Sodium ion secondary battery and method of manufacturing the same
By using an electrode with an organic binder that emits fluorescence at 532 nm and undergoes controlled decomposition, the electrode achieves improved charge/discharge capacity through enhanced ionic conductivity and binding properties.
Patent Information
- Application Number
- JP2019171540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-09-20
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2039-09-20
AI Technical Summary
Existing secondary battery electrodes face issues with insufficient sinterability of raw material powders, leading to inadequate charge/discharge capacity due to insufficient adhesion and poor ionic conductivity of organic binders.
Incorporating an electrode active material powder and an organic binder that emits fluorescence at a specific wavelength (532 nm) and undergoes partial decomposition within a controlled temperature range, ensuring excellent ionic conductivity and charge/discharge capacity.
The electrode achieves enhanced charge/discharge capacity by maintaining the organic binder's structural integrity and ionic conductivity, even after partial decomposition, thereby improving binding properties and reducing mass loss.
Smart Images

Figure 0007577917000005 
Figure 0007577917000001 
Figure 0007577917000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode, which is a component of a secondary battery used in portable electronic devices, electric vehicles, etc., and a method for manufacturing the same. [Background technology]
[0002] Lithium ion secondary batteries have established a position as a high-capacity, lightweight power source that is indispensable for mobile devices, electric vehicles, and the like. Current lithium ion secondary batteries mainly use flammable organic electrolytes as the electrolyte, raising concerns about the risk of fire, etc. As a method for solving this problem, development of all-solid-state lithium ion batteries that use solid electrolytes instead of organic electrolytes is underway (see, for example, Patent Document 1).
[0003] In addition, because of concerns about the global rise in the cost of lithium as a raw material, sodium is also attracting attention as an alternative to lithium, and NASICON-type Na3Zr2Si2PO 12 A sodium ion all-solid-state battery using a sodium ion conductive crystal made of the above has been proposed (see, for example, Patent Document 2). In addition, β-alumina (theoretical composition: Na2O·11Al2O3), β"-alumina (theoretical composition: Na2O·5.3Al2O3), Li2O-stabilized β"-alumina (Na 1.7 Li 0.3 Al 10.7 O 17 ), MgO-stabilized β”-alumina ((Al 10.32 Mg 0.68 O 16 )(Na 1.68 O)) and beta-alumina-based solid electrolytes such as Na5YSi4O 12 It is known that these solid electrolytes also exhibit high sodium ion conductivity, and these solid electrolytes can also be used for sodium ion all-solid-state batteries. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-205741 [Patent Document 2] JP 2010-15782 A Summary of the Invention [Problem to be solved by the invention]
[0005] As an electrode layer in a secondary battery, there is a sintered body of a raw material powder containing an electrode active material powder. However, the sinterability of the raw material powder is insufficient, and a dense sintered body cannot be obtained, and as a result, sufficient charge / discharge capacity may not be obtained. Therefore, a method of binding the raw material powder with an organic binder to increase the adhesion between the powders has been proposed. However, since the organic binder itself has poor ionic conductivity, the desired charge / discharge capacity may still not be obtained.
[0006] In view of the above, an object of the present invention is to provide an electrode for a secondary battery that is capable of achieving excellent charge / discharge capacity. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved when a secondary battery electrode containing an electrode active material powder and an organic binder emits fluorescence at a specific wavelength in Raman spectroscopy measurement.
[0008] That is, the secondary battery electrode of the present invention is characterized by containing an electrode active material powder and an organic binder, and emitting fluorescence in Raman spectroscopy at a wavelength of 532 nm. As described below, it has been found that in a secondary battery electrode containing an electrode active material powder and an organic binder, when the organic binder is denatured by baking at a predetermined temperature to partially decompose it, it emits fluorescence in Raman spectroscopy at a wavelength of 532 nm. It has also been found that in this way, when the organic binder is denatured and a structural change occurs, the ion conductivity of the organic binder is excellent, and a desired charge / discharge capacity can be obtained.
[0009] Another aspect of the present invention is an electrode for a secondary battery, which contains an electrode active material powder and an organic binder, and is characterized in that the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50 ° C is 5% or less. Usually, when heat-treated at the decomposition temperature of the organic binder + 50 ° C, the decomposition of the organic binder proceeds, and CO2 gas, CO gas, H2O gas, etc. are generated, resulting in a large decrease in mass. On the other hand, the electrode for a secondary battery of the present invention is characterized in that the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50 ° C is as small as 5% or less. This means that the organic binder is already in a partially decomposed and denatured state, and therefore further decomposition hardly proceeds. In this case, the ionic conductivity of the organic binder is excellent as described above, and it is possible to obtain a desired charge / discharge capacity.
