Composite positive electrode active material, positive electrode and lithium battery using the same, and manufacturing method thereof
A composite positive electrode active material with a lithium transition metal oxide core and a carbon-based shell improves lithium battery performance by suppressing side reactions and enhancing cycle and rate characteristics.
Patent Information
- Application Number
- JP2022189323
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-26
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-11-28
AI Technical Summary
Conventional cathode active materials in lithium batteries suffer from reduced lifetime characteristics due to side reactions and low thermal stability, necessitating a solution to prevent battery performance deterioration.
A composite positive electrode active material is developed, comprising a lithium transition metal oxide core coated with a shell made of a first metal oxide, a first carbon-based material, and a second fibrous carbon-based material, which forms a conductive network to suppress side reactions and improve electrode reversibility.
The composite active material enhances high-temperature cycle characteristics and reduces internal resistance, while maintaining high rate characteristics and energy density by preventing side reactions and cation mixing.
Smart Images

Figure 0007577721000004 
Figure 0007577721000005 
Figure 0007577721000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite positive electrode active material, a positive electrode and a lithium battery using the same, and a method for producing the composite positive electrode active material. [Background technology]
[0002] In order to meet the trend of miniaturization and high performance of various devices, it is becoming increasingly important to make lithium batteries not only smaller and lighter, but also to have higher energy density, i.e., high-capacity lithium batteries.
[0003] In order to realize a lithium battery that meets the above-mentioned applications, positive electrode active materials having high capacity are being investigated.
[0004] Conventional positive electrode active materials suffer from reduced life characteristics due to side reactions and also have low thermal stability. Therefore, a method is required that can prevent deterioration of battery performance while containing a positive electrode active material. Summary of the Invention [Problem to be solved by the invention]
[0005] One aspect of the present invention is to provide a novel composite positive electrode active material that can suppress side reactions of the composite positive electrode active material and improve the reversibility of the electrode reaction, thereby preventing deterioration of lithium battery performance.
[0006] Another aspect is to provide a cathode comprising the composite cathode active material. Yet another aspect is to provide a lithium battery employing the positive electrode. Yet another aspect is to provide a method for making a composite cathode active material. [Means for solving the problem]
[0007] According to one aspect, a lithium transition metal oxide (LiO2) is provided comprising a core comprising a lithium transition metal oxide; a shell disposed along a surface of the core; and the shell having a chemical formula M a Ob (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer) one or more first metal oxides; a first carbon-based material; and a second carbon-based material; wherein the first metal oxide is disposed within a first carbon-based material matrix, M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements, and the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more, a composite cathode active material is provided.
[0008] On another aspect, a cathode including the composite cathode active material is provided. On yet another aspect, a lithium battery including the cathode is provided.
[0009] On yet another aspect, providing a lithium transition metal oxide; providing a composite; providing a second carbon-based material; and mechanically milling the lithium transition metal oxide, the composite, and the second carbon-based material; wherein the composite has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer) one or more first metal oxides; and a first carbon-based material; wherein the first metal oxide is disposed within a first carbon-based material matrix, M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements, and the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more, a method for manufacturing a composite cathode active material is provided.
Advantages of the Invention
[0010] According to one aspect, the composite cathode active material includes a shell containing a first metal oxide, a first carbon-based material, and a second carbon-based material, thereby improving the high-temperature cycle characteristics of the lithium battery, suppressing an increase in internal resistance, and improving high-rate characteristics.
Brief Description of the Drawings
[0011] [Figure 1] It is a cross-sectional schematic view of composite cathode active material particles according to an embodiment. [Diagram 2] 1 is a scanning electron microscope image of the surface of a particle of the composite positive electrode active material used in Example 1. [Diagram 3] 1 shows XPS images of bare NCA91 prepared in Comparative Example 1, the composite prepared in Preparation Example 1, and the composite positive electrode active material prepared in Example 1. [Figure 4] 2 shows Raman spectrum images of the composite prepared in Preparation Example 1 and the composite positive electrode active material prepared in Example 1. [Diagram 5] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 6] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 7] 1 is a schematic diagram of a lithium battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present inventive concept described below can be modified in various ways and can have various embodiments, and specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, this is not intended to limit the present inventive concept to a specific embodiment, and it should be understood that the present inventive concept includes any modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.
[0013] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In the following, terms such as "include" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the situation.
[0014] In the drawings, thicknesses are exaggerated or reduced to clearly depict multiple layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part such as a layer, film, region, plate, etc. is described as being "on" or "above" another part, this does not only include the case where it is directly on top of the other part, but also the case where there is another part in between. Throughout the specification, terms such as first, second, etc. may be used to describe various components, but the components should not be limited by the terms. Terms are used only to distinguish one component from another.
[0015] In this specification, the "particle size" of a particle refers to the average diameter when the particle is spherical, and refers to the average major axis length when the particle is non-spherical. The particle size of a particle can be measured using a particle size analyzer (PSA). The "particle size" of a particle is the average particle size. The average particle size is, for example, the median diameter (D50). The median diameter (D50) is a particle size that corresponds to a 50% cumulative value calculated from the particle side having the smallest particle size in a cumulative distribution curve of particle sizes in which particles are accumulated in order of particle size from the smallest particle to the largest particle. The cumulative value is, for example, also a cumulative volume. The median diameter (D50) can be measured, for example, by a laser diffraction method.
[0016] Hereinafter, a composite positive electrode active material according to an example embodiment, a positive electrode and a lithium battery including the same, and a method for manufacturing the same will be described in more detail.
[0017] The composite active cathode material includes a core comprising a lithium transition metal oxide; a shell disposed along a surface of the core; and the shell has the formula M a O bOne or more first metal oxides represented by (0 < a ≤ 3, 0 < b < 4; if a is 1, 2, or 3, b is not an integer); a first carbon-based material; and a second carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements, and the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more.
[0018] Hereinafter, the theoretical basis for the excellent effects provided by the composite cathode active material according to an embodiment will be described. This is for the purpose of assisting the understanding related to the creative idea and is not intended to limit the creative idea in any way.
[0019] Referring to FIG. 1, the composite positive electrode active material 100 includes a core 10 and a shell 20 disposed continuously or discontinuously along the surface of the core 10. The shell 20 may cover all or a part of the core 10. The core 10 includes a lithium transition metal oxide, and the shell 20 includes a first metal oxide 21, a first carbon-based material 22, and a second carbon-based material 23. The second carbon-based material 23 includes fibrous carbon having an aspect ratio of 10 or more. When manufacturing the composite positive electrode active material 100, the shell 20 may be disposed on the lithium transition metal oxide core 10 using a composite including a plurality of first metal oxides 21 disposed in a matrix of the first carbon-based material 22. Thus, the shell 20 may be disposed uniformly on the core 10 while preventing the aggregation of the first carbon-based material 22. The shell 20 disposed on the core 10 may effectively block contact between the core 10 and the electrolyte. The shell 20 effectively blocks contact between the core 10 and the electrolyte, thereby preventing side reactions caused by contact between the core 10 and the electrolyte. In addition, the shell 20 is disposed on the core 10, thereby suppressing cation mixing caused by contact between the core 10 and the electrolyte. The suppression of cation mixing caused by contact between the core 10 and the electrolyte can suppress the generation of a resistance layer inside and / or on the surface of the composite positive electrode active material 100. In addition, the shell 20 is disposed on the core 10, thereby suppressing the elution of transition metal ions from the lithium transition metal oxide core 10. The first carbon-based material may be, for example, a crystalline carbon-based material. The first carbon-based material may be, for example, a carbon-based nanostructure. The first carbon-based material may be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material may be, for example, graphene. In this case, the shell containing graphene and / or its matrix has flexibility and can easily accommodate the volume change of the composite positive electrode active material during charging and discharging, thereby suppressing the occurrence of cracks inside the composite positive electrode active material. Graphene has high electrical conductivity and can reduce the interfacial resistance between the composite positive electrode active material and the electrolyte. Therefore, despite the introduction of a shell containing graphene, the internal resistance of the lithium battery can be maintained or reduced.On the other hand, conventional carbon-based materials easily agglomerate, making it difficult to achieve a uniform coating on the lithium transition metal oxide core.
[0020] The shell includes a second carbon-based material, which is fibrous carbon having an aspect ratio of 10 or more. Therefore, the conductive path of the composite positive electrode active material is further lengthened. The second carbon-based material may form a three-dimensional conductive network between the composite positive electrode active materials, thereby reducing the internal resistance of the positive electrode including the composite positive electrode active material. Since the fibrous carbon is fixed on the composite positive electrode active material, a uniform and stable three-dimensional conductive network may be formed between the composite positive electrode active materials. Therefore, since the composite positive electrode active material includes the second carbon-based material, the high rate characteristics of the lithium battery including the composite positive electrode active material may be improved. Meanwhile, a simple mixture of the lithium transition metal oxide core and the fibrous carbon, which is the second carbon-based material, is difficult to form a uniform three-dimensional conductive network between the lithium transition metal oxide particles due to the aggregation of the fibrous carbon. As shown in FIG. 1 and FIG. 2, the second carbon-based material 23 may be disposed on the surface of the composite positive electrode active material 100. Also, as shown in FIG. 1, the second carbon-based material 23 may protrude from the surface of the composite positive electrode active material 100. Therefore, the second carbon-based material 23 can effectively provide a conductive network between a plurality of composite positive electrode active materials 100. The second carbon-based material 23 may be easily coated on the core 10 by being disposed in the matrix of the first carbon-based material 22. The matrix of the first carbon-based material 22 acts as a binder that binds the core and the second carbon-based material 23. Therefore, without the matrix of the first carbon-based material 22, the second carbon-based material 23 may be difficult to attach onto the core 10 or the second carbon-based material 23 may be easily detached from the core 10 during the process of preparing the slurry for the positive electrode. When a binder is added to bind the lithium transition metal oxide core 20 and the second carbon-based material 23, the core 10 is covered with the insulating binder, and the internal resistance of the composite positive electrode active material 100 increases. When the core coated with the second carbon-based material and the binder is subjected to a high-temperature heat treatment to carbonize the binder, the core 10 and the second carbon-based material 23 may be deteriorated during the heat treatment.
