Method for producing transferable hard-coated film, transferable hard-coated film, and hard-coated laminate
The hard coat film composition with controlled hydroxyl value and isocyanate curing agent balances flexibility and blocking resistance, improving scratch resistance and manufacturing efficiency in hard coat films for transfer.
Patent Information
- Application Number
- JP2019068957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-03-29
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-03-29
AI Technical Summary
Existing hard coat films for transfer face a trade-off between flexibility and blocking resistance, particularly in after-cure type transfers, making it difficult to optimize both properties simultaneously.
A hard coat film composition with a hydroxyl value above a certain level before coating, adjusted by the amount of isocyanate curing agent, is used to form a hard coat layer with a hydroxyl value of 150 mgKOH/g or less after coating, achieving a balanced flexibility and blocking resistance.
The film achieves both flexibility and blocking resistance at a good level before final curing, enhancing scratch resistance and manufacturing efficiency in roll-to-roll processes.
Smart Images

Figure 0007577916000002 
Figure 0007577916000003 
Figure 0007577916000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a hard-coated film for transfer, a hard-coated film for transfer, and a hard-coated laminate. [Background technology]
[0002] Conventionally, a transfer hard coat film has been used to form a hard coat layer on a resin molded product. As an example of the transfer hard coat film, a decorative sheet in which a base layer, an adhesive layer, and a hard coat layer made of a curable resin are laminated in this order has been disclosed (see Patent Document 1).
[0003] This hard coat film for transfer is required to have sufficient hardness after curing in order to impart sufficient scratch resistance to a molded article with a hard coat layer, but on the other hand, the hard coat film for transfer is also required to have a certain degree of flexibility before the final curing stage in order to enable transfer to molded article substrates of various shapes.
[0004] Here, the transfer process of the hard coat layer onto the molded product using the transfer hard coat film is often carried out in a roll-to-roll manufacturing facility, as with general film-like resin materials. The transfer hard coat film, which is in the stage prior to the final curing, is also required to have blocking resistance in order to maintain a good level of productivity in the roll-to-roll manufacturing facility (see Patent Document 2).
[0005] Patent Document 2 discloses, for example, that by setting the glass transition point of the curable resin (acrylate resin) forming the hard coat layer to 30° C. or higher, tackiness can be suppressed and blocking resistance can be imparted, and that by setting the glass transition point to 150° C. or lower, flexibility during molding can be maintained.
[0006] However, the "flexibility" and "blocking resistance" of the hard coat layer before curing are in a trade-off relationship, and it has been difficult to optimize both at a good level. This problem is particularly serious in so-called after-cure type transfer hard coat films that undergo a final curing process after transfer to a molded article substrate, and Patent Document 2 only vaguely exemplifies a wide range of cured resins that are not impossible to use when considering the compatibility of "flexibility" and "blocking resistance," and does not disclose any specific means for actually achieving a good level of compatibility between "flexibility" and "blocking resistance." [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-193211 A [Patent Document 2] JP 2012-51247 A Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a transfer hard coat film capable of forming a scratch-resistant hard coat layer on a molded article (hard coat laminate) that has both good levels of "flexibility" and "blocking resistance" at the stage before final curing. [Means for solving the problem]
[0009] The present inventors have conducted intensive research to solve the above problems, and have found that the above problems can be solved by a transfer hard coat film that can be produced by a unique production method in which the resin composition for forming the hard coat layer is specified to have a hydroxyl value of a certain level or more in the material stage before the coating film is formed, and the hydroxyl value of the resin composition after the coating film is formed is suppressed to a certain level or less by adjusting the amount of isocyanate-based curing agent added, and thus the present invention has been developed. More specifically, the present invention provides the following.
[0010] (1) A method for producing a transfer hard coat film having a hard coat layer laminated on a substrate film, the method comprising: a hard coat layer forming step of applying a resin composition for a hard coat layer onto the substrate film and then semi-curing the applied composition to form a hard coat layer; and an adhesive layer forming step of forming an adhesive layer on the hard coat layer, the resin composition for a hard coat layer having an acrylate group as a base resin and containing an isocyanate-based curing agent, the hydroxyl value of the resin composition for a hard coat layer before the formation of a coating film being 160 mgKOH / g or more, and the amount of the isocyanate-based curing agent added to the resin composition for a hard coat layer being adjusted to an amount such that the hydroxyl value of the resin composition for a hard coat layer after the formation of a coating film is 150 mgKOH / g or less.
[0011] (2) The method for producing a transfer hard coat film according to (1), wherein the resin composition for the hard coat layer has a hydroxyl value of 200 mgKOH / g or more before forming a coating film.
