Electromagnetic Shielding Materials
The flexible electromagnetic shielding material with a skin layer and protective layer improves shielding performance and flexibility by forming the metal layer on the skin layer and using a protective layer to prevent cracking.
Patent Information
- Application Number
- JP2023044401
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2038-10-30
AI Technical Summary
Existing electromagnetic shielding materials require improvement in shielding performance and are prone to cracking and deterioration when bent or deformed.
A flexible electromagnetic shielding material comprising a porous sheet-like base material with a skin layer and a metal sprayed layer, covered by a protective layer of hot melt resin, where the metal sprayed layer is formed on the skin layer to ensure uniform thickness and prevent cracking.
The configuration enhances shielding performance and flexibility by preventing metal penetration into the base material and covering the metal layer with a protective layer to suppress cracking and deterioration.
Smart Images

Figure 0007577778000001 
Figure 0007577778000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a flexible electromagnetic wave shielding material. [Background technology]
[0002] Patent Document 1 discloses an electromagnetic wave shielding material having a metal sprayed layer formed by spraying a metal onto the surface of a nonwoven fabric sheet. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 5-347493 A (paragraph
[0016] , Figure 1) Summary of the Invention [Problem to be solved by the invention]
[0004] There is a demand for improved shielding performance for the electromagnetic wave shielding material of Patent Document 1. [Means for solving the problem]
[0005] A first aspect of the invention made to solve the above problems is an electromagnetic wave shielding material comprising a flexible sheet-like substrate made of a porous body, and a metal sprayed layer formed by spraying a metal onto the surface of the sheet-like substrate, wherein a skin layer is formed on a surface portion of the sheet-like substrate, and the metal sprayed layer is formed on the skin layer.
[0006] A second aspect of the invention is the electromagnetic shielding material according to the first aspect, wherein the sheet-like substrate is a foamed sheet having a skin layer as the surface layer.
[0007] A third aspect of the invention is the electromagnetic shielding material according to the second aspect, which is composed of a foam of a resin selected from the group consisting of polyolefin resins, polyurethane resins, acrylic resins, and blends thereof.
[0008] In a fourth aspect of the invention, the metal sprayed layer has a coating weight of 90 g / m 2 The electromagnetic shielding material according to any one of the first to third aspects is as described above.
[0009] A fifth aspect of the invention is the electromagnetic shielding material according to any one of the first to fourth aspects, further comprising a protective layer made of a hot melt resin and covering the metal sprayed layer.
[0010] In a sixth aspect of the invention, the metal sprayed layer has a basis weight of 280 g / m 2 The electromagnetic wave shielding material according to a fifth aspect is as follows. Effect of the Invention
[0011] In the first aspect of the invention, a skin layer is formed on the surface layer portion of the sheet-like substrate on the side where the metal sprayed layer is formed, and a metal sprayed layer is formed on the skin layer. This skin layer has low air permeability or has lower air permeability than the inner layer portion of the sheet-like substrate. Here, when a metal sprayed layer is formed on a porous body, the metal sprayed layer may become thin due to pores in the porous body, or a region where no metal is present may occur in the metal sprayed layer, resulting in an uneven thickness of the metal sprayed layer. However, in the configuration of the first aspect of the invention, the metal sprayed on the sheet-like substrate is prevented from penetrating into the inside of the sheet-like substrate, and the reduction in the basis weight of the metal sprayed layer, which occurs when a metal sprayed layer is formed on a porous body, is suppressed, and the thickness of the metal sprayed layer is made uniform. This improves the shielding performance of the electromagnetic wave shielding material. However, when a metal sprayed layer is formed on the skin layer, it is considered that when the electromagnetic wave shielding material is bent and deformed, cracks may occur in the metal sprayed layer, causing damage to the electromagnetic wave shielding material. Therefore, by configuring the metal sprayed layer to be covered with a protective layer made of hot melt resin (fifth aspect of the invention), it is possible to prevent parts of the metal sprayed layer from falling off and to prevent cracks from occurring in the metal sprayed layer when the electromagnetic shielding material is bent and deformed, thereby suppressing deterioration of the electromagnetic shielding material.