[0010] A secondary battery electrode according to yet another aspect of the present invention is an electrode for a secondary battery containing an electrode active material powder and an organic binder, characterized in that no exothermic peak or endothermic peak appears in the range of the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100 ° C. in DTA (differential thermal analysis) measurement. As described above, when heat treatment is usually performed at a temperature higher than the decomposition temperature of the organic binder, the decomposition of the organic binder proceeds and CO2 gas, CO gas, H2O gas, etc. are generated, but in this case, an exothermic peak or endothermic peak appears in DTA measurement. On the other hand, the secondary battery electrode of the present invention is characterized in that no exothermic peak or endothermic peak appears in DTA measurement in the range of the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100 ° C. This means that the organic binder is already in a partially decomposed and denatured state, and further decomposition hardly proceeds. In this case, as described above, the ionic conductivity of the organic binder is excellent, and it is possible to obtain a desired charge / discharge capacity.
[0011] The secondary battery electrode of the present invention preferably comprises a sintered body of a material containing an electrode active material powder and an organic binder.
[0012] The secondary battery electrode of the present invention preferably contains 0.1 to 30% by mass of an organic binder.
[0013] In the secondary battery electrode of the present invention, the organic binder is preferably at least one selected from polyacrylic acid, sodium polyacrylate, sodium methylcellulose, polyvinylidene fluoride, styrene-butadiene rubber, polyimide, and polyethylene oxide.
[0014] In the secondary battery electrode of the present invention, the electrode active material powder is preferably graphite, hard carbon, titanium oxide, Si, Sn or Bi.
[0015] The secondary battery electrode of the present invention may further contain a solid electrolyte powder, which allows an ion conductive path to be formed within the electrode.
[0016] In the secondary battery electrode of the present invention, the solid electrolyte powder is preferably a sodium ion conductive crystalline powder.
[0017] In the secondary battery electrode of the present invention, the sodium ion conductive solid electrolyte powder is preferably at least one selected from β-alumina, β″-alumina, and NASICON crystal.
[0018] The method for producing an electrode for a secondary battery of the present invention is characterized by including a step of firing a material containing an electrode active material powder and an organic binder at a temperature within a range of −50° C. to +250° C. with respect to the decomposition temperature of the organic binder. In this way, the organic binder is modified and undergoes a structural change, and a part of it remains in the electrode without being completely burned off. In this case, the obtained electrode emits fluorescence in Raman spectroscopy at a wavelength of 532 nm, and as described above, the ionic conductivity of the organic binder is excellent, and a desired charge / discharge capacity can be obtained. Effect of the Invention
[0019] According to the present invention, it is possible to provide an electrode for a secondary battery that is capable of obtaining excellent charge / discharge capacity. [Brief description of the drawings]
[0020] [Figure 1] 1 is a graph showing an initial charge / discharge curve of a test battery No. 4 in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The secondary battery electrode of the present invention contains an electrode active material powder and an organic binder. Each of the components will be described below.
[0022] (electrode active material powder) The electrode active material powder includes a positive electrode active material powder and a negative electrode active material powder.
[0023] The positive electrode active material powder is NaCrO2, Na 0.7 MnO2, NaFe 0.2 Mn 0.4 Ni 0.4 O2, Na2FeP2O7, NaFePO4, Na3V2(PO4)3, Na2CoP2O7, Na2NiP2O7, Na 2 / 3 Ni 2 / 3 Mn 2 / 3 Examples of active material powders for sodium ion secondary batteries include those containing Na, M (M is at least one transition metal element selected from Cr, Fe, Mn, Co, and Ni), P, and O, such as O2. In particular, crystals containing Na, M, P, and O are preferred because they have high capacity and excellent chemical stability. Among them, triclinic crystals belonging to space group P1 or P-1, particularly those having the general formula Na x A crystal represented by MyP2O7 (1.20≦x≦2.80, 0.95≦y≦1.60) is preferred because of its excellent cycle characteristics.
[0024] As the positive electrode active material powder, there may be mentioned active material powders for lithium ion secondary batteries, such as LiCoO2, LiFePO4, and LiMn2O4.
