Radio wave absorber, housing, and power conversion device
The radio wave absorber with a soft magnetic material and electrical resistance layer addresses insulation issues at higher voltages, ensuring effective insulation and compact device design by enhancing withstand voltage performance.
Patent Information
- Application Number
- JP2022194114
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Conventional radio wave absorbers with insulating resin layers fail to provide sufficient insulation performance at higher voltages, leading to increased device size due to the need for greater distance between high-voltage equipment and absorbers.
A radio wave absorber comprising a soft magnetic material and a resin with a dielectric breakdown strength of 8 kV/mm or more, combined with an electrical resistance layer, enhances insulation while maintaining a compact device size by reducing the required distance between high-voltage equipment.
The absorber ensures improved withstand voltage performance and insulation, allowing for a reduction in the overall device size by suppressing dielectric breakdown without the need for additional space, suitable for high-voltage environments.
Smart Images

Figure 0007577724000001 
Figure 0007577724000002 
Figure 0007577724000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a radio wave absorber, a housing, and a power conversion device. [Background technology]
[0002] Conventionally, wave absorbers that absorb electromagnetic waves have been used to suppress the effects of electromagnetic waves emitted from various electric circuits, electronic devices, etc. For example, Patent Document 1 discloses an electromagnetic wave shielding film that is attached to wiring on a printed wiring board and includes an insulating resin layer made of resin and a conductive layer. Here, the conductive layer of the electromagnetic wave shielding film includes an electromagnetic wave blocking layer that is configured as a metal layer and blocks electromagnetic waves, and an electromagnetic wave absorbing layer that is configured as a metal layer, a conductive metal compound layer, or the like and absorbs electromagnetic waves, thereby suppressing the effects of electromagnetic waves. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-21837 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as various devices are becoming higher in voltage and the demand for insulating properties in radio wave absorbers increases, the insulating performance of the radio wave absorber may become insufficient even when the radio wave absorber has an insulating resin layer as in the configuration described in the cited document 1. As a configuration for ensuring the insulating properties, for example, a measure of providing a space between the radio wave absorber and the high-voltage device or the high-voltage wiring connected to the high-voltage device and using air as an insulating layer may be considered. However, such a configuration may be difficult to adopt because the higher the voltage of the high-voltage device, the greater the need to increase the distance between the high-voltage device and the radio wave absorber, which increases the size of the entire device including the high-voltage device. Therefore, there has been a demand for a radio wave absorber that can ensure voltage resistance performance while suppressing the increase in size of the entire device. [Means for solving the problem]
[0005] The present disclosure can be realized in the following forms. (1) According to one embodiment of the present disclosure, there is provided a radio wave absorber for absorbing electromagnetic waves, comprising: a radio wave absorbing layer including a soft magnetic material and a resin; and an electrical resistance layer disposed on one surface of the radio wave absorbing layer, the electrical resistance layer including a ceramic having a dielectric breakdown strength of 8 kV / mm or more and a resin having a dielectric breakdown strength higher than that of air. According to the radio wave absorber of this embodiment, it is possible to improve the voltage resistance of the radio wave absorber having radio wave absorbing properties. (2) In the radio wave absorber of the above embodiment, the dielectric breakdown strength may be 3 kV / mm or more. With such a configuration, the dielectric breakdown strength of the radio wave absorber is equal to or greater than the dielectric breakdown strength of air, so that it is possible to reduce the air layer provided on the radio wave absorber in order to ensure insulation and to suppress dielectric breakdown of the radio wave absorber. (3) In the radio wave absorber of the above embodiment, the real component of the complex relative permeability may be 3 or more in the range of 1 MHz to 100 MHz. With this configuration, the radio wave absorber can function as a radio wave absorber for electromagnetic waves of 1 MHz to 100 MHz. (4) In the radio wave absorber of the above embodiment, the soft magnetic material may be manganese zinc ferrite. With this configuration, the function of the radio wave absorber for electromagnetic waves of 1 MHz to 100 MHz can be improved. (5) In the radio wave absorber of the above form, the Young's modulus may be 10 MPa or less. With such a configuration, the flexibility and pliability of the radio wave absorber can be increased, and therefore, by bending the radio wave absorber, it becomes easy to dispose the radio wave absorber on the surface of a member of any shape. (6) In the radio wave absorber of the above embodiment, the Young's modulus after treatment in the atmosphere at 100° C. for 1000 hours may be 11 MPa or less. With such a configuration, even when the radio wave absorber is placed in a device that becomes relatively hot and used for a long time, the flexibility of the radio wave absorber can be ensured, and the heat resistance and durability of the radio wave absorber can be improved. (7) According to another aspect of the present disclosure, there is provided a housing made of a conductive material for housing an electronic component module, the housing including the radio wave absorber according to any one of (1) to (6), the radio wave absorber being attached to an inner wall surface of the housing with the radio wave absorbing layer facing the inner wall surface of the housing. According to this embodiment of the housing, the radio wave absorber is attached to the inner wall surface of the housing, thereby suppressing the influence of electromagnetic waves on the electronic component module and ensuring insulation between the housing and the electronic component module. At this time, since the radio wave absorber is attached to the inner wall surface of the housing so that the radio wave absorbing layer faces the inner wall surface of the housing, the electrical resistance layer can suppress dielectric breakdown of the radio wave absorbing layer. (8) According to yet another embodiment of the present disclosure, there is provided a power converter including a power module having a semiconductor, a harness electrically connected to the power module, and a housing made of a conductive material that houses the power module and the harness. In this power converter, the housing includes the radio wave absorber according to any one of (1) to (6), and the radio wave absorber is attached to an inner wall surface of the housing with the electric wave absorbing layer facing the inner wall surface of the housing. According to the power converter of this embodiment, the electromagnetic wave absorber is attached to the inner wall surface of the housing, thereby suppressing the influence of electromagnetic waves on the power module and ensuring insulation between the housing and the power module. At this time, since the electromagnetic wave absorber is attached to the inner wall surface of the housing so that the electromagnetic wave absorbing layer faces the inner wall surface of the housing, the electrical resistance layer can suppress dielectric breakdown of the electromagnetic wave absorbing layer. The present disclosure may be realized in various forms other than those described above, for example, in the form of a radio wave absorbing sheet, a method for manufacturing a radio wave absorber, a method for preventing the emission or intrusion of electromagnetic waves in electronic devices, etc. [Brief description of the drawings]
[0006] [Figure 1] 1 is a schematic cross-sectional view illustrating a schematic configuration of a radio wave absorber according to a first embodiment. [Diagram 2] FIG. 4 is an explanatory diagram showing the state near the inner wall surface of a housing that houses high-voltage equipment. [Diagram 3] FIG. 11 is a schematic cross-sectional view illustrating a schematic configuration of a radio wave absorber according to a second embodiment. [Figure 4] FIG. 13 is an explanatory diagram showing the configuration of a radio wave absorber and the results of investigating its performance. [Diagram 5] FIG. 13 is an explanatory diagram showing evaluation results of radio wave absorbers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] A. First embodiment: 1 is a schematic cross-sectional view illustrating a schematic configuration of a radio wave absorber 10 according to a first embodiment of the present disclosure. The radio wave absorber 10 includes a radio wave absorbing layer 12 and an electric resistance layer 14 disposed on one surface of the radio wave absorbing layer 12.