[0012] The sheet-like substrate may be a nonwoven fabric sheet or a foamed sheet with a resin film attached as a facing material, or a foamed sheet having a skin layer on at least one of the front and back surfaces (a second aspect of the invention). In the latter case, if the foamed sheet is made of a foamed resin selected from the group consisting of polyolefin resins, polyurethane resins, acrylic resins, and blends thereof, the metal spray layer can be easily formed (a third aspect of the invention).
[0013] The weight of the metal sprayed layer is 90g / m 2 It is preferable that the weight per unit area is 90 g / m or more (fourth aspect of the invention). 2 If the thickness is less than 280g / m, the shielding performance will be reduced. If the metal sprayed layer is covered with a protective layer, the weight of the metal sprayed layer is 280g / m 2 It is preferable that the weight per unit area is 280 g / m or less (sixth aspect of the invention). 2 If the content is greater than this, the flexibility of the electromagnetic shielding material is impaired, and cracks are more likely to occur in the metal spray layer when the material is bent. [Brief description of the drawings]
[0014] [Figure 1] (A) Cross-sectional view of electromagnetic wave shielding material, (B) Enlarged cross-sectional view of the metal sprayed layer [Diagram 2] Data table showing the results of the confirmatory experiment DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As shown in FIG. 1(A), an electromagnetic shielding material 10 of this embodiment is formed by laminating a flexible and pliable sheet-like substrate 11, a metal sprayed layer 21, and a protective layer 31.
[0016] The sheet-like substrate 11 is made of a porous material. A skin layer 12 is formed on at least one of the surface layers of the front and back sides of the sheet-like substrate 11. The skin layer 12 has low air permeability or has a higher density than the inner layer portion 13 of the sheet-like substrate 11, resulting in low air permeability. Here, the skin layer 12 has low air permeability when the air permeability of the skin layer 12 measured using a Frazier type air permeability tester in accordance with the JIS L 1096A method is 80 ml / (cm 2 / s). The air permeability of the epidermis layer 12 is less than 2 ml / (cm 2 / s) or more 50ml / (cm 2 / s) or less.
[0017] Specifically, the sheet-like substrate 11 is made of a foamed sheet, and the surface layer 12 is made of a skin layer formed on the surface of the foamed sheet. The resin constituting the foamed sheet is, for example, a polyolefin resin, a polyurethane resin, an acrylic resin, or a blend of these. When the sheet-like substrate 11 is made of a foamed sheet having a low-air-permeability surface layer 12, the foamed sheet includes a foamed sheet with a semi-open cell structure. Here, the "semi-open cell structure" means a structure in which the cells have small pores, unlike closed cells, and in which the pores between adjacent cells are smaller than in an open cell structure, and specifically, an air permeability of 2 ml / (cm) or less according to the Frazier type method of JIS L 1096A method. 2 / s) or more 80ml / (cm 2 / s).
[0018] The metal sprayed layer 21 is formed by spraying a metal onto the surface of the sheet-like substrate 11. From the viewpoint of the shielding performance of the electromagnetic wave shielding material 10, the weight of the metal sprayed layer 21 is set to 90 g / m 2 From the viewpoint of the flexibility of the electromagnetic shielding material 10, it is preferable that the thickness is 280 g / m or more. 2 It is preferable that:
[0019] In metal spraying, a large number of metal particles 22 are collided with the surface of the sheet-like substrate 11, and the metal sprayed layer 21 is formed by accumulating the flattened metal particles 22 (see FIG. 1(B)). The types of metals used in metal spraying include, for example, zinc, aluminum, copper, and alloys of these metals. As metal spraying, flame spraying using combustion gas as a heat source, high-velocity flame spraying, detonation spraying, arc spraying using electricity as a heat source, plasma spraying, RF plasma spraying, wire explosion spraying, and the like can be used. Among these, arc spraying is preferred in that the formation speed of the metal sprayed layer 21 is high and the basis weight of the metal sprayed layer 21 can be precisely controlled.
