Composite negative electrode active material, negative electrode and lithium battery using the same
The composite negative electrode active material with a silicon core and carbon-based shell addresses the deterioration issue in silicon-based materials by stabilizing volume changes, improving cycle characteristics and reducing resistance in lithium batteries.
Patent Information
- Application Number
- JP2022189322
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-26
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-28
AI Technical Summary
Conventional silicon-based negative electrode active materials in lithium batteries deteriorate easily due to volume changes during charging and discharging, leading to poor cycle characteristics and increased internal resistance.
A composite negative electrode active material is developed, comprising a silicon-containing core coated with a shell made of a first metal oxide and a carbon-based material, where the shell is disposed within a carbon-based material matrix, effectively preventing volume changes and reducing side reactions.
The composite material improves the cycle characteristics of lithium batteries by suppressing volume changes and reducing internal resistance, thereby enhancing the battery's performance and longevity.
Smart Images

Figure 0007577720000006 
Figure 0007577720000007 
Figure 0007577720000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite positive electrode active material, and a negative electrode and a lithium battery employing the same. [Background technology]
[0002] In order to meet the trend of miniaturization and high performance of various devices, it is becoming increasingly important to make lithium batteries not only smaller and lighter, but also to have higher energy density, i.e., high-capacity lithium batteries.
[0003] In order to realize a lithium battery that meets the above-mentioned applications, negative electrode active materials having high capacity have been investigated.
[0004] Conventional silicon-based negative electrode active materials are more easily degraded than carbon-based negative electrode active materials due to volume changes caused by charging and discharging.
[0005] There is a demand for lithium batteries that contain silicon-based negative electrode active materials and provide excellent cycle characteristics. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a novel composite negative electrode active material capable of preventing deterioration of a lithium battery.
[0007] Another object of the present invention is to provide a negative electrode comprising the composite negative electrode active material.
[0008] Still another object of the present invention is to provide a lithium battery using the negative electrode. [Means for solving the problem]
[0009] On one side, it includes a core; and a shell disposed along the surface of the core; wherein the core includes a silicon-containing structure, a silicon-containing compound or a combination thereof, and the shell has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, if a is 1, 2, or 3, then b is not an integer) and includes one or more first metal oxides; and a first carbon-based material; wherein the first metal oxide is disposed within the first carbon-based material matrix, and M is one or more selected metals from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements, and a composite negative electrode active material is provided.
[0010] On another side, a negative electrode including the composite negative electrode active material is provided.
[0011] On still another side, it includes a dry composite negative electrode active material, a dry conductive material, and a dry binder. The dry composite negative electrode active material includes a core; and a shell disposed along the surface of the core; wherein the core includes a silicon-containing structure, a silicon-containing compound or a combination thereof, and the shell has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, if a is 1, 2, or 3, then b is not an integer) and includes one or more first metal oxides; and a first carbon-based material; wherein the first metal oxide is disposed within the first carbon-based material matrix, and M is one or more selected metals from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements, and a negative electrode is provided.
[0012] On still another side, a lithium battery including the negative electrode is provided.
Advantages of the Invention
[0013] According to one side, the composite negative electrode active material includes a shell containing a first metal oxide and a first carbon-based material, thereby improving the cycle characteristics of the lithium battery and suppressing volume change.
Brief Description of the Drawings
[0014] [Figure 1] 1 is a schematic cross-sectional view of a composite negative electrode active material according to an embodiment; [Figure 2A] 1 shows XPS spectra of the C 1s orbital of the silicon composite structure prepared in Preparation Example 3 and the composite negative electrode active material prepared in Example 1. [Figure 2B] 1 shows XPS spectra of O1s orbitals of the silicon composite structure prepared in Preparation Example 3 and the composite negative electrode active material prepared in Example 1. [Figure 2C] 1 shows XPS spectra of Si 2p orbitals of the silicon composite structure prepared in Preparation Example 3 and the composite negative electrode active material prepared in Example 1. [Figure 2D] 1 shows XPS spectra of Al 2p orbitals of the silicon composite structure prepared in Comparative Example 5 and the composite negative electrode active material prepared in Example 1. [Figure 3A] 1 shows XPS spectra of the C 1s orbital of the silicon composite structure prepared in Comparative Example 3 and the composite negative electrode active material prepared in Example 8. [Figure 3B] 1 shows XPS spectra of O1s orbitals of the silicon composite structure prepared in Comparative Example 3 and the composite negative electrode active material prepared in Example 8. [Figure 3C] 13 shows XPS spectra of Si 2p orbitals of the silicon composite structure prepared in Comparative Example 3 and the composite negative electrode active material prepared in Example 8. [Figure 3D] 13 shows XPS spectra of the Al 2p orbital of the silicon composite structure prepared in Comparative Example 3 and the composite negative electrode active material prepared in Example 8. [Figure 4A] 1 is a scanning electron microscope image of the composite negative electrode active material of Example 1. [Figure 4B] 1 is a SEM-EDS mapping image of the composite negative electrode active material of Example 1. [Figure 4C] 1 is a scanning electron microscope image of the composite negative electrode active material of Example 8. [Figure 4D]1 is a SEM-EDS mapping image of the composite negative electrode active material of Example 8. [Diagram 5] FIG. 4 is a schematic cross-sectional view of a composite negative electrode active material according to another embodiment. [Figure 6] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 7] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 8] 1 is a schematic diagram of a lithium battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventive concept described below can be modified in various ways and can have various embodiments, and specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present inventive concept to a specific embodiment, and it should be understood that the present inventive concept includes any modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.
[0016] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In the following, terms such as "include" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the situation.
[0017] In the drawings, thicknesses are exaggerated or reduced to clearly depict multiple layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part such as a layer, film, region, plate, etc. is described as being "on" or "above" another part, this does not only mean that it is directly on top of the other part, but also includes cases where there is another part in between. Throughout the specification, terms such as first, second, etc. may be used to describe various components, but the components should not be limited by the terms. Terms are used only to distinguish one component from another.
[0018] In this specification, the "particle size" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle size of a particle can be measured using a particle size analyzer (PSA). The "particle size" of a particle is, for example, the average particle size. The average particle size is the median size (D50) unless otherwise specified above. The median size (D50) is the particle size that corresponds to the 50% cumulative value calculated from the particle side having the smallest particle size in a cumulative distribution curve of particle sizes in which particles are accumulated in order of particle size from the smallest particle to the largest particle. The cumulative value is, for example, the cumulative volume. The median size (D50) can be measured, for example, by a laser diffraction method.
[0019] In this specification, the particle size (D10) is a particle size corresponding to a 10% cumulative value calculated from the particle side having a small particle size in a cumulative distribution curve of particle sizes.
[0020] In this specification, particle size (D90) is a particle size corresponding to a 90% cumulative value calculated from the particle side having a small particle size in a cumulative distribution curve of particle sizes.
[0021] As used herein, "silicon suboxide" refers to, for example, SiO xIt has a single composition represented by (0 < x < 2). Alternatively, "silicon suboxide" contains, for example, one or more selected from Si and SiO2, and has an average composition of SiO x It has a composition represented by (0 < x < 2). Alternatively, "silicon suboxide" also includes, for example, silicon-suboxide-like materials. Silicon-suboxide-like materials are substances having properties similar to those of silicon suboxide, and include, for example, one or more selected from Si and SiO2, and have an average composition of SiO x It can have a composition represented by (0 < x < 2).
[0022] Hereinafter, the composite negative electrode active material, the negative electrode containing the same, and the lithium battery according to exemplary embodiments will be described in more detail.
[0023] The composite negative electrode active material includes a core; and a shell disposed along the surface of the core, wherein the core includes a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, if a is 1, 2, or 3, then b is not an integer) of one or more first metal oxides; and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the periodic table of the elements. Referring to FIG. 1, the composite negative electrode active material 100 includes a core 10 and a shell 20 disposed continuously or discontinuously along the surface of the core 10. The shell 20 can cover all or part of the core 10. The core 10 includes a silicon-containing negative electrode active material such as a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell 20 includes a first metal oxide 21 and a first carbon-based material 22.
[0024] Hereinafter, the theoretical basis for why the composite negative electrode active material according to one embodiment provides excellent effects will be described. However, this is intended to aid in understanding the present invention and is not intended to limit the present invention in any manner.
[0025] The composite negative electrode active material includes a matrix of a first carbon-based material, and a composite including a plurality of first metal oxides disposed within the matrix is used to prevent aggregation of the first carbon-based material while a uniform shell is disposed on the core. Therefore, by effectively blocking contact between the core and the electrolyte, side reactions due to contact between the core and the electrolyte are effectively prevented. The first carbon-based material is, for example, a crystalline carbon-based material. The first carbon-based material is, for example, a carbon-based nanostructure. The first carbon-based material is, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material is, for example, a carbon-based flake. As an example, the first carbon-based material is graphene. The shell including graphene and / or its matrix has flexibility, so that it can easily accommodate the volume change of the core during charging and discharging. Therefore, the occurrence of cracks on the surface and / or inside of the composite negative electrode active material during charging and discharging is suppressed, and the formation of a solid electrolyte membrane (SEI) on the surface and / or inside of the composite negative electrode active material is suppressed. As a result, the deterioration of the lithium battery containing the composite anode active material is suppressed. Meanwhile, conventional silicon-based anode active materials generally undergo volumetric changes during charging and discharging, which causes cracks on the surface and / or inside the silicon-containing anode active material. The cracks create new surfaces inside and / or outside the silicon-based anode active material. On such new surfaces, a solid electrolyte interlayer (SEI) is formed by a side reaction between the silicon-based anode active material and the electrolyte. The continuous formation of the solid electrolyte interlayer (SEI) as charging and discharging proceeds increases the internal resistance of the silicon-based anode active material, which results in a decrease in the performance of the lithium battery. In addition, conventional carbon-based materials are easily agglomerated during the coating process, making it difficult to uniformly coat the core.
[0026] The core of the composite negative electrode active material contains a negative electrode active material containing silicon, such as a silicon-containing structure, a silicon-containing compound, or a combination thereof. The silicon-containing structure is also, for example, a silicon composite structure. The silicon composite structure is also, for example, a silicon-carbon composite. The silicon-carbon composite is also, for example, a silicon-carbon nano composite. The silicon-carbon nano composite means a composite in which one or more of silicon and carbon have a nano size of less than 1 μm. For example, the silicon-carbon nano composite is also a composite in which silicon nanoparticles and carbon nanoparticles are combined. The silicon-containing compound contains, for example, silicon, a silicon alloy, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a combination thereof. The silicon-containing compound can contain, for example, SiO x (0 < x < 2).
[0027] The silicon composite structure contains, for example, porous silicon secondary particles; and a first carbon flake disposed on the porous silicon secondary particles, wherein the porous silicon secondary particles are an aggregate of a plurality of silicon composite primary particles, and the silicon composite primary particles contain silicon; silicon suboxide (SiO x , 0 < x < 2) disposed on the silicon; and a second carbon flake disposed on the silicon suboxide.
[0028] The silicon composite structure includes porous silicon secondary particles including agglomerates of a plurality of silicon composite primary particles, and first carbon flakes disposed on the porous silicon secondary particles. The first carbon flakes disposed on the porous silicon secondary particles may be disposed so as to cover at least one surface of the porous silicon secondary particles. The first carbon flakes may be disposed directly on the porous silicon secondary particles. The first carbon flakes may be grown directly on the silicon suboxide of the porous silicon secondary particles. The first carbon flakes may grow directly from the surface of the porous silicon secondary particles and be disposed directly on the surface of the porous silicon secondary particles. The first carbon flakes may entirely or partially cover the surface of the porous silicon secondary particles. The coverage rate of the first carbon flakes is, for example, 5 to 100%, 10 to 99%, 20 to 95%, or 40 to 90% based on the total surface area of the porous silicon secondary particles. The carbon of the first carbon flakes is present on the surface of the porous silicon secondary particles and can effectively buffer the volume change of the porous silicon secondary particles. The size of the porous silicon secondary particles can be, for example, 1 to 20 μm, 2 to 18 μm, or 3 to 10 μm. The size of the first carbon flakes can be, for example, 1 to 200 nm, 5 to 150 nm, or 10 to 100 nm. Here, size refers to the diameter or major axis length.