[0008] The electromagnetic wave absorbing layer 12 includes a soft magnetic material and a resin. The resin included in the electromagnetic wave absorbing layer 12 is hereinafter also referred to as a "first resin." In the electromagnetic wave absorbing layer 12, the soft magnetic material is dispersed in the first resin in the form of powder particles.
[0009] The soft magnetic material is, for example, at least one of a soft magnetic alloy and a metal oxide. Examples of soft magnetic alloys include Fe-Si alloys, Fe-Si-Cr alloys, sendust (Fe-Si-Al alloys), and permalloy (Fe-Ni alloys). Examples of metal oxides include ferrites such as Ni-Zn ferrite (nickel zinc ferrite) and Mn-Zn ferrite (manganese zinc ferrite), and iron oxides such as magnetite and maghemite.
[0010] The soft magnetic material may be appropriately selected according to the frequency band of the electromagnetic waves to be absorbed by the radio wave absorber 10. Since the frequency band of the electromagnetic waves emitted from a general electronic device is kHz to MHz, a soft magnetic material that functions in a wide frequency band from kHz to MHz is preferable. The above-mentioned Ni-Zn ferrite, Mn-Zn ferrite, magnetite, Fe-Si alloy, Fe-Si-Cr alloy, sendust, permalloy, etc. are useful for electromagnetic waves in such a frequency band, and Mn-Zn ferrite is particularly preferable because it has a relatively high magnetic permeability in a frequency band ranging from kHz to MHz. Furthermore, when the radio wave absorber 10 is used in the vicinity of a high-voltage device, it is desirable that the soft magnetic material is a material with a higher electric resistance. From the viewpoint of high electric resistance, ferrites such as Ni-Zn ferrite and Mn-Zn ferrite are preferable, and Ni-Zn ferrite is particularly preferable. The amount of the soft magnetic material added to the radio wave absorbing layer 12 is preferably 40% by volume to 60% by volume from the viewpoint of increasing the real component μ' of the complex relative magnetic permeability in the radio wave absorber 10.
[0011] The first resin is preferably a resin having a relatively large electric resistance, and more preferably an insulating resin. In this way, even when the radio wave absorber 10 is used by being disposed in the vicinity of or in contact with an electronic device or a wiring connected to the electronic device, it is possible to suppress the dielectric breakdown of the radio wave absorber 10. The dielectric breakdown strength of the first resin is preferably equal to or greater than the dielectric breakdown strength of air, specifically, equal to or greater than 3 kV / mm. Examples of such resins include acrylic resin, butyral resin, epoxy resin, polyimide resin, and silicone resin, and silicone resin is particularly preferred from the viewpoints of heat resistance and flexibility.
[0012] The electrical resistance layer 14 is a layer for increasing the electrical resistance of the entire radio wave absorber 10, and comprises ceramic and resin. The ceramic contained in the electrical resistance layer 14 is also referred to as "high resistance ceramic" below. In the electrical resistance layer 14, the high resistance ceramic is dispersed in the second resin in the form of powder particles. The resin contained in the electrical resistance layer 14 is also referred to as "second resin" below.
[0013] In this embodiment, ceramics having a dielectric breakdown strength of 8 kV / mm or more are used as the high resistance ceramic. From the viewpoint of increasing the electrical resistance of the electrical resistance layer 14 and the entire radio wave absorber 10, it is desirable that the dielectric breakdown strength of the high resistance ceramic is 10 kV / mm or more. As such a high resistance ceramic, for example, alumina (Al2O3), zirconia (ZrO2), silicon nitride, aluminum nitride, mullite (aluminosilicate represented by 3Al2O3·2SiO2 to 2Al2O3·SiO2), etc. can be used. Since the high resistance ceramic is mixed into the second resin as a filling material, it is particularly preferable to use alumina, which is easy to control the particle size and shape. The amount of the high resistance ceramic added to the electrical resistance layer 14 is preferably 40% by volume to 60% by volume.
[0014] The second resin is preferably a resin having a relatively large electrical resistance, similar to the first resin, and more preferably an insulating resin. In this embodiment, the dielectric breakdown strength of the second resin is higher than the dielectric breakdown strength of air (3 kV / mm). The second resin may be the same resin as that described in the description of the first resin. The first resin and the second resin may be the same type of resin, or different types of resin. If the first resin and the second resin are the same type of resin, it is preferable because it is easier to ensure the adhesive strength between the radio wave absorbing layer 12 and the electrical resistance layer 14.
[0015] In the radio wave absorber 10, the dielectric breakdown strength of the entire radio wave absorber 10, which is the combination of the radio wave absorbing layer 12 and the electrical resistance layer 14, is desirably equal to or greater than the dielectric breakdown strength of air, and specifically, is desirably equal to or greater than 3 kV / mm. In this way, by making the dielectric breakdown strength of the radio wave absorber 10 equal to or greater than the dielectric breakdown strength of air, when the radio wave absorber 10 is used in the vicinity of high-voltage equipment, it is possible to suppress dielectric breakdown of the radio wave absorber 10 without providing an additional air layer between the high-voltage equipment and the radio wave absorber 10 to increase insulation.