[0020] The protective layer 31 is made of a hot melt resin. Examples of the hot melt resin constituting the protective layer 31 include thermoplastic polyurethane elastomer (TPU), ethylene-vinyl acetate copolymer (EVA), and a blend of polyethylene and ethylene-acrylic acid copolymer (PE / EAA). The thickness of the protective layer 31 does not affect the shielding performance of the metal spray layer 21, but from the viewpoint of the flexibility of the electromagnetic wave shielding material 10, the thickness is preferably 80 μm or less, and more preferably 35 μm or less.
[0021] 1(B), a part of the hot melt resin constituting the protective layer 31 penetrates into the metal sprayed layer 21 and enters into the gaps between the metal particles 22 in the surface layer portion of the metal sprayed layer 21 on the side opposite to the sheet-like substrate 11. This prevents the metal particles 22 from peeling off and the occurrence of cracks between the metal particles 22 when the electromagnetic wave shielding material 10 is bent and deformed. The protective layer 31 may be formed, for example, by overlapping a hot melt film on the metal sprayed layer 21 and heat-pressing the film, or by applying a hot melt resin to the metal sprayed layer 21.
[0022] As described above, in the electromagnetic shielding material 10 of the present embodiment, the skin layer 12 is formed on the surface layer of the sheet-like substrate 11, and the skin layer 12 has low air permeability or has lower air permeability than the inner layer portion 13 of the sheet-like substrate 11, and the metal sprayed layer 21 is formed on the skin layer 12, so that the metal particles 22 sprayed on the sheet-like substrate 11 are prevented from penetrating into the inside of the sheet-like substrate 11, and the reduction in the basis weight of the metal sprayed layer 21 is prevented more than when the metal sprayed layer 21 is formed on a porous body, and the thickness of the metal sprayed layer 21 is made uniform. As a result, the shielding performance of the electromagnetic shielding material 10 is improved.
[0023] In addition, since the metal sprayed layer 21 is covered with a protective layer 31 made of hot melt resin, it is possible to prevent parts of the metal sprayed layer 21 from falling off and to prevent cracks from occurring in the metal sprayed layer 21 when the electromagnetic wave shielding material 10 is bent and deformed, thereby suppressing deterioration of the electromagnetic wave shielding material 10.
[0024] [Confirmatory experiment] 1. Experimental Example The structure of the electromagnetic shielding material 10 of the above embodiment was modified as necessary to create Experimental Examples 1 to 12 and Comparative Experimental Examples 1 and 2 shown in Fig. 2, and an evaluation experiment was conducted on the shielding properties (electric field shielding properties and magnetic field shielding properties) and flexibility for each of the Experimental Examples. In Experimental Examples 1 to 12, a soft polyurethane foam sheet with a skin layer (specifically, PureCell UC 150PR (manufactured by Inoac Corporation, thickness 1.0 mm, air permeability 10 ml / (cm 2 In Experimental Examples 1 to 11, PE / EAA (manufactured by Enshu Chemical Industry Co., Ltd.) was used as the hot melt film, and in Experimental Example 12, no hot melt film was used. In Comparative Experimental Example 1, a nonwoven fabric (specifically, a polypropylene spunbond nonwoven fabric (manufactured by Maeda Kosen Co., Ltd., basis weight 50 g / m)) was used as the sheet-like substrate. 2 , breathability 175ml / (cm 2 / s))) was used. In Comparative Experimental Example 2, an aluminum sheet (thickness 40 μm) was used as the electromagnetic wave shielding material. The measured value of the air permeability was based on the Frazier type method of JIS L 1096A method.