[0029] The silicon composite primary particles are comprised of silicon; silicon suboxide (SiO x, (0 < x < 2); and a second carbon flake disposed on one surface of the silicon suboxide. The silicon can be, for example, plate-shaped, needle-shaped, spherical, or a combination thereof. The shape of the silicon is not particularly limited, and for example, it can be spherical, nanowire, needle-shaped, rod-shaped, particle, nanotube, nanorod, wafer, and nanoribbon, or a combination thereof. The average size of the silicon is, for example, 10 nm to 1 μm, 10 nm to 500 nm, 20 to 150 nm, or 100 nm. The average size of the silicon means the average particle diameter when the silicon is spherical particles, and means the major axis length, length, or thickness when it is non-spherical particles, such as plate-shaped particles or needle-shaped particles. The silicon suboxide (SiO x )(0 < x < 2) disposed on the silicon can be arranged to cover at least one surface of the silicon. The silicon suboxide can be disposed directly on the silicon. The silicon suboxide can cover the surface of the silicon entirely or partially. The coverage rate of the silicon suboxide is, for example, based on the total surface area of the silicon, for example, 1 to 100%, 5 to 99%, 10 to 95%, or 20 to 90%. The second carbon flake disposed on the silicon suboxide can be arranged to cover at least one surface of the silicon suboxide. The second carbon flake can be disposed directly on the silicon suboxide. The second carbon flake can grow directly from the surface of the silicon suboxide and be disposed directly on the surface of the silicon suboxide. The second carbon flake can cover, for example, the surface of the silicon suboxide entirely or partially. The coverage rate of the second carbon flake is, for example, based on the total surface area of the silicon suboxide, for example, 10 to 100%, 10 to 99%, 20 to 95%, or 40 to 90%. The carbon of the second carbon flake is present on the surface of the silicon and / or the silicon suboxide and can effectively buffer the volume change of the silicon composite primary particles. The size of the second carbon flake is, for example, 1 to 200 nm, 5 to 150 nm, or 10 to 100 nm. Here, the size means the diameter or the major axis length.
[0030] The silicon composite structure includes porous silicon secondary particles and second carbon flakes disposed on the porous silicon secondary particles. The second carbon flakes may be disposed in a form that entirely or partially covers the porous silicon secondary particles. For example, the second carbon flakes may be disposed in a form that entirely or partially surrounds the porous silicon secondary particles. The silicon composite primary particles include first carbon flakes. During volumetric expansion / contraction of the silicon composite structure, silicon included in the porous silicon secondary particles can maintain contact with the first carbon flakes and / or the second carbon flakes. The porous secondary particles include pores, and thus act as an internal buffer space during volumetric expansion / contraction of the silicon composite structure. Therefore, unlike conventional silicon-based negative electrode active materials, the silicon composite structure can effectively accommodate volumetric changes of the silicon composite structure during charging / discharging while suppressing an increase in internal resistance.
[0031] The porosity of the silicon composite structure may be, for example, 60% or less, or 30% to 60%. Alternatively, the silicon composite structure may be non-porous. A non-porous structure may be, for example, a porosity of 10% or less, or 5% or less. A non-porous structure may be, for example, a porosity of 0.01% to 5%, or 0%. The porosity may be measured by mercury adsorption or nitrogen adsorption.
[0032] The silicon composite structure has, for example, a non-spherical shape. The sphericity of the silicon composite structure is, for example, 0.9 or less. The sphericity of the silicon composite structure is, for example, 0.7 to 0.9, 0.8 to 0.9, or 0.85 to 0.9. The circularity is, for example, 4πA / P 2 (A is the area and P is the perimeter).
[0033] The silicon composite structure includes a first carbon flake and a second carbon flake. The first carbon flake and the second carbon flake may be, for example, identical carbon flakes. Any carbon-based material having a flake shape may be used as the first carbon flake and the second carbon flake. The first carbon flake and the second carbon flake may be, independently of each other, graphene, graphite, carbon fiber, graphitic carbon, graphene oxide, or a mixture thereof. The porous composite structure includes, for example, a first graphene and a second graphene as the first carbon flake and the second carbon flake. The first graphene and the second graphene each have a structure such as a nanosheet, a membrane (or film), or a flake. The nanosheet means a form irregularly formed on a silicon suboxide or a porous silicon secondary particle with a thickness of about 1000 nm or less, for example, 1 to 1000 nm. The term "film" refers to a form formed continuously and uniformly on silicon suboxide or porous silicon secondary particles.
[0034] The silicon-containing structure may further include a carbon-based coating layer disposed on the silicon composite structure. The carbon-based coating layer can improve the physical stability of the silicon composite structure and more effectively prevent side reactions between silicon and the electrolyte during charging and discharging. The carbon-based coating layer includes, for example, a first amorphous carbon. The carbon-based coating layer includes a first amorphous carbon having a high density. The first amorphous carbon includes, for example, pitch-based carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a mixture thereof. The carbon-based coating layer may further include crystalline carbon. The carbon-based coating layer further includes crystalline carbon, so that the silicon composite structure can more effectively perform a buffering role against the volume change. The crystalline carbon can be, for example, natural graphite, artificial graphite, graphene, fullerene, carbon nanotube, or a mixture thereof. The thickness of the carbon-based coating layer can be, for example, 1 nm to 5000 nm, 10 nm to 2000 nm, or 5 nm to 2500 nm.
[0035] The silicon-containing structure may further include, for example, a second amorphous carbon disposed within the silicon composite structure. For example, the silicon composite structure may include porous silicon secondary particles, and the second amorphous carbon may be disposed within the pores of the porous silicon secondary particles. The second amorphous carbon may be disposed between a plurality of silicon composite primary particles that make up the porous silicon secondary particles. The silicon composite primary particles include, for example, silicon; silicon suboxide (SiO x , 0 < x < 2) disposed on the silicon; and a second carbon flake disposed on the silicon suboxide; and a second amorphous carbon disposed on the second carbon flake. The silicon composite structure has a dense structure with a non-porous structure by filling the internal pores thereof with the dense second amorphous carbon. Since the silicon composite structure has such a non-porous structure, side reactions with the electrolyte during charge and discharge can be further reduced, and the volume change of silicon can be more effectively alleviated. The second amorphous carbon includes, for example, pitch-based carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a mixture thereof.
[0036] In the silicon composite structure, the mixing ratio of the total weight of the first carbon, which is the sum of the carbon of the first carbon flake and the carbon of the second carbon flake, to the weight of the second carbon, which is the carbon of the carbon-based coating layer, is, for example, 30:1 to 1:3, 20:1 to 1:1, or 10:1 to 1:0.9. By having such a mixing ratio of the first carbon and the second carbon, a lithium battery with improved cycle characteristics is provided. The mixing ratio of the first carbon and the second carbon can be confirmed through thermogravimetric analysis. The first carbon is related to the peak shown in the region of 700 to 750 °C, and the second carbon is related to the peak shown in the region of 600 to 650 °C. The thermogravimetric analysis is carried out, for example, at a heating rate of about 10 °C / min in an air atmosphere in the range of 25 to 1,000 °C. The first carbon is, for example, crystalline carbon, and the second carbon is, for example, amorphous carbon. The mixing ratio of the total weight of the carbon of the first carbon flake and the carbon of the second carbon flake to the total weight of the first amorphous carbon and the second amorphous carbon is, for example, 1:99 to 99:1, 1:20 to 80:1, or 1:1 to 1:10.
[0037] The core is a silicon-containing negative electrode active material, which is a silicon-containing compound SiO x (0 < x < 2). SiO x (0 < x < 2) has an average particle size of, for example, 1 μm or more, 3 μm or more, or 5 μm or more. SiO x (0 < x < 2) has an average particle size of, for example, 1 μm to 30 μm, 3 μm to 20 μm, or 5 μm to 15 μm.
[0038] The shell contains a first metal oxide and a first carbon-based material.
[0039] The first carbon-based material, for example, graphene, has high electrical conductivity, so that the interfacial resistance between the composite negative electrode active material and the electrolyte can be reduced. Therefore, even though a shell including the first carbon-based material is introduced, an increase in the internal resistance of the lithium battery is suppressed. Since the first carbon-based material included in the shell of the composite negative electrode active material is derived from a graphene matrix, it has a relatively low density and a high porosity compared to conventional carbon-based materials derived from graphite-based materials. The d002 interplanar distance of the first carbon-based material included in the shell of the composite negative electrode active material is, for example, 3.38 Å or more, 3.40 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or 4.00 Å or more. The d002 interplanar distance of the first carbonaceous material contained in the shell of the composite anode active material is, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. Meanwhile, the d002 interplanar distance of the conventional carbonaceous material derived from the graphite-based material is, for example, 3.38 Å or less, or 3.35 to 3.38 Å. Since the first metal oxide has a voltage resistance, it is possible to prevent the deterioration of the core during charging and discharging at a high voltage. The shell contains, for example, one kind of the first metal oxide or two or more kinds of different first metal oxides. As a result, the cycle characteristics of the lithium battery containing the above-mentioned composite anode active material can be improved and the volume change can be suppressed.
[0040] The content of the shell may be 0.1 wt% to 5 wt%, 0.1 wt% to 4 wt%, 0.1 wt% to 3 wt%, or 0.1 wt% to 2 wt% of the total weight of the composite negative electrode active material. The content of the first metal oxide may be, for example, 0.06 wt% to 3 wt%, 0.06 wt% to 2.4 wt%, 0.06 wt% to 1.8 wt%, or 0.06 wt% to 1.2 wt% of the total weight of the composite negative electrode active material. When the composite negative electrode active material contains the shell and the first metal oxide in such a content range, the cycle characteristics of the lithium battery are further improved.
[0041] The shell includes a first metal, and the content of the first metal is, for example, 0.1 to 10 at%, 0.5 to 7 at%, or 1 to 5 at% based on the total number of atoms in the shell. When the shell includes the first metal having such a content range, the cycle characteristics of a lithium battery including the composite negative electrode active material can be further improved. The content of the first metal element included in the shell can be determined, for example, from a peak obtained by measuring an XPS spectrum of the surface of the composite negative electrode active material. The first metal is a metal included in the first metal oxide.
[0042] The shell contains oxygen (O), and the oxygen (O) content is, for example, 6 to 20 at%, 7 to 15 at%, 8 to 15 at%, or 10 to 15 at% based on the total number of atoms in the shell. When the shell contains oxygen having such a content range, the cycle characteristics of a lithium battery including the composite negative electrode active material can be further improved. The oxygen (O) content of the shell can be determined, for example, from a peak obtained by measuring an XPS spectrum of the surface of the composite negative electrode active material.
[0043] The shell contains aluminum (Al), and the aluminum (Al) content is, for example, 0.1 to 10 at%, 0.5 to 10 at%, 1 to 9 at%, 1 to 7 at%, or 1 to 5 at% based on the total number of atoms in the shell. When the shell contains aluminum (Al) having such a content range, the cycle characteristics of a lithium battery including the composite negative electrode active material can be further improved. The aluminum (Al) content of the shell can be determined, for example, from a peak obtained by measuring an XPS spectrum of the surface of the composite negative electrode active material.
[0044] The shell contains carbon (C), and the carbon (C) content is, for example, 70 to 95 at%, 70 to 90 at%, 75 to 90 at%, 80 to 90 at%, 80 to 87 at%, or 80 to 85 at% based on the total number of atoms in the shell. By the shell containing carbon within such a content range, the cycle characteristics of a lithium battery containing a composite negative electrode active material can be further improved. The carbon content contained in the shell can be determined, for example, from the peaks obtained by measuring the XPS spectrum with respect to the surface of the composite negative electrode active material.
[0045] The first metal oxide contains a first metal, and the first metal is, for example, also one or more selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide is, for example, Al2O z (0 < z < 3), NbO x (0 < x < 2.5), MgO x (0 < x < 1), Sc2O z (0 < z < 3), TiO y (0 < y < 2), ZrO y (0 < y < 2), V2O z (0 < z < 3), WO y (0 < y < 2), MnO y (0 < y < 2), Fe2O z (0 < z < 3), Co3O w (0 < w < 4), PdO x (0 < x < 1), CuO x (0 < x < 1), AgO x (0 < x < 1), ZnO x (0 < x < 1), Sb2O z (0 < z < 3), and SeO y (0 < y < 2) and is also one or more selected therefrom. By disposing such a first metal oxide within the matrix of the carbon-based material, the uniformity of the shell disposed on the core is improved, and the voltage resistance of the composite negative electrode active material is further improved. For example, the shell contains Al2O x (0 < x < 3).
[0046] The shell has the chemical formula M a Oc (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer), one or more second metal oxides represented thereby may be further included. The M is one or more selected metals from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements. For example, the second metal oxide contains the same metal as the first metal oxide, and c / a, which is the ratio of c to a of the second metal oxide, has a larger value compared to b / a, which is the ratio of b to a of the first metal oxide. For example, c / a > b / a. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is, for example, a reduction product of the second metal oxide. By reducing part or all of the second metal oxide, the first metal oxide is obtained. Therefore, the first metal oxide has a lower oxygen content and a lower oxidation number of the metal compared to the second metal oxide. For example, the shell is the first metal oxide Al2O x (0 < x < 3) and contains Al2O3 which is a second metal oxide.