[0016] Fig. 2 is an explanatory diagram showing the state near the inner wall surface of the housing 20 in an apparatus in which high-voltage equipment is stored inside the housing 20. Fig. 2 shows, as an example, an enlarged view of the area between the wiring 22 connected to the high-voltage equipment and the housing 20. Fig. 2(A) shows a case where no radio wave absorber is arranged, Fig. 2(B) shows a state where a radio wave absorber composed only of a radio wave absorbing layer 12 is arranged on the inner wall surface of the housing 20, and Fig. 2(C) shows a state where a radio wave absorber 10 including the radio wave absorbing layer 12 and an electric resistance layer 14 is arranged on the inner wall surface of the housing 20.
[0017] As shown in FIG. 2(A), the distance between the housing 20 and the wiring 22 may be set to a distance α so that insulation between the housing 20 and the wiring 22 can be ensured. In such a device, when the radio wave absorbing layer 12 is disposed on the inner wall surface of the housing 20 as shown in FIG. 2(B), the distance between the radio wave absorbing layer 12 and the wiring 22 becomes a distance β shorter than the distance α. In this case, if the dielectric breakdown strength of the radio wave absorbing layer 12 designed to obtain the desired radio wave absorption performance is insufficient, the distance between the radio wave absorbing layer 12 and the inner wall surface of the housing 20 becomes shorter than the distance α, and dielectric breakdown may occur in the radio wave absorbing layer 12. In contrast, as shown in FIG. 2(C), when a radio wave absorber 10 further including an electric resistance layer 14 is used, even if the distance between the radio wave absorber 10 and the wiring 22 becomes a distance γ shorter than the distance β, the dielectric breakdown strength of the entire radio wave absorber 10 is equal to or greater than the dielectric breakdown strength of air, so that insulation between the housing 20 and the wiring 22 can be ensured. That is, without changing the distance α between the inner wall surface of the housing 20 and the wiring 22, it is possible to ensure insulation between the housing 20 and the wiring 22 while suppressing an increase in size of the entire device.
[0018] The dielectric breakdown strength of the entire radio wave absorber 10 is affected by the dielectric breakdown strength, capacitance, and thickness of each of the radio wave absorbing layer 12 and the electrical resistance layer 14. The higher the dielectric breakdown strength of each layer, the higher the dielectric breakdown strength of the entire radio wave absorber 10. Also, the thicker the electrical resistance layer 14, which has a higher dielectric breakdown strength, the higher the dielectric breakdown strength of the entire radio wave absorber 10. The dielectric breakdown strength of each layer can be adjusted by the type and amount of filler used (soft magnetic material of the radio wave absorbing layer 12 and high resistance ceramic of the electrical resistance layer 14). The capacitance is affected by the relative dielectric constant, but when the same type of resin is used in each layer, for example, the capacitance of each layer is approximately the same. In this case, the dielectric breakdown strength and thickness of each layer are major factors that affect the dielectric breakdown strength of the entire radio wave absorber 10. In addition, defects such as voids (bubbles) and cracks that occur during the production of each layer also affect the dielectric breakdown strength. Therefore, when manufacturing the radio wave absorber 10, in order to suppress the effects of the above-mentioned defects, it is desirable to perform a degassing process on the material (paste) before forming each layer, and to perform a sufficient stirring process to suppress secondary aggregation of the filler.
[0019] The real component μ' of the complex relative magnetic permeability in the radio wave absorber 10 is desirably 3 or more in the range of 1 MHz to 100 MHz. In this way, the radio wave absorber 10 can function well as a radio wave absorber for electromagnetic waves in the above frequency band. The real component μ' of the complex relative magnetic permeability in the radio wave absorber 10 can be adjusted, for example, by the type and amount of the soft magnetic material contained in the radio wave absorbing layer 12. In addition, the thickness fraction of the radio wave absorbing layer 12 in the radio wave absorber 10 in which the radio wave absorbing layer 12 and the electric resistance layer 14 are laminated also affects the real component μ'. The larger the thickness fraction of the radio wave absorbing layer 12, the larger the real component μ' of the complex relative magnetic permeability in the radio wave absorber 10.
[0020] In order to make the real component μ' of the complex relative permeability equal to or greater than 3, it is desirable to use Mn-Zn ferrite as the soft magnetic material of the radio wave absorbing layer 12. Since Mn-Zn ferrite has a relatively high permeability in a frequency band ranging from kHz to MHz, using Mn-Zn ferrite as the soft magnetic material makes it easy to make the real component μ' of the complex relative permeability equal to or greater than 3 in the range from 1 MHz to 100 MHz.
[0021] Moreover, the Young's modulus of the radio wave absorber 10 is preferably 15 MPa or less, and more preferably 10 MPa or less. This ensures the flexibility of the radio wave absorber 10. By ensuring the flexibility of the radio wave absorber 10, it becomes easy to attach the radio wave absorber 10 along a shape different from a flat surface. For example, when attaching the radio wave absorber 10 to at least a part of the inner wall surface of a housing that contains a device that emits electromagnetic waves or is affected by electromagnetic waves, even if the attachment portion is a curved surface, the radio wave absorber 10 can be easily attached. Moreover, the Young's modulus of the radio wave absorber 10 is preferably 0.5 MPa or more, and more preferably 1 MPa or more.
[0022] The Young's modulus of the radio wave absorber 10 can be adjusted by, for example, the type, molecular weight, or crosslink density of the first and second resins. For example, when the molecular weight of the resin is small, the crosslink density is likely to be high, and the Young's modulus is likely to be large. In particular, a resin with a high crosslink density such as an epoxy resin is likely to have a high Young's modulus. The Young's modulus of the radio wave absorber 10 can be adjusted by the type and content of the soft magnetic material in the radio wave absorbing layer 12, or the type and content of the high resistance ceramic in the electrical resistance layer 14. The lower the content of the filler in each layer, the lower the Young's modulus of the radio wave absorber 10 can be.