[0025] 2. Evaluation of shielding effectiveness For Experimental Examples 1 to 12 and Comparative Experimental Example 1, a metal sprayed layer 21 was formed on the skin layer 12 of the sheet-like substrate 11 by metal spraying, and the resulting specimen was cut into a test piece of 120 mm x 120 mm. Then, for Experimental Examples 1 to 11, the outer periphery of the test piece (specifically, within a range of 10 mm from the outer edge) was masked, and a hot melt film was laminated and heated to produce a test piece on which a protective layer 31 of 100 mm x 100 mm was laminated. For Comparative Experimental Example 2, an aluminum sheet was cut into a test piece of 120 mm x 120 mm. The electromagnetic shielding effects (electric shielding effect and magnetic field shielding effect) of the test pieces of Experimental Examples 1 to 12 and Comparative Experimental Examples 1 and 2 were measured in accordance with the KEC method in the near electric field range of 10 MHz to 1 GHz. Figure 2 shows the values and evaluations of the electric field shielding effect and magnetic field shielding effect at 100 MHz. The evaluation of each shielding effect was as follows: if the shielding effect value was 40 dB or more, it was considered good ("○"), if it was 30 dB or more and less than 40 dB, it was considered fair ("△"), and if it was less than 30 dB, it was considered poor ("×"). The coating weight (g / m2) of the sprayed metal was also measured. 2 ) was calculated from the change in weight before and after thermal spraying.
[0026] 3. Evaluation of flexibility In Experimental Examples 1 to 11, a metal sprayed layer 21 was formed on a sheet-like substrate 11 by metal spraying, and then a hot melt film was laminated and heated to produce a laminate in which a protective layer 31 was laminated. The laminate was then cut to produce test pieces of 120 mm x 20 mm. In Experimental Example 12 and Comparative Experimental Example 1, a metal sprayed layer 21 was formed on a sheet-like substrate 11 by metal spraying, and the resultant was cut to produce test pieces of 120 mm x 20 mm. In Comparative Experimental Example 2, an aluminum sheet was cut to produce test pieces of 120 mm x 20 mm. For Experimental Examples 1 to 12 and Comparative Experimental Examples 1 and 2, one end (10 mm) in the longitudinal direction of the test piece was fixed, and then the other end (10 mm) was gripped and moved toward one end until the distance from the other end became 50 mm, and then returned to the original position. This extension and contraction motion was repeated 20 times. After these 20 extension and contraction motions, those without cracks or breaks in the metal sprayed layer 21 (see FIG. 1) were rated as good ("◯"), and those with cracks or breaks were rated as poor ("X").
[0027] 4. Experimental Results FIG. 2 shows the experimental results of Experimental Examples 1 to 12. Focusing on the electric field shielding effect, it is greater than 40 dB in all of Experimental Examples 1 to 12. On the other hand, focusing on the magnetic field shielding effect, it is greater than 40 dB in Experimental Examples 3 to 12, but less than 40 dB in Experimental Examples 1 and 2. In both the electric field shielding effect and the magnetic field shielding effect, the shielding effect increases as the basis weight of the metal sprayed layer 21 increases. And when the basis weight of the metal sprayed layer is 90 g / m 2 If it is equal to or greater than this, it is understood that the magnetic field shielding effect is good ("◯").
[0028] Furthermore, for example, a comparison between Experimental Example 3 and Experimental Example 4 reveals that the thickness of protective layer 31 does not affect either the electrolytic shielding effect or the magnetic field shielding effect. Note that Experimental Example 12, which does not include protective layer 31, also exhibits the same electric field shielding effect and magnetic field shielding effect as Experimental Examples 3 and 4, which have the same basis weight of metal sprayed layer 21. This shows that even a configuration not including protective layer 31 exhibits excellent electric field shielding effect and magnetic field shielding effect.