[0021] The aspect ratio of the second carbon-based material is 10 or more, or 20 or more. The aspect ratio of the second carbon-based material is, for example, 10 to 100,000, 10 to 80,000, 10 to 50,000, 10 to 10,000, 10 to 5000, 10 to 1000, 10 to 500, 10 to 100, or 10 to 50. The aspect ratio of the second carbon-based material is, for example, the ratio of the length of the major axis passing through the center of the second carbon-based material, that is, the length of the minor axis passing through the center of the second carbon-based material and perpendicular to the major axis, that is, the diameter of the second carbon-based material.
[0022] The diameter of the second carbon-based material is, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbon-based material is, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. If the diameter of the second carbon-based material is too large, the absolute number per volume decreases, and the effect of reducing internal resistance is negligible. If the diameter of the second carbon-based material is too small, it is difficult to uniformly disperse it.
[0023] The length of the second carbon-based material is, for example, 1000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbon-based material is, for example, 100 nm to 1000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material is, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or 500 nm to 2 μm. As the length of the second carbon-based material increases, the internal resistance of the electrode decreases. If the length of the second carbon-based material is too short, it is difficult to provide an effective conductive path.
[0024] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.
[0025] The carbon nanotubes include, for example, a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof.
[0026] The primary structure of a carbon nanotube is one carbon nanotube unit. A carbon nanotube unit has a graphite sheet with a cylindrical shape of nano-sized diameter and an sp2 bond structure. Depending on the angle and structure of the curved graphite sheet, it exhibits conductive or semiconductive properties. Carbon nanotube units can be classified into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT), depending on the number of bonds that make up the wall. The thinner the wall thickness of a carbon nanotube unit, the lower the resistance.
[0027] The carbon nanotube primary structure includes, for example, single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure is, for example, 1 nm or more, or 2 nm or more. The diameter of the carbon nanotube primary structure is, for example, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube primary structure is, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 1 nm to 10 nm. The length of the carbon nanotube primary structure is, for example, 100 nm or more, or 200 nm or more. The length of the carbon nanotube primary structure is, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the carbon nanotube primary structure may be, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure may be measured from a scanning electron microscope (SEM) or a transmission electron microscope (TEM) image. Alternatively, the diameter and / or length of the carbon nanotube primary structure may be measured by a laser diffraction method.
[0028] The carbon nanotube secondary structure is a structure formed by assembling the carbon nanotube primary structures to form a bundle or a bundle shape entirely or partially. The carbon nanotube secondary structure includes, for example, bundle-type carbon nanotubes, rope-type carbon nanotubes, or a combination thereof. The diameter of the carbon nanotube secondary structure is, for example, 2 nm or more or 3 nm or more. The diameter of the carbon nanotube secondary structure is, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure is, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure is, for example, 500 nm or more, 700 nm or more, 1 μm or more, or 10 μm or more. The length of the carbon nanotube secondary structure may be, for example, 1000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure may be, for example, 500 nm to 1000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure may be measured from a scanning electron microscope (SEM) image or an optical microscope. Alternatively, the diameter and / or length of the carbon nanotube secondary structure may be measured by a laser diffraction method.
[0029] The carbon nanotube secondary structure can be converted into a carbon nanotube primary structure by, for example, dispersing it in a solvent, and then used to manufacture a composite positive electrode active material.
[0030] The content of the second carbon-based material is, for example, 0.1wt% to 50wt%, 1wt% to 40wt%, or 5wt% to 30wt% based on the total weight of the first carbon-based material and the second carbon-based material. When the composite positive electrode active material includes the first carbon-based material and the second carbon-based material in such a range, a conduction path is more effectively secured in the composite positive electrode active material, and the internal resistance of the composite positive electrode active material may be further reduced. As a result, the cycle characteristics of a lithium battery including the composite positive electrode active material may be further improved. The content of the second carbon-based material is, for example, 0.001wt% to 5wt%, 0.01wt% to 3wt%, 0.01wt% to 1wt%, 0.01wt% to 0.5wt%, or 0.01wt% to 0.1wt% based on the total weight of the composite positive electrode active material. When the composite positive electrode active material includes the second carbon-based material in such a range, a conduction path is secured within the composite positive electrode active material, and the internal resistance of the composite positive electrode active material may be further reduced, and as a result, the cycle characteristics of a lithium battery including the composite positive electrode active material may be further improved.
[0031] The shell also includes a first metal oxide and a first carbonaceous material. The first carbonaceous material is derived from, for example, a graphene matrix, and therefore has a relatively low density and a high porosity compared to conventional carbonaceous materials derived from graphite-based materials. The d002 interplanar distance of the first carbonaceous material is, for example, 3.38 Å or more, 3.40 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or 4.00 Å or more. The d002 interplanar distance of the first carbonaceous material included in the shell is, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. On the other hand, the d002 interplanar distance of conventional carbon-based materials derived from graphite-based materials is, for example, 3.38 Å or less, or 3.35 to 3.38 Å. The first metal oxide has voltage resistance, so that it is possible to prevent the deterioration of the lithium transition metal oxide contained in the core during charging and discharging at high voltage. The shell contains, for example, one type of first metal oxide or two or more different first metal oxides. As a result, the high-temperature cycle characteristics of a lithium battery containing the above-mentioned composite positive electrode active material are improved. The content of the shell is, for example, 0.1 wt% to 5 wt%, 0.1 wt% to 4 wt%, 0.1 wt% to 3 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2 wt%, or 0.1 wt% to 1.5 wt% of the total weight of the composite positive electrode active material. The content of the first metal oxide is, for example, 0.06 wt% to 3 wt%, 0.06 wt% to 2.4 wt%, 0.06 wt% to 1.8 wt%, 0.06 wt% to 1.5 wt%, 0.06 wt% to 1.2 wt%, or 0.06 wt% to 0.9 wt% of the total weight of the composite positive electrode active material. When the composite positive electrode active material contains the shell and the first metal oxide in such a content range, respectively, the cycle characteristics of the lithium battery are further improved.
[0032] The first metal oxide includes a first metal, and the first metal may be, for example, one or more selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, AlO z (0 <z<3),NbOx (0 < x < 2.5), MgO x (0 < x < 1), Sc2O z (0 < z < 3), TiO y (0 < y < 2), ZrO y (0 < y < 2), V2O z (0 < z < 3), WO y (0 < y < 2), MnO y (0 < y < 2), Fe2O z (0 < z < 3), Co3O w (0 < w < 4), PdO x (0 < x < 1), CuO x (0 < x < 1), AgO x (0 < x < 1), ZnO x (0 < x < 1), Sb2O z (0 < z < 3), and SeO y (0 < y < 2) is also one or more selected therefrom. By arranging such a first metal oxide in the first carbon-based material matrix, the uniformity of the shell disposed on the core is improved, and the voltage resistance of the composite positive electrode active material is further improved. For example, the shell is Al2O as the first metal oxide x (0 < x < 3) is included.
[0033] The shell has the chemical formula M a O cOne or more second metal oxides represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) may be further included. The M is one or more selected metals from Groups 2 to 13, Group 15, and Group 16 of the periodic table of the elements. For example, the second metal oxide contains the same metal as the first metal oxide, and c / a, which is the ratio of c to a of the second metal oxide, has a value further larger than b / a, which is the ratio of b to a of the first metal oxide. For example, c / a > b / a. The second metal oxide is selected from, for example, Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide is, for example, a reduction product of the second metal oxide. By reducing part or all of the second metal oxide, the first metal oxide is obtained. Therefore, the first metal oxide has a lower oxygen content and a lower oxidation number of the metal compared to the second metal oxide. The shell is, for example, the first metal oxide Al2O x contains (0 < x < 3) and Al2O3 which is the second metal oxide.
[0034] The shell contains, for example, a first carbon-based material, and the core contains, for example, a lithium transition metal oxide. And the transition metal of the first carbon-based material and the lithium transition metal oxide can be chemically bonded, for example, through a chemical bond. The carbon atom (C) of the first carbon-based material and the transition metal (Me) of the lithium transition metal oxide are chemically bonded, for example, through an oxygen atom via a C-O-Me bond (for example, a C-O-Ni bond or a C-O-Co bond). By chemically bonding the first carbon-based material arranged in the shell and the lithium transition metal oxide arranged in the core through a chemical bond, the core and the shell are complexed. Therefore, the composite positive electrode active material is distinguished from a mere physical mixture of the first carbon-based material and the lithium transition metal oxide. Also, the first metal oxide and the first carbon-based material can be chemically bonded through a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond.
[0035] The shell may include, for example, one or more selected from the first metal oxide and the second metal oxide, and the particle size of the selected one or more of the first metal oxide and the second metal oxide may be, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may be more uniformly distributed in the first carbon-based material matrix by having such a nano-range particle size. If the particle size of one or more of the first metal oxide and the second metal oxide is excessively increased, the thickness of the shell may increase, and the internal resistance of the composite negative electrode active material may increase. If the particle size of one or more of the first metal oxide and the second metal oxide is excessively decreased, uniform dispersion may be difficult.
[0036] The shell includes a first metal oxide and / or a second metal oxide and includes a first carbon-based material. The first carbon-based material can be arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface. The first carbon-based material can be arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface by directly growing from the first metal oxide and / or the second metal oxide surface. The first carbon-based material arranged in a direction protruding from the first metal oxide and / or the second metal oxide surface is, for example, a carbon-based two-dimensional nanostructure, a carbon-based flake, or graphene.
[0037] The thickness of the shell is, for example, 1 nm to 5 μm, 1 nm to 1 μm, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 90 nm, 1 nm to 80 nm, 1 nm to 70 nm, 1 nm to 60 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, or 1 nm to 20 nm. When the shell has a thickness in such a range, the electronic conductivity of the positive electrode containing the composite positive electrode active material can be further improved.
[0038] The composite positive electrode active material may further include, for example, a third metal doped on the core and / or a third metal oxide coated on the core. Then, a shell may be disposed on the third metal doped on the core and / or the third metal oxide coated on the core. For example, the surface of the lithium transition metal oxide core may be doped with a third metal, or the surface of the lithium transition metal oxide may be coated with a third metal oxide, and then a shell may be disposed on the third metal and / or the third metal oxide. For example, the composite positive electrode active material may include a core; an intermediate layer disposed on the core; and a shell disposed on the intermediate layer, the intermediate layer including a third metal or a third metal oxide. The third metal may be one or more metals selected from Al, Zr, W, and Co, and the third metal oxide may be Al2O3, Li2O-ZrO2, WO2, CoO, Co2O3, Co3O4, or a combination thereof.