[0023] Furthermore, the Young's modulus of the radio wave absorber 10 after being treated in the atmosphere at 100° C. for 1000 hours is preferably 15 MPa or less, more preferably 11 MPa or less. This ensures the flexibility of the radio wave absorber 10 even when the radio wave absorber 10 is placed in a device that is relatively hot and used for a long time, and can improve the heat resistance and durability of the radio wave absorber. The Young's modulus of the radio wave absorber 10 after the above-mentioned heat treatment can be adjusted, for example, by the type of the first resin or the second resin, the crosslinking density, or the temperature at which the resin is cured. For example, assuming that the amount of functional groups is the same, the larger the molecular weight of the first resin or the second resin, the lower the crosslinking density is likely to be, and the smaller the Young's modulus after the heat treatment is likely to be. For example, when a silicone resin is used as the resin, the molecular weight of the main agent of the silicone resin is preferably 20,000 or more, more preferably 50,000 or more, and even more preferably 70,000 or more. Although epoxy resin, acrylic resin, and the like are cured at a relatively low temperature, when cured at a low temperature, the Young's modulus may increase and change significantly when the resin is subsequently placed in a high-temperature environment for a long period of time. The Young's modulus of the wave absorber 10 after the above-mentioned heat treatment is preferably 0.5 MPa or more, and more preferably 1 MPa or more.
[0024] An adhesive layer may be provided on one surface of the radio wave absorber 10 (a surface different from the surface of the radio wave absorbing layer 12 that contacts the electrical resistance layer 14, and the surface shown as the adhesive surface 13 in FIG. 1). This adhesive layer is a structure for attaching the radio wave absorber 10 to a location where the radio wave absorber 10 is to be disposed, such as the inner wall surface of a housing 20 that houses a high-voltage device shown in FIG. 2. The adhesive layer can be formed by applying an adhesive or pressure-sensitive adhesive such as a silicone resin, an acrylic resin, or an epoxy resin. Note that when the radio wave absorber 10 is disposed by being mechanically fixed using, for example, a fastener, instead of being attached, the above-mentioned adhesive layer may not be provided.
[0025] In addition, when the radio wave absorber 10 is arranged by pasting, no adhesive layer is provided, e.g. For example, an alkoxide such as a silane coupling agent may be added to the first resin constituting the radio wave absorbing layer 12, and the radio wave absorber 10 may be used as an adhesive sheet. In this case, after preparing the radio wave absorber 10 in a state in which a part of the first resin is cured, the radio wave absorber 10 can be bonded to the adherend by attaching the radio wave absorber 10 to a desired location (an adherend such as an inner wall surface of a housing) and thermally curing the radio wave absorber 10. The silane coupling agent to be added to the first resin is not particularly limited, and can be appropriately selected from conventionally known silane coupling agents such as those having any one of a vinyl group, an epoxy group, a methacryl group, an amino group, a mercapto group, and an isocyanate group as an organic reactive group.
[0026] The radio wave absorber 10 of the present embodiment configured as described above includes the radio wave absorbing layer 12 including a soft magnetic material and a first resin, and the electric resistance layer 14 including a high resistance ceramic and a second resin, which is disposed on one surface of the radio wave absorbing layer 12. Since the radio wave absorber 10 includes the electric resistance layer 14 including the high resistance ceramic, the voltage resistance performance of the radio wave absorber 10 can be improved. In this case, when the radio wave absorber 10 is disposed on the inner wall surface of a housing that contains a device that emits electromagnetic waves or is affected by electromagnetic waves, the electric resistance layer 14 ensures insulation, so that the space provided to enhance insulation between the radio wave absorber 10 and the device can be reduced. As a result, it is possible to suppress an increase in the size of the entire device including the device and the housing.
[0027] The effect of suppressing the increase in size of the device will be further explained below. As described above, the dielectric breakdown strength of the electric resistance layer 14 can be adjusted by the type and content of the high resistance ceramic. For example, when a high resistance ceramic having a dielectric breakdown strength of 10 kV / mm or more such as alumina is used, an electric resistance layer 14 having a dielectric breakdown strength of 70 kV / mm or more can be obtained. Assuming that such an electric resistance layer 14 is arranged on the inner wall surface of the housing 20 that houses the high voltage device to ensure voltage resistance performance, if the voltage resistance requirement determined according to the voltage used by the high voltage device is, for example, 1 kV, the thickness of the electric resistance layer 14 (having a dielectric breakdown strength of 70 kV / mm) required to realize a voltage resistance of 1 kV is about 0.015 mm. In contrast, when an insulating resin layer made of resin is disposed on the inner wall surface of the housing 20 as in the electromagnetic shielding film described in Patent Document 1, the dielectric breakdown strength of the resin layer is generally considered to be 10 to 20 kV / mm, so the thickness of the insulating resin layer required to realize a withstand voltage of 1 kV is 0.05 to 0.1 mm. In this way, by employing the electrical resistance layer 14 of this embodiment, the thickness of the insulating layer required to realize a desired withstand voltage can be significantly reduced, and an effect of suppressing the size of the device can be obtained. In consideration of the above-mentioned placement location, the thickness of the radio wave absorber 10 is preferably 2 mm or less.
[0028] An example of an apparatus including such a high-voltage device is a power conversion device such as a power control unit (PCU) mounted on a hybrid vehicle or an electric vehicle that runs using a motor to control power. The PCU generally includes a boost converter that boosts the battery voltage, a step-down converter that steps down the high voltage, and a three-phase inverter that converts direct current to alternating current and controls frequency before supplying power to the motor. The PCU generally includes a housing made of a conductive material such as aluminum. In such an apparatus, there is generally almost no space between the high-voltage device or wiring and the housing. Therefore, by applying the radio wave absorber 10 of this embodiment, the effect of suppressing the size of the apparatus from increasing can be significantly obtained. That is, even if the radio wave absorber 10 contacts the high-voltage device or wiring 22, it is possible to ensure insulation between the high-voltage device or wiring 22 and the housing 20.