[0047] The shell contains one or more selected from the first metal oxide and the second metal oxide. The particle size of one or more selected from the first metal oxide and the second metal oxide is, for example, also 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. By having such a nano-scale particle size for the first metal oxide and / or the second metal oxide, it can be more uniformly distributed within the first carbon-based material matrix of the shell. If the particle size of one or more of the first metal oxide and the second metal oxide increases excessively, the thickness of the shell increases, thereby increasing the internal resistance of the composite negative electrode active material. If the particle size of one or more of the first metal oxide and the second metal oxide decreases excessively, uniform dispersion is difficult.
[0048] The shell includes a first metal oxide and / or a second metal oxide and includes a first carbon-based material. The first carbon-based material can be arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface. The first carbon-based material can be arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface by directly growing from the first metal oxide and / or the second metal oxide surface. The first carbon-based material arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface can be, for example, a carbon-based two-dimensional nanostructure, a carbon-based flake, or graphene.
[0049] The shell includes, for example, a first carbon-based material, and the core includes, for example, a silicon-containing structure and / or a silicon-containing compound as a silicon-containing negative active material. For example, the first carbon-based material may be composited with the silicon-containing structure and / or the silicon-containing compound through a mechanochemical reaction. The first carbon-based material may be chemically bonded with the silicon-containing structure and / or the silicon-containing compound through a chemical bond. The first carbon-based material disposed in the shell and the silicon-containing structure and / or the silicon-containing compound disposed in the core are chemically bonded through a chemical bond, thereby composited with the core and the shell. Therefore, the composite negative active material is distinguished from a simple physical mixture of the first carbon-based material and the silicon-containing structure and / or the silicon-containing compound. The first metal oxide and the carbon-based material contained in the shell may also be chemically bound through a chemical bond. Here, the chemical bond may be, for example, a covalent bond or an ionic bond.
[0050] The thickness of the shell is, for example, 1 nm to 5 μm, 1 nm to 1 μm, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 20 nm. When the shell has a thickness in such a range, the electronic conductivity of the negative electrode containing the composite negative electrode active material can be further improved.
[0051] The shell disposed along the surface of the core may include at least one selected from a composite including a first metal oxide and a first carbon-based material, such as graphene, and a milling result of the composite. The first metal oxide is disposed in a matrix of the first carbon-based material, such as a graphene matrix. The shell may be prepared, for example, from a composite including a first metal oxide and a first carbon-based material, such as graphene. The composite may further include a second metal oxide in addition to the first metal oxide. The composite may include, for example, two or more types of first metal oxides. The composite may include, for example, two or more types of first metal oxides and two or more types of second metal oxides.
[0052] The content of one or more of the composite and milling products thereof may be 5 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or 0.5 wt% or less of the total weight of the composite negative electrode active material. The content of one or more of the composite and milling products thereof included in the composite negative electrode active material may be, for example, 0.1 wt% to 5 wt%, 0.1 wt% to 4 wt%, 0.1 wt% to 3 wt%, or 0.1 wt% to 2 wt% of the total weight of the composite negative electrode active material. When the composite negative electrode active material includes one or more of the composite and milling products thereof within such ranges, the cycle characteristics of a lithium battery including the composite negative electrode active material may be further improved.
[0053] The composite includes one or more selected from the first metal oxide and the second metal oxide. The particle size of the selected one or more of the first metal oxide and the second metal oxide may be, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may have such a nano-range particle size, so that they can be more uniformly distributed in the first carbon-based material matrix of the composite. Therefore, such a composite may be uniformly coated on the core without aggregation to form a shell. In addition, the first metal oxide and / or the second metal oxide may have such a particle size range, so that they may be more uniformly arranged on the core. Therefore, the first metal oxide and / or the second metal oxide may be uniformly arranged on the core, so that the voltage resistance characteristics may be more effectively exhibited. The average particle size of the first metal oxide and the second metal oxide may be measured, for example, using a measuring device of a laser diffraction method or a dynamic light scattering method. The particle size is measured, for example, using a laser scattering particle size distribution analyzer (e.g., HORIBA LA-920), and is the median diameter (D50) value when 50% is accumulated from the elementary particle side in volume conversion. The uniformity deviation of one or more selected from the first metal oxide and the second metal oxide is 3% or less, 2% or less, or 1% or less. The uniformity can also be determined, for example, by XPS. Therefore, the selected one or more of the first metal oxide and the second metal oxide can have a deviation of 3% or less, 2% or less, or 1% or less and be uniformly distributed in the composite.
[0054] The composite includes a first carbon-based material. The first carbon-based material may have, for example, a branched structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the branched structure of the first carbon-based material. The branched structure of the first carbon-based material may include, for example, a plurality of first carbon-based material particles in contact with each other. The first carbon-based material may have a branched structure, and various conductive paths may be provided. The first carbon-based material may be, for example, graphene. The graphene may have, for example, a branched structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the branched structure of graphene. The branched structure of graphene may include, for example, a plurality of graphene particles in contact with each other. The graphene may have a branched structure, and various conductive paths may be provided.
[0055] The first carbon-based material may have, for example, a spherical structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material is 50 nm to 300 nm. There may be a plurality of first carbon-based materials having a spherical structure. Since the first carbon-based material has a spherical structure, the composite may have a robust structure. The first carbon-based material may be, for example, graphene. Graphene may have, for example, a spherical structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of graphene is 50 nm to 300 nm. There may be a plurality of graphenes having a spherical structure. Since the graphene has a spherical structure, the composite may have a robust structure.
[0056] The first carbon-based material may have a spiral structure in which a plurality of spherical structures are connected, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the spiral structure. The size of the spiral structure of the first carbon-based material is 500 nm to 100 μm. Since the first carbon-based material has a spiral structure, the composite may have a robust structure. The first carbon-based material may be, for example, graphene. The graphene may have a spiral structure in which a plurality of spherical structures are connected, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the spiral structure. The size of the spiral structure of graphene is 500 nm to 100 μm. Since the graphene has a spiral structure, the composite may have a robust structure.
[0057] The first carbon-based material may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the cluster structure of the first carbon-based material is 0.5 mm to 10 mm. Since the first carbon-based material has a cluster structure, the composite may have a robust structure. The first carbon-based material may also be graphene, for example. Graphene may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the cluster structure of graphene is 0.5 mm to 10 mm. Since the graphene has a cluster structure, the composite may have a robust structure.
[0058] The composite may be, for example, a wrinkled faceted-ball structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. By the composite having such a faceted-ball structure, the composite may be easily coated onto the irregular surface of the core.
[0059] The composite may be, for example, a planar structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the planar structure. Because the composite has such a two-dimensional planar structure, the composite may be easily coated on the irregular surface of the core.
[0060] The first carbon-based material extends over the first metal oxide for a distance of 10 nm or less and includes at least 1 to 20 layers of the first carbon-based material. For example, a plurality of layers of the first carbon-based material may be stacked to provide a first carbon-based material having a total thickness of 12 nm or less on the first metal oxide. For example, the total thickness of the carbon-based material is 0.6 nm to 12 nm. The first carbon-based material may also be graphene. The graphene extends over the first metal oxide for a distance of 10 nm or less and includes at least 1 to 20 layers of graphene. For example, a plurality of graphene layers may be stacked to provide a first carbon-based material having a total thickness of 12 nm or less on the first metal oxide. For example, the total thickness of the graphene is 0.6 nm to 12 nm.
[0061] The shell may further include a second carbon-based material that is fibrous carbon. The second carbon-based material may include fibrous carbon.
[0062] The composite anode active material further includes a second carbon-based material, which is fibrous carbon, so that the conductive path of the composite anode active material is longer. The second carbon-based material may form a three-dimensional conductive network between the composite anode active materials to reduce the internal resistance of the anode including the composite anode active material. The fibrous carbon may be fixed on the composite anode active material to form a uniform and stable three-dimensional conductive network between the composite anode active materials. Therefore, the high rate characteristics of a lithium battery including the composite anode active material including the second carbon-based material may be improved. Referring to FIG. 5, the composite anode active material 100 includes a core 10 and a shell 20 disposed along a surface of the core 10. The core 10 includes a lithium transition metal oxide, and the shell 20 includes a first metal oxide 21, a first carbon-based material 22, and a second carbon-based material 23. The second carbon-based material 23 includes, for example, fibrous carbon having an aspect ratio of 10 or more. On the other hand, a simple mixture of the core and fibrous carbon is difficult to form a uniform three-dimensional conductive network between a plurality of core particles due to aggregation of the fibrous carbon. The second carbon-based material 23 is disposed in the matrix of the first carbon-based material 22, so that it can be easily coated on the core 10. The matrix of the first carbon-based material 22 acts as a binder that binds the core 10 and the second carbon-based material 23. Therefore, without the matrix of the first carbon-based material 22, the second carbon-based material 23 is difficult to attach to the core 10, or the second carbon-based material 23 is easily detached from the core 10 during the process of preparing the slurry for the negative electrode. When a binder is added to bind the core 10 and the second carbon-based material 23, the core 10 is covered with the insulating binder, so that the internal resistance of the composite negative electrode active material 100 increases. When the core 10 coated with the second carbon-based material 23 and the binder is subjected to a high-temperature heat treatment to carbonize the binder, the core 10 and the second carbon-based material 23 may be deteriorated during the heat treatment.
[0063] The aspect ratio of the second carbon-based material is 10 or more, or 20 or more. The aspect ratio of the second carbon-based material is, for example, 10 to 100,000, 10 to 80,000, 10 to 50,000, 10 to 10,000, 10 to 5000, 10 to 1000, 10 to 500, 10 to 100, or 10 to 50. The aspect ratio of the second carbon-based material is, for example, the ratio of the major axis length passing through the center of the second carbon-based material, i.e., the second carbon-based material to the minor axis length passing through the center of the second carbon-based material and perpendicular to the major axis, i.e., the diameter of the second carbon-based material.
[0064] The diameter of the second carbon-based material is, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbon-based material is, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. If the diameter of the second carbon-based material is too large, the absolute number per volume decreases, and the effect of reducing internal resistance is small. If the diameter of the second carbon-based material is too small, it is difficult to uniformly disperse it.
[0065] The length of the second carbon-based material is, for example, 1000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbon-based material is, for example, 100 nm to 1000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material is, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or 500 nm to 2 μm. As the length of the second carbon-based material increases, the internal resistance of the electrode decreases. If the length of the second carbon-based material is too short, it is difficult to provide an effective conductive path.
[0066] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.
[0067] The carbon nanotubes include, for example, a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof.
[0068] The primary structure of a carbon nanotube is one carbon nanotube unit. A carbon nanotube unit has a graphite sheet with a cylindrical shape of nano-sized diameter and an sp2 bond structure. It exhibits conductive or semiconductive properties depending on the bending angle and structure of the graphite sheet. Carbon nanotube units can be classified into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT), depending on the number of bonds that make up the wall. The thinner the wall thickness of a carbon nanotube unit, the lower the resistance.
[0069] The carbon nanotube primary structure includes, for example, a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), and a multi-walled carbon nanotube (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure is, for example, 1 nm or more, or 2 nm or more. The diameter of the carbon nanotube primary structure is, for example, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube primary structure is, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 2 nm to 10 nm. The length of the carbon nanotube primary structure is, for example, 100 nm or more, or 200 nm or more. The length of the carbon nanotube primary structure is, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the carbon nanotube primary structure is, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure can be measured from a scanning electron microscope (SEM) image. Alternatively, the diameter and / or length of the carbon nanotube primary structure can be measured by a laser diffraction method.
[0070] The carbon nanotube secondary structure is a structure formed by assembling the carbon nanotube primary structures entirely or partially into a bundle or bundle shape. The carbon nanotube secondary structure includes, for example, bundle-type carbon nanotubes, rope-type canon nanotubes, or a combination thereof. The diameter of the carbon nanotube secondary structure is, for example, 2 nm or more or 3 nm or more. The diameter of the carbon nanotube secondary structure is, for example, 50 nm or less, 30 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure is, for example, 50 nm or less, 30 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure is, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure is, for example, 500 nm or more, 700 nm or more, 1 μm or more, or 10 μm or more. The length of the carbon nanotube secondary structure is, for example, 1000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure is, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured from a scanning electron microscope (SEM) image or an optical microscope. Alternatively, the diameter and / or length of the carbon nanotube secondary structure can be measured by a laser diffraction method. The carbon nanotube secondary structure can be, for example, dispersed in a solvent or the like to be converted into a carbon nanotube primary structure, and then used to manufacture a composite negative electrode active material.