[0012] (3) A hard-coat film for transfer comprising a base film, a hard-coat layer, and an adhesive layer laminated in this order, the hard-coat layer having an acrylic acrylate as a base resin, a hydroxyl value of 150 mgKOH / g or less, and an intensity ratio of urethane bonds to C-H bonds of 1.5 or more as measured by infrared absorption spectroscopy.
[0013] (4) A hard coat laminate comprising a hard coat layer laminated on a molded article substrate, the hard coat layer being the hard coat layer of the transfer hard coat film described in (3). Effect of the Invention
[0014] According to the present invention, in a transfer hard coat film capable of forming a scratch-resistant hard coat layer on a molded article (hard coat laminate), it is possible to achieve both "flexibility" and "blocking resistance" at a good level at the stage before final curing. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic cross-sectional view showing a layer structure of a transferable hard coat film of the present invention. [Diagram 2] FIG. 1 is a cross-sectional schematic diagram showing an example of a hard coat laminate that can be produced using the transfer hard coat film of the present invention, in which (a) the shape of the laminate before the base film is peeled off, and (b) the shape of the laminate after the base film is peeled off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments. Furthermore, the present invention can be practiced with appropriate modifications within the scope of its purpose.
[0017] <Hard coat film for transfer> A transferable hard coat film 10 which is a preferred embodiment of the present invention is a laminate in which a hard coat layer 12 and an adhesive layer 13 are laminated in this order on a substrate film 11 (see FIG. 1).
[0018] In producing a hard coat laminate 100 in which a hard coat layer is formed on the surface of a molded article substrate 20, this transfer hard coat film 10 is used to transfer a hard coat film transfer body 1 comprising a hard coat layer 12 and an adhesive layer 13 to the molded article substrate 20, thereby obtaining a hard coat laminate 100 with excellent scratch resistance (see Figure 2).
[0019] The hard coat layer 12 of the transfer hard coat film 10 is made mainly of a curable resin such as an ultraviolet curable resin, and is a layer that imparts excellent scratch resistance to the surface of the molded article substrate 20 constituting the hard coat laminate 100 .
[0020] The adhesive layer 13 of the hard coat film for transfer 10 is a layer that exhibits sufficient adhesion to the surface of the molded article substrate 20 in the hard coat film transfer body 1. It is more preferable that the adhesive layer 13 has a multilayer structure in which a primer layer 131 and a heat seal layer 132 are laminated in this order from the surface side of the hard coat layer 12.
[0021] [Base film] The base film 11 is preferably made of a polyester resin film or a polyolefin resin film, and more preferably made of a stretched film among the above resin films.
[0022] Polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate, polyethylene naphthalate, polyarylate, polycarbonate, and ethylene terephthalate-isophthalate copolymers can be preferably used as the polyester resin film constituting the base film 11. Among these, polyethylene terephthalate (PET) is particularly preferred because it is less susceptible to thermal shrinkage and is economical.
[0023] As the polyolefin resin film constituting the base film 11, a stretched resin film or the like made of a polyolefin resin such as a polyethylene resin, a polypropylene resin, a polybutene resin, an ethylene-propylene copolymer resin, an ethylene-propylene-butene copolymer resin, or an olefin thermoplastic elastomer can be preferably used. Among these, a stretched polypropylene resin film is preferable because it has excellent heat resistance and is less likely to undergo thermal shrinkage.
[0024] The thickness of the base film 11 is preferably 4 μm or more and 200 μm or less. By making the thickness of the base film 11 4 μm or more, the occurrence of curl deformation and wrinkles can be suppressed. Furthermore, by making the thickness of the base film 11 200 μm or less, the transfer performance when transferring the hard coat film transfer body 1 to the surface of the molded article substrate 20 by heat and pressure bonding can be maintained well.
[0025] A release layer (not shown) may be further disposed on the surface of the base film 11 on which the hard coat layer is disposed, for facilitating peeling of the hard coat film transfer body 1 from the base film 11 when transferring to the surface of the molded article substrate 20. Examples of resins that can be used to form the release layer include acrylic resins, melamine resins, epoxy resins, silicone resins, and ionizing radiation curable resins.
[0026] [Hard coat layer] The hard coat layer 12 is a cured film made of a resin composition for hard coat layer containing a predetermined curable resin and a predetermined curing agent. The details of the composition of the resin composition for hard coat layer will be described later.
[0027] Here, in the transfer hard coat film 10, it is assumed that the hard coat layer 12 is transferred to the surface of the molded article substrate 20 and then undergoes a curing treatment such as ultraviolet irradiation to progress to final curing. That is, in the stage before transfer, final curing has not progressed in the hard coat layer 12 of the transfer hard coat film 10, and in this uncured stage, the transfer hard coat film 10 can exhibit advantageous curing over conventional products by achieving both flexibility and blocking resistance as a film material at a good level.