[0029] In such a power converter, for example, when the inverter converts direct current into alternating current, electromagnetic noise with a frequency of several MHz to several hundred MHz is generated. The material may be appropriately selected according to the frequency band of the electromagnetic waves to be absorbed and attenuated, and Mn-Zn ferrite and soft magnetic alloys are suitable for absorbing the above-mentioned electromagnetic noise. Thus, even when using a soft magnetic material having a relatively low electrical resistance compared to Ni-Zn ferrite, by providing the electrical resistance layer 14, it is possible to ensure that the radio wave absorber 10 as a whole has an insulating property suitable for the above-mentioned power converter.
[0030] The device to which the radio wave absorber 10 of this embodiment is applied may be other than the above-mentioned PCU, and may be any of various power conversion devices including a power module having a semiconductor, a harness which is wiring electrically connected to the power module, and a housing which contains the power module and the harness and is made of a conductive material. An example of such other power conversion device is an SCU (Solar Charging Unit) which converts the voltage generated by a solar panel and sends it to a storage battery. In this case, the radio wave absorber 10 converts the voltage The radio wave absorber 10 may be attached to the inner wall surface of the housing 20 so that the radio wave absorbing layer 12 faces the inner wall surface of the housing 20. This makes it possible to suppress dielectric breakdown of the radio wave absorbing layer 12. The radio wave absorber 10 of this embodiment may also be used in an apparatus including equipment (electronic component modules operating at a relatively low voltage) different from the high voltage equipment described above, and for example, by arranging the radio wave absorber 10 on the inner wall surface of a housing that contains the equipment, the same effect as in the above embodiment can be obtained.
[0031] B. Second embodiment: 3 is a cross-sectional schematic diagram showing a schematic configuration of a radio wave absorber 130 of the second embodiment. The radio wave absorber 130 of the second embodiment further includes a reflective layer 116 on one surface (the surface on the radio wave absorbing layer 12 side in contact with an adherend) of the radio wave absorber 10 in addition to the radio wave absorber 10 similar to that of the first embodiment.
[0032] The reflective layer 116 is a layer that reflects electromagnetic waves that have passed through the radio wave absorber 10. The reflective layer 116 may be formed of any metal that can reflect electromagnetic waves, such as copper, nickel, iron, stainless steel, precious metals such as gold and silver, and aluminum. The reflective layer 116 may be formed, for example, by attaching a metal film that has been prepared in advance to one surface of the radio wave absorber 10. At this time, the reflective layer 116 and the radio wave absorber 10 may be attached to each other using an adhesive, or a silane coupling agent or the like may be added to the first resin that constitutes the radio wave absorbing layer 12 to make the radio wave absorber 10 into an adhesive sheet, and the reflective layer 116 and the radio wave absorber 10 may be joined together. In addition, when a metal that can form a plated film is used as the material of the reflective layer 116, the reflective layer 116 may be formed by performing plating treatment such as electrolytic plating or electroless plating on the surface of the radio wave absorber 10. When the radio wave absorber 10 of the second embodiment is disposed on a desired adherend, for example, the reflective layer 116 attached to the radio wave absorber 10 and the adherend may be fixed together using an adhesive.
[0033] With such a configuration, the same effect as that of the radio wave absorber 10 of the first embodiment can be obtained, and by providing the reflective layer 116 overlapping the radio wave absorber 10, it is possible to block electromagnetic waves that pass through the radio wave absorber 10. Therefore, even if a housing that contains a device that emits electromagnetic waves or is affected by electromagnetic waves is made of a material other than a material that reflects electromagnetic waves, such as metal, by using the radio wave absorber 130, it is possible to absorb electromagnetic waves with the radio wave absorber 10 and suppress leakage of the electromagnetic waves to the outside of the housing with the reflective layer 116.
[0034] C. Other embodiments: In the above-described embodiments, the radio wave absorber is formed in a sheet shape, but may be formed in a different shape, however, forming the radio wave absorber in a sheet shape makes it easier to arrange the radio wave absorber along the surface of an adherend of any shape. EXAMPLES
[0035] FIG. 4 is an explanatory diagram showing the results of investigating the configurations and performances of 13 types of radio wave absorbers, samples S1 to S13, produced. FIG. 5 is an explanatory diagram showing the results of evaluating the radio wave absorbers, samples S1 to S13. The configurations and manufacturing methods of each sample, and the results of evaluating the performances, are described below. The types of materials used and the mixing ratios of the materials are different for each sample. Samples S10 to S13 are comparative samples that do not satisfy the conditions related to the soft magnetic material and high resistance ceramic described in the embodiment. In each sample described below, the first resin constituting the radio wave absorbing layer and the second resin constituting the electric resistance layer are the same resin.
[0036] <Preparation of each sample> [Sample S1] A paste was prepared by adding 50% by volume of Mn-Zn ferrite (arithmetic mean particle size: about 1.5 μm), an acrylic dispersion material (molecular weight about 10,000), an antifoaming agent, and water as a dispersion solvent to an acrylic resin (molecular weight about 200,000), and wet mixing. After adjusting the viscosity of the obtained paste, it was spun by a doctor blade method to a thickness of 900 μm. The electromagnetic wave absorbing layer was obtained by forming the sample into a sheet shape and volatilizing the solvent at a temperature of 100° C. or less. In FIG. 4, for each sample including sample S1, the thickness of the sheet when formed into a sheet shape is indicated as “layer 12 thickness”.
[0037] Similarly, acrylic resin (molecular weight approximately 200,000) is mixed with 45% by volume of alumina (arithmetic mean particle size: approximately 10 μm), an acrylic dispersion material (molecular weight approximately 10,000), and an antifoaming material. Water was added as a dispersion solvent, and the mixture was wet mixed to prepare a paste. After adjusting the viscosity of the obtained paste, the paste was cut into a sheet having a thickness of 100 μm by a doctor blade method. The sheet was molded into a sheet shape, and the solvent was evaporated at a temperature of 100° C. or less to obtain an electrical resistance layer. In FIG. 4, for each sample including sample S1, the thickness of the sheet when molded into a sheet shape is indicated as “layer 14 thickness.”
[0038] The electromagnetic wave absorbing layer and the electrical resistance layer prepared as described above were laminated and integrated by thermocompression bonding at 100° C. to obtain the electromagnetic wave absorber of sample S1.
