid, and the resulting solid phase was washed with a sufficient amount of water and dried at 105°C to obtain the product. Powder X-ray diffraction analysis confirmed that the product was a single phase of CHA zeolite. Furthermore, fluorescent X-ray analysis showed that the silica-alumina ratio (SiO2 / Al2O3) of the obtained CHA-type aluminosilicate was 13.4.

[0229] The obtained CHA-type zeolite of Comparative Example A4 was treated with NH4 + type CHA zeolite) was obtained.

[0230] (Cu support on CHA type zeolite) The obtained NH4 + 160.0 g of the CHA-type zeolite was impregnated with a mixture of 42.0 g of 50% copper nitrate trihydrate aqueous solution and 42.0 g of water, and then dried at 100 to 120°C to obtain Cu-loaded CHA-type zeolite. The amount of Cu loaded in terms of solid content measured by fluorescent X-ray analysis was 4.8 mass%, and the SAR (SiO2 / Al2O3 ratio) was 13.4. Figure 19 shows an SEM image. The average particle diameter was about 0.3 μm. On the other hand, the primary particle diameter was even finer, less than 0.1 μm.

[0231] (Manufacturing honeycomb laminated catalysts) A honeycomb laminated catalyst of Comparative Example A4 was obtained in the same manner as in Example A7, except that the obtained Cu-supported CHA-type zeolite of Comparative Example A4 was used.

[0232] <Laboratory measurement of nitrogen oxide reduction efficiency> The honeycomb laminated catalysts of Example A7, Comparative Example A3 and Comparative Example A4 were cut into a cylindrical shape with a diameter of 25.4 mmφ×length of 50 mm, and placed in an electric furnace (product name OXK-600X, manufactured by Kyoei Electric Furnace Manufacturing Co., Ltd.) connected to a gas humidifier (product name RMG-1000, manufactured by J Science Lab Co., Ltd.), and were held at 650°C for 100 hours under a flow rate of 70 L / min of air containing 10% water vapor, to measure hydrothermal durability. The sample after hydrothermal durability was set in a catalyst evaluation device (product name SIGU-2000, manufactured by Horiba, Ltd.), and the gas composition was analyzed with an automobile exhaust gas measurement device (product name MEXA-6000FT, manufactured by Horiba, Ltd.) to measure the nitrogen oxide reduction efficiency in a steady air flow of a model gas. Here, a model gas containing 210 ppm NO, 40 ppm NO2, 250 ppm NH3, 4% H2O, 10% O2, and the balance N2 was used. Measurements were performed in the temperature range of 170°C to 500°C, with a space velocity of SV = 59,000 h -1 So I went. The results are shown in Table 12.

[0233] [Table 12]

[0234] In this way, the compound of the present invention can obtain a single phase of AFX zeolite whether in the form of an iodide or hydroxide. In other words, the compound of the present invention can be used to prepare AFX zeolite without the need to convert the iodide into another salt, and the desired AFX zeolite can be obtained as a single substance, so the compound has high performance as an OSDA.

[0235] [Production Example B1: Preparation of Pt-V / HAP catalyst] Pt(acac)2 (platinum acetylacetonate, 0.4 mmol) from N.E. Chemcat and VO(acac)2 (vanadyl acetylacetonate, 0.4 mmol) from Sigma-Aldrich were added to 90 mL of acetone and stirred at room temperature for 30 minutes. 1.0 g of HAP (trade name "tricalcium phosphate") from Wako Pure Chemical Industries was added and stirred at room temperature for 4 hours. The solvent was removed from the mixture using a rotary evaporator to obtain a pale green powder. The powder was dried at 110°C overnight. The dried powder was then crushed in an agate bowl and calcined at 300°C for 3 hours in air to obtain a dark gray powder (Pt-V / HAP).

[0236] [Example B1: Synthesis of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide] (Synthesis of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine) 0.3 g of Pt-V / HAP obtained in Production Example B1, 0.3 mmol of N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarbonyldiimide synthesized according to the method of Patent Document 2, and 0.1 g of molecular sieves 4Å from Wako Pure Chemical Industries, Ltd. were added to a 50 mL stainless steel autoclave, and 5 mL of 1,2-dimethoxyethane (DME) as a solvent was added, and the hydrogenation reaction was carried out for 48 hours at a reaction temperature of 150°C and a hydrogen pressure of 5 MPa. After the reaction, the yield of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine was measured using GC-MS, and the yield was 77%. The product was isolated and the results of NMR measurement are shown below. 1 H NMR (400 MHz, CDCl3) δ = 2.72 (t, J = 17 Hz, 4H), 2.49 (dd, J = 30, 14 Hz, 4H), 2.43 (dd, J = 18, 10 Hz, 4H), 2.21 (s, 4H), 1.57 (s, 4H), 1.40 (s, 2H), 1.14 (t, J = 15 Hz, 6H); 13C NMR (100 MHz, CDCl3) δ = 57.0(×4), 50.2(×2), 40.7(×4), 30.6(×2), 14.6(×2), 13.9(×2).