[0028] The hard coat layer 12 is a cured film made of a resin composition for hard coat layers, which contains a predetermined curable resin and a predetermined curing material. However, in the transfer hard coat film 10, it is assumed that the hard coat layer 12 is transferred to the surface of the molded article substrate 20, and then cured by UV irradiation or the like to progress to final curing. That is, in the stage before transfer, the final curing does not progress in the hard coat layer 12 of the transfer hard coat film 10, and in this uncured stage, the transfer hard coat film 10 can exhibit an advantageous effect over conventional products in that it has a good level of flexibility and blocking resistance as a film material.
[0029] The hard coat layer 12 is a resin layer that uses acrylic acrylate as a base resin and has a hydroxyl value of 150 mgKOH / g or less after coating formation and an "intensity ratio of urethane bonds to C-H bonds" of 1.5 or more as measured by infrared absorption spectroscopy or the like. The "intensity ratio of urethane bonds to C-H bonds" is calculated by infrared absorption spectroscopy by transferring the layer to a resin molded product, irradiating the layer with ultraviolet light (800 mJ / cm 2 ) was irradiated and cured, and the 1400 cm wavelength derived from the C-H bond was measured by the ATR method. -1 The peak intensity around 1740 cm originating from the urethane bond -1 It can be calculated from the ratio of the peak intensities in the vicinity.
[0030] (Resin composition for hard coat layer) The resin composition for hard coat layer forming the hard coat layer 12 contains a resin having an acrylate group as a base resin and an isocyanate-based curing agent in an appropriate amount range described in detail below. In this specification, "acrylate" may also be "methacrylate".
[0031] The resin composition for the hard coat layer must have a hydroxyl value of 160 mgKOH / g or more, preferably 200 mgKOH / g or more, before the coating film is formed (for example, in the form of an ink for forming a hard coat layer), and must have a hydroxyl value of 150 mgKOH / g or less after the coating film is formed as the hard coat layer 12.
[0032] As described above, in the resin composition for hard coat layer, a certain number of hydroxyl groups are present at the initial stage, and a certain percentage of the hydroxyl groups react with the curing agent to crosslink and form urethane bonds during the process of forming the coating film. This allows the hard coat layer 12 after the coating film is formed to have appropriate flexibility and blocking resistance. The formation of the above-mentioned urethane bonds during the coating film formation gives the hard coat layer 12 sufficient blocking resistance. On the other hand, the flexibility of the urethane bonds at the crosslinking points is sufficiently large compared to the curing caused by crosslinking of the acrylate groups in the resin composition for hard coat layer when the final curing is completed by ultraviolet irradiation or the like after the hard coat film transfer body 1 is transferred to the molded article substrate 20. Therefore, in the transfer hard coat film 10, it is possible to achieve both "flexibility" and "blocking resistance" at a good level after the coating film is formed and before the final curing.
[0033] The base resin of the hard coat layer resin composition may be a resin having an acrylate group, which can make the hydroxyl value of the composition at the initial stage 160 mgKOH / g or more. Specifically, acrylic acrylate, polyester acrylate, epoxy acrylate, urethane acrylate, polyether acrylate, polyol acrylate, melamine acrylate, etc. may be used as the base resin of the hard coat layer resin composition. Among these, acrylic acrylate is particularly preferably used as the base resin of the hard coat layer resin composition. In this specification, the "base resin" means a resin contained in the resin composition at a ratio of at least 30% by mass or more, 50% by mass or more in the resin components, and the resin with the largest content ratio among the resin components. In addition to the above-mentioned base resin, the hard coat layer resin composition may contain a resin other than the base resin at a ratio below the above range.
[0034] As the curing agent to be added to the resin composition for hard coat layer, an isocyanate-based curing agent can be used. As the isocyanate-based curing agent to be added to the resin composition for hard coat layer, any known curing agent can be appropriately selected and used as long as it contains isocyanate and is capable of forming a urethane bond by crosslinking hydroxyl groups present in the resin composition for hard coat layer at the material stage. Specific examples of such curing agents include various isocyanate-based curing agents each containing tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, cyclohexane phenylene diisocyanate, naphthalene-1,5-diisocyanate, etc. Among these, hexamethylene diisocyanate and its multimers can be particularly preferably used as the curing agent to be added to the resin composition for hard coat layer.