[0071] The content of the second carbon-based material is, for example, 0.1 wt% to 50 wt%, 1 wt% to 40 wt%, or 5 wt% to 30 wt% based on the total weight of the first carbon-based material and the second carbon-based material. When the composite negative electrode active material includes the first carbon-based material and the second carbon-based material in such a range, a conduction path is more effectively secured in the composite positive electrode active material, and the internal resistance of the composite negative electrode active material may be further reduced. As a result, the cycle characteristics of a lithium battery including the composite negative electrode active material may be further improved. The content of the second carbon-based material is, for example, 0.001 wt% to 5 wt%, 0.01 wt% to 3 wt%, or 0.01 wt% to 1 wt% based on the total weight of the composite negative electrode active material. When the composite negative electrode active material includes the second carbon-based material in such a range, a conduction path is more effectively secured in the composite negative electrode active material, and the internal resistance of the composite negative electrode active material may be further reduced. As a result, the cycle characteristics of a lithium battery including the composite negative electrode active material can be further improved.
[0072] The specific surface area of the composite negative electrode active material is, for example, 1 m 2 / g~100m 2 / g, 1m 2 / g~50m 2 / g, or 1m 2 / g~30m 2 / g. When the composite negative electrode active material has a specific surface area in such a range, the cycle characteristics of a lithium battery employing such a composite negative electrode active material can be further improved. The average particle size (D50) of the composite negative electrode active material is, for example, 1 μm to 30 μm, 3 μm to 20 μm, or 5 μm to 15 μm. The particle size (D10) of the composite negative electrode active material is, for example, 0.1 μm to 10 μm, 0.5 μm to 10 μm, or 1 μm to 10 μm. The particle size (D90) of the composite negative electrode active material is, for example, 10 μm to 50 μm, 10 μm to 30 μm, or 10 μm to 25 μm. When the composite negative electrode active material has an average particle size (D50), particle size (D10), and / or particle size (D90) in such a range, the cycle characteristics of a lithium battery employing such a composite negative electrode active material can be further improved.
[0073] According to another embodiment, a negative electrode includes the above-described composite negative electrode active material, which provides improved cycle characteristics and reduced volume change.
[0074] The negative electrode may be prepared, for example, by a wet method. The negative electrode may be prepared by the following exemplary method, but is not limited to such a method and may be adjusted according to required conditions.
[0075] First, the composite negative active material, conductive material, binder, and solvent are mixed to prepare a negative active material composition. The prepared negative active material composition is directly coated on a copper current collector and dried to manufacture a negative electrode plate having a negative active material layer. Alternatively, the negative active material composition is cast on a separate support, and then peeled off from the support to obtain a film, which is then laminated on a copper current collector to manufacture a negative electrode plate having a negative active material layer.
[0076] Examples of conductive materials include carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fibers, carbon nanotubes, metal powders or metal fibers or metal tubes of copper, nickel, aluminum, silver, etc., and conductive polymers such as polyphenylene derivatives. However, the conductive material is not limited to these, and any material used as a conductive material in the relevant technical field can be used.
[0077] Examples of the binder that can be used include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above-mentioned polymers, styrene-butadiene rubber-based polymers, polyacrylic acid, lithium-substituted polyacrylic acid, polyamide-imide, and polyimide, but are not limited to these. Any binder that can be used in the relevant technical field can be used.
[0078] As the solvent, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but the solvent is not limited to these, and any solvent available in the art can be used.
[0079] A plasticizer or pore-forming agent may be further added to the negative electrode active material composition to form pores within the electrode plate.
[0080] The contents of the composite negative electrode active material, conductive material, binder, and solvent used in the negative electrode are at levels typically used in lithium batteries. Depending on the application and configuration of the lithium battery, one or more of the conductive material, binder, and solvent may be omitted.
[0081] The content of the binder contained in the negative electrode is 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the negative electrode active material layer. The content of the conductive material contained in the negative electrode is 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the negative electrode active material layer. The content of the composite negative electrode active material contained in the negative electrode is 0.1 wt% to 99 wt%, 0.1 wt% to 90 wt%, 0.1 wt% to 50 wt%, 0.1 wt% to 30 wt%, 0.1 wt% to 20 wt%, or 0.1 wt% to 10 wt% of the total weight of the negative electrode active material layer.
[0082] The negative electrode may further include other conventional negative electrode active materials in addition to the composite negative electrode active material described above.
[0083] Examples of conventional negative electrode active materials include, but are not limited to, one or more selected from the group consisting of lithium metal, metals capable of being alloyed with lithium, transition metal oxides, non-transition metal oxides, and carbon-based materials. Any material used as a negative electrode active material for lithium batteries in the art may be used.
[0084] Examples of metals that can be alloyed with lithium include Si, Sn, Al, Ge, Pb, Bi, Sb, Si-X alloys (X is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, but is not Si), and Sn-X alloys (X is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, but is not Sn). The element X is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.
[0085] Examples of the transition metal oxide include lithium titanium oxide, vanadium oxide, and lithium vanadium oxide. The non-transition metal oxide is, for example, SnO2.
[0086] The carbon-based material is, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is, for example, graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite. The amorphous carbon is, for example, soft carbon (low-temperature sintered carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0087] The total content of the composite negative electrode active material and the conventional negative electrode active material contained in the negative electrode is 80 wt% to 99 wt%, 90 wt% to 99 wt%, or 90 wt% to 95 wt% of the total weight of the negative electrode active material layer. On the other hand, the negative electrode is also a dry negative electrode produced by a dry process.
[0088] The dry-type negative electrode includes a dry composite negative electrode active material, a dry conductive material, and a dry binder. The dry composite negative electrode active material includes a core; and a shell disposed along the surface of the core. The core includes a silicon-containing structure, a silicon-containing compound, or a combination thereof. The shell has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4. If a is 1, 2, or 3, then b is not an integer) and includes one or more first metal oxides; and a first carbon-based material. The first metal oxide is disposed within the first carbon-based material matrix. M is one or more metals selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.
[0089] The method for manufacturing a dry-type negative electrode includes, for example, the steps of dry-mixing a dry composite negative electrode active material, a dry conductive material, and a dry binder to prepare a dry mixture; providing a negative electrode current collector; disposing an intermediate layer on one surface of the negative electrode current collector; and disposing the dry mixture on the intermediate layer and rolling it to manufacture a negative electrode having a negative electrode active material layer disposed on one surface of the negative electrode current collector.
[0090] First, a composite negative electrode active material, a dry conductive material, and a dry binder are dry-mixed to prepare a dry mixture. Dry mixing means mixing in a state without including a process solvent. The process solvent is, for example, a solvent used in the manufacture of an electrode slurry. The process solvent is, for example, water, NMP, etc., but is not limited thereto, as long as it is a process solvent used during the manufacture of an electrode slurry. Dry mixing can be performed using a stirrer, for example, at a temperature of 25 to 65°C. Dry mixing can be performed using a stirrer, for example, at a rotational speed of 10 to 10,000 rpm, or 100 to 10,000 rpm. Dry mixing can be performed using a stirrer, for example, for 1 to 200 minutes, or 1 to 150 minutes. The composite negative electrode active material is a dry composite negative electrode active material.
[0091] The dry mixing may be performed, for example, one or more times. First, the dry composite negative active material, the dry conductive material, and the dry binder may be primarily dry mixed to prepare a first mixture. The primary dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 2000 rpm or less for a time period of 15 minutes or less. The primary dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 500 to 2000 rpm for 5 to 15 minutes. The primary dry mixing may allow the dry composite negative active material, the dry conductive material, and the dry binder to be uniformly mixed. Then, the dry composite negative active material, the dry conductive material, and the dry binder may be secondarily dry mixed to prepare a second mixture. The secondary dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 4000 rpm or more for 10 minutes or more. The secondary dry mixing may be carried out, for example, at a temperature of 25 to 65° C. and a rotation speed of 4000 to 9000 rpm for 10 to 60 minutes. A dry mixture containing a fibrillated dry binder is obtained by the secondary dry mixing.
[0092] The agitator is, for example, a kneader. The agitator includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and a blade rotatably coupled to the rotating shaft and disposed in the longitudinal direction of the rotating shaft. The blade may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blade, the dry negative electrode composite active material, the dry conductive material, and the dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0093] The produced dry mixture can be put into an extrusion device and extruded into a sheet. The pressure during extrusion is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The obtained sheet-like extrudate is also a sheet for a negative electrode active material layer.
[0094] Examples of the dry conductive material include carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fiber, carbon nanotubes, metal powder or metal fiber or metal tube such as copper, nickel, aluminum, silver, etc., and conductive polymers such as polyphenylene derivatives, but are not limited thereto. Any material used as a conductive material in the art can be used. The conductive material is, for example, a carbon-based conductive material. The dry conductive material is a conductive material that is not in contact with a process solvent.
[0095] Examples of the dry binder include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above polymers, and styrene-butadiene rubber-based polymers, but are not limited thereto. Any material available in the art may be used. An example of the dry binder is polytetrafluoroethylene (PTFE). The dry binder is a binder that has not come into contact with a process solvent.
[0096] A plasticizer or pore-forming agent may be further added to the dry mixture to form pores within the negative electrode active material layer.
[0097] The contents of the dry composite negative electrode active material, the dry conductive material, and the dry binder used in the negative electrode active material layer are in the same ranges as those of the wet negative electrode.
[0098] Next, a negative electrode current collector is provided, which may be, for example, an aluminum foil. Next, an intermediate layer is disposed on at least one surface of the negative electrode current collector. The intermediate layer includes a carbon-based conductive material and a binder. The intermediate layer may be omitted.
[0099] Next, the sheet for the negative electrode active material layer provided on the intermediate layer is placed and rolled to produce a negative electrode in which the negative electrode active material layer is placed on one side of the negative electrode current collector. The intermediate layer is placed between the negative electrode current collector and the negative electrode active material layer. The rolling may be, for example, a roll press or a flat plate press, but is not necessarily limited thereto. The pressure during rolling may be, for example, 0.1 ton / cm. 2 ~10.0ton / cm 2 However, the range is not limited thereto. If the pressure during rolling is too high, cracks may occur in the negative electrode current collector. If the pressure during rolling is too low, the adhesive strength between the negative electrode current collector and the negative electrode active material layer may decrease.
[0100] According to yet another embodiment, a lithium battery employs a negative electrode including the composite negative electrode active material described above.
[0101] The lithium battery employs a positive electrode containing the above-mentioned composite positive electrode active material, thereby providing improved cycle characteristics and reduced volume change.
[0102] The lithium battery can be manufactured, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to the required conditions.
[0103] First, the negative electrode is manufactured by the above-mentioned method for manufacturing the negative electrode. Next, a positive electrode active material composition is prepared by mixing a positive electrode active material, a conductive material, a binder, and a solvent. The positive electrode active material composition is directly coated on an aluminum current collector and dried to manufacture a positive electrode plate. Alternatively, the positive electrode active material composition may be cast on a separate support, and the film peeled off from the support may be laminated on an aluminum current collector to manufacture a positive electrode plate.
[0104] The positive electrode active material may be any lithium-containing metal oxide that is commonly used in the art. The positive electrode active material may be one or more of composite oxides of metals and lithium selected from cobalt, manganese, nickel, and combinations thereof. The positive electrode active material may be, but is not limited to, one or more selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide. Any positive electrode active material may be used in the art as long as it is used as a positive electrode active material for lithium batteries.
[0105] The positive electrode active material is, for example, Li a A 1-b B b D2 (wherein, 0.90≦a≦1.8 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1.8, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-αF2 (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F α (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (wherein, 0.90≦a≦1.8, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein, 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d GeO2 (wherein, 0.90≦a≦1.8, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, 0.90≦a≦1.8, 0.001≦b≦0.1); Li a CoG b O2 (wherein, 0.90≦a≦1.8, 0.001≦b≦0.1); Li a MnG b O2 (wherein, 0.90≦a≦1.8, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1.8, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f)J2(PO4)3(0≦f≦2);Li (3-f) This includes compounds expressed by any one of the chemical formulas Fe2(PO4)3(0≦f≦2); and LiFePO4.
[0106] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0107] It is also possible to use a compound in which a coating layer is added to the surface of the above-mentioned compound, and it is also possible to use a mixture of the above-mentioned compound and the above-mentioned compound to which a coating layer is added. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of the coating element of the coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A detailed description of the specific coating method is omitted because it is well understood by those engaged in the field.
[0108] The positive electrode active material is, for example, LiNiO2, LiCoO2, LiMn x O2x (x = 1, 2), LiNi 1-x Mn x O2(0 < x < 1), LiNi 1-x-y Co x Mn y O2(0 ≦ x ≦ 0.5, 0 ≦ y ≦ 0.5), LiFeO2, V2O5, TiS, MoS, etc. can be used.