[0237] (Synthesis of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide) A 50 mL ethanol solution of 2.2 g of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine (molecular weight 248.41) synthesized above was placed in a 100 mL flask, and 6.0 g of ethyl iodide (molecular weight 155.97, liquid, Tokyo Chemical Industry) was added dropwise. After refluxing for 2 days under a nitrogen atmosphere, the solution was allowed to cool, filtered, washed with acetone, and dried to obtain 2.6 g (yield 52%) of the target product, N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide, as a white powder. The white powder obtained 1 H-NMR and 13 The C-NMR is shown below. 1 H NMR(400MHz, D2O) δ: 3.82 (dd, 4H), 3.49 (q4, 4H), 3.38 (q4, 4H), 3.33 (d, 4H), 2.68(m, 4H), 1.80 (s, 2H), 1.64 (s, 4H), 1.36 (t, 6H), 1.31 (t, 6H) 13 C NMR(400Hz, CDCl3) δ: 65.00(×4), 58.51(×2), 54.41(×2), 40.11(×4), 28.33(×2), 14.86(×2), 11.01(×2), 10.1(×2) N,N,N',N'-Tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide 1 The HNMR spectrum data is shown in Figure 20. 13 The CNMR spectrum data is shown in FIG.

[0238] [Reference Example B1: Synthesis of AFX-type zeolite] 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62), 8.4 g of 4.8 mass% sodium hydroxide solution, 2.7 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 3.3 g of water were stirred in a SUS beaker for 48 hours. The composition of the mixture was as follows:

[0239] [Table 13]

[0240] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 50 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and allowed to stand at 170° C. for 48 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of water and dried at 105° C. to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. FIG. 22 shows the XRD data of the AFX zeolite.

[0241] [Reference Example B2: Synthesis of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide] 370.0 g of N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-dipyrrolidine (molecular weight 246.39) synthesized according to Patent Document 2 was dissolved in 1,200 mL of isopropyl alcohol (IPA) modified alcohol, and 31.08 g of 5% palladium carbon catalyst (K-type water-containing product manufactured by N.E. Chemcat) was added in dry mass equivalent (equivalent to 1.0 mol% of the substrate as palladium), and the reaction was carried out for 190 hours at 50°C under normal pressure hydrogen. The conversion rate of the substrate was 99% or more by gas chromatography (GC). After filtering to remove the catalyst, 516.0 g of ethyl iodide (molecular weight 155.11, 2.2 equivalents) was added dropwise while stirring. After gently refluxing for 16 hours under a nitrogen atmosphere, the mixture was allowed to cool, filtered, washed with acetone, and dried to obtain 703.0 g (90% yield) of the desired product, N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide as a white powder. The resulting white powder 1 H-NMR and 13 The C-NMR spectrum is shown below. 1 H-NMR (400MHz, D2O) δ: 3.82 (dd, 4H), 3.49 (q4, 4H), 3.38 (q4, 4H), 3.33 (d, 4H), 2.69 (m, 4H), 1.80 (s, 2H), 1.64 (s, 4H), 1.36 (t, 6H), 1.31 (t, 6H). 13 C-NMR(100Hz, D2O) δ: 65.00(×4), 58.51(×2), 54.41(×2), 40.11(×4), 28.33(×2), 14.86(×2), 11.01(×2), 10.17(×2) N,N,N',N'-Tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide 1 The HNMR spectrum data is shown in Figure 23. 13 The CNMR spectrum data is shown in FIG.

[0242] [Reference Example B3: Synthesis of AFX zeolite] 28.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62) of Reference Example B2, 116.0 g of 4.8 mass% sodium hydroxide solution, 37.5 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 47.0 g of water were stirred in a polyethylene beaker for 48 hours. The composition of the mixture was as follows.

[0243] [Table 14]

[0244] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 300 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and allowed to stand at 170° C. for 40 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the resulting solid phase was washed with a sufficient amount of water and dried at 105° C. to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. FIG. 25 shows the XRD data of the AFX zeolite.