[0035] The amount of the isocyanate-based curing agent added to the hard coat layer resin composition is such that the hydroxyl value of the hard coat layer resin composition after the coating film is formed is 150 mgKOH / g or less. As described above, the hydroxyl value of the hard coat layer resin composition at the initial stage is 160 mgKOH / g or more, preferably 200 mgKOH / g or more. The amount of the isocyanate-based curing agent added is an amount that can reduce the hydroxyl value of the composition at the initial stage to 150 mgKOH / g or less by the formation of the above-mentioned urethane bond. As a specific guideline, for example, when a resin material made of acrylic acrylate is used as the main resin of the hard coat layer resin composition, the amount of the isocyanate-based curing agent added is preferably 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the resin component. With this range as a guideline, it is sufficient to adjust the amount to be able to vary the hydroxyl value before and after the coating film formation as described above.
[0036] In addition, the resin composition for hard coat layer may further contain a scratch-resistant filler or a weathering agent. The scratch-resistant filler that may be contained in the resin composition for hard coat layer may be inorganic or organic, and inorganic particles such as alumina, silica, kaolinite, iron oxide, diamond, zirconia, silicon carbide, etc. may be used. Among these inorganic scratch-resistant fillers, silica particles may be preferably used when transparency is required for the hard coat layer 12. This is because silica particles improve the scratch resistance of the hard coat layer 12 and do not inhibit the transparency of the hard coat layer 12. As the silica particles, any silica particles known in the art may be appropriately selected and used, and colloidal silica particles may also be preferably used. Even if the amount of colloidal silica particles added is increased, the transparency is less affected.
[0037] The resin composition for the hard coat layer may further contain various light resistance agents such as ultraviolet absorbers and light stabilizers. The ultraviolet absorbers absorb harmful ultraviolet rays and improve the long-term weather resistance and stability of the hard coat laminate 100. The light stabilizers themselves hardly absorb ultraviolet rays, but efficiently capture harmful free radicals generated by ultraviolet rays to obtain stabilization. Preferred examples of the ultraviolet absorbers include inorganic ones such as titanium dioxide, cerium oxide, and zinc oxide, and organic ones such as benzotriazole and triazine ultraviolet absorbers, and among them, triazine ultraviolet absorbers can be preferably used. Preferred examples of the light stabilizers include hindered amine light stabilizers (HALS).
[0038] The thickness of the hard coat layer 12 is preferably 1 μm or more and 20 μm or less, more preferably 2 μm or more and 10 μm or less, and most preferably 2 μm or more and 6 μm or less. By making the thickness of the hard coat layer 12 1 μm or more, it is possible to ensure the scratch resistance that is usually required. In addition, by making the thickness of the hard coat layer 12 20 μm or less, it is possible to maintain the manufacturing stability and economic efficiency at a good level.
[0039] [Adhesive layer] The adhesive layer 13 is a layer having a function of adhering the hard coat film transfer body 1 to the surface of the molded article substrate 20. This adhesive layer 13 may be a single layer, but as described above, it is preferable that it has a two-layer structure in which a primer layer 131 and a heat seal layer 132 are laminated in this order from the side of the hard coat layer 12. Hereinafter, the case where the adhesive layer 13 has such a two-layer structure will be described.
[0040] The weather resistance agent and light resistance agent that can be contained in the hard coat layer can also be contained in the adhesive layer 13 as necessary. In particular, when the adhesive layer 13 has a two-layer structure as described above, the weather resistance agent and light resistance agent are contained in the primer layer 131, and the heat seal layer 132 does not contain these additives, so that the weather resistance and light resistance of the molded article substrate 20 can be maintained at a high level while avoiding a decrease in the adhesiveness and adhesive durability of the heat seal layer 132.
[0041] [Primer layer] The primer layer 131 functions as a stress relaxation layer for the hard coat layer 12, and also has a function of improving the adhesion of the hard coat film transfer body 1, which includes the hard coat layer 12, to the molded article substrate 20. This primer layer 131 is composed of a resin composition for forming a primer layer, which contains a binder resin and various additives, such as an antiblocking agent, which are added as necessary.
[0042] The binder resin constituting the primer layer 131 is preferably a two-component curing resin consisting of a base agent and a curing agent. The base agent of the binder resin constituting the primer layer 131 is not particularly limited. Examples of the base agent of the binder resin that can be preferably used include polyurethane resin, (meth)acrylic resin, vinyl chloride-vinyl acetate copolymer, polyester resin, butyral resin, chlorinated polypropylene, and chlorinated polyethylene. These binder resins can be used alone or in combination of two or more. Among these binder resins, polyurethane resin is particularly preferred from the viewpoints of adhesion and weather resistance.