[0039] The shell disposed along the surface of the core may include one or more selected from a composite including a first metal oxide and a first carbon-based material, such as graphene, a second carbon-based material, and / or a milling result of the composite and the second carbon-based material. The first metal oxide is disposed in a matrix of a carbon-based material, such as a graphene matrix. The shell may be prepared, for example, from a composite including a first metal oxide and a first carbon-based material, such as graphene. The composite may further include a second metal oxide in addition to the first metal oxide. The composite may include, for example, two or more types of first metal oxides. The composite may include, for example, two or more types of first metal oxides and two or more types of second metal oxides.
[0040] The content of one or more of the composite and milling products thereof may be, for example, 5 wt% or less, 3 wt% or less, 2 wt% or less, 2.5 wt% or less, or 1.5 wt% or less of the total weight of the composite positive electrode active material. The content of one or more of the composite and milling products thereof may be 0.01 wt% to 5 wt%, 0.01 wt% to 4 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 2.5 wt%, 0.01 wt% to 2 wt%, or 0.01 wt% to 1.5 wt% of the total weight of the composite positive electrode active material. When the composite positive electrode active material includes one or more of the composite and milling products thereof within such ranges, the cycle characteristics of a lithium battery including the composite positive electrode active material are further improved.
[0041] The composite includes one or more selected from the first metal oxide and the second metal oxide. The particle size of the selected one or more of the first metal oxide and the second metal oxide may be 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or even 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may have such a nano-range particle size, so that they can be more uniformly distributed in the first carbon-based material matrix of the composite. Therefore, such a composite may be uniformly coated on the core without aggregation to form a shell. In addition, the first metal oxide and / or the second metal oxide may have such a particle size range, so that they may be more uniformly arranged on the core. Therefore, the first metal oxide and / or the second metal oxide may be uniformly arranged on the core, so that the voltage resistance characteristics may be more effectively exhibited. The particle size of the first metal oxide and / or the second metal oxide may be measured using, for example, a measuring device of a laser diffraction method or a dynamic light scattering method. The particle size is measured, for example, using a laser scattering particle size distribution analyzer (e.g., HORIBA LA-920), and is the median diameter (D50) value when 50% is accumulated from the elementary particle side in volume conversion. The uniformity deviation of one or more selected from the first metal oxide and / or the second metal oxide is 3% or less, 2% or less, or 1% or less. The uniformity can also be determined, for example, by XPS. Therefore, the selected one or more of the first metal oxide and the second metal oxide can have a deviation of 3% or less, 2% or less, or 1% or less and be uniformly distributed in the composite.
[0042] The composite includes a first carbon-based material. The first carbon-based material may have, for example, a branched structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the branched structure of the first carbon-based material. The branched structure of the first carbon-based material may include, for example, a plurality of first carbon-based material particles in contact with each other. The first carbon-based material may have a branched structure, and various conductive paths may be provided. The first carbon-based material may be, for example, graphene. The graphene may have, for example, a branched structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the branched structure of graphene. The branched structure of graphene may include, for example, a plurality of graphene particles in contact with each other. The graphene may have a branched structure, and various conductive paths may be provided.
[0043] The first carbon-based material may have, for example, a spherical structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material is 50 nm to 300 nm. There may be a plurality of first carbon-based materials having a spherical structure. Since the first carbon-based material has a spherical structure, the composite may have a robust structure. The first carbon-based material may be, for example, graphene. Graphene may have, for example, a spherical structure, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of graphene is 50 nm to 300 nm. There may be a plurality of graphenes having a spherical structure. Since the graphene has a spherical structure, the composite may have a robust structure.
[0044] The first carbon-based material may have a helical structure in which a plurality of spherical structures are connected, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the helical spherical structures. The size of the helical structure of the first carbon-based material is 500 nm to 100 μm. Since the first carbon-based material has a helical structure, the composite may have a robust structure. The first carbon-based material may also be graphene. For example, graphene may have a helical structure in which a plurality of spherical structures are connected, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed in the helical spherical structures. The size of the helical structure of graphene is 500 nm to 100 μm. Since the graphene has a helical structure, the composite may have a robust structure.
[0045] The first carbon-based material may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the cluster structure of the first carbon-based material is 0.5 mm to 10 cm. Since the first carbon-based material has a cluster structure, the composite may have a robust structure. The first carbon-based material may also be graphene, for example. Graphene may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more selected metal oxides from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the graphene cluster structure is 0.5 mm to 10 cm. Since the graphene has a cluster structure, the composite may have a robust structure.
[0046] The composite may be, for example, a wrinkled polyhedral ball structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. By the composite having such a polyhedral ball structure, the composite may be easily coated on the irregular surface irregularities of the core.
[0047] The composite may be, for example, a faceted-ball structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. Since the composite has such a two-dimensional faceted-ball structure, the composite may be easily coated on the irregular surface irregularities of the core.
[0048] The first carbon-based material extends over the first metal oxide by a distance of 10 nm or less and includes at least 1 to 20 carbon-based material layers. For example, a first carbon-based material having a total thickness of 12 nm or less can be disposed on the first metal oxide by stacking a plurality of first carbon-based material layers. For example, the total thickness of the first carbon-based material is 0.6 nm to 12 nm. The first carbon-based material can also be, for example, graphene. The graphene extends over the first metal oxide by a distance of 10 nm or less and includes at least 1 to 20 graphene layers. For example, a plurality of graphene layers can be stacked to dispose the first metal oxide with a total thickness of 12 nm or less. For example, the total thickness of the graphene is 0.6 nm to 12 nm.
[0049] The composite positive electrode active material includes a core, and the core includes, for example, a lithium transition metal oxide represented by the following formulas 1 to 8:
[0050] [Chemical formula 1] Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 1, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.8 ≤ x < 1, 0 < y ≤ 0.3, 0 < z ≤ 0.3, and x + y + z = 1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof.
[0051] [Chemical Formula 2] LiNi x Co y Mn z O2
[0052] [Chemical Formula 3] LiNi x Co y Al z O2 In the Chemical Formulas 2 and 3, 0.8 ≤ x ≤ 0.95, 0 ≤ y ≤ 0.2, 0 < z ≤ 0.2 and x + y + z = 1.
[0053] [Chemical Formula 4] LiNi x Co y Mn z Al w O2 In the Chemical Formula 4, 0.8 ≤ x ≤ 0.95, 0 ≤ y ≤ 0.2, 0 < z ≤ 0.2, 0 < w ≤ 0.2, and x + y + z + w = 1.
[0054] The lithium transition metal oxides of Chemical Formulas 1 to 4 have a high nickel content of 80 mol% or more, 85 mol% or more, 90 mol% or more, or 90 mol% or more based on the total number of moles of transition metals, and provide excellent initial capacity, normal temperature life characteristics, and high temperature life characteristics. For example, the nickel content in the lithium transition metal oxides of Chemical Formulas 1 to 4 is 80 mol% to 99 mol%, 85 mol% to 99 mol%, or 90 mol% to 97 mol% based on the total number of moles of transition metals.
[0055] [Chemical Formula 5] Li a Co x M y O 2-b A b In the above Chemical Formula 5, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.9 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, and x + y = 1, M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof.
[0056] [Chemical Formula 6] Li a Ni x Mn y M’ z O 2-b A b In the above Chemical Formula 6, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0 < x ≤ 0.3, 0.5 ≤ y < 1, 0 < z ≤ 0.3, and x + y + z = 1, M’ is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A is F, S, Cl, Br or a combination thereof.
[0057] [Chemical Formula 7] Li a M1 x M2 y PO 4-b X b In the above Chemical Formula 7, 0.90 ≤ a ≤ 1.1, 0 ≤ x ≤ 0.9, 0 ≤ y ≤ 0.5, 0.9 < x + y < 1.1, 0 ≤ b ≤ 2, M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr) or a combination thereof; M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y), or a combination thereof; and X is O, F, S, P, or a combination thereof.
[0058] [Chemical formula 8] Li a M3 z PO4 In the above Chemical Formula 8, 0.90≦a≦1.1 and 0.9≦z≦1.1; M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
[0059] According to another embodiment, a positive electrode includes the above-described composite positive electrode active material. By including the above-described composite positive electrode active material in a positive electrode, improved energy density, improved cycle characteristics, and increased conductivity can be provided.
[0060] Since the shell of the composite positive electrode active material includes the second carbon-based material, the composite positive electrode active material can further perform the role of a conductive material. Therefore, the content of the conductive material used in the positive electrode can be reduced. The conductive material is necessary for improving the conductivity of the battery, but if the content of the conductive material increases, the composite density of the positive electrode decreases, and as a result, the energy density of the lithium battery decreases. Meanwhile, the positive electrode of the present invention can reduce the content of the conductive material without increasing the internal resistance by using the above-mentioned composite positive electrode active material. Therefore, the composite density of the positive electrode increases, and as a result, the energy density of the lithium battery can be improved. In particular, in a high-capacity lithium battery, the energy density of the lithium battery can be significantly increased by decreasing the content of the conductive material and increasing the content of the composite positive electrode active material.
[0061] The positive electrode may be prepared, for example, by a wet method. The positive electrode may be prepared, for example, by the following exemplary method, but is not necessarily limited to such a method and may be adjusted according to required conditions.
[0062] First, the composite positive active material, conductive material, binder, and solvent are mixed to prepare a positive active material composition. The prepared positive active material composition is directly coated on an aluminum current collector and dried to manufacture a positive electrode plate having a positive active material layer. Alternatively, the positive active material composition is cast on a separate support, and then peeled off from the support to obtain a film, which is then laminated on the aluminum current collector to manufacture a positive electrode plate having a positive active material layer.
[0063] Examples of the conductive material include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fibers, carbon nanotubes, metal powders or metal fibers or metal tubes such as copper, nickel, aluminum, and silver, and conductive polymers such as polyphenylene derivatives. In contrast, the positive electrode does not include, for example, a separate conductive material.