[0025] Examples of the negative electrode active material powder include carbon powders such as graphite and hard carbon, ceramic powders such as titanium oxide (anatase type or rutile type), and metal powders such as Si, Sn, and Bi. Note that graphite, hard carbon, ceramic powder, Si, and the like are not easily softened and deformed by heat, and therefore, in order to obtain a dense sintered body, it is basically necessary to add an organic binder. Therefore, when using such an electrode active material powder that is not easily softened and deformed by heat, it is easy to enjoy the effects of the present invention.
[0026] (organic binder) Examples of organic binders include polyacrylic acid, sodium polyacrylate, sodium methylcellulose, polyvinylidene fluoride, styrene-butadiene rubber, polyimide, and polyethylene oxide. These may be used alone or in combination of two or more.
[0027] The secondary battery electrode of the present invention is characterized by emitting fluorescence in Raman spectroscopy at a wavelength of 532 nm, which indicates that the organic binder is modified by firing and undergoes a structural change (rubbery state). In this state in which the organic binder is modified and undergoes a structural change, the organic binder has excellent ion conductivity and is likely to have improved charge / discharge capacity.
[0028] In addition, the secondary battery electrode according to another aspect of the present invention is characterized in that the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50°C is 5% or less, which also indicates that the organic binder is denatured by firing and further decomposition hardly progresses. In this case, too, the organic binder has excellent ion conductivity, and the charge / discharge capacity is easily improved. In addition, the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50°C is preferably 3% or less, 1% or less, and particularly 0%.
[0029] In addition, the secondary battery electrode according to still another aspect of the present invention is characterized in that no exothermic or endothermic peak appears in the DTA measurement in the range from the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100°C, which also indicates that the organic binder is modified by firing and undergoes a structural change. In this case as well, the organic binder has excellent ion conductivity, which facilitates an improvement in charge / discharge capacity.
[0030] The content of the organic binder in the secondary battery electrode of the present invention is preferably 0.1 to 30 mass%, 0.2 to 20 mass%, 0.3 to 10 mass%, and particularly preferably 0.5 to 5 mass%. If the content of the organic binder is too small, the electrode active material powders and the electrode active material powder and the solid electrolyte powder cannot be bonded together, and an ion conduction path cannot be secured, so that the charge / discharge capacity is likely to decrease. Alternatively, in the case of an all-solid-state battery, it becomes difficult to obtain the bond between the electrode and the solid electrolyte layer, and there is a risk that the electrode will peel off from the solid electrolyte layer. On the other hand, if the content of the organic binder is too large, the internal resistance of the electrode will increase, and there is a risk that the charge / discharge capacity will decrease significantly. In addition, the volume of the electrode active material in the electrode will decrease, and the energy density will decrease.
[0031] (Other Ingredients) The secondary battery electrode of the present invention may contain, in addition to the above components, a solid electrolyte powder and a conductive assistant.
[0032] In addition, a solid electrolyte powder may be contained in the electrode to form an ion conductive path. Examples of the solid electrolyte powder include sodium ion conductive crystal powder such as β-alumina, β”-alumina, and NASICON crystal, and LLZ (Ga-doped Li7La3Zr2O 12 ) and other lithium ion conductive crystal powders.
[0033] By incorporating a conductive assistant, the conductivity in the electrode is improved, and an excellent charge / discharge capacity can be obtained. In addition, a high rate can be achieved. Specific examples of the conductive assistant include highly conductive carbon black such as acetylene black and ketjen black, graphite, coke, and metal powders such as Ni powder, Cu powder, and Ag powder. Among them, it is preferable to use any one of highly conductive carbon black, Ni powder, and Cu powder, which exhibits excellent conductivity with the addition of a very small amount.
[0034] (Method of manufacturing electrodes for secondary batteries) The secondary battery electrode of the present invention can be produced, for example, by firing a material containing an electrode active material powder and an organic binder at a predetermined temperature.
[0035] Specifically, the electrode active material powder and the organic binder are first kneaded to form a slurry. When forming the slurry, a solvent such as N-methylpyrrolidone or water may be added. If necessary, a conductive assistant or a solid electrolyte powder may also be added.