[0043] As the curing agent for the binder resin constituting the primer layer 131, for example, an isocyanate curing agent such as tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, cyclohexane phenylene diisocyanate, naphthalene-1,5-diisocyanate, etc. can be used. The amount of the curing agent used is preferably 1 part by mass or more and 40 parts by mass or less, more preferably 10 parts by mass or more and 30 parts by mass or less, and even more preferably 20 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the resin as the main agent.
[0044] If necessary, various additives other than those mentioned above can be blended into the primer layer 131 within a range that does not impair the effects of the present invention. Examples of such additives include weather resistance improvers such as ultraviolet absorbers and light stabilizers, abrasion resistance improvers, infrared absorbers, light stabilizers, antistatic agents, adhesion improvers, leveling agents, thixotropy imparting agents, coupling agents, plasticizers, defoamers, fillers, solvents, colorants, etc. These additives can be appropriately selected from those commonly used.
[0045] The thickness of the primer layer 131 is not particularly limited, but is preferably 0.1 μm or more and 10 μm or less, and more preferably 0.1 μm or more and 5 μm or less.
[0046] [Heat seal layer] The heat seal layer 132 is a layer that, together with the primer layer 131, functions to adhere the hard coat film transfer body 1 to the surface of the molded article substrate 20, and is composed of an adhesive resin such as a heat-sealing resin so that transfer to the molded article substrate 20 can be performed satisfactorily by heating and pressurization.
[0047] The adhesive resin contained in the heat seal layer 132 is determined according to the material of the molded article substrate 20, the transfer temperature and pressure during transfer, the use of the transferred product, etc., and is not particularly limited. In general, as the adhesive resin, heat-sealing resins such as acrylic resin, vinyl chloride-vinyl acetate copolymer, polyamide resin, polyester resin, chlorinated polypropylene, chlorinated rubber, urethane resin, epoxy resin, styrene resin, etc. can be appropriately used. Each of these resins can be used alone, or two or more types can be used in combination.
[0048] The thickness of the heat seal layer 132 is preferably thicker than that of the primer layer 131. From the viewpoint of ensuring the function of adhering the hard coat film transfer body 1 including the hard coat layer 12 to the molded article substrate 20 and excellent transparency, the thickness of the heat seal layer 132 is preferably thicker than that of the primer layer 131 and is 1 μm or more and 7 μm or less, and more preferably thicker than that of the primer layer 131 and is 1 μm or more and 3 μm or less.
[0049] The surface of the hard coat film 10 for transfer can also be protected by attaching a cover film (protective film) made of a resin such as polyethylene resin on the heat seal layer 132. When a cover film is provided on the hard coat film 10 for transfer, this cover film is peeled off to expose the heat seal layer 132, and then the hard coat film transfer body 1 is transferred to the molded article substrate 20 via the surface of the heat seal layer 132.
[0050] <Method of manufacturing hard coat film for transfer> The transfer hard coat film 10 can be efficiently produced while maintaining a high level of quality stability by the "production method for a transfer hard coat film" according to the present invention, which will be described in detail below.
[0051] The method for producing a hard coat film for transfer of the present invention is a method for producing at least a "hard coat layer forming step" in which a "resin composition for hard coat layer", the composition of which is described in detail above, is applied to a substrate film 11, and then semi-cured to form a hard coat layer, and an "adhesive layer forming step" in which an adhesive layer is further formed on the hard coat layer 12. The main feature of the method is that the hydroxyl value and the number of urethane bonds of the hard coat layer at the stage after the coating film is formed and before the final curing are optimized in a well-balanced manner by adjusting the amount of curing agent added to the "resin composition for hard coat layer" used in the "hard coat layer forming step". In addition, "semi-cured" in this specification means that the coating film formation as the hard coat layer of the hard coat film for transfer is completed, but the final curing leading to the completion stage of the final product (hard coat laminate) is not yet completed. For example, the "ultraviolet ray irradiation step" in the "method for producing a hard coat laminate" described later corresponds to this step of "completing the final curing".
[0052] [Hard coat layer formation process] In this step, as described above, a "resin composition for hard coat layer" having a hydroxyl value of 160 or more before the coating film is formed, the resin composition containing an acrylate group as a base resin and an isocyanate-based curing agent is applied onto a substrate film to form a hard coat layer.
[0053] The amount of the curing agent added is adjusted so that the hydroxyl value of the hard coat layer resin composition after coating is 150 mgKOH / g or less, as described above, which allows the intensity ratio of the C-H bond to the urethane bond in the infrared absorption spectrum of the hard coat layer after coating to be 1.5 or more.