[0064] Examples of binders that can be used include vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, and styrene-butadiene rubber-based polymers. Examples of solvents that can be used include, but are not limited to, N-methylpyrrolidone (NMP), acetone, and water, and any solvent that is used in the relevant technical field can be used.
[0065] A plasticizer or pore-forming agent may be further added to the positive electrode active material composition to form pores inside the electrode plate.
[0066] The contents of the composite positive electrode active material, conductive material, binder, and solvent used in the positive electrode are at levels typically used in lithium batteries. Depending on the application and configuration of the lithium battery, one or more of the conductive material, binder, and solvent may be omitted.
[0067] The content of the binder used in the positive electrode is also 0.1wt% to 10wt% or 0.1wt% to 5wt% of the total weight of the positive electrode active material layer. The content of the composite positive electrode active material used in the positive electrode is also 80wt% to 99wt%, 90wt% to 99wt%, or 95wt% to 99wt% of the total weight of the positive electrode active material layer. The content of the conductive material used in the positive electrode is also 0.01wt% to 10wt%, 0.01wt% to 5wt%, 0.01wt% to 3wt%, 0.01wt% to 1wt%, 0.01wt% to 0.5wt%, or 0.01wt% to 0.1wt% of the total weight of the positive electrode active material layer. The conductive material may be omitted.
[0068] In addition, the positive electrode may further include other common positive electrode active materials in addition to the above-mentioned composite positive electrode active material.
[0069] The general positive electrode active material may be any lithium-containing metal oxide that is commonly used in the art. For example, one or more of composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. Specific examples thereof include Li a A 1-b B b D2 (wherein, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Co b B c O 2-α F α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F α(wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d GeO2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn2G b O4 (wherein 0.90≦a≦1, 0.001≦b≦0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≦f≦2);Li (3-f) A compound expressed by any one of the chemical formulas Fe2(PO4)3(0≦f≦2);LiFePO4 can be used.
[0070] In the chemical formula representing the above-mentioned compound, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-mentioned compound, and it is also possible to use a mixture of the above-mentioned compound and a compound having a coating layer added thereto. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound such as an oxide, hydroxide, oxyhydroxide, oxycarbonate, or hydroxycarbonate of the coating element of the coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method of forming the coating layer is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A specific coating method is a content that can be understood by those skilled in the art, so a detailed description will be omitted.
[0071] On the other hand, the positive electrode is also a dry type positive electrode manufactured by a dry method. The dry negative electrode includes a dry composite positive electrode active material, a dry conductive material, and a dry binder. The dry composite positive electrode active material includes a core including a lithium transition metal oxide and a shell disposed along a surface of the core. The shell has a chemical formula M a O bOne or more first metal oxides represented by (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, b is not an integer); a first carbon-based material; and a second carbon-based material; wherein the first metal oxide is disposed within a first carbon-based material matrix, M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements, and the second carbon-based material is fibrous carbon having an aspect ratio of 10 or more.
[0072] The method for manufacturing a dry cathode includes, for example, a step of dry-mixing a dry composite cathode active material, a dry conductive material, and a dry binder to prepare a dry mixture; a step of providing a cathode current collector; a step of disposing an intermediate layer on one surface of the cathode current collector; and a step of disposing the dry mixture on the intermediate layer and rolling to manufacture a cathode having a cathode active material layer disposed on one surface of the cathode current collector.
[0073] First, a composite anode active material, a dry conductive material, and a dry binder are dry-mixed to prepare a dry mixture. Dry mixing means mixing in a state without containing a process solvent. The process solvent is, for example, a solvent used in the manufacture of an electrode slurry. The process solvent is, for example, water, NMP, etc., but is not limited thereto, and is not limited as long as it is a process solvent used during the manufacture of an electrode slurry. Dry mixing can be performed using a stirrer, for example, at a temperature of 25 to 65°C. Dry mixing can be performed using a stirrer, for example, at a rotational speed of 10 to 10,000 rpm, or 100 to 10,000 rpm. Dry mixing can be performed using a stirrer, for example, for 1 to 200 minutes, or 1 to 150 minutes. The composite anode active material is a dry composite anode active material.
[0074] The dry mixing may be performed, for example, one or more times. First, the composite positive electrode active material, the dry conductive material, and the dry binder are dry-mixed for a first time to prepare a first mixture. The first dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 2000 rpm or less for a time of 15 minutes or less. The first dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 500 to 2000 rpm for 5 to 15 minutes. The composite positive electrode active material, the dry conductive material, and the dry binder may be uniformly mixed by the first dry mixing. Then, the composite positive electrode active material, the dry conductive material, and the dry binder are dry-mixed for a second time to prepare a second mixture. The second dry mixing may be performed, for example, at a temperature of 25 to 65° C. and a rotation speed of 4000 rpm or more for 10 minutes or more. The secondary dry mixing may be carried out, for example, at a temperature of 25 to 65° C. and a rotation speed of 4000 to 9000 rpm for 10 to 60 minutes. A dry mixture containing a fibrillated dry binder is obtained by the secondary dry mixing.
[0075] The agitator is, for example, a kneader. The agitator includes, for example, a chamber; one or more rotating shafts disposed inside the chamber and rotating; and a blade rotatably coupled to the rotating shaft and disposed in the longitudinal direction of the rotating shaft. The blade may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blade, the dry composite positive electrode active material, the dry conductive material, and the dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0076] The produced dry mixture can be put into an extrusion device and extruded into a sheet. The pressure during extrusion is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The obtained sheet-like extrudate is also a sheet for a positive electrode active material layer.
[0077] Examples of the dry conductive material include carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fiber, carbon nanotubes, metal powder or metal fiber or metal tube such as copper, nickel, aluminum, silver, etc., and conductive polymers such as polyphenylene derivatives, but are not limited thereto. Any material used as a conductive material in the art can be used. The conductive material is, for example, a carbon-based conductive material. The dry conductive material is a conductive material that has not come into contact with a process solvent.
[0078] Examples of the dry binder include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above polymers, and styrene-butadiene rubber-based polymers, but are not limited thereto. Any binder used in the art can be used. An example of the dry binder is polytetrafluoroethylene (PTFE). The dry binder is a binder that does not come into contact with the process solvent.
[0079] A plasticizer or pore former may further be added to the dry mixture to form pores within the positive electrode active material layer.
[0080] The contents of the dry composite positive electrode active material, the dry conductive material, and the dry binder used in the dry positive electrode are in the same ranges as the contents of the composite positive electrode active material, the conductive material, and the binder used in the wet positive electrode.
[0081] A positive current collector is then provided, which may be, for example, an aluminum foil. Next, an intermediate layer is disposed on at least one surface of the positive electrode current collector. The intermediate layer includes a carbon-based conductive material and a binder. The intermediate layer may be omitted.
[0082] Next, the sheet for the positive electrode active material layer provided on the intermediate layer is placed and rolled to produce a positive electrode in which the positive electrode active material layer is placed on one side of the positive electrode current collector. The intermediate layer is placed between the positive electrode current collector and the positive electrode active material layer. The rolling may be, for example, a roll press or a flat plate press, but is not necessarily limited thereto. The pressure during rolling may be, for example, 0.1 ton / cm. 2 ~10.0ton / cm 2 However, the range is not limited thereto. If the pressure during rolling is excessively high, cracks may occur in the positive electrode current collector. If the pressure during rolling is excessively low, the adhesive strength between the positive electrode current collector and the positive electrode active material layer may decrease.
[0083] According to yet another embodiment, a lithium battery employs a positive electrode including the composite positive electrode active material described above.
[0084] The lithium battery employs a positive electrode containing the above-mentioned composite positive electrode active material, thereby providing improved energy density, cycle characteristics and thermal stability.
[0085] The lithium battery can be manufactured, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to the required conditions.
[0086] First, the positive electrode is manufactured by the above-mentioned positive electrode manufacturing method. Next, the negative electrode is prepared as follows. The negative electrode is prepared in a substantially similar manner to the positive electrode, except that, for example, a negative electrode active material is used instead of the composite positive electrode active material. In addition, the conductive material, binder, and solvent in the negative electrode active material composition may be substantially the same as those in the positive electrode.
[0087] For example, a negative active material, a conductive material, a binder, and a solvent are mixed to prepare a negative active material composition, which is then directly coated onto a copper current collector to prepare a negative electrode plate. Alternatively, the prepared negative active material composition is cast onto a separate support, and a negative active material film that is peeled off from the support is laminated onto a copper current collector to prepare a negative electrode plate.
[0088] Any negative electrode active material can be used as long as it is used as a negative electrode active material for a lithium battery in the relevant technical field. For example, it includes one or more selected from the group consisting of lithium metal, a metal alloyable with lithium, a transition metal oxide, a non-transition metal oxide, and a carbon-based material. The metal alloyable with lithium is, for example, Si, Sn, Al, Ge, Pb, Bi, Sb, a Si-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combined element thereof and is not Si), a Sn-Y alloy (wherein Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combined element thereof and is not Sn), etc. The element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof. The transition metal oxide is, for example, lithium titanate, vanadium oxide, lithium vanadate, etc. The non-transition metal oxide is, for example, SnO2, SiO x (0 < x < 2), etc. The carbon-based material is, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is, for example, graphite such as amorphous, plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. The amorphous carbon is, for example, soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0089] The contents of the negative electrode active material, the conductive material, the binder, and the solvent are at levels normally used in lithium batteries. Depending on the use and configuration of the lithium battery, one or more of the conductive material, the binder, and the solvent can be omitted.
[0090] The content of the binder used in the negative electrode is, for example, 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the negative electrode active material layer. The content of the conductive material used in the negative electrode is, for example, 0.1 wt% to 10 wt% or 0.1 wt% to 5 wt% of the total weight of the negative electrode active material layer. The content of the negative electrode active material used in the negative electrode is, for example, 80 wt% to 99 wt%, 90 wt% to 99 wt%, or 95 wt% to 99 wt% of the total weight of the negative electrode active material layer. When the negative electrode active material is lithium metal, the negative electrode does not include a binder and a conductive material.