[0109] The positive electrode active material is, for example, Li a Ni x Co y M z O 2-b A b (1.0 ≦ a ≦ 1.2, 0 ≦ b ≦ 0.2, 0.8 ≦ x < 1, 0 ≦ y ≦ 0.3, 0 < z ≦ 0.3, x + y + z = 1, M is one or more selected from the group consisting of manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), and boron (B), A is F, S, Cl, Br, or a combination thereof), LiNi x Co y Mn z O2(0.8 ≦ x ≦ 0.95, 0 < y ≦ 0.2, 0 < z ≦ 0.2 and x + y + z = 1), LiNi x Co y Al z O2(0.8 ≦ x ≦ 0.95, 0 ≦ y ≦ 0.2, 0 < z ≦ 0.2, x + y + z = 1), LiNi x Co y Al v Mn w O2(0.8 ≦ x ≦ 0.95, 0 ≦ y ≦ 0.2, 0 < v ≦ 0.2, 0 < w ≦ 0.2, x + y + v + w = 1), Li a Ni x Mn y M’ z O 2-b A b(1.0 ≦ a ≦ 1.2, 0 ≦ b ≦ 0.2, 0 < x ≦ 0.3, 0.5 ≦ y < 1, 0 < z ≦ 0.3, and x + y + z = 1, M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, A is F, S, Cl, Br or a combination thereof, etc. can be used.)
[0110] In the positive electrode active material composition, the conductive material, binder and solvent are the same as those in the case of the negative electrode active material composition. On the other hand, a plasticizer may be further added to the positive electrode active material composition and / or the negative electrode active material composition to form pores inside the electrode plate.
[0111] The contents of the positive electrode active material, conductive material, binder and solvent are at levels commonly used in lithium batteries. Depending on the use and configuration of the lithium battery, one or more of the above-mentioned conductive material, binder and solvent may be omitted.
[0112] The binder content contained in the positive electrode is, for example, 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The content of the conductive material contained in the positive electrode is also, for example, 0.1 to 10 wt% or 0.1 to 5 wt% of the total weight of the positive electrode active material layer. The positive electrode active material content contained in the positive electrode is, for example, 70 wt% to 99 wt%, 90 wt% to 99 wt%, or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer.
[0113] Next, a separator inserted between the positive electrode and the negative electrode is prepared.
[0114] Any separator that is generally used in lithium batteries can be used. The separator is, for example, one that has low resistance to ion movement of the electrolyte and has excellent electrolyte moisture-absorbing ability. The separator is, for example, one selected from glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene (PTFE), or a combination thereof, and is in the form of a nonwoven fabric or a woven fabric. For lithium ion batteries, a separator that can be wound, such as polyethylene or polypropylene, is used, and for lithium ion polymer batteries, a separator that has excellent organic electrolyte impregnation ability is used.
[0115] The separator is manufactured by the following exemplary method, but is not necessarily limited to such method, and may be adjusted according to the required conditions.
[0116] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated on the top of an electrode and dried to form a separator. Alternatively, the separator composition is cast on a support and dried, and the separator film is peeled off from the support and laminated on the top of an electrode to form a separator.
[0117] The polymer used in the manufacture of the separator is not particularly limited, and any polymer that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0118] The electrolyte is then prepared. The electrolyte is, for example, an organic electrolyte solution, which is produced by dissolving a lithium salt in an organic solvent, for example.
[0119] The organic solvent can be any organic solvent used in the art. The organic solvent can be, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a mixture thereof.
[0120] Any lithium salt that is used as a lithium salt in the art can be used. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(CyF 2y+1 SO2) (1≦x≦20, 1≦y≦20), LiCl, LiI or a mixture thereof.
[0121] Meanwhile, the electrolyte is a solid electrolyte. The solid electrolyte is, for example, boron oxide, lithium oxynitride, etc., but is not limited thereto, and any solid electrolyte used as a solid electrolyte in the art can be used. The solid electrolyte is formed on the negative electrode by a method such as sputtering, or a separate solid electrolyte sheet is laminated on the negative electrode.
[0122] The solid electrolyte is, for example, an oxide-based solid electrolyte or a sulfide-based solid electrolyte.
[0123] The solid electrolyte is, for example, an oxide-based solid electrolyte. The oxide-based solid electrolyte is Li 1+x+y Al x Ti 2-x S y P 3-y O 12 (0 <x<2,0≦y<3),BaTiO3,Pb(Zr,Ti)O3(PZT),Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≦x<1,O≦y<1),PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT),HfO2,SrTiO3,SnO2,CeO2,Na2O,MgO,NiO,CaO,BaO,ZnO,ZrO2,Y2O3,Al2O3,TiO2,SiO2,Li3PO4,Li x Ti y (PO4)3(0 <x<2,0<y<3),Li x Al y Ti z (PO4)3(0 <x<2,0<y<1,0<z<3),Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x S y P 3-y O 12 (0≦x≦10≦y≦1), Li x La y TiO3(0 <x<2,0<y<3),Li2O,LiOH,Li2CO3,LiAlO2,Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2,Li 3+x La3M2O 12 (M=Te, Nb, or Zr, x is an integer from 1 to 10). The solid electrolyte is produced by a sintering method or the like. For example, an oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer of 1 to 10) is a garnet-type solid electrolyte selected from the group consisting of:
[0124] Sulfide-based solid electrolytes include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or combinations thereof. Sulfide-based solid electrolyte particles include Li2S, P2S5, SiS2, GeS2, B2S3, or combinations thereof. Sulfide-based solid electrolyte particles are also Li2S or P2S5. Sulfide-based solid electrolyte particles are known to have high lithium ion conductivity compared to other inorganic compounds. For example, sulfide-based solid electrolytes include Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte contains Li2S-P2S5, the mixed molar ratio of Li2S:P2S5 is, for example, also in the range of about 50:50 to about 90:10. Also, Li3PO4, halogens, halogen compounds, Li 2+2x Zn 1-x GeO4 (“LISICON”, 0 ≦ x < 1), Li 3+y PO 4-x N x( “LIPON”, 0 < x < 4, 0 < y < 3), Li 3.25 Ge 0.25 P 0.75 S4 (“ThioLISICON”), Li2O - Al2O3 - TiO2 - P2O 5( “LATP”), etc., are added to inorganic solid electrolytes such as Li2S - P2S5, SiS2, GeS2, B2S3, or combinations thereof to produce inorganic solid electrolytes that can be used as sulfide solid electrolytes. Non-limiting examples of sulfide solid electrolyte materials are Li2S - P2S5; Li2S - P2S5 - LiX (X = halogen element); Li2S - P2S5 - Li2O; Li2S - P2S5 - Li2O - LiI; Li2S - SiS2; Li2S - SiS2 - LiI; Li2S - SiS2 - LiBr; Li2S - SiS2 - LiCl; Li2S - SiS2 - B2S3 - LiI; Li2S - SiS2 - P2S5 - LiI; Li2S - B2S3; Li2S - P2S5 - Z m S n (0 < m < 10, 0 < n < 10, Z = Ge, Zn or Ga); Li2S - GeS2; Li2S - SiS2 - Li3PO4; and Li2S - SiS2 - Li p MO qIt contains (0 < p < 10, 0 < q < 10, M = P, Si, Ge, B, Al, Ga or In). In this regard, the sulfide-based solid electrolyte material can be manufactured by treating the raw starting materials of the sulfide-based solid electrolyte substance (for example, Li2S, P2S5, etc.) by methods such as the melt quenching method or the mechanical milling method. Also, a calcination process can be performed after the above treatment. The sulfide-based solid electrolyte can be amorphous, crystalline, or a mixture of these.
[0125] Referring to FIG. 6, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. An organic electrolyte is injected into the battery case 5 and sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to such a form, and can be, for example, angular, thin-film-like, etc.
[0126] Referring to FIG. 7, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. A separator 4 is disposed between the positive electrode 3 and the negative electrode 2, and the positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. It includes an electrode tab 8 that serves as an electrical path for guiding the current formed by the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is angular, but is not necessarily limited to such a form, and can also be, for example, cylindrical, thin-film-like, etc.
[0127] Referring to FIG. 8, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2 to form a battery structure. Battery structures 7 are stacked in a bi-cell structure and then housed in a battery case 5. The battery structure 7 includes electrode tabs 8 that act as electrical paths for conducting current generated in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape and may be cylindrical, thin film, etc.
[0128] The pouch-type lithium battery corresponds to the lithium batteries of FIGS. 6 to 8, respectively, in which a pouch is used as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, and then impregnated with an organic electrolyte, and then housed in a pouch and sealed to complete the pouch-type lithium battery. For example, although not shown, the above-mentioned positive electrode, negative electrode, and separator are simply stacked and housed in a pouch in the form of an electrode assembly, or wound into a jelly-roll-shaped electrode assembly, or folded and then housed in a pouch. Then, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0129] Lithium batteries have excellent life characteristics and high rate characteristics, and are therefore used, for example, in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and fields requiring large amounts of power storage, such as electric bicycles and power tools.
[0130] Lithium batteries are stacked in multiple numbers to form a battery module, and multiple battery modules form a battery pack. Such a battery pack can be used in all devices that require high capacity and high output. For example, it can be used in notebook computers, smartphones, electric vehicles, etc. The battery module includes, for example, a plurality of batteries and a frame that holds them. The battery pack includes, for example, a plurality of battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. A plurality of battery packs are regulated by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0131] Furthermore, a method for manufacturing a composite negative electrode active material according to still another embodiment includes providing a silicon-containing negative electrode active material such as a silicon-containing structure, a silicon-containing compound, or a combination thereof; providing a composite; and mechanically milling the silicon-containing structure, the silicon-containing compound, or a combination thereof with the composite; The composite has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer) of one or more first metal oxides; and a first carbon-based material; wherein the first metal oxide is disposed within the first carbon-based material matrix, and said M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements.
[0132] A silicon-containing negative electrode active material is provided. The silicon-containing negative electrode active material is, for example, a silicon-containing structure, a silicon-containing compound, or a combination thereof. The silicon-containing structure is, for example, the silicon composite structure described above. The silicon-containing compound is, for example, SiO x (0 < x < 2).
[0133] The step of providing the composite includes, for example, M a O c(0 < a ≤ 3, 0 < c ≤ 4, and when a is 1, 2, or 3, b is an integer), supplying a reaction gas composed of a carbon source gas to one or more second metal oxides represented thereby, and including a step of producing a composite by heat treatment, wherein M is one or more selected metals from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.
[0134] The carbon source gas is a compound represented by the following Chemical Formula 1, or one or more mixed gases selected from the group consisting of a compound represented by the following Chemical Formula 1, a compound represented by the following Chemical Formula 2, and an oxygen-containing gas represented by the following Chemical Formula 3.
[0135] <Chemical Formula 1> C n H (2n+2-a) [OH] a In the Chemical Formula 1, n is 1 to 20, and a is 0 or 1; <Chemical Formula 2> C n H 2n In the Chemical Formula 2, n is 2 to 6; <Chemical Formula 3> C x H y O z In the Chemical Formula 3, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.
[0136] The compound represented by Chemical Formula 1 and the compound represented by Chemical Formula 2 are one or more selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 3 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.
[0137] M a O cA reaction gas composed of a carbon source gas is supplied to a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer), and after the heat treatment step, a cooling step using one or more inert gases selected from the group consisting of nitrogen, helium, and argon is further performed. The cooling step refers to the step of adjusting to room temperature (20 - 25°C). The carbon source gas contains one or more inert gases selected from the group consisting of nitrogen, helium, and argon.
[0138] In the method for producing a composite, the growth process of a carbon-based material, such as graphene, by gas-phase reaction can be carried out under various conditions.
[0139] According to the first condition, for example, M a O c Methane is first supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is placed, and the temperature is raised to the heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700 - 1100°C. Heat treatment is carried out during the reaction time at the heat treatment temperature (T). The reaction time is, for example, 4 - 8 hours. The heat-treated product is cooled to room temperature to produce a composite. The time taken for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 1 - 5 hours.
[0140] According to the second condition, for example, M a O c Hydrogen is first supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is placed, and the temperature is raised to the heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700 - 1100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), methane gas is supplied, and heat treatment is carried out during the remaining reaction time. The reaction time is, for example, 4 - 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 1 - 5 hours.
[0141] According to the third condition, for example, M a O c (0 < a ≤ 3, 0 < c ≤ 4, if a is 1, 2, or 3, then c is an integer), hydrogen is first supplied to a reactor in which the second metal oxide is disposed, and the temperature is raised to the heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700 to 1100 °C. After heat treatment for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and heat treatment is carried out during the remaining reaction time. The reaction time is, for example, 4 to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for the cooling process from the heat treatment temperature (T) to room temperature is, for example, 1 to 5 hours.
[0142] In the process of producing the composite, when the carbon source gas contains water vapor, a composite having very excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited and is, for example, 0.01 to 10% by volume based on 100% by volume of the total carbon source gas. The carbon source gas is, for example, methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.