[0054] The method of forming the hard coat layer 12 on the substrate film 11 includes coating the resin composition for forming the hard coat layer by a method such as gravure coating, bar coating, roll coating, reverse roll coating, comma coating, etc., preferably gravure coating, so that the thickness of the hard coat layer 12 after coating is the desired thickness, and curing the composition. When the resin composition contains a solvent, it is preferable to heat and dry the coating layer in advance using a hot air dryer or the like after coating, and then further heat treatment. This further heat treatment, etc., more quickly promotes the formation of urethane bonds by the reaction of the hydroxyl group of the base resin with isocyanate.
[0055] [Adhesive layer formation process] In this step, an adhesive layer 13 is formed on the hard coat layer 12 obtained in the hard coat layer forming step. As described above, the adhesive layer 13 preferably has a multi-layer structure consisting of a primer layer 131 and a heat seal layer 132. Hereinafter, a preferred embodiment of this step in which the adhesive layer 13 has such a layer structure will be described.
[0056] The primer layer 131 can be formed by using the above-mentioned composition for forming a primer layer, by a coating method such as gravure coating, bar coating, roll coating, reverse roll coating, comma coating, slit coating, die coating, or a transfer coating method. Here, the transfer coating method is a method in which a coating film of the primer layer 131 is formed on a thin sheet (film substrate), and then the surface of the hard coat layer 12 is coated with the primer layer 131. It is preferably performed by gravure coating.
[0057] The heat seal layer 132 can also be formed on the primer layer 131 using an adhesive resin such as the above-mentioned heat fusion resin in the same manner as in the formation of the primer layer, such as gravure coating.
[0058] <Hard coat laminate> The hard coat laminate 100 according to the present invention is a laminate in which the hard coat layer 12 of the above-mentioned hard coat film 10 for transfer, i.e., the hard coat layer 12 of the hard coat film transfer body 1, is formed as a cured film that enhances the scratch resistance of the surface of the molded article on the molded article substrate 20. The substrate film 11 may be disposed arbitrarily, and as shown in Fig. 2(b), the substrate film 11 may be peeled off from the hard coat film transfer body 1 at any stage during use.
[0059] [Molded product base] Various resin bases and the like may be appropriately selected according to the desired molded product for the molded article base 20. When the molded article base 20 is a resin base, specific examples of the resin constituting the molded article base 20 include polycarbonate resin, ABS resin, acrylic resin, and olefin resins such as polypropylene and polyethylene.
[0060] This hard coat laminate 100 can be obtained by the manufacturing method of the hard coat laminate described below. As described below, this hard coat laminate is assumed to be manufactured by integrally molding the molded article substrate 20 and the hard coat film transfer body 1 in a mold or the like, and then completing the final curing of the hard coat layer 12 by ultraviolet irradiation (so-called after-cure). Therefore, the hard coat film transfer body 1 has extremely good conformability to molded article substrates of various surface shapes, and the crosslinking process for curing can be performed by a relatively simple device, and the crosslinking conditions can be easily controlled. In other words, the hard coat laminate 100 is a molded article that has excellent characteristics in that the moldability and hardness of the hard coat layer 12 can be easily optimized.
[0061] <Method of Manufacturing Hard Coat Laminate> The method for producing the hard coat laminate 100 of the present invention is not limited to a specific method, but as described in detail below, the hard coat laminate 100 can be produced by a production method that sequentially performs a lamination step for obtaining a material laminate and an ultraviolet irradiation step for irradiating the material laminate after lamination with ultraviolet light to complete the final curing of the resin that forms the hard coat layer 12.
[0062] (Lamination process) The lamination step is a step of obtaining a material laminate by laminating a hard coat layer 12 on the surface of a molded article substrate 20 via an adhesive layer 13, for example, in a mode as shown in Fig. 2. The material laminate thus obtained is integrated by subjecting it to the next step, which is an energy wave irradiation step.
[0063] (Ultraviolet irradiation process) The ultraviolet ray irradiation process is a process in which the material laminate obtained in the above lamination process is irradiated with ultraviolet rays to crosslink the resin that forms the hard coat layer 12, thereby completing the final curing of the hard coat layer 12. EXAMPLES
[0064] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0065] <Preparation of hard coat film for transfer> (Release layer forming process) A release layer-forming resin composition was applied to one surface of the substrate film and dried at a temperature of 150° C. or higher to form a release layer (layer thickness: 1 μm). (Hard coat layer forming process) A curable resin composition for forming a hard coat layer was applied onto the surface on which the release layer was formed to form an uncured resin layer. (Adhesive layer formation process) A resin composition for forming a primer layer was applied to the surface of the hard coat layer opposite the substrate film to form a primer layer (layer thickness: 2 μm), and a resin composition for forming a heat seal layer was further applied onto the primer layer to form a heat seal layer (layer thickness: 1.5 μm).