[0091] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared. Any separator that is generally used in lithium batteries can be used. The separator is, for example, one that has low resistance to ion movement of the electrolyte and has excellent electrolyte moisture-absorbing ability. The separator is, for example, one selected from glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene (PTFE), or a combination thereof, and is in the form of a nonwoven fabric or a woven fabric. For lithium ion batteries, a separator that can be wound, such as polyethylene or polypropylene, is used, and for lithium ion polymer batteries, a separator that has excellent organic electrolyte impregnation ability is used.
[0092] The separator is manufactured by the following exemplary method, but is not necessarily limited to such method, and may be adjusted according to the required conditions.
[0093] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated on the top of an electrode and dried to form a separator. Alternatively, the separator composition is cast on a support and dried, and the separator film is peeled off from the support and laminated on the top of an electrode to form a separator.
[0094] The polymer used in the manufacture of the separator is not particularly limited, and any polymer that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0095] Next, the electrolyte is prepared. The electrolyte is, for example, an organic electrolyte solution, which is produced by dissolving a lithium salt in an organic solvent, for example.
[0096] The organic solvent can be any organic solvent used in the art. The organic solvent can be, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a mixture thereof.
[0097] Any lithium salt that is used as a lithium salt in the art can be used. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(CyF 2y+1 SO2) (wherein x and y are each a natural number from 1 to 20), LiCl, LiI, or a mixture thereof.
[0098] Meanwhile, the electrolyte may be a solid electrolyte. The solid electrolyte may be, for example, boron oxide, lithium oxynitride, etc., but is not limited thereto, and any solid electrolyte used as a solid electrolyte in the art may be used. The solid electrolyte may be formed on the negative electrode by a method such as sputtering, or a separate solid electrolyte sheet may be laminated on the negative electrode.
[0099] The solid electrolyte is, for example, an oxide-based solid electrolyte or a sulfide-based solid electrolyte. The solid electrolyte is, for example, an oxide-based solid electrolyte. The oxide-based solid electrolyte is Li 1+x+y Al x Ti 2-x S y P 3-y O 12 (0 <x<2,0≦y<3),BaTiO3,Pb(Zr,Ti)O3(PZT),Pb 1-x La x Zr 1-y Ti y O3(PLZT)(O≦x<1,O≦y<1),PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT),HfO2,SrTiO3,SnO2,CeO2,Na2O,MgO,NiO,CaO,BaO,ZnO,ZrO2,Y2O3,Al2O3,TiO2,SiO2,Li3PO4,Li x Ti y (PO4)3(0 <x<2,0<y<3),Li x Al y Ti z (PO4)3(0 <x<2,0<y<1,0<z<3),Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x S y P 3-y O 12 (0≦x≦10≦y≦1), Li x La y TiO3(0 <x<2,0<y<3),Li2O,LiOH,Li2CO3,LiAlO2,Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2,Li 3+x La3M2O 12(M=Te, Nb, or Zr, x is an integer from 1 to 10). The solid electrolyte is produced by a sintering method or the like. For example, an oxide-based solid electrolyte is Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M doped LLZO, M=Ga, W, Nb, Ta, or Al, x is an integer of 1 to 10) is a garnet-type solid electrolyte selected from the group consisting of:
[0100] The sulfide-based solid electrolyte includes, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles are Li2S or P2S5. The sulfide-based solid electrolyte particles are known to have a higher lithium ion conductivity than other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixed molar ratio of Li2S:P2S5 is, for example, in the range of about 50:50 to about 90:10. In addition, Li3PO4, halogen, halogen compound, Li 2+2x Zinc 1-x GeO4(“LISICON”,0≦x<1),Li 3+y PO 4-x N x "LIPON", 0 <x<4,0<y<3),Li 3.25 Ge 0.25 P 0.75 S4(“Thio-LISICON”),Li2O-Al2O3-TiO2-P2O 5(Inorganic solid electrolytes produced by adding, for example, “LATP” to inorganic solid electrolytes of Li2S-P2S5, SiS2, GeS2, B2S3 or combinations thereof can be used as sulfide solid electrolytes. Non-limiting examples of sulfide solid electrolyte materials include Li2S-P2S5; Li2S-P2S5-LiX (X = halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n (0 < m < 10, 0 < n < 10, Z = Ge, Zn or Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; and Li2S-SiS2-Li p MO q (0 < p < 10, 0 < q < 10, M = P, Si, Ge, B, Al, Ga or In). In this regard, sulfide-based solid electrolyte materials can be produced by treating raw starting materials of sulfide-based solid electrolyte substances (such as Li2S, P2S5, etc.) by methods such as the melt quenching method, mechanical milling method, etc. Further, a calcination process can be performed after the said treatment. Sulfide-based solid electrolytes can be amorphous, crystalline, or in a mixed state of these.
[0101] Referring to FIG. 5, a lithium battery 1 according to one embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, negative electrode 2, and separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. An organic electrolyte solution is injected into the battery case 5 and sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to such a form, and can be, for example, square-shaped, thin-film-shaped, etc.
[0102] Referring to FIG. 6, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2, and the positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. The battery structure 7 includes electrode tabs 8 that serve as electrical paths for conducting current formed in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape and may be, for example, cylindrical or thin film.
[0103] Referring to FIG. 7, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2 to form a battery structure. The battery structure 7 is stacked in a bi-cell structure and then housed in a battery case 5. The battery structure 7 includes electrode tabs 8 that act as electrical paths for conducting current generated in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape and may be, for example, cylindrical or thin film.
[0104] The pouch-type lithium battery corresponds to the lithium batteries of FIGS. 5 to 7, in which a pouch is used as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, impregnated with an organic electrolyte, and housed in a pouch and sealed to complete the pouch-type lithium battery. For example, although not shown, the above-mentioned positive electrode, negative electrode, and separator are simply stacked and housed in a pouch in the form of an electrode assembly, or wound into a jelly-roll-shaped electrode assembly, or folded and housed in a pouch. Then, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0105] Since lithium batteries are excellent in terms of life characteristics and high-rate characteristics, they are used, for example, in electric vehicles (EVs). For example, they are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). They are also used in fields where a large amount of power storage is required. For example, they are used in electric bicycles, power tools, etc.
[0106] Multiple lithium batteries are stacked to form a battery module, and multiple battery modules form a battery pack. Such a battery pack can be used in all devices that require high capacity and high output. For example, it can be used in notebook computers, smartphones, electric vehicles, etc. A battery module includes, for example, multiple batteries and a frame that holds them. A battery pack includes, for example, multiple battery modules and a bus bar that connects them. The battery module and / or the battery pack may further include a cooling device. Multiple battery packs are regulated by a battery management system. The battery management system includes a battery pack and a battery control device connected to the battery pack.
[0107] A method for manufacturing a composite cathode active material according to still another embodiment includes the steps of providing a lithium metal oxide; providing a composite; providing a second carbon-based material; and mechanically milling the lithium metal oxide, the composite, and the second carbon-based material, where the composite has the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer) represents one or more first metal oxides; and includes a first carbon-based material, the first metal oxide is disposed within the first carbon-based material matrix, where M is one or more metals selected from Groups 2 to 13, 15, and 16 of the periodic table of elements, and the second carbon-based material includes fibrous carbon with an aspect ratio of 10 or more.
[0108] A lithium transition metal oxide is provided. The lithium transition metal oxide is, for example, a compound represented by Chemical Formulas 1 to 6 described above.
[0109] A composite is provided. The step of providing the composite includes, for example, supplying a reaction gas composed of a carbon source gas to a structure containing a second metal oxide and performing a heat treatment to provide the composite. The step of providing the composite includes, for example, M a O c (0 < a ≤ 3, 0 < c ≤ 4, when a is 1, 2, or 3, b is a constant) supplying a reaction gas composed of a carbon source gas to one or more second metal oxides represented by and performing a heat treatment to produce a composite, wherein M is one or more selected metals from Groups 2 to 13, 15, and 16 of the Periodic Table of the Elements.
[0110] The carbon source gas is a gas composed of a compound represented by the following Chemical Formula 9, or one or more mixed gases selected from the group consisting of a compound represented by the following Chemical Formula 9, a compound represented by the following Chemical Formula 10, and an oxygen-containing gas represented by the following Chemical Formula 11.
[0111] [Chemical Formula 9] C n H (2n+2-a) [OH] a In the above Chemical Formula 9, n is 1 to 20, and a is 0 or 1;
[0112] [Chemical Formula 10] C n H 2n In the above Chemical Formula 10, n is 2 to 6;
[0113] [Chemical Formula 11] C x H y O z In the above Chemical Formula 11, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.
[0114] The compound represented by Chemical Formula 9 and the compound represented by Chemical Formula 10 are one or more selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 11 includes, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.
[0115] M a O c After the step of supplying a reaction gas composed of a carbon source gas to the second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4; if a is 1, 2, or 3, c is an integer) and performing heat treatment, a cooling step using one or more inert gases selected from the group consisting of nitrogen, helium, and argon is further carried out. The cooling step refers to the step of adjusting to room temperature (20 - 25°C). The carbon source gas includes one or more inert gases selected from the group consisting of nitrogen, helium, and argon.
[0116] In the method for producing a composite, the growth process of a carbon-based material, such as graphene, by a gas-phase reaction can be carried out under various conditions.
[0117] According to the first condition, for example, M a O c First, methane is supplied to a reactor in which the second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4; if a is 1, 2, or 3, c is an integer) is arranged, and the temperature is raised to the heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1100°C. Heat treatment is carried out during the reaction time at the heat treatment temperature (T). The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. The time taken for the process of cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0118] According to the second condition, for example, M a O cHydrogen is first supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), methane gas is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for the process of cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0119] According to the third condition, for example, M a O c Hydrogen is first supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature raising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for the process of cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0120] In the process of producing the composite, when the carbon source gas contains water vapor, a composite having very excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited, and is, for example, 0.01% by volume to 10% by volume based on 100% by volume of the total carbon source gas. The carbon source gas is, for example, methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.
[0121] The carbon supply gas may be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20-1:0.50, about 1:0.25-1:0.45, or about 1:0.30-1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane to carbon dioxide to water vapor is about 1:0.20-0.50:0.01-1.45, about 1:0.25-0.45:0.10-1.35, or about 1:0.30-0.40:0.50-1.0.