[0245] The gas chromatography conditions in Example B and Reference Example B were as follows. Instrument name: GCMS-QP2010 (Shimadzu Corporation) Column: SHIMADZU SH-Rtx-200MS Carrier gas: Helium Total flow rate: 98.9mL / min Column flow rate: 2.56mL / min Temperature: The column oven was heated from 40° C. to 300° C. at a rate of 10° C. / min. Then, the temperature was kept at 300° C. for 10 min.

[0246] The NMR measurement conditions in Example B and Reference Example B were as follows. Device name: Ascend4000 (BRUKER) Measurement method: 1 HNMR and 13 CNMR was measured by dissolving the sample in deuterium oxide.

[0247] The conditions for powder X-ray diffraction measurements in Example B and Reference Example B were as follows. Device name: X'Pert Pro (Spectris Corporation) Measurement method: The powder sample was filled into a grooved glass sample plate container and used for measurement. The X-ray source was CuKα radiation, the tube voltage was 45 kV, and the tube current was 40 mA.

[0248] According to the production method of the present invention, since it is not necessary to use a strong reducing agent that is difficult to handle, such as a reducing agent that poses a risk of ignition, etc., it is possible to safely and easily produce N,N,N',N'-tetraalkylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium. Furthermore, according to this production method, since the synthesis can be performed under relatively safe conditions, the burden on equipment is small and large-scale production is possible, thereby improving the productivity and economic efficiency of the compound.

[0249] [Production Example C1: Preparation of Pt-V / HAP catalyst] Pt(acac)2 (platinum acetylacetonate, 0.4 mmol) from N.E. Chemcat and VO(acac)2 (vanadyl acetylacetonate, 0.4 mmol) from Sigma-Aldrich were added to 90 mL of acetone and stirred at room temperature for 30 minutes. 1.0 g of HAP (trade name "tricalcium phosphate") from Wako Pure Chemical Industries was added and stirred at room temperature for 4 hours. The solvent was removed from the mixture using a rotary evaporator to obtain a pale green powder. The powder was dried at 110°C overnight. The dried powder was then crushed in an agate bowl and calcined at 300°C for 3 hours in air to obtain a dark gray powder (Pt-V / HAP).

[0250] [Production Example C2: Synthesis of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine] 0.3 g of Pt-V / HAP obtained in Production Example C1, 0.3 mmol of N,N'-diethylbicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarbonyldiimide synthesized according to the method of Patent Document 2, and 0.1 g of molecular sieves 4Å from Wako Pure Chemical Industries, Ltd. were added to a 50 mL stainless steel autoclave, and 5 mL of 1,2-dimethoxyethane (DME) as a solvent was added, and the hydrogenation reaction was carried out for 48 hours at a reaction temperature of 150°C and a hydrogen pressure of 5 MPa. After the reaction, the yield of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine was measured using GC-MS, and the yield was 77%. The product was isolated and the results of NMR measurement are shown below. 1 H NMR (400 MHz, CDCl3) δ = 2.72 (t, J = 17 Hz, 4H), 2.49 (dd, J = 30, 14 Hz, 4H), 2.43 (dd, J = 18, 10 Hz, 4H), 2.21 (s, 4H), 1.57 (s, 4H), 1.40 (s, 2H), 1.14 (t, J = 15 Hz, 6H); 13 C NMR (100 MHz, CDCl3) δ = 57.0(×4), 50.2(×2), 40.7(×4), 30.6(×2), 14.6(×2), 13.9(×2).

[0251] [Production Example C3: Synthesis of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide] A 50 mL ethanol solution of 2.2 g of N,N'-diethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidine (molecular weight 248.41) synthesized according to Production Example C2 was placed in a 100 mL flask, and 6.0 g of ethyl iodide (molecular weight 155.97, liquid, Tokyo Chemical Industry) was added dropwise. After refluxing for 2 days under a nitrogen atmosphere, the mixture was allowed to cool, filtered, washed with acetone, and dried to obtain 2.6 g (yield 52%) of the target product, N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide, as a white powder. The white powder obtained 1 HNMR and 13 The CNMR spectrum is shown below. 1 H NMR(400MHz, D2O) δ: 3.82 (dd, 4H), 3.49 (q4, 4H), 3.38 (q4, 4H), 3.33 (d, 4H), 2.68(m, 4H), 1.80 (s, 2H), 1.64 (s, 4H), 1.36 (t, 6H), 1.31 (t, 6H) 13 C NMR(400Hz, CDCl3) δ: 65.00(×4), 58.51(×2), 54.41(×2), 40.11(×4), 28.33(×2), 14.86(×2), 11.01(×2), 10.1(×2) Also, 1 The HNMR spectrum data is shown in Figure 26. 13 The CNMR spectrum data is shown in FIG.