[0039] [Sample S2] Mn-Zn ferrite (arithmetic mean particle size: about 1.5μm) was added to the liquid epoxy resin so that the volume was 50%, and mixed with a mixer using a stirring blade and a three-roll mill to obtain a paste. After adding and mixing a curing agent, the obtained paste was formed into a sheet by the doctor blade method to a thickness of 900μm, and thermally cured at a temperature of 60℃ or less to obtain an electromagnetic wave absorbing layer.
[0040] Similarly, alumina (arithmetic mean particle size: about 10 μm) was added to liquid epoxy resin to make a paste of 45 volume % and mixed with a stirrer using a stirring blade and a three-roll mill. After adding and mixing a curing agent, the paste was formed into a sheet of 100 μm thickness by the doctor blade method and thermally cured at a temperature of 60°C or less to obtain an electrical resistance layer.
[0041] An epoxy adhesive was applied between the electromagnetic wave absorbing layer and the electrical resistance layer prepared as described above, and the two were laminated and integrated to obtain a electromagnetic wave absorber of sample S2.
[0042] [Sample S3] Silicone resin (molecular weight approximately 30,000) with vinyl groups as functional groups, 50% by volume Mn-Zn ferrite (arithmetic mean particle size: about 1.5 μm), a silane coupling agent, a crosslinking agent, and a metal catalyst were added, and mixed with a stirrer using a stirring blade and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape with a thickness of 900 μm by the doctor blade method, and heat-cured (semi-cured) at a temperature of 100°C or less to obtain an electromagnetic wave absorbing layer.
[0043] Similarly, 45% by volume of alumina (arithmetic mean particle size: about 10 μm), a silane coupling agent, a crosslinking agent, and a metal catalyst were added to a silicone resin (molecular weight about 30,000) having a vinyl group as a functional group, and mixed with a stirrer using a stirring blade and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet having a thickness of 100 μm by the doctor blade method, and thermally cured (semi-cured) at a temperature of 100°C or less to obtain an electrical resistance layer.
[0044] The electromagnetic wave absorbing layer and the electrical resistance layer prepared as described above were laminated and further heat-cured at 100° C. or higher to integrate them, thereby obtaining an electromagnetic wave absorber of sample S3.
[0045] [Sample S4] The electromagnetic wave absorbing layer was prepared using the paste prepared for the electromagnetic wave absorbing layer of sample S3. This paste was formed into a sheet having a thickness of 450 μm by a doctor blade method, and heat cured at a temperature of 100° C. or less to obtain an electromagnetic wave absorbing layer.
[0046] The electrical resistance layer was prepared using the paste prepared for the electrical resistance layer of sample S3. This paste was formed into a sheet having a thickness of 50 μm by a doctor blade method, and thermally cured at a temperature of 100° C. or less to obtain an electrical resistance layer.
[0047] The radio wave absorbing layer and the electrical resistance layer prepared as described above were laminated and further heat-cured at 100° C. or higher to integrate them, thereby obtaining a radio wave absorber of sample S4.
[0048] [Sample S5] 50% by volume of Mn-Zn ferrite (arithmetic mean particle size: about 1.5μm), silane coupling agent, crosslinking agent, and metal catalyst were added to silicone resin (molecular weight about 70000) having vinyl groups as functional groups, and mixed with a stirrer using a stirring blade and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape with a thickness of 450μm by the doctor blade method, and heat-cured (semi-cured) at a temperature of 100℃ or less to obtain an electromagnetic wave absorbing layer.
[0049] Similarly, 45% by volume of alumina (arithmetic mean particle size: about 10 μm), a silane coupling agent, a crosslinking agent, and a metal catalyst were added to a silicone resin (molecular weight about 70,000) having a vinyl group as a functional group, and mixed with a stirrer using a stirring blade and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet shape with a thickness of 50 μm by the doctor blade method, and thermally cured (semi-cured) at a temperature of 100°C or less to obtain an electrical resistance layer.
[0050] The electromagnetic wave absorbing layer and the electrical resistance layer prepared as described above were laminated and further heat-cured at 100° C. or higher to integrate them, thereby obtaining the electromagnetic wave absorber of sample S5.
[0051] [Sample S6] The electromagnetic wave absorbing layer was fabricated in the same manner as the electromagnetic wave absorbing layer of sample S3. The electrical resistance layer was fabricated by using 45 volume % aluminum nitride (arithmetic mean particle size: about 15 μm) instead of 45 volume % alumina (arithmetic mean particle size: about 10 μm) as the high resistance ceramic. The other parts were prepared in the same manner as the electric resistance layer of sample S3. The electromagnetic wave absorbing layer and the electric resistance layer prepared as described above were laminated and further heat-cured at 100°C or higher to be integrated, thereby obtaining the electromagnetic wave absorber of sample S6.
[0052] [Sample S7] The electromagnetic wave absorbing layer was fabricated in the same manner as the electromagnetic wave absorbing layer of sample S3. The electrical resistance layer was fabricated in the same manner as the electrical resistance layer of sample S3, except that 45 volume % zirconia (arithmetic mean particle size: about 2 μm) was used as the high resistance ceramic instead of 45 volume % alumina (arithmetic mean particle size: about 10 μm). The electromagnetic wave absorbing layer and the electrical resistance layer fabricated as described above were laminated, and further heat cured at 100° C. or higher to integrate them, thereby obtaining the electromagnetic wave absorber of sample S7.
[0053] [Sample S8] The electromagnetic wave absorbing layer was fabricated in the same manner as the electromagnetic wave absorbing layer of sample S5, except that 50% by volume of Ni-Zn ferrite (arithmetic mean particle diameter: about 1.5 μm) was used as the soft magnetic material instead of 50% by volume of Mn-Zn ferrite (arithmetic mean particle diameter: about 1.5 μm). The electric resistance layer was fabricated in the same manner as the electric resistance layer of sample S5. The electromagnetic wave absorbing layer and the electric resistance layer fabricated as described above were laminated, and further heat cured at 100° C. or higher to integrate them, thereby obtaining the electromagnetic wave absorber of sample S8.