[0122] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas does not include an inert gas such as nitrogen.
[0123] The heat treatment pressure can be selected in consideration of the heat treatment temperature, the composition of the gas mixture, the desired amount of carbon coating, and the like. The heat treatment pressure can be controlled by adjusting the amount of the inflowing gas mixture and the amount of the outflowing gas mixture. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more. The heat treatment pressure is, for example, 0.5 atm to 10 atm, 1 atm to 10 atm, 2 atm to 10 atm, 3 atm to 10 atm, 4 atm to 10 atm, or 5 atm to 10 atm.
[0124] The heat treatment time is not particularly limited and can be appropriately adjusted according to the heat treatment temperature, the pressure during heat treatment, the composition of the gas mixture, and the amount of the desired carbon coating. For example, the reaction time at the heat treatment temperature is, for example, 10 minutes to 100 hours, 30 minutes to 90 hours, or 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene (carbon), increases, whereby the electrical properties of the composite can be improved. However, such a tendency is not necessarily directly proportional to the time. For example, after a predetermined time has elapsed, no further carbon deposition, for example, graphene deposition, occurs or the deposition rate decreases.
[0125] Even at a relatively low temperature through the gas-phase reaction of the above-described carbon source gas, M a O c (0 < a ≤ 3, 0 < c ≤ 4, if a is 1, 2, or 3, then c is an integer), a second metal oxide represented thereby and its reduction product M a O b Among the first metal oxides represented by (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer), by providing a uniform coating of the first carbon-based material, for example, a graphene coating, on one or more selected ones, a composite is obtained.
[0126] The composite is, for example, a matrix of a first carbon-based material having one or more structures selected from a spherical structure, a helical structure in which a plurality of spherical structures are connected, a cluster structure in which a plurality of spherical structures are aggregated, and a sponge structure, for example, a graphene matrix, and M disposed within the graphene matrix a O b (0 < a ≤ 3, 0 < b < 4, a is 1, 2, or 3, and b is not an integer), a first metal oxide represented thereby and M a O cIt contains one or more selected from the second metal oxides represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer).
[0127] Next, the lithium transition metal oxide, the composite, and the second carbon-based material are mechanically milled. In the step of mechanical milling, the milling method is not particularly limited and is a method of bringing the lithium transition metal oxide, the composite, and the second carbon-based material into contact using a machine, and any method that can be used in the technical field can be used.
[0128] For example, a Nobilta mixer is used during milling. The rotation speed of the mixer during milling is, for example, 1000 rpm to 5000 rpm or 2000 rpm to 4000 rpm. If the milling speed is too low, the shear force applied to the lithium transition metal oxide, the composite, and the second carbon-based material is weak, making it difficult for the lithium transition metal oxide and the composite to form a chemical bond. If the milling speed is too high, the composite is formed in an excessively short time, making it difficult for the composite and the second carbon-based material to be uniformly coated on the lithium transition metal oxide and to form a uniform and continuous shell. The milling time is, for example, 5 minutes to 100 minutes, 5 minutes to 60 minutes, or 5 minutes to 30 minutes. If the milling time is too short, it is difficult for the composite and the second carbon-based material to be uniformly coated on the lithium transition metal oxide and to form a uniform shell. If the milling time is too long, production efficiency decreases. The content of the complex may be 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, or 1 wt% or less of the total weight of the lithium transition metal oxide and the complex. The content of the complex may be, for example, 0.01 to 5 wt%, 0.01 to 4 wt%, 0.01 to 3 wt%, 0.1 to 2 wt%, or 0.1 to 1 wt% of the total weight of the first lithium transition metal oxide and the complex. For example, the content of the complex relative to 100 parts by weight of the mixture of the first lithium transition metal oxide and the complex may be 0.01 to 5 parts by weight, 0.01 to 4 parts by weight, 0.01 to 3 parts by weight, 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, or 0.1 to 1 part by weight. The average particle size (D50) of the composite used in the mechanical milling of the first lithium transition metal oxide and the composite is, for example, 50 nm to 200 nm, 100 nm to 300 nm, or 200 nm to 500 nm.
[0129] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are merely for the purpose of illustrating the present invention and are not intended to limit the scope of the present invention.
[0130] (Production of the complex) Production example 1: Al 2 O3 @Gr complex After placing Al2O3 particles (average particle size: about 20 nm) in the reactor, the internal temperature of the reactor was raised to 1000 °C under the condition that CH4 was supplied at about 300 sccm and 1 atm for about 30 minutes in the reactor.
[0131] Next, heat treatment was performed by holding at the said temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20 - 25 °C), and a composite in which Al2O3 particles and Al2O z (0 < z < 3) particles were embedded in graphene was obtained. The alumina content contained in the composite was 60 wt%.
[0132] Production example 2: Al 2 O 3 @Gr complex A composite was produced in the same manner as in Production Example 1, except that Al2O3 particles (average particle size: about 200 nm) were used instead of Al2O3 particles (average particle size: about 20 nm).
[0133] Comparative production example 1: SiO 2 @Gr complex After placing SiO2 particles (average particle size: about 15 nm) in the reactor, the internal temperature of the reactor was raised to 1000 °C under the condition that CH4 was supplied at about 300 sccm and 1 atm for about 30 minutes in the reactor.
[0134] Next, heat treatment was performed by holding at the said temperature for 7 hours. Then, the internal temperature of the reactor was adjusted to room temperature (20 - 25 °C), and SiO2 particles and SiO y (0 < y < 2) particles were embedded in graphene was obtained.
[0135] (Production of Composite Cathode Active Material) Example 1: Al 2 O 3 @NCA91 coated with 0.2wt% Gr composite (0.12wt% alumina) and 0.05wt% CNT LiNi with an average particle size of 10 μm 0.91 Co 0.05 Al 0.04A composite positive electrode active material was prepared by milling O2 (hereinafter referred to as NCA91), the composite prepared in Preparation Example 1, and carbon nanotubes (hereinafter referred to as CNTs) using a Nobilta Mixer (Hosokawa, Japan) at a rotation speed of about 1000 to 2000 rpm for about 5 to 30 minutes. NCA91, the composite, and CNTs were mixed in a ratio of 99.75:0.2:0.05 to prepare a composite positive electrode active material.
[0136] It was confirmed that carbon nanotubes were disposed on the surface of the composite positive electrode active material, as shown in Fig. 2. The carbon nanotubes include a carbon nanotube primary structure and a carbon nanotube secondary structure formed by agglomerating a plurality of carbon nanotube units.
[0137] The carbon nanotube primary structure is composed of one carbon nanotube unit, the length of which is 200 nm to 300 nm, and the diameter of the carbon nanotube is about 10 nm.
[0138] The carbon nanotube secondary structure was formed by agglomerating a plurality of carbon nanotube units, and had a length of 500 nm or more and a diameter of about 40 nm.
[0139] Example 2: Al 2 O 3 @NCA91 coated with 0.15wt% Gr composite and 0.05wt% CNT A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixture ratio of the composite and the carbon nanotubes was changed from 0.2:0.05 to 0.15:0.05.
[0140] Example 3: Al 2 O 3 @NCA91 coated with 0.18wt% Gr composite and 0.02wt% CNT A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixture ratio of the composite and the carbon nanotubes was changed from 0.2:0.05 to 0.18:0.02.
[0141] Example 4: Al 2 O 3 @Gr composite 0.1wt% and CNT 0.1wt% coating NCA91 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixture ratio of the composite and the carbon nanotubes was changed from 0.2:0.05 to 0.1:0.1.
[0142] Example 5: Al 2 O 3 @Gr composite 0.2wt% and CNT 0.05wt% coating NCA91, alumina particle size 200nm A composite positive electrode active material was prepared in the same manner as in Example 1, except that the composite obtained in Preparation Example 2 was used instead of the composite obtained in Preparation Example 1.
[0143] Comparative example 1: bare NCA91 NCA91 with an average particle size of 10 μm was used as it is as a composite positive electrode active material.
[0144] Comparative Example 2: CNT 0.25wt% coated NCA91 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the composite prepared in Preparation Example 1 was not used and 0.25 wt % of carbon nanotubes was used.
[0145] Comparative example 3: SiO 2 @Gr composite 0.25wt% coating silicon composite structure A composite positive electrode active material was prepared in the same manner as in Example 1, except that the composite prepared in Comparative Preparation Example 1 was used instead of the composite prepared in Preparation Example 1.
[0146] Comparative example 4: Al 2 O 3 @A simple mixture of 0.2 wt% Gr composite and 0.05 wt% CNT LiNi with an average particle size of 10 μm 0.91 Co 0.05 Al 0.04 A simple mixture of O2 (hereinafter referred to as NCA91), the composite prepared in Preparation Example 1, and carbon nanotubes (hereinafter referred to as CNT) in a weight ratio of 97.5:0.2:0.05 was used as a composite positive electrode active material.
[0147] (Lithium battery (half cell) manufacturing, wet type) Example 6 (Production of positive electrodes) The composite positive electrode active material prepared in Example 1, a carbon conductive material (Denka Black), and polyvinylidene fluoride (PVdF) were mixed in a weight ratio of 98.85:0.5:0.65, and the mixture was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0148] The slurry was bar-coated on an aluminum current collector having a thickness of 15 μm, dried at room temperature, and then dried again under vacuum at 120° C., followed by rolling and punching to prepare a positive electrode having a thickness of 60 μm.
[0149] (Coin cell manufacturing) Coin cells were fabricated using the positive electrode prepared above, lithium metal as a counter electrode, a PTFE separator, and a solution of 1.5 M LiPF6 dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (volume ratio 2:1:7) as an electrolyte.
[0150] Examples 7 to 10 Coin cells were manufactured in the same manner as in Example 6, except that the composite positive electrode active materials prepared in Examples 2 to 5 were used instead of the composite positive electrode active material prepared in Example 1.
[0151] Comparative Examples 5 to 8 Coin cells were manufactured in the same manner as in Example 6, except that the composite positive electrode active materials prepared in Comparative Examples 1 to 4 were used instead of the composite positive electrode active material prepared in Example 1.