[0252] [Example C1: Synthesis of AFX-type zeolite] 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octane-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62), 8.4 g of 4.8 mass% sodium hydroxide solution, 2.7 g of FAU type zeolite CBV712 (manufactured by Zeolyst, silica-alumina ratio SAR 10.9), and 3.3 g of water were stirred in a SUS beaker for 48 hours. The composition of the mixture was as follows:

[0253] [Table 15]

[0254] The numerical value of each component in the above mixture means the ratio of the amount of substance when the amount of substance of SiO2 is set to 1. Next, this raw material composition (mixture) was placed in a 50 cc stainless steel sealed pressure vessel with a Teflon inner cylinder and allowed to stand at 170°C for 48 hours. The product after this hydrothermal treatment was subjected to solid-liquid separation, and the obtained solid phase was washed with a sufficient amount of water and dried at 105°C to obtain a product. Powder X-ray diffraction analysis confirmed that the product was a single phase of AFX zeolite. Figure 28 shows an XRD chart of the AFX zeolite obtained in Example C1.

[0255] [Comparative Example C1: Synthesis of AFX-type zeolite] A product was obtained in the same manner as in Example C1, except that 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octa-2,3:5,6-dipyrrolidinium diiodide (molecular weight 556.61) synthesized according to the method of Patent Document 2 was used instead of 2.0 g of N,N,N',N'-tetraethylbicyclo[2.2.2]octa-2,3:5,6-dipyrrolidinium diiodide (molecular weight 558.62). When powder X-ray diffraction analysis was performed, it was confirmed that beta zeolite was produced in addition to AFX zeolite in the product. FIG. 29 shows an XRD chart of the AFX zeolite obtained by Comparative Example C1.

[0256] Thus, according to the production method of the present invention, it is possible to obtain a single-phase AFX zeolite even if the OSDA is still in the iodide form, which is useful. In addition, it is possible to avoid the use of dangerous reducing agents such as lithium aluminum hydride (LiAlH4) when mass-producing AFX zeolite.

[0257] The diffraction peaks obtained as a result of powder X-ray diffraction analysis of the AFX zeolite produced in Example C1 are shown in the following table.

[0258] [Table 16] [Industrial Applicability]

[0259] According to the present invention, it is possible to realize a relatively stable and low-cost supply of, for example, zeolite, which is a type of hydrous aluminosilicate, which is useful as a material for OSDA. According to the manufacturing method of the present invention, it is possible to easily and safely provide compounds that are materials for OSDA, and it is possible to realize a relatively stable and low-cost supply of, for example, zeolite, which is a type of hydrous aluminosilicate. According to the present invention, it is possible to realize a relatively stable and low-cost supply of, for example, AFX-type zeolite, which is a type of hydrous aluminosilicate, and it is possible to achieve highly efficient purification of nitrogen oxides using a reducing component, for example, by using an embodiment such as a honeycomb stacked catalyst in which AFX-type zeolite is applied to a honeycomb carrier. Therefore, the present invention can be widely and effectively used in applications such as adsorbents or separators for various inorganic or organic molecules, as well as desiccants, dehydrants, ion exchangers, oil refining catalysts, petrochemical catalysts, solid acid catalysts, three-way catalysts, exhaust gas purification catalysts, and NOx storage materials.

Claims

1. A step (Step I) of preparing a compound represented by formula (A); a step (step II) of reacting the compound represented by formula (A) with a hydrogen source using a catalyst containing platinum to obtain a compound represented by formula (2); A step of N-alkylating the compound represented by the formula (2) using an alkylating agent (step III); A method for producing a compound represented by formula (1) or a salt thereof, comprising: [Formula 1] (In the above formulas (A), (1) and (2), R 1 ~R 4 are each independently an alkyl group.

2. The catalyst further contains vanadium. The method of claim 1 .

3. The catalyst further comprises a carrier selected from the group consisting of silica, titania, zirconia, alumina, magnesium oxide, tricalcium phosphate, and composites of two or more of these inorganic oxides. The method according to claim 1 or 2.

4. The catalyst further comprises tricalcium phosphate. The method according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for producing AFX-type zeolite

    JP2016169139A

  • AFX type zeolite and production method thereof

    JP2017128457A

  • Catalytic converter

    JP2017508605A

  • JPP7442142B

  • Synthetic porous crystalline MCM-70, its synthesis and use

    US20020174824A1