[0143] The carbon source gas is also, for example, methane; a mixed gas of methane and carbon dioxide; or a mixed gas of methane, carbon dioxide, and water vapor. In the mixed gas of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixed gas of methane, carbon dioxide, and water vapor, the molar ratio of methane to carbon dioxide to water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.
[0144] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixed gas of methane and nitrogen. In the mixed gas of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas does not contain an inert gas such as nitrogen.
[0145] The heat treatment pressure is selected in consideration of factors such as the heat treatment temperature, the composition of the gas mixture, and the amount of the desired carbon coating. The heat treatment pressure is controlled by adjusting the amount of the inflowing gas mixture and the amount of the outflowing gas mixture. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more.
[0146] The heat treatment time is not particularly limited and can be appropriately adjusted according to the heat treatment temperature, the pressure during the heat treatment, the composition of the gas mixture, and the amount of the desired carbon coating. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene (carbon), increases, and thereby the electrical physical properties of the composite can be improved. However, such a tendency is not necessarily directly proportional to time. For example, after a predetermined time has elapsed, no further carbon deposition, for example, graphene deposition, occurs, or the deposition rate decreases.
[0147] Even at a relatively low temperature through the gas-phase reaction of the above-described carbon source gas, M a O c (0 < a ≤ 3, 0 < c ≤ 4, if a is 1, 2, or 3, then c is an integer), and the reduced product thereof, M a O b (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer), a composite is obtained by providing a uniform carbon-based material coating, for example, a graphene coating, on one or more selected from the first metal oxides represented by the formula.
[0148] The composite has, for example, a matrix of a carbon-based material having one or more structures selected from a spherical structure, a spiral structure in which a plurality of spherical structures are connected, a cluster structure in which a plurality of spherical structures are aggregated, and a sponge structure, for example, a graphene matrix, and M disposed within the matrix of the carbon-based material a O b a first metal oxide represented by (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer) and M a O c and includes one or more selected from a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and c is an integer if a is 1, 2, or 3).
[0149] Next, the silicon-containing structure, the silicon-containing compound, or a combination thereof and the composite are mechanically milled. In the step of mechanical milling, the milling method is not particularly limited and is a method of bringing the silicon-containing structure, the silicon-containing compound, or a combination thereof and the composite into contact and applying pressure using a machine, and any method that can be used in the art can be used. When milling, a nobel tumbler or the like is used. The rotation speed of the mixer during milling is, for example, 2000 rpm or more, or 3000 rpm or more. The rotation speed of the mixer during milling is, for example, 4000 rpm or less. The rotation speed of the mixer during milling is, for example, 2000 rpm to 4000 rpm, or 3000 rpm to 4000 rpm.
[0150] If the milling speed is too low, the shear force applied to the silicon-containing structure, silicon-containing compound, or combination thereof and the composite is weak, so that the silicon-containing structure, silicon-containing compound, or combination thereof and the composite are difficult to be composited. If the milling speed is too high, the composite is uniformly coated on the silicon-containing structure and / or silicon-containing compound, and it is difficult to form a uniform and continuous shell. The milling time is, for example, 5 minutes to 100 minutes, 5 minutes to 60 minutes, or 5 minutes to 30 minutes. If the milling time is too short, the composite is uniformly coated on the silicon-containing structure and / or silicon-containing compound, and it is difficult to form a uniform and continuous shell. If the milling time is too long, the production efficiency is reduced. The content of the composite is 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, or 1 wt% or less of the total weight of the silicon-containing negative electrode active material and the composite. The content of the composite is, for example, 0.01 to 5 wt%, 0.01 to 4 wt%, 0.01 to 3 wt%, 0.1 to 2 wt%, or 0.1 to 1 wt% of the total weight of the silicon-containing negative electrode active material and the composite. For example, the content of the composite relative to 100 parts by weight of the mixture of the silicon-containing negative electrode active material and the composite is 0.01 to 5 parts by weight, 0.01 to 4 parts by weight, 0.01 to 3 parts by weight, 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, or 0.1 to 1 part by weight. The average particle size (D50) of the composite used for mechanical milling of the silicon-containing negative electrode active material and the composite is, for example, 50 nm to 200 nm, 100 nm to 300 nm, or 200 nm to 500 nm.
[0151] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are merely for the purpose of illustrating the present invention and are not intended to limit the scope of the present invention.
[0152] (Production of the complex) Production example 1: Al 2 O 3 @Gr complex After placing Al2O3 particles (average particle size: about 20 nm) inside the reactor, the temperature inside the reactor was raised to 1000 °C at a heating rate of about 23 °C / min under the condition that CH4 was supplied at about 300 sccm and 1 atm for about 30 minutes inside the reactor.
[0153] Next, heat treatment was carried out by holding at the said temperature for 7 hours. Next, the supply of CH4 was interrupted, the temperature inside the reactor was adjusted to room temperature (25 °C), and a composite in which Al2O3 particles and Al2O z (0 < z < 3) particles were embedded in graphene was obtained. The alumina content contained in the composite was 60 wt%.
[0154] Production example 2: Al 2 O 3 @Gr complex A composite was produced in the same manner as in Production Example 1, except that Al2O3 particles (average particle size: about 200 nm) were used instead of Al2O3 particles (average particle size: about 20 nm).
[0155] Comparative production example 1: SiO 2 @Gr complex After placing SiO2 particles (average particle size: about 15 nm) inside the reactor, the temperature inside the reactor was raised to 1000 °C at a heating rate of about 23 °C / min under the condition that CH4 was supplied at about 300 sccm and 1 atm for about 30 minutes inside the reactor.
[0156] Next, heat treatment was carried out by holding at the said temperature for 7 hours. Next, the supply of CH4 was interrupted, the temperature inside the reactor was adjusted to room temperature (25 °C), and SiO2 particles and SiO y (0 < y < 2) particles were embedded in graphene was obtained.
[0157] (Production of silicon-based negative electrode active material) Manufacturing example 3: Silicon composite structure Needle-shaped silicon was pulverized to obtain silicon suboxide (SiO x, plate-like and needle-like silicon particles with a length of about 125 nm and a thickness of about 40 nm, on the surface of which a film (0 < x < 2) was formed, were obtained.
[0158] A composition containing 30 parts by weight of plate-like and needle-like silicon particles, 10 parts by weight of stearic acid, and 60 parts by weight of isopropyl alcohol was prepared. The prepared composition was spray-dried and dried to obtain porous silicon secondary particles with an average particle size of about 5 μm.
[0159] For spray drying, a spray dryer (Micro Mist Spray Dryers, Fujisaki electric) was used. Under a nitrogen atmosphere, the spray nozzle size was about 5 μm, the pressure during spray drying was about 0.4 MPa, and the powder injection atmosphere temperature was about 200 °C. The composition prepared under such spray drying conditions was sprayed to remove isopropyl alcohol, and porous silicon secondary particles were produced.
[0160] The produced porous silicon secondary particles were placed in a reactor. Under the condition of supplying CH4 at about 300 sccm and 1 atm in the reactor, the temperature inside the reactor was raised to 1000 °C at a heating rate of about 23 °C / min.
[0161] Next, heat treatment was performed by holding at the above temperature for 5 hours. Then, the supply of CH4 was interrupted, and the temperature inside the reactor was adjusted to room temperature (25 °C) to obtain a porous silicon composite structure.
[0162] The porous silicon composite structure includes porous silicon secondary particles and high-crystalline first graphene flakes arranged on top of the porous silicon secondary particles. The porous silicon secondary particles include aggregates of two or more silicon composite primary particles. The silicon composite primary particles include silicon; silicon suboxide (SiO x , 0 < x < 2) and second graphene flakes arranged on the silicon suboxide.
[0163] The content of the first graphene flakes and the second graphene flakes in the silicon-containing composite structure was about 25 parts by weight based on 100 parts by weight of the total weight of the porous silicon composite. The silicon-containing composite structure was porous.
[0164] Manufacturing Example 4: Silicon composite structure + amorphous carbon coating layer 60 parts by weight of the silicon-containing composite structure produced in Production Example 3, 40 parts by weight of coal tar pitch, and 10 parts by weight of N-methylpyrrolidone were added to a planetary mixer, and a mixing step was carried out.
[0165] The mixing process allowed the coal tar pitch to infiltrate into the gaps of the porous silicon secondary particles contained in the silicon composite structure. The mixing process for infiltrating the coal tar pitch was performed in a total of four cycles, with stirring-degassing-stirring being performed in that order for 5 minutes each, for a total of 15 minutes. The stirring step had a revolution speed of 1000 rpm and a rotation speed of 1000 rpm, and the degassing step had a revolution speed of 2000 rpm and a rotation speed of 64 rpm. The coal tar pitch was divided into four portions by weight and added for each cycle. The mixing temperature was controlled at about 70°C. The mixed product was heat-treated in a nitrogen gas atmosphere at about 1,000°C for four hours.
[0166] A silicon composite structure was manufactured in which a carbon-based coating film including a first amorphous carbon was disposed on the silicon composite structure, and a second amorphous carbon was disposed inside the silicon composite structure. The second amorphous carbon was disposed in the pores of the porous silicon secondary particles contained in the silicon composite structure. The weight ratio of the first amorphous carbon to the second amorphous carbon was 1:2. The weight ratio of the carbon of the graphene flakes to the carbon of the amorphous carbon in the manufactured silicon composite structure was 2:8. The graphene flakes were a combination of both the first graphene flakes and the second graphene flakes. The amorphous carbon was a combination of both the first amorphous carbon and the second amorphous carbon.
[0167] (Production of composite negative electrode active material) Example 1: Al 2 O 3 @Gr composite 1wt% (alumina 0.6wt%) coating silicon composite structure The silicon composite structure manufactured in Manufacturing Example 3 and the composite prepared in Manufacturing Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 2000 rpm to about 4000 rpm using a Nobilta mixer (Hosokawa, Japan) to obtain a composite negative electrode active material. The composite negative electrode active material had a structure in which a shell including the composite and / or the milling product thereof was coated on a silicon-based negative electrode active material core.
[0168] The mixing weight ratio of the silicon composite structure obtained in Production Example 3 to the composite obtained in Production Example 1 was 99:1.
[0169] Example 2: Al 2 O 3 @Gr composite 0.1wt% coating silicon composite structure A composite negative electrode active material was prepared in the same manner as in Example 1, except that the weight ratio of the silicon composite structure obtained in Preparation Example 3 to the composite obtained in Preparation Example 1 was changed to 99.9:0.1.
[0170] Example 3: Al 2 O 3 @Gr composite 0.5wt% coating silicon composite structure A composite negative electrode active material was prepared in the same manner as in Example 1, except that the weight ratio of the silicon composite structure obtained in Preparation Example 3 to the composite obtained in Preparation Example 1 was changed to 99.5:0.5.
[0171] Example 4: Al 2 O 3 @Gr composite 5wt% coating silicon composite structure A composite negative electrode active material was prepared in the same manner as in Example 1, except that the weight ratio of the silicon composite structure obtained in Preparation Example 3 and the composite obtained in Preparation Example 1 was changed to 95:5.
[0172] Example 5: Al 2 O 3 @Gr composite 1wt% + CNT 0.1wt% coated silicon composite structure A composite negative electrode active material was produced in the same manner as in Example 1, except that the weight ratio of the silicon composite structure obtained by Production Example 3, the composite obtained by Production Example 1, and carbon nanotubes (CNT) was changed to 98.9:1.0:0.1.
[0173] In addition to the silicon composite structure obtained by Production Example 3 and the composite obtained by Production Example 1, carbon nanotubes (CNT) were additionally used. The length of the carbon nanotubes was 200 nm to 300 nm, and the diameter of the carbon nanotubes was about 10 nm.
[0174] Example 6: Al 2 O 3 @Gr composite 1wt% coating silicon composite structure, alumina particle size 200nm A composite negative electrode active material was produced in the same manner as in Example 1, except that the composite obtained by Production Example 2 was used instead of the composite obtained by Production Example 1.
[0175] Example 7: Al 2 O 3 @Gr composite 1wt% coating [amorphous carbon coated silicon composite structure] A composite negative electrode active material was produced in the same manner as in Example 1, except that the amorphous carbon-coated silicon composite structure obtained by Production Example 4 was used instead of the silicon composite structure obtained by Production Example 3.
[0176] Example 8: Al 2 O 3 @Gr composite 1wt% coating SiO x A composite negative electrode active material was produced in the same manner as in Example 1, except that SiO with an average particle size of 6 μm x (0 < x < 2) was used as the silicon-based negative electrode active material.
[0177] Comparative Example 1: Bare Silicon Composite Structure The silicon composite structure produced by Production Example 3 was used as the negative electrode active material as it was.