[0029] Comparing Experimental Examples 5 to 7 and Comparative Experimental Example 1, which have the same basis weight of the metal sprayed layer 21, it is found that the magnetic field shielding effect is better when a soft polyurethane foam sheet with a skin layer is used as the sheet-like substrate than when a nonwoven fabric is used as the sheet-like substrate. In Comparative Experimental Example 2, the electric field shielding effect is greater than 40 dB, but the magnetic field shielding effect is less than 40 dB. In addition, comparing Example 12 and Comparative Experimental Example 1, which have a smaller basis weight of the metal sprayed layer 21, it is found that the magnetic field shielding effect is better when a soft polyurethane foam sheet with a skin layer is used as the sheet-like substrate 11 than when a nonwoven fabric is used as the sheet-like substrate 11. From the above, it is found that the soft polyurethane foam sheet with a skin layer on which a metal sprayed layer is formed has excellent magnetic field shielding properties.
[0030] Next, focusing on the flexibility, the flexibility was good ("◯") in Experimental Examples 1 to 9, and was poor ("×") in Experimental Examples 10 and 11. From this, it can be seen that when a soft polyurethane foam sheet with a skin layer was used as the sheet-like substrate, the weight of the metal sprayed layer 21 was 280 g / m 2 It can be seen that when the weight of the metal sprayed layer 21 exceeds 280 g / m, cracks or breaks occur in the metal sprayed layer 21. In addition, in the experimental example 12, the bending property is poor ("x"), so that the weight of the metal sprayed layer 21 is 280 g / m 2 It can be seen that even if the temperature is below this level, if protective layer 31 is not provided, cracks or breaks will occur in metal sprayed layer 21.
[0031] It should be noted that Experimental Examples 1 to 12 correspond to "Examples", and Comparative Experimental Examples 1 and 2 correspond to "Comparative Examples".
[0032] [Other embodiments] (1) The sheet-like substrate 11 may be formed by melting and solidifying the surface of a foamed sheet having an open-cell structure.
[0033] (2) The sheet-like substrate 11 may have a structure in which a surface material having a semi-open cell structure is laminated to a foamed sheet having an open cell structure. In this case, the foamed sheet constitutes the inner layer 13, and the surface material constitutes the skin layer 12.
[0034] (3) The protective layer 31 does not necessarily cover the entirety of the metal sprayed layer 21, but may cover at least a portion of the metal sprayed layer 21.
[0035] (4) Skin layers 12 may be formed on both the front and back surfaces of the sheet-like substrate 11 .
[0036] (5) The electromagnetic shielding material 10 may have a structure that does not include the protective layer 31. Even with this structure, as shown by the results of the confirmatory experiment, a good electric field shielding effect and a good magnetic field shielding effect can be achieved. [Explanation of symbols]
[0037] 10 Electromagnetic shielding materials 11 Sheet-shaped substrate 12 Epidermal layer 21 Metal sprayed layer 31 Protective layer
Claims
1. The porous sheet-like substrate and the metal sprayed layer formed by spraying a metal on the surface of the sheet-like substrate, a surface layer is formed on a surface layer portion of the sheet-like substrate, and the metal spray layer is formed on the surface layer, the air permeability of the surface layer measured using a Frazier type air permeability tester in accordance with JIS L 1096A method is less than 80 ml / (cm 2 / s); An electromagnetic wave shielding material having a magnetic field shielding effect of 30 dB or more in the 100 MHz frequency band, in compliance with the KEC method.
2. 2. The electromagnetic wave shielding material according to claim 1, which has an electric field shielding effect of 30 dB or more in a frequency band of 100 MHz according to the KEC method.
3. 3. The electromagnetic shielding material according to claim 1, further comprising a protective layer made of a hot melt resin and covering the metal sprayed layer.
Citation Information
Patent Citations
Electromagnetic wave shielding sheet for electronic device
JP1983106899A
Preparation of metal composite resin molded article
JP1987299312A
Electromagnetic shielding material and molding method therefor
JP1993347493A
Highly incombustible gasket for shielding electromagnetic wave and manufacturing method therefor
JP2001111285A
Flame-retardant electrically-conductive material and method for manufacturing it
JP2003175565A