[0152] (Lithium battery (halfcell) manufacturing, dry type) Example 11 (Production of positive electrodes) The composite positive electrode active material prepared in Example 1, a carbon conductive material (Denka Black), and polyvinylidene fluoride (PVdF) were mixed in a weight ratio of 98.85:0.5:0.65, and the mixture was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0153] The slurry was bar-coated on an aluminum current collector having a thickness of 15 μm, dried at room temperature, and then dried again under vacuum at 120° C., followed by rolling and punching to prepare a positive electrode having a thickness of 60 μm.
[0154] The composite cathode active material prepared in Example 1 as a dry cathode active material, a carbon conductive material (Denka Black) as a dry conductive material, and polytetrafluoroethylene (PTFE) as a dry binder were charged into a blade mixer in a weight ratio of 92:4:4, and then primary dry mixing was performed at 25° C. and 1000 rpm for 10 minutes to prepare a first mixture in which the dry cathode active material, the dry conductive material, and the dry binder were uniformly mixed.
[0155] Then, in order to promote fiberization of the binder, the first mixture was further mixed at 25° C. and 5000 rpm for 20 minutes to prepare a second mixture. No separate solvent was used in the preparation of the first and second mixtures.
[0156] The prepared second mixture was put into an extruder and extruded to prepare a sheet-shaped positive electrode active material layer self-standing film under a pressure of 50 MPa.
[0157] A carbon layer was disposed as an interlayer on one surface of a 12 μm-thick aluminum thin film, and the interlayer was disposed on one surface of a second positive electrode current collector to prepare a first laminate.
[0158] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was about 1 μm.
[0159] A positive electrode active material layer free-standing film was placed on the intermediate layer of the prepared first laminate, and rolled to produce a positive electrode.
[0160] (Coin cell manufacturing) Coin cells were fabricated using the positive electrode prepared above, lithium metal as a counter electrode, a PTFE separator, and a solution of 1.5 M LiPF6 dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (volume ratio 2:1:7) as an electrolyte.
[0161] Comparative Example 9 Coin cells were prepared in the same manner as in Example 11, except that the composite positive electrode active material prepared in Comparative Example 1 was used instead of the composite positive electrode active material prepared in Example 1.
[0162] Evaluation example 1: XPS spectrum evaluation XPS spectra were measured over time using a Qunatum 2000 (Physical Electronics) during the manufacturing process of the composite manufactured in Manufacturing Example 1. XPS spectra of the C 1s orbital and Al 2p orbital were measured for the sample before heating, after 1 minute, 5 minutes, 30 minutes, 1 hour, and 4 hours. At the beginning of the heating, only the peak for the Al 2p orbital was shown, and no peak for the C 1s orbital was shown. After 30 minutes, the peak for the C 1s orbital was clearly shown, and the magnitude of the peak for the Al 2p orbital was significantly reduced.
[0163] After 30 minutes, peaks for the C 1s orbital due to C-C and C=C bonds caused by the growth of graphene were clearly shown near 284.5 eV.
[0164] With the passage of the reaction time, the oxidation number of aluminum decreased, and the peak position of the Al 2p orbital shifted to the side with a lower binding energy (eV).
[0165] Therefore, as the reaction proceeded, graphene grew on the Al2O3 particles, and it was confirmed that Al2O x (0 < x < 3) which is the reduction product of Al2O3 was produced.
[0166] Through XPS analysis results of 10 regions of the composite sample produced in Production Example 1, the average contents of carbon and aluminum were measured. For the measurement results, the deviation of the aluminum content for each region was calculated. The deviation of the aluminum content was shown as a percentage with respect to the average value, and this was referred to as the uniformity. The percentage with respect to the average value of the deviation of the aluminum content, that is, the uniformity of the aluminum content was 1%. Therefore, it was confirmed that alumina was uniformly distributed in the composite produced in Production Example 1.
[0167] Evaluation example 2: SEM, HR-TEM and SEM-EDS analysis Scanning electron microscopy, high-resolution transmission electron microscopy, and EDS (Energy-dispersive X-ray spectroscopy) analysis were performed on the composite produced in Production Example 1, the composite positive electrode active material produced in Example 1, and the composite positive electrode active material produced in Comparative Example 1.
[0168] During SEM-EDS analysis, FEI Titan 80-300 from Philips was used.
[0169] The composite produced in Production Example 1 is composed of Al2O3 particles and Al2O which is its reduction product zIt was shown that the structure has (0 < z < 3) particles embedded in graphene. Al2O3 particles and Al2O z It was confirmed that a graphene layer is disposed on the outer contour of one or more particles selected from (0 < z < 3). Al2O3 particles and Al2O z One or more particles selected from (0 < z < 3) were uniformly dispersed in the graphene matrix. Al2O3 particles and Al2O z One or more particle sizes in the (0 < z < 3) particles are about 20 nm. The particle size of the composite produced in Production Example 1 is about 50 nm to 200 nm. It was confirmed that a shell formed of a composite containing graphene is disposed on the NCA core in the composite positive electrode active material produced in Example 1.
[0170] In the SEM-EDS mapping analysis of the composite positive electrode active materials produced in Comparative Example 1 and Example 1, it was confirmed that the concentration of aluminum (Al) distributed on the surface of the composite positive electrode active material of Example 1 increased compared to the surface of the composite positive electrode active material of Comparative Example 1.
[0171] It was confirmed that the composite produced in Production Example 1 is uniformly coated on the NCA core in the composite positive electrode active material of Example 1 to form a shell.
[0172] Evaluation example 3: XPS spectrum evaluation (graphene-NCA chemical bond) The XPS spectrum for the O 1s orbital was measured for the composite produced in Production Example 1, the NCA of Comparative Example 1, and the composite positive electrode active material produced in Example 1 using Quantum 2000 (Physical Electronics), and the results are shown in FIG. 3.
[0173] As shown in FIG. 3, a peak due to a CO-Ni bond was observed near 530.2 eV for the composite cathode active material of Example 1. This peak was determined to be a peak due to a bond formed between the NiO phase present on the NCM surface and the carbon of graphene. Therefore, it was confirmed that the graphene contained in the shell formed on the core forms a covalent bond with Ni, which is a transition metal contained in the core.
[0174] Evaluation example 4: Raman spectrum evaluation (graphene-NCA chemical bond) The Raman spectra of the composite prepared in Preparation Example 1 and the composite positive electrode active material prepared in Example 1 were measured, and the results are shown in FIG.
[0175] As shown in FIG. 4, the composite produced in Production Example 1 had a peak at 1338.7 cm -1 D band peak at 1575.0 cm -1 The G-band peak at
[0176] On the other hand, in the composite positive electrode active material of Example 1, the D band peak is 1351.3 cm due to the graphene-containing shell. -1 And it is about 12cm -1 The G-band peak shifted to 1593.6 cm -1 And it is about 18cm -1 Shifted.
[0177] The shift in the D-band peak was determined to be due to the strain of the graphene bonded onto the core by milling to form the shell.
[0178] The shift in the G-band peak was determined to be due to charge transfer between the core and graphene in the complex formed by the CO-Ni bond.
[0179] Therefore, it was confirmed that the graphene contained in the shell formed on the core forms a covalent bond with Ni, the transition metal contained in the core.
[0180] Evaluation example 4: High temperature (45℃) charge / discharge characteristic evaluation The lithium batteries manufactured in Examples 6 to 10 and Comparative Examples 5 to 8 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.3 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) during discharge (formation cycle).
[0181] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2 C rate at 45°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. It was then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (1 st 50 such cycles. th The cycle was repeated under the same conditions.
[0182] In all charge / discharge cycles, a rest time of 10 minutes was allowed after one charge / discharge cycle. Some results of the room temperature charge / discharge experiments are shown in Tables 1 and 2 below. The initial efficiency is defined by the following Equation 1, and the capacity retention is defined by the following Equation 2.
[0183] [Formula 1] Initial efficiency [%] = [1 st Discharge capacity in cycles / 1 st Charging capacity in cycles x 100 [Formula 2] Capacity retention rate [%]=[50 th Discharge capacity in cycles / 1 st Discharge capacity in cycles x 100
[0184] Evaluation example 5: Evaluation of direct current internal resistance (DC-IR) before and after high-temperature charge / discharge For the lithium batteries produced in Examples 6 to 10 and Comparative Examples 5 to 8, the direct current internal resistance (DC-IR) was measured before and after the high temperature charge / discharge evaluation by the following method.
[0185] 1 st In the cycle, the battery was charged to a voltage of 50% SOC (state of charge) at a current of 0.5C, then cut off at 0.02C and rested for 10 minutes. Discharge at a constant current of 0.5C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 30 seconds, then rest for 10 minutes, Discharge at a constant current of 1.0C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 1 minute, and rest for 10 minutes. Discharge at a constant current of 2.0C for 30 seconds, then rest for 30 seconds, charge at a constant current of 0.5C for 2 minutes, rest for 10 minutes, The battery was discharged at a constant current of 3.0 C for 30 seconds, then rested for 30 seconds, charged at a constant current of 0.5 C for 3 minutes, and rested for 10 minutes.
[0186] The DC internal resistance (DC-IR, R = ΔV / ΔI) was calculated from the ratio of the average voltage change (ΔV) and the average current change (ΔI) during constant current discharge at each C-rate, and the average value was taken as the measured value.
[0187] Some of the measurement results of the DC internal resistance before the high-temperature charge-discharge evaluation and after the room-temperature charge-discharge evaluation are shown in Table 2 below.
[0188] [Table 1]
[0189] As shown in Table 1, the lithium batteries of Examples 7 to 10 had improved high-temperature life characteristics compared to the lithium batteries of Comparative Examples 5 to 8.
[0190] The lithium battery of Comparative Example 6 has inferior high-temperature life characteristics compared to the lithium battery of Example 6. This is believed to be because in the lithium battery of Comparative Example 6, only CNTs were arranged on the NCA91 core, and side reactions between the NCA91 core and the electrolyte could not be efficiently blocked.
[0191] The lithium battery of Comparative Example 7 has inferior high-temperature life characteristics compared to the lithium battery of Example 6. This was determined to be due to the inferior high-voltage stability of the SiO2@Gr composite disposed on the NCA91 core in the lithium battery of Comparative Example 6.