[0178] Comparative example 2: [Al 2 O3 + graphene (Gr)] mixture 1wt% coated silicon composite structure A composite negative electrode active material was produced in the same manner as in Example 1, except that a simple mixture of Al2O3 particles (average particle size: about 20 nm) and graphene at a weight ratio of 60:40 was used instead of the composite produced in Production Example 1.
[0179] Comparative example 3: Al 2 O 3 Simple mixtures of @Gr and silicon composite structures A simple mixture of the silicon composite structure produced in Production Example 3 and the composite produced in Production Example 1 at a weight ratio of 99:1 was used as the negative electrode active material as it was.
[0180] Comparative example 4: SiO 2 @Gr composite 1wt% coating silicon composite structure A composite negative electrode active material was produced in the same manner as in Example 1, except that the composite obtained in Comparative Production Example 1 was used instead of the composite produced in Production Example 1.
[0181] Comparative example 5: bare SiO x SiO with an average particle size of 6 μm x (0 < x < 2) was used as the negative electrode active material as it was.
[0182] (Manufacture of Lithium Battery (Full Cell), Wet Anode) Example 9 (Manufacture of Anode) The composite negative electrode active material produced in Example 1, graphite, a CMC / SBR binder (a 1:1 weight ratio mixture), and deionized water were mixed to produce a slurry. The mixing ratio of the solid content of the mixture of the composite negative electrode active material and graphite and the CMC / SBR binder was 97.5:2.5 by weight. The weight ratio of the composite negative electrode active material to graphite in the mixture of the composite negative electrode active material and graphite produced according to Example 1 was 2:98.
[0183] The slurry was bar-coated to a thickness of 100 μm on a copper foil current collector, dried at room temperature, then vacuum-dried again under vacuum conditions at 120 °C, and rolled to produce an anode.
[0184] (Production of positive electrodes) LiNi 0.91 Co 0.05 Al 0.04 A mixture of O2 (hereinafter referred to as NCA91) composite positive electrode active material, carbon conductive material (Denka Black), and polyvinylidene fluoride (PVdF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0185] The slurry was bar-coated on an aluminum current collector to a thickness of 40 μm, dried at room temperature, and then dried again under vacuum at 120° C. and rolled to prepare a positive electrode.
[0186] (Coin cell manufacturing) Coin cells were fabricated using the fabricated positive and negative electrodes, polypropylene separators (Celgard 3510), and a solution of 1.15M LiPF6 and 1.5wt% vinylene carbonate (VC) dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (volume ratio 2:4:4) as an electrolyte.
[0187] Examples 10 to 16 Coin cells were prepared in the same manner as in Example 9, except that the composite negative electrode active materials prepared in Examples 2 to 8 were used instead of the composite negative electrode active material prepared in Example 1.
[0188] Comparative Examples 6 to 10 Coin cells were prepared in the same manner as in Example 9, except that the negative active materials prepared in Comparative Examples 1 to 5 were used instead of the composite negative active material prepared in Example 1.
[0189] (Lithium battery (full cell) manufacturing, dry anode) Example 17 (Production of negative electrodes) The composite negative electrode active material prepared in Example 1 as a dry first negative electrode active material, graphite as a dry second negative electrode active material, a carbon conductive material (Denka Black) as a dry conductive material, and polytetrafluoroethylene (PTFE) as a dry binder were charged into a blade mixer in a weight ratio of 1.8:90.2:4:4, and then primary dry mixing was performed at 25° C. and 1000 rpm for 10 minutes to prepare a first mixture in which the first negative electrode active material, the second negative electrode active material, the conductive material, and the binder were uniformly mixed.
[0190] Then, in order to promote fiberization of the binder, the first mixture was further mixed at 25° C. and 5000 rpm for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0191] The prepared second mixture was put into an extruder and extruded to prepare a sheet-shaped negative electrode active material layer self-standing film under a pressure of 50 MPa.
[0192] A carbon layer was disposed as an interlayer on one surface of a copper thin film having a thickness of 12 μm, and the interlayer was disposed on one surface of a second positive electrode current collector to prepare a first laminate.
[0193] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was about 1 μm.
[0194] A negative electrode active material layer free-standing film was placed on the intermediate layer of the prepared first laminate, and rolled to produce a negative electrode.
[0195] (Production of positive electrodes) LiNi 0.91 Co 0.05 Al 0.04A mixture of a composite cathode active material of O2 (hereinafter referred to as NCA91), a carbon conductive material (Denka Black), and polyvinylidene fluoride (PVdF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to produce a slurry.
[0196] The slurry was bar-coated on an aluminum current collector to a thickness of 40 μm, dried at room temperature, then dried again under vacuum conditions at 120 °C, and rolled to produce a cathode.
[0197] (Manufacture of coin cells) Using the cathode and anode manufactured above, a polypropylene separator (Celgard 3510) and a solution in which 1.15 M LiPF6 and 1.5 wt% vinylene carbonate (VC) are dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (volume ratio of 2:4:4) were used as electrolytes to manufacture coin cells respectively.
[0198] Comparative Example 11 Coin cells were manufactured in the same manner as in Example 17, except that the anode active material prepared in Comparative Example 1 was used instead of the composite anode active material manufactured in Example 1 as the dried first anode active material.
[0199] Evaluation example 1: Specific surface area and particle size evaluation The specific surface area and particle size of the silicon composite structure manufactured in Production Example 3, the composite anode active material manufactured in Example 1, SiO prepared in Comparative Example 5 x (0 < x < 1) and the composite anode active material manufactured in Example 8 were measured, and the results are shown in Table 1 below. The specific surface area was measured by the nitrogen adsorption method. The particle size was measured using a laser scattering particle size distribution analyzer.
[0200]
Table 1
[0201] As shown in Table 1, the composite negative electrode active material produced in Example 1 had an increased specific surface area and decreased D10, D50, and D90 particle sizes compared to the silicon composite structure produced in Production Example 3.
[0202] Also, the composite negative electrode active material produced in Example 8 had an increased specific surface area and decreased D10 and D50 particle sizes compared to SiO x (0 < x < 2).
[0203] Evaluation example 2: XPS spectrum evaluation (I) During the production process of the composite produced in Production Example 1, XPS spectra were measured using Quantum 2000 (Physical Electronics) over time. The XPS spectra of the C 1s orbital and Al 2p orbital were measured for samples before heating, after 1 minute, after 5 minutes, after 30 minutes, after 1 hour, and after 4 hours, respectively. At the initial stage of heating, only a peak for the Al 2p orbital was shown, and no peak for the C 1s orbital was shown. After 30 minutes, a peak for the C 1s orbital was clearly shown, and the magnitude of the peak for the Al 2p orbital decreased significantly.
[0204] After 30 minutes, a peak for the C 1s orbital due to C-C bonds and C=C bonds resulting from the growth of graphene was clearly shown near 284.5 eV.
[0205] As the reaction time elapsed, the oxidation number of aluminum decreased, causing the peak position of the Al 2p orbital to shift further to the side with lower binding energy (eV).
[0206] Therefore, it was confirmed that as the reaction proceeded, graphene grew on the Al2O3 particles and Al2O x (0 < x < 3) was generated.
[0207] The average contents of carbon and aluminum were measured through XPS analysis results in 10 regions of the composite sample manufactured in Production Example 1. The deviation of the aluminum content for each region was calculated for the measurement results. The deviation of the aluminum content was shown as a percentage with respect to the average value, and this was referred to as the uniformity. The percentage with respect to the average value of the deviation of the aluminum content, that is, the uniformity of the aluminum content, was 1%. Therefore, it was confirmed that alumina was uniformly distributed in the composite manufactured in Production Example 1.
[0208] Evaluation example 3: XPS spectrum evaluation (II) The silicon composite structure manufactured in Production Example 3, the composite negative electrode active material manufactured in Example 1 (silicon composite structure coated with an Al2O3@Gr composite), SiO prepared in Comparative Example 5 x (0 < x < 2), and the XPS spectra of the composite negative electrode active material manufactured in Example 8 (SiO coated with an Al2O3@Gr composite) x (0 < x < 2)) are shown in FIGS. 2A to 3D.
[0209] As shown in FIGS. 2A to 2D, for the composite negative electrode active material manufactured in Example 1, compared with the silicon composite structure manufactured in Production Example 3, the size of the carbon peak was partially decreased, the size of the oxygen peak was increased, the size of the silicon peak was partially decreased, and the size of the aluminum peak was significantly increased. Therefore, it was confirmed that a composite containing aluminum and oxygen was coated on the surface of the silicon composite structure.
[0210] As shown in FIGS. 3A to 3D, for the composite negative electrode active material manufactured in Example 8, compared with SiO prepared in Comparative Example 5 x (0 < x < 2), the size of the carbon peak was partially decreased, the size of the oxygen peak was increased, the size of the silicon peak was partially decreased, and the size of the aluminum peak was significantly increased. Therefore, it was confirmed that a composite containing aluminum and oxygen was coated on the surface of the silicon composite structure.
[0211] The silicon composite structure manufactured in Production Example 3, the composite negative electrode active material manufactured in Example 1, SiO prepared in Comparative Example 5 x (0 < x < 2), and the contents of the elements obtained from the XPS spectra of the composite negative electrode active material manufactured in Example 8 are shown in Table 2 below.
[0212]
Table 2
[0213] As shown in Table 1, the silicon composite structure manufactured in Production Example 3 and SiO prepared in Comparative Example 5 x do not contain the aluminum (Al) element.
[0214] On the other hand, the aluminum (Al) element contents of the composite negative electrode active materials in Example 1 and Example 8 were 1.2 at% and 3.3 at%, respectively.
[0215] Evaluation example 4: SEM, HR-TEM and SEM-EDS analysis The composite negative electrode active material (silicon composite structure coated with Al2O3@Gr composite) manufactured in Example 1 and the composite negative electrode active material (SiO coated with Al2O3@Gr composite) manufactured in Example 8 x (0 < x < 2)) were subjected to scanning electron microscopy, high-resolution transmission electron microscopy, and SEM-EDS (Energy-dispersive X-ray spectroscopy) analysis. Philips' FEI Titan 80-300 was used for SEM-EDS analysis.
[0216] The composite manufactured in Production Example 1 was shown to have a structure in which Al2O3 particles and Al2O z (0 < z < 3) particles are embedded in graphene. It was confirmed that a graphene layer is disposed on the outer contour of one or more particles selected from Al2O3 particles and Al2O z (0 < z < 3). Al2O3 particles and Al2O zOne or more particles selected from among (0 < z < 3) were uniformly dispersed within the graphene matrix. Al2O3 particles and Al2O z Among the (0 < z < 3) particles, one or more particle sizes are approximately 20 nm. The particle size of the composite produced in Production Example 1 is approximately 50 nm to 200 nm.
[0217] It was confirmed that a shell formed by a composite containing graphene is disposed on the silicon composite structure core or on the SiO x core (0 < x < 2).
[0218] SEM-EDS mapping analysis was performed on the composite positive electrode active materials produced in Example 1 and Example 8.
[0219] Figure 4A is an SEM image of the composite negative electrode active material of Example 1. Figure 3B is an image obtained by performing SEM-EDS mapping on the composite negative electrode active material of Example 1.
[0220] As shown in Figure 4B, aluminum (Al) distributed on the surface of the composite negative electrode active material of Example 1 was confirmed.
[0221] Figure 4C is an SEM image of the composite negative electrode active material of Example 8. Figure 3D is an image obtained by performing SEM-EDS mapping on the composite negative electrode active material of Example 8.
[0222] As shown in Figure 4D, aluminum (Al) distributed on the surface of the composite negative electrode active material of Example 8 was confirmed.
[0223] It was confirmed that the composite produced in Production Example 1 uniformly coats the silicon composite structure core or the SiO x core (0 < x < 2) to form a shell in the composite negative electrode active materials produced in Example 1 and Example 8.
[0224] Evaluation example 5: Normal temperature (25℃) charge / discharge characteristic evaluation The lithium batteries prepared in Examples 9 to 16 and Comparative Examples 6 to 10 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.5 V (vs. Li), and then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.75 V (vs. Li) during discharge (formation cycle).
[0225] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.5 V (vs. Li), and then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. It was then discharged at a constant current of 0.2 C rate until the voltage reached 2.75 V (vs. Li) during discharge (1 st 50 such cycles. th The cycle was repeated (50 times) under the same conditions.
[0226] In all charge / discharge cycles, a rest time of 10 minutes was allowed after one charge / discharge cycle. Some results of the room temperature charge / discharge experiments are shown in Table 3 below. The initial efficiency is defined by the following Equation 1, and the capacity retention is defined by the following Equation 2.