[0054] [Sample S9] The electromagnetic wave absorbing layer was prepared in the same manner as the electromagnetic wave absorbing layer of sample S5, except that 50% by volume of Fe-Si-Cr alloy (arithmetic mean particle size: about 9 μm) was used as the soft magnetic material instead of 50% by volume of Mn-Zn ferrite (arithmetic mean particle size: about 1.5 μm), and the thickness when formed into a sheet was set to 900 μm instead of 450 μm. The electrical resistance layer was prepared in the same manner as the electrical resistance layer of sample S5, except that the thickness when formed into a sheet was set to 100 μm instead of 50 μm. The electromagnetic wave absorbing layer and the electrical resistance layer prepared as above were laminated, and further heat cured at 100° C. or higher to integrate them, thereby obtaining the electromagnetic wave absorber of sample S9.
[0055] [Sample S10] Sample S10 does not have a radio wave absorbing layer, but only has an electrical resistance layer. The electrical resistance layer was made using the paste made for the electrical resistance layer of sample S5. This paste was formed into a sheet shape with a thickness of 100 μm by a doctor blade method, and thermally cured at a temperature of 100° C. or less to obtain sample S10.
[0056] [Sample S11] Sample S11 does not have an electric resistance layer, but only has an electromagnetic wave absorbing layer. The paste prepared for the electromagnetic wave absorbing layer of sample S5 was used to prepare the electromagnetic wave absorbing layer. This paste was formed into a sheet having a thickness of 900 μm by a doctor blade method, and heat cured at a temperature of 100° C. or less to obtain sample S11.
[0057] [Sample S12] A silane coupling agent, a crosslinking agent, and a metal catalyst were added to a silicone resin (molecular weight approximately 30,000) having a vinyl group as a functional group, and the mixture was mixed with a stirrer using a stirring blade and a three-roll mill to obtain a paste. The obtained paste was formed into a sheet having a thickness of 100 μm by a doctor blade method, and heat-cured (semi-cured) at a temperature of 100° C. or less to obtain an electromagnetic wave absorbing layer. In other words, the electromagnetic wave absorbing layer of sample S12 does not contain a soft magnetic material.
[0058] The electric resistance layer was prepared in the same manner as the electric resistance layer of sample S3. The electromagnetic wave absorbing layer and the electric resistance layer prepared as described above were laminated and further heat-cured at 100°C or higher to be integrated, thereby obtaining the electromagnetic wave absorber of sample S12.
[0059] [Sample S13] The electromagnetic wave absorbing layer was prepared in the same manner as the electromagnetic wave absorbing layer of sample S3. The electrical resistance layer was prepared in the same manner as the electrical resistance layer of sample S3, except that it did not contain high resistance ceramic. The electromagnetic wave absorbing layer and the electrical resistance layer prepared as described above were laminated and further heat cured at 100°C or higher to be integrated, thereby obtaining the electromagnetic wave absorber of sample S9.
[0060] <Measurement of dielectric breakdown strength> The dielectric breakdown strength was measured according to JIS C 2110-1:2016. For the measurement, each sample was cut into a rectangular shape of 100 mm x 100 mm. Samples with a thickness of 1 mm were measured as is to obtain the dielectric breakdown strength value. For samples with different thicknesses, the dielectric breakdown voltage was measured and then the dielectric breakdown strength per mm of thickness was calculated.
[0061] <Derivation of complex relative permeability> The real component μ' of the complex relative permeability was measured using an E4991B impedance analyzer (Keysight Technologies). For the measurement, each sample was cut into a toroidal shape with an outer diameter of 20 mm and an inner diameter of 10 mm. The real component of the complex relative permeability was read from the region where the value of μ' was constant.
[0062] <Measurement of Young's modulus> The Young's modulus was measured at room temperature using a tensile tester (Shimadzu Autograph (AG-IS)). Each sample was cut into a rectangular test piece with a width of 1 cm and a length of 7 cm, and a tensile test was performed on the middle part with a length of 3 cm while holding the test piece with a jig at a position 2 cm from both ends. The Young's modulus was obtained from the SS curve (stress-strain curve). Specifically, the change in the sample length and the load was measured over time while pulling each test piece until it broke. The tensile stress was calculated by dividing the measured load by the cross-sectional area of the test piece before the tensile test. The Young's modulus was calculated as the slope in the elastic deformation region in a graph (stress-strain curve) with the strain calculated by the following formula (1) on the horizontal axis and the tensile stress on the vertical axis.
[0063] Strain (%) = [sample length during tension – original sample length] / original sample length (1)
[0064] <Heat resistance test> Each sample was placed in a dryer at 100° C. in air and subjected to a continuous heat resistance test for 1000 hours. After the heat resistance test, the Young's modulus of each sample was measured by the same method as in the "Measurement of Young's modulus" described above.
[0065] <Evaluation method> As shown in FIG. 5, each item was evaluated by comparing it with the reference value. The "MHz band performance" is an evaluation item related to the suitability of the sample as an electromagnetic wave absorber for the MHz band. In each sample, if the electromagnetic wave absorbing layer contains Mn-Zn ferrite as a soft magnetic material, it is marked as "○", and if it does not contain Mn-Zn ferrite, it is marked as "×". In the "dielectric breakdown strength", if the dielectric breakdown strength of each sample is 3 kV / mm or more, it is marked as "○", and if it is less than 3 kV / mm, it is marked as "×". In the "μ'" category, if the real component μ' of the complex relative permeability in the range of 1 MHz to 100 MHz of each sample is 3 or more, it is marked as "○", and if it is less than 3, it is marked as "×". In the "Young's modulus", if the Young's modulus of each sample is 10 MPa or less, it is marked as "○", and if it exceeds 10 MPa, it is marked as "×". In the "Young's modulus after heat resistance", if the Young's modulus of each sample after the heat resistance test is 11M If it was less than 11 MPa, it was marked as "○", and if it was more than 11 MPa, it was marked as "×".