[0066] By the above-mentioned operation, the hard coat film for transfer of each of the examples and comparative examples was obtained, in which the base film, the release layer, the hard coat layer, and the adhesive layer (primer layer and heat seal layer) were laminated in this order. Details of the materials used are as follows.
[0067] (Base film) Product name: Lumirror 50T60, manufactured by Toray Industries, Inc. (a 50μm thick film made of polyethylene terephthalate resin (PET)) (Resin composition for forming release layer) : 100 parts by mass of acrylic melamine resin composition (EX-114D-B medium (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.)); 6 parts by mass of curing agent (PTC No. 7 curing agent (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.)). (Curable resin composition for forming hard coat layer) Acrylic acrylate 1 (used in Example 1 and Comparative Example 1) 100 parts of acrylic acrylate resin (molecular weight approximately 65,000, hydroxyl value 211 mgKOH / g); 4 parts of photopolymerization initiator (IRGCURE184 (manufactured by BASF Japan Ltd.)) Acrylic acrylate 2 (used in Example 2 and Comparative Example 2) 100 parts of acrylic acrylate resin (molecular weight approximately 65,000, hydroxyl value 160 mgKOH / g); 4 parts of photopolymerization initiator (IRGCURE184 (manufactured by BASF Japan Ltd.)) Acrylic acrylate 3 (used in Comparative Example 3) 100 parts of acrylic acrylate resin (molecular weight approximately 65,000, hydroxyl value 10 mgKOH / g); 4 parts of photopolymerization initiator (IRGCURE184 (manufactured by BASF Japan Ltd.)) Urethane acrylate (used in Comparative Example 4) : 100 parts by weight of hexafunctional ionizing radiation curable resin (a mixture of 60 parts by weight of hexafunctional urethane acrylate (molecular weight of about 1,000) and 40 parts by weight of bifunctional caprolactone-modified urethane acrylate (molecular weight of about several thousand)); 0.7 parts by weight of hydroxyphenyltriazine-based ultraviolet absorber (Tinuvin 479 (manufactured by BASF Japan Ltd.)); 4.2 parts by weight of light stabilizer having reactive functional group (Sanol LS-3410 (manufactured by Nippon Nyukazai Co., Ltd.)); 0.3 parts by weight of non-reactive silicone compound (polyether-modified silicone oil); 2 parts by weight of scratch-resistant filler (silica particles, average particle size: 2 μm) Curing agent (hexamethylene diisocyanate-based polyfunctional isocyanate): Added in the amount (unit: parts by mass) shown in Table 1 relative to 100 parts by mass of the acrylic acrylates 1 to 3 or the urethane acrylate. In addition, only in Comparative Example 4, the resin composition for hard coat layer was coated and then irradiated with electron beams under conditions of 90 kV and 7 Mrad (70 KGy) to crosslink and harden the composition, thereby forming a hard coat layer.
[0068] (Resin composition for forming primer layer) Polyester urethane-acrylic copolymer 100 parts by weight; hydroxyphenyl triazine ultraviolet absorber (Tinuvin 400 (BASF Japan Ltd.)) 17 parts by weight; hydroxyphenyl triazine ultraviolet absorber (Tinuvin 479 (BASF Japan Ltd.)) 13 parts by weight; hindered amine light stabilizer 8 parts by weight (Tinuvin 123 (BASF Japan Ltd.)); antiblocking agent 9 parts by weight; curing agent (hexamethylene diisocyanate) 25 parts by weight; silica particles (average particle size: 3 μm)
[0069] (Resin composition for forming heat seal layer) Acrylic resin (molecular weight approx. 100,000, glass transition temperature (Tg) approx. 105°C)
[0070] <Preparation of hard coat laminate> The transfer hard coat films of the Examples and Comparative Examples produced as described above were inserted into the mold of an injection molding machine, and the following "resin composition for resin molding" was injected to perform injection molding, and a molded product was obtained, and at the same time, the substrate film was peeled off to obtain a resin molded product provided with a hard coat layer. The molded product was then removed from the mold, and the substrate film was peeled off. The hard coat layer in a semi-cured state was finally cured by ultraviolet irradiation under the following "ultraviolet irradiation conditions", to obtain a hard coat laminate. (Resin composition for resin molded body) Polycarbonate resin (Panlite L-1225Z100M (Teijin Limited)) (Ultraviolet irradiation conditions) Air atmosphere, H bulb, 800mJ / cm 2 It was irradiated and cured.
[0071] <Test Example 1: Hydroxyl value of the resin composition for hard coat layer before and after coating film formation> The hydroxyl value of the resin composition for the hard coat layer before the coating film was measured according to JIS K 0070: 1992. The hydroxyl value after the coating film was measured in the same manner after dissolving the hard coat layer in a semi-cured state before the final curing treatment in methyl ethyl ketone.