[0227] <Number 1> Initial efficiency [%] = [discharge capacity in formation cycle / charge capacity in formation cycle] 100 <Number 2> Capacity retention rate [%]=[50 th Discharge capacity in cycles / 1 st Discharge capacity in cycles x 100
[0228] [Table 3]
[0229] As shown in Table 3, the lithium batteries of Examples 9 to 16 had improved life characteristics compared to the lithium batteries of Comparative Examples 1 to 5.
[0230] The improved life characteristics were believed to be due to the composite coating suppressing the formation of a solid electrolyte membrane (SEI) on the surface and / or inside the negative electrode active material, thereby reducing the internal resistance of the lithium battery.
[0231] The lithium batteries of Examples 9 to 12 had improved life characteristics due to the use of the composite-coated composite negative electrode active material.
[0232] The lithium battery of Example 13 further improved its life characteristics by using a composite negative electrode active material that additionally contained carbon nanotubes in addition to the composite.
[0233] The lithium battery of Example 14 has relatively poor life characteristics compared to the lithium batteries of Examples 9 to 13 due to the increase in thickness of the coating layer caused by using alumina having a particle size of 200 nm.
[0234] The lithium battery of Comparative Example 7 used a composite negative electrode active material in which a simple mixture of alumina and graphene was coated on a core, and a uniform coating was not obtained on the core due to the aggregation of graphene.
[0235] In the lithium battery of Comparative Example 8, a simple mixture of the composite and the silicon composite structure was used as the negative electrode active material, and therefore it was impossible to form a coating layer on the silicon composite structure.
[0236] Although not shown in the table, the lithium battery of Example 17 had improved life characteristics compared to the lithium battery of Comparative Example 11.
[0237] Evaluation example 6: Room temperature high-efficiency charging characteristics evaluation The lithium batteries prepared in Examples 9 to 18 and Comparative Examples 6 to 10 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.5 V (vs. Li), and then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.2 C rate until the voltage reached 2.75 V (vs. Li) during discharge (formation cycle).
[0238] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.5 V (vs. Li), and then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. It was then discharged at a constant current of 0.2 C rate until the voltage reached 2.75 V (vs. Li) during discharge (1 st cycle).
[0239] 1 st The cycled lithium battery was charged at 25°C at a constant current of 0.5C rate until the voltage reached 4.5V (vs. Li), and then cut off at a current of 0.02C rate while maintaining 4.5V in constant voltage mode. It was then discharged at a constant current of 0.2C rate until the voltage reached 2.8V (vs. Li) (2 nd cycle).
[0240] 2 nd The cycled lithium battery was charged at 25°C at a constant current of 1.0 C rate until the voltage reached 4.5 V (vs. Li), and then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode. It was then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) during discharge (3 rd cycle).
[0241] 3 rdThe cycled lithium battery was charged at 25°C at a constant current of 2.0 C rate until the voltage reached 4.5 V (vs. Li), then cut-off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (4th cycle).
[0242] 4 th The cycled lithium battery was charged at 25°C at a constant current of 3.0 C rate until the voltage reached 4.5 V (vs. Li), then cut off at a current of 0.02 C rate while maintaining 4.5 V in constant voltage mode, and then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (5th cycle).
[0243] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle. Some of the room temperature high-rate charge characteristic test results are shown in Table 4 below. The high-rate characteristic is defined by the following Equation 3.
[0244] <Number 3> High rate characteristics [%] = [3.0C rate charging capacity (5 th Cycle charge capacity) / 0.1C rate charge capacity (chemical cycle charge capacity)] x 100
[0245] [Table 4]
[0246] As shown in Table 4, the lithium batteries of Example 9 and Example 16, which were coated with the composite of Preparation Example 1, had improved high rate characteristics compared to the lithium batteries of Comparative Example 1 and Comparative Example 10, which did not have a coating layer.
[0247] Evaluation example 7: Evaluation of negative electrode expansion rate at high temperature (55°C) The lithium batteries prepared in Examples 9 to 16 and Comparative Examples 6 to 10 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.4 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.4 V in constant voltage mode. Then, they were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) during discharge (formation cycle).
[0248] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.7 C rate at 25° C. until the voltage reached 4.5 V (vs. Li), at which point it was cut off.
[0249] The charged lithium battery was then subjected to floating charging at a constant voltage of 4.5V (vs. Li) at 55°C for 7, 10, 14, 17 and 20 days, after which the negative electrode expansion rate was measured and the results are shown in Table 5. The negative electrode expansion rate is expressed by Equation 4 below.
[0250] <Number 4> Thickness expansion rate (%) = [(negative electrode thickness after 20 days of storage - negative electrode thickness before assembly) / negative electrode thickness before assembly] × 100 "Negative electrode thickness before assembly" is the negative electrode thickness measured before assembling the lithium battery. "Negative electrode thickness after 20 days of storage" is the thickness of the negative electrode measured by disassembling the lithium battery after it was taken out from the oven after 20 days of storage.
[0251] [Table 5]
[0252] As shown in Table 5, the lithium battery of Example 9 had a significantly reduced negative electrode expansion rate compared to the lithium battery of Comparative Example 6.
[0253] The lithium battery of Example 16 had a significantly reduced negative electrode expansion rate as compared with the lithium battery of Comparative Example 10.
[0254] This decrease in expansion rate was believed to be due to the fact that the composite coating significantly reduced side reactions between the negative electrode active material and the electrolyte, thereby suppressing the formation of a thick solid electrolyte membrane (SEI). [Explanation of symbols]
[0255] 1 Lithium battery 2 negative electrode 3 Positive electrode 4. Separator 5 Battery case 6 Cap Assembly 7 Battery structure 8 Electrode tab 10 cores 20 Shell 21 First metal oxide 22 Carbon-based materials No. 1 23 Secondary carbon-based materials 100 Composite negative electrode active material
Claims
1. A core, a shell disposed along a surface of the core; the core comprises a silicon-containing structure, a silicon-containing compound, or a combination thereof; The shell has the formula M a O b (wherein 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer); and a first carbon-based material, The first metal oxide is disposed in a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of Elements; The silicon-containing structure comprises a silicon composite structure, and the silicon-containing compound comprises SiOx (0<x<2); The silicon composite structure is a porous silicon secondary particle; and a first carbon flake disposed on the porous silicon secondary particle; the porous silicon secondary particles are aggregates of a plurality of silicon composite primary particles; The silicon composite primary particles include silicon, a silicon suboxide (SiOx, 0<x<2) disposed on the silicon, and a second carbon flake disposed on the silicon suboxide.
2. 2. The composite anode active material of claim 1, wherein the silicon composite structure has a porosity of 60% or less or is non-porous, and the silicon composite structure has a non-spherical morphology.
3. the first carbon flake and the second carbon flake are the same flake; 2. The composite anode active material of claim 1, wherein the first carbon flakes and the second carbon flakes each independently comprise graphene, graphite, carbon fiber, graphitic carbon, graphene oxide, or a mixture thereof.
4. the silicon-containing structure further comprises a carbon-based coating layer disposed on the silicon composite structure, the carbon-based coating layer comprising a first amorphous carbon; The silicon-containing structure further comprises a second amorphous carbon disposed within a silicon composite structure, the silicon composite structure comprises porous silicon secondary particles, and the second amorphous carbon is disposed within pores of the porous silicon secondary particles; 2. The composite anode active material of claim 1, wherein the first amorphous carbon and the second amorphous carbon independently comprise pitch-based carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a mixture thereof.
5. 2. The composite anode active material of claim 1, wherein the first metal oxide comprises a first metal, the first metal being one or more selected from the group consisting of Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se.
6. The first metal oxide is Al 2 O z (0<z<3), NbO x (0<x<2.5), MgO x (0<x<1), Sc 2 O z (0<z<3), TiO y (0<y<2), ZrO y (0<y<2), V 2 O z (0<z<3), WO y (0<y<2), MnO y (0<y<2), Fe 2 O z (0<z<3), Co 3 O w (0<w<4), PdO x (0<x<1),CuO x (0<x<1), AgO x (0<x<1), ZnO x (0<x<1), Sb 2 O z (0<z<3), and SeO y 2. The composite negative electrode active material of claim 1 , wherein y is one or more selected from the group consisting of (0<y<2).
7. The shell has the formula M a O c (0<a≦3, 0<c≦4, and if a is 1, 2, or 3, then c is an integer), the second metal oxide comprises the same metal as the first metal oxide; 2 . The composite anode active material of claim 1 , wherein a ratio c / a between a and c of the second metal oxide is greater than a ratio b / a between a and b of the first metal oxide.
8. The second metal oxide is Al 2 O 3 , NbO, NbO 2 , Nb 2 O 5 , MgO, Sc 2 O 3 , TiO 2 , ZrO 2 , V 2 O 3 , W.O. 2 , MnO 2 , Fe 2 O 3 , Co 3 O 4 , PdO, CuO, AgO, ZnO, Sb 2 O 3 , and SeO 2 is selected from 8. The composite anode active material of claim 7, wherein the first metal oxide is a reduction product of the second metal oxide.
9. 8. The composite negative electrode active material of claim 7, wherein a particle size of at least one of the first metal oxide and the second metal oxide is in the range of 1 nm to 100 nm.
10. The shell includes a first carbon-based material disposed in a direction protruding from a surface of one or more of the first metal oxide and the second metal oxide, 2. The composite anode active material of claim 1, wherein the shell has a thickness of 1 nm to 5 μm.
11. the shell includes at least one selected from the group consisting of a composite including the first metal oxide and a first carbon-based material and a milling result of the composite, 2. The composite negative electrode active material of claim 1, wherein a content of at least one of the composite and the milled product of the composite is 0.1 wt % to 5 wt % of a total weight of the composite negative electrode active material.
12. the first carbon-based material has a branched structure and the first metal oxide is distributed within the branched structure; 12. The composite anode active material of claim 11, wherein the branched structure comprises a plurality of particles of the first carbon-based material in contact with one another.
13. the first carbon-based material has at least one structure selected from a spherical structure, a helical structure in which the spherical structures are connected, and a cluster structure in which the spherical structures are aggregated; the first metal oxide is distributed within the spherical structures, the size of the spherical structures is 50 nm to 300 nm, and the size of the helical structures is 500 nm to 100 μm; The composite is a wrinkled polyhedral ball structure or a planar structure, and one or more selected from a first metal oxide and a second metal oxide are distributed inside or on the surface of the structure; 12. The composite anode active material of claim 11, wherein the first carbon-based material extends a distance of 10 nm or less from the first metal oxide and comprises at least 1 to 20 layers of the first carbon-based material, the total thickness of the first carbon-based material being 0.6 nm to 12 nm.
14. The shell further comprises a second carbon-based material, the second carbon-based material comprises fibrous carbon, and the second carbon-based material comprises at least one selected from the group consisting of carbon nanofibers and carbon nanotubes; The length of the second carbon-based material is 1000 μm or less, and the diameter of the second carbon-based material is 50 nm or less; 2. The composite negative electrode active material of claim 1, wherein the second carbon-based material is present in an amount of 0.001 wt % to 1 wt % of the total weight of the composite negative electrode active material.
15. The specific surface area of the composite negative electrode active material is 1 m 2 / g to 100m 2 / g, 2. The composite anode active material of claim 1, wherein the composite anode active material has an average particle size (D50) of 1 μm to 30 μm, a D10 of 0.1 μm to 10 μm, and a D90 of 10 μm to 50 μm.
16. 16. A negative electrode comprising the composite negative electrode active material of claim 1.
17. a dry composite negative electrode active material, a dry conductive material, and a dry binder; The dry composite negative electrode active material is A core, a shell disposed along a surface of the core; the core comprises a silicon-containing structure, a silicon-containing compound, or a combination thereof; The shell has the formula M a O b (wherein 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer); and a first carbon-based material, The first metal oxide is disposed in a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of Elements; The silicon-containing structure comprises a silicon composite structure, and the silicon-containing compound comprises SiOx (0<x<2); The silicon composite structure is a porous silicon secondary particle; and a first carbon flake disposed on the porous silicon secondary particle; the porous silicon secondary particles are aggregates of a plurality of silicon composite primary particles; a negative electrode, wherein the silicon composite primary particles include silicon, a silicon suboxide (SiOx, 0<x<2) disposed on the silicon, and a second carbon flake disposed on the silicon suboxide.
18. A positive electrode, a negative electrode according to claim 16, and a lithium battery comprising an electrolyte disposed between the positive electrode and the negative electrode.
Citation Information
Patent Citations
Anode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery using the same
JP2008153117A
Negative electrode for energy storage device and energy storage device having the same
JP2011238585A
Composite active material for lithium secondary battery and method for producing the same
JP2014187007A
Negative electrode active material for secondary batteries, and method for manufacturing the same
JP2016021393A
Method for producing negative electrode active material for lithium ion secondary batteries
WO2017175812A1