[0066] Fig. 5 further shows the result of the overall evaluation. The "overall evaluation" was marked as "X" when at least one of the evaluation items corresponding to the basic performance related to the effect achieved by the radio wave absorber of the present disclosure, i.e., "dielectric breakdown strength" and "μ'", was marked as "X". In addition, when the overall evaluation was other than "X", and there was no evaluation item marked as "X" among the remaining evaluation items, it was marked as "◎", when there was one evaluation item marked as "X", it was marked as "○", and when there were two or more evaluation items marked as "X", it was marked as "△".
[0067] <Evaluation Results> As shown in FIG. 5, it was confirmed that the "wave absorbing layer 12 including a soft magnetic material and a resin" and the "electrical resistance layer 14 disposed on one surface of the wave absorbing layer 12 and including a ceramic having a dielectric breakdown strength of 8 kV / mm or more and a resin having a dielectric breakdown strength higher than that of air" can improve insulation while ensuring wave absorbing ability for electromagnetic waves in the range of 1 MHz to 100 MHz (comparison between samples S1 to S9 and samples S10 to S13). It was also confirmed that the use of silicone resin as the resin constituting the wave absorber provides an effect of improving the flexibility of the wave absorber, and that such an effect is sustained even after long-term treatment under high-temperature conditions (comparison between sample S3 and samples S1 and 2, for example). It was also confirmed that the greater the molecular weight of the resin constituting the wave absorber, the smaller the Young's modulus and the Young's modulus after a heat resistance test become, and the greater the flexibility and heat resistance of the wave absorber become (comparison between samples S4 and S5, for example).
[0068] The present disclosure is not limited to the above-mentioned embodiments, etc., and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features in the embodiments corresponding to the technical features in each form described in the Summary of the Invention column can be appropriately replaced or combined in order to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted.
[0069] The present disclosure can also be realized in the following forms. [Application example 1] A radio wave absorber that absorbs electromagnetic waves, a radio wave absorbing layer including a soft magnetic material and a resin; an electrical resistance layer disposed on one surface of the radio wave absorbing layer, the electrical resistance layer comprising a ceramic having a dielectric breakdown strength of 8 kV / mm or more and a resin having a dielectric breakdown strength higher than the dielectric breakdown strength of air; A radio wave absorber comprising: [Application example 2] The radio wave absorber according to Application Example 1, Characterized by a dielectric breakdown strength of 3 kV / mm or more Radio wave absorber. [Application example 3] The radio wave absorber according to Application Example 1 or 2, The real component of the complex relative permeability is 3 or more in the range of 1 MHz to 100 MHz. Radio wave absorber. [Application example 4] The radio wave absorber according to any one of Application Examples 1 to 3, The soft magnetic material is manganese zinc ferrite. Radio wave absorber. [Application example 5] The radio wave absorber according to any one of Application Examples 1 to 4, The Young's modulus is 10 MPa or less. Radio wave absorber. [Application Example 6] The radio wave absorber according to any one of Application Examples 1 to 5, The Young's modulus after treatment in air at 100°C for 1000 hours is 11 MPa or less. Radio wave absorber. [Application Example 7] A housing made of a conductive material for housing an electronic component module, A radio wave absorber according to any one of Application Examples 1 to 6, The radio wave absorber is attached to the inner wall surface of the housing in a direction facing the inner wall surface of the housing. Housing. [Application Example 8] A power conversion device comprising: a power module having a semiconductor; a harness electrically connected to the power module; and a housing that contains the power module and the harness and is made of a conductive material, The housing includes the radio wave absorber according to any one of Application Examples 1 to 6. The radio wave absorber is attached to the inner wall surface of the housing in a direction facing the inner wall surface of the housing. Power conversion equipment. [Explanation of symbols]
[0070] 10,130…Radio wave absorber 12...Electromagnetic wave absorbing layer 13...Adhesive surface 14...Electrical resistance layer 20…Housing 22…Wiring 116...Reflection layer
Claims
1. A radio wave absorber that absorbs electromagnetic waves, an electromagnetic wave absorbing layer including a soft magnetic material and a first resin, the soft magnetic material being dispersed in the first resin; an electrical resistance layer disposed on one surface of the electromagnetic wave absorbing layer, the electrical resistance layer comprising: a ceramic having a dielectric breakdown strength of 8 kV / mm or more; and a second resin having a dielectric breakdown strength higher than the dielectric breakdown strength of air, the ceramic being dispersed in the second resin; A radio wave absorber comprising:
2. 2. The radio wave absorber according to claim 1, The dielectric breakdown strength is 3 kV / mm or more. Radio wave absorber.
3. 2. The radio wave absorber according to claim 1, The real component of the complex relative permeability is 3 or more in the range of 1 MHz to 100 MHz. Radio wave absorber.
4. 2. The radio wave absorber according to claim 1, The soft magnetic material is manganese zinc ferrite. Radio wave absorber.
5. 2. The radio wave absorber according to claim 1, The Young's modulus is 10 MPa or less. Radio wave absorber.
6. A radio wave absorber that absorbs electromagnetic waves, a radio wave absorbing layer including a soft magnetic material and a resin; an electrical resistance layer disposed on one surface of the radio wave absorbing layer, the electrical resistance layer comprising a ceramic having a dielectric breakdown strength of 8 kV / mm or more and a resin having a dielectric breakdown strength higher than the dielectric breakdown strength of air; Equipped with The Young's modulus is 10 MPa or less. Radio wave absorber.
7. A housing made of a conductive material for housing an electronic component module, A radio wave absorber according to any one of claims 1 to 6, The radio wave absorber is characterized in that the radio wave absorbing layer is attached to the inner wall surface of the housing in a direction facing the inner wall surface of the housing. Housing.
8. A power conversion device comprising: a power module having a semiconductor; a harness electrically connected to the power module; and a housing that contains the power module and the harness and is made of a conductive material, The housing includes the radio wave absorber according to any one of claims 1 to 6, The radio wave absorber is characterized in that the radio wave absorbing layer is attached to the inner wall surface of the housing in a direction facing the inner wall surface of the housing. Power conversion equipment.
Citation Information
Patent Citations
Radio wave absorber
JP2002158484A
Resin composition and phase change type heat-conductive member
JP2005187567A
Electromagnetic wave shield film
JP2018088510A
Electromagnetic wave absorber and electromagnetic wave absorber equipped molded article