[0072] <Test Example 2: Intensity ratio of C-H bond to urethane bond in infrared absorption spectrum of hard coat layer> For each of the hard coat laminates of the Examples and Comparative Examples produced as described above, the infrared absorption spectrum of the hard coat layer was measured by the following method. -1 The peak intensity around 1740 cm is for C-H bonds. -1 The peak intensity in the vicinity was determined as the peak intensity attributable to the urethane bond, and the intensity ratio (peak intensity of the urethane bond / peak intensity of the C-H bond) was calculated. (Measuring device): "FT / IR-6100 (manufactured by JASCO Corporation)" (Measurement conditions): Wavelength range is 400 cm -1 ~4000cm -1The absorbance was measured using the ATR method.
[0073] <Evaluation Example 1> [Evaluation of blocking resistance] (Test Method) For each of the transfer hard coat films of the Examples and Comparative Examples produced as described above, the coating appearance was evaluated after the coating surface after the hard coat layer was formed (semi-cured) by touching it with a finger for 5 seconds. (Evaluation Criteria) A: There is no change in the appearance of the coating film, and the coating film-forming resin does not adhere to fingers. B: There is a slight change in the appearance of the coating film, but the film-forming resin does not adhere to the fingers. C: There is a noticeable change in the appearance of the coating film, and the coating film-forming resin adheres to the fingers.
[0074] <Evaluation example 2> [Evaluation of moldability] The appearance of the surface of each of the hard coat laminates of the Examples and Comparative Examples produced as described above was observed, and the moldability was evaluated according to the following evaluation criteria. (Evaluation Criteria) A: The molding is done without any cracks. B: Minor cracks only on the edges C: Cracks have occurred all over the surface
[0075] <Evaluation Example 3> [Weather resistance evaluation] (Test Method) Using a super xenon weather meter (SX-75, manufactured by Suga Test Instruments), the appearance of the test sample was evaluated after 1000 hours had elapsed in the following "test cycle." (Test Cycle) "STEP1 (irradiation)": Illuminance 180W / m 2 ;BP temperature 63℃; humidity 50%; time 102 minutes "STEP 2 (irradiation + rain)": Illuminance 180W / m 2 ;BP temperature 30℃; humidity 98%; time 18 minutes (Evaluation Criteria) A: No change in appearance B: Slight changes in appearance C: Significant changes in appearance such as cracks or loss of gloss are observed.
[0076] [Table 1]
[0077] As can be seen from Table 1, the present invention makes it possible to obtain a transfer hard coat film capable of forming a scratch-resistant hard coat layer on a molded article (hard coat laminate), which has both good levels of "flexibility" and "blocking resistance" before the final curing stage. [Explanation of symbols]
[0078] 1 Hard coat film transfer 10 Hard coat film for transfer 11 Base film 12 Hard coat layer 13 Adhesive layer 131 Primer layer 132 Heat seal layer 123 Adhesive layer 20 Molded product base 100 Hard coat laminate
Claims
[Claim 1] A method for producing a transferable hard coat film in which a hard coat layer is laminated on a substrate film, comprising the steps of: a hard coat layer forming step of applying a resin composition for a hard coat layer onto a substrate film and then semi-curing the composition to form a hard coat layer; and forming an adhesive layer on the hard coat layer, The resin composition for the hard coat layer contains a resin having an acrylate group as a base resin, an isocyanate-based curing agent, and a solvent, The hydroxyl value of the resin composition for hard coat layer before forming a coating film is 211 mgKOH / g or more, The amount of the isocyanate-based curing agent added to the resin composition for hard coat layer is adjusted so that the hydroxyl value of the resin composition for hard coat layer after forming a coating film is 150 mgKOH / g or less; In the hard coat layer forming step, after coating the resin composition for hard coat layer, the coating layer made of the resin composition for hard coat layer is preheated and dried, and then additionally heated, so that the intensity ratio of C-H bond to urethane bond (peak intensity of urethane bond / peak intensity of C-H bond) in the infrared absorption spectrum of the hard coat layer after coating film formation is 3.7 or more. A method for producing a hard coat film for transfer.
Citation Information
Patent Citations
Active energy ray hardening resin composition used for transfer material and protective layer for transfer material and manufacture of molded product of superior wear resistance and chemical resistance using transfer material
JP1998058895A
Active energy ray-curable resin composition
JP2004131587A
Hard coating agent composition, hard coat film and molded product
JP2011126921A
Decorative hard coat film, decorative film and decorative molded product
JP2012051247A
Protective layer transfer sheet and intermediate transfer medium
JP2014198435A