[0192] The lithium battery of Comparative Example 8 has inferior high-temperature life characteristics compared to the lithium battery of Example 6. This is believed to be because, in the lithium battery of Comparative Example 8, NCA91, the composite, and CNTs are simply mixed, and a shell is not formed on the NCA91 core, so that side reactions of the electrolyte are not efficiently blocked.
[0193] Although not shown in Table 1, the lithium battery of Example 11 had improved life characteristics compared to the lithium battery of Comparative Example 9.
[0194] [Table 2]
[0195] As shown in Tables 1 and 2, the lithium batteries of Examples 6 and 7 had improved initial efficiency and high-temperature life characteristics, and an increase in DC internal resistance was suppressed, compared to the lithium battery of Comparative Example 5.
[0196] Although not shown in Table 2, the lithium batteries of Examples 7 to 10 had improved initial efficiency and suppressed increase in DC internal resistance compared to the lithium battery of Comparative Example 5.
[0197] Evaluation Example 6: Evaluation of room temperature high rate characteristics and reversibility of electrode reactions The lithium batteries prepared in Examples 6 to 10 and Comparative Examples 5 to 8 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 2.8 V (vs. Li) during discharge (formation cycle).
[0198] The lithium battery that had undergone the chemical cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. It was then discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V (vs. Li) (1 st cycle).
[0199] 1 st The cycled lithium battery was charged at 25°C at a constant current of 0.2C rate until the voltage reached 4.3V (vs. Li), and then cut off at a current of 0.05C rate while maintaining 4.3V in constant voltage mode. It was then discharged at a constant current of 0.5C rate until the voltage reached 2.8V (vs. Li) (2 nd cycle).
[0200] 2 nd The cycled lithium battery was charged at 25°C at a constant current of 0.2 C rate until the voltage reached 4.3 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.3 V in constant voltage mode. It was then discharged at a constant current of 1.0 C rate until the voltage reached 2.8 V (vs. Li) (3 rd cycle).
[0201] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle. Some results of the room temperature charge / discharge experiments are shown in Table 3 below. The high rate characteristic is defined by the following Equation 3.
[0202] The reversibility of the electrode reaction is expressed by the following Equation 4. The reversibility of the electrode reaction is the ratio of the capacity charged in a constant current mode to the total charging capacity.
[0203] [Formula 3] High rate characteristic [%] = [1.0C rate discharge capacity (3 rd Cycle discharge capacity) / 0.2C rate discharge capacity (1 st Cycle discharge capacity)] x 100
[0204] [Formula 4] Electrode reaction reversibility [%] = [0.2C rate constant current mode charge capacity (1 st Cycle CC charging capacity) / 0.2C rate Constant current mode and constant voltage mode charging capacity (1 st Cycle CC+CV charging capacity)] x 100
[0205] [Table 3]
[0206] As shown in Table 3, the lithium batteries of Examples 6 to 10 had improved high rate characteristics and reversibility of the electrode reaction compared to the lithium battery of Comparative Example 5. [Explanation of symbols]
[0207] 1 Lithium battery 2 negative electrode 3 Positive electrode 4. Separator 5 Battery case 6 Cap Assembly 7 Battery structure 8 Electrode tab 10 cores 20 Shell 21 First metal oxide 22 Carbon-based materials No. 1 23 Secondary carbon-based materials 100 Composite positive electrode active material
Claims
1. A core comprising a lithium transition metal oxide having a nickel content of 80 mol% or more based on the total transition metal mole number; a shell disposed along a surface of the core; The shell has the formula M a O b (0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer), the first metal oxide is disposed within a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of Elements; the second carbonaceous material comprises fibrous carbon having an aspect ratio of 10 or more.
2. 10. The composite active cathode material of claim 1, wherein the second carbon-based material comprises carbon nanofibers, carbon nanotubes, or a combination thereof.
3. The carbon nanotubes include a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof; The composite positive electrode active material of claim 2 , wherein the carbon nanotube primary structure is a single carbon nanotube unit.
4. 4. The composite cathode active material of claim 3, wherein the carbon nanotube primary structures comprise single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-walled carbon nanotubes, or combinations thereof.
5. 4. The composite positive electrode active material of claim 3, wherein the carbon nanotube primary structure has a diameter of 1 nm to 20 nm and a length of 100 nm to 2 μm.
6. 4. The composite active cathode material of claim 3, wherein the carbon nanotube secondary structures comprise bundled carbon nanotubes, bundled carbon nanotubes, or combinations thereof.
7. 4. The composite positive electrode active material according to claim 3, wherein the carbon nanotube secondary structures have a diameter of 2 nm to 50 nm and a length of 500 nm to 1000 μm.
8. The content of the second carbon-based material is 0.1 wt % to 50 wt % based on the total weight of the first carbon-based material and the second carbon-based material; The content of the second carbon-based material is 0.001 wt % to 1 wt % based on the total weight of the composite positive electrode active material; 10. The composite active cathode material of claim 1 , wherein the second carbon-based material is disposed on a surface of the composite active cathode material.
9. The first metal contained in the first metal oxide is one or more metals selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se; The first metal oxide is Al 2 O z (0<z<3), NbO x (0<x<2.5), MgO x (0<x<1), Sc 2 O z (0<z<3), TiO y (0<y<2), ZrO y (0<y<2), V 2 O z (0<z<3), WO y (0<y<2), MnO y (0<y<2), Fe 2 O z (0<z<3), Co 3 O w (0<w<4), PdO x (0<x<1),CuO x (0<x<1), AgO x (0<x<1), ZnO x (0<x<1), Sb 2 O z (0<z<3), and SeO y 2. The composite positive electrode active material of claim 1 , wherein y is one or more selected from the group consisting of (0<y<2).
10. The shell has the formula M a O c (0<a≦3, 0<c≦4, and if a is 1, 2, or 3, then c is an integer), the second metal oxide comprises the same metal as the first metal oxide; 2. The composite positive electrode active material of claim 1, wherein a ratio c / a between a and c of the second metal oxide is greater than a ratio b / a between a and b of the first metal oxide.
11. The second metal oxide is Al 2 O 3 , NbO, NbO 2 , Nb 2 O 5 , MgO, Sc 2 O 3 , TiO 2 , ZrO 2 , V 2 O 3 , W.O. 2 , MnO 2 , Fe 2 O 3 , Co 3 O 4 , PdO, CuO, AgO, ZnO, Sb 2 O 3 , and SeO 2 is selected from 11. The composite active cathode material of claim 10, wherein the first metal oxide is a reduction product of the second metal oxide.
12. 12. The composite positive electrode active material according to claim 11, wherein an average particle size of one or more selected from the first metal oxide and the second metal oxide is 1 nm to 100 nm, and the average particle size is a volume-based median diameter (D50) measured using a laser scattering particle size distribution meter.
13. The shell includes a first carbon-based material disposed in a direction protruding from a surface of one or more of the first metal oxide and the second metal oxide, 2. The composite cathode active material of claim 1, wherein the shell has a thickness of 1 nm to 5 μm.
14. the shell includes at least one selected from the group consisting of a composite including the first metal oxide, a first carbon-based material, and a second carbon-based material, and a milling result of the composite; 2. The composite positive electrode active material of claim 1, wherein a content of at least one of the composite and the milled product of the composite is 0.01 wt % to 5 wt % of a total weight of the composite positive electrode active material.
15. the first carbon-based material has a branched structure and the first metal oxide is distributed within the branched structure; 15. The composite active cathode material of claim 14, wherein the branched structure comprises a plurality of particles of the first carbon-based material in contact with one another.
16. 2. The composite positive electrode active material of claim 1, wherein the lithium transition metal oxide is represented by a formula selected from the following Formulas 1 to 8: [Chemical formula 1] Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 1, 1.0≦a≦1.2, 0≦b≦0.2, 0.8≦x<1, 0≦y≦0.3, 0<z≦0.3, and x+y+z=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br or a combination thereof; [Chemical formula 2] L)) x Co y Mn z O 2 [Chemical formula 3] L)) x Co y Al z O 2 In the formulas 2 and 3, 0.8≦x≦0.95, 0≦y≦0.2, 0<z≦0.2, and x+y+z=1; [Chemical formula 4] L)) x Co y Mn z Al w O 2 In the formula 4, 0.8≦x≦0.95, 0≦y≦0.2, 0<z≦0.2, 0<w≦0.2, and x+y+z+w=1; [Chemical formula 7] Li a M1 x M2 y PO 4-b X b In the formula 7, 0.90≦a≦1.1, 0≦x≦0.9, 0≦y≦0.5, 0.9<x+y<1.1, and 0≦b≦2; M1 is nickel (Ni); M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y), or a combination thereof; and X is O, F, S, P, or a combination thereof.
17. A positive electrode comprising the composite positive electrode active material of claim 1 .
18. a dry composite positive electrode active material, a dry conductive material, and a dry binder; The dry composite positive electrode active material is a core including a lithium transition metal oxide having a nickel content of 80 mol% or more based on the total transition metal moles; a shell disposed along a surface of the core; The shell has the formula M a O b (wherein 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer); a first carbon-based material; and a second carbon-based material, the first metal oxide is disposed within a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of Elements; The second carbonaceous material comprises fibrous carbon having an aspect ratio of 10 or more.
19. The positive electrode of claim 18; a negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode.
20. The method of claim 1, further comprising providing a lithium transition metal oxide having a nickel content of 80 mol% or more based on the total transition metal moles; Providing a complex; providing a second carbon-based material; and mechanically milling the lithium transition metal oxide, the composite, and the second carbon-based material; The complex has the formula M a O b (wherein 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer); and a first carbon-based material; the first metal oxide is disposed within a first carbon-based material matrix, and the M is one or more metals selected from Groups 2 to 13, 15, and 16 of the Periodic Table of Elements; the second carbonaceous material comprises fibrous carbon having an aspect ratio of 10 or more.
Citation Information
Patent Citations
Positive electrode activator and positive electrode using the same, lithium ion battery and lithium polymer battery using positive electrode
JP2004220909A
Positive electrode active material and lithium battery including the same
JP2012043787A
Positive electrode active material for lithium ion secondary battery, and method for manufacturing the same
JP2012169217A
Positive electrode material for lithium secondary battery
JP2021176123A
Lithium ion secondary cell
WO2016098783A1