[0036] The content of the organic binder in the material (solid material) is preferably 0.1 to 50 mass%, 1 to 40 mass%, 5 to 30 mass%, and particularly preferably 10 to 25 mass%. If the content of the organic binder is too small, the electrode active material powders and the electrode active material powder and the solid electrolyte powder cannot be bonded together, and an ion conduction path cannot be secured, so that the charge / discharge capacity is likely to decrease. Alternatively, in the case of an all-solid-state battery, it becomes difficult to obtain the bond between the electrode and the solid electrolyte layer, and there is a risk that the electrode will peel off from the solid electrolyte layer. On the other hand, if the content of the organic binder is too large, the internal resistance of the electrode will increase, and there is a risk that the charge / discharge capacity will decrease significantly. In addition, the volume of the electrode active material in the electrode will decrease, and the energy density will decrease.
[0037] Next, the obtained slurry is formed into a film to obtain a secondary battery electrode precursor. For example, in the case of an all-solid-state battery, the secondary battery electrode precursor may be formed by applying the slurry to a desired thickness on the surface of a solid electrolyte layer.
[0038] The slurry may be applied to a substrate such as a PET (polyethylene terephthalate) film and dried to prepare a green sheet, which may be used as the electrode precursor for a secondary battery. In the case of an all-solid-state battery, the obtained green sheet is laminated and pressed onto the surface of a solid electrolyte layer to form an electrode precursor for a secondary battery.
[0039] Alternatively, the electrode active material powder and the powdered organic binder may be mixed, and the mixture may be press-molded into pellets to prepare a secondary battery electrode precursor, which can omit the step of forming a slurry, thereby reducing the manufacturing cost.
[0040] Further, the electrode precursor for secondary batteries is fired to obtain an electrode for secondary batteries. The firing temperature is within the range of -50°C to +250°C relative to the decomposition temperature of the organic binder, preferably within the range of -30°C to +180°C relative to the decomposition temperature of the organic binder, more preferably within the range of -10°C to +160°C relative to the decomposition temperature of the organic binder, more preferably within the range of the decomposition temperature of the organic binder to the decomposition temperature of the organic binder +140°C, and particularly preferably within the range of +10°C to +120°C relative to the decomposition temperature of the organic binder. If the firing temperature is too low, the modification of the organic binder is insufficient, making it difficult to obtain an electrode for secondary batteries having the desired characteristics as described above. On the other hand, if the firing temperature is too high, the organic binder is completely decomposed and carbonized, losing its binding force, so that the binding between the electrode active materials and between the electrode layer and the solid electrolyte layer decreases, and the charge / discharge capacity tends to decrease significantly.
[0041] After the secondary battery electrode is obtained by carrying out the firing as described above, it is preferable not to carry out high-temperature firing (specifically, firing at a temperature higher than the decomposition temperature of the organic binder + 250°C), such as firing for sintering the electrode active materials together, because such firing after obtaining the secondary battery electrode promotes decomposition and carbonization of the organic binder, making it difficult to obtain a secondary battery electrode having desired characteristics. EXAMPLES
[0042] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0043] Tables 1 to 4 show examples (Nos. 3 to 6, 9 to 23) and comparative examples (Nos. 1, 2, 7, and 8).
[0044] [Table 1]
[0045] [Table 2]
[0046] [Table 3]
[0047] [Table 4]
[0048] (Samples No. 1 to 8) The electrode active material powder (negative electrode active material powder) was hard carbon powder (AT Electrode Co., Ltd., Bellfine® LN-0001, D 50 The raw materials were obtained by weighing out 80% of the powder (μm = 1), 5% of acetylene black (SUPER C65 manufactured by TIMCAL) as a conductive additive, and 15% of polyacrylic acid (PAH manufactured by Wako Pure Chemical Industries, Ltd., cross-linking degree 0%) as an organic binder. An equal amount of N-methylpyrrolidone was added to the raw materials, and the mixture was made into a slurry by thoroughly stirring using a planetary centrifugal mixer. All of the above operations were carried out in an environment with a dew point of -50°C or less. For No. 8, no organic binder was added, and the electrode active material powder and conductive additive were added in the ratios shown in Table 1.
[0049] The obtained slurry was mixed with β”-alumina (manufactured by Ionotec, composition formula: Na 1.7 Li0.3 Al 10.7 O 17 ) on one surface of a 0.5 mm thick solid electrolyte layer. 2 The coating was applied to an area of 100 μm and a thickness of 100 μm, and dried at 70° C. for 1 hour. Thereafter, the coating was held in air for 15 minutes at the firing temperature shown in Table 1 to form an electrode (negative electrode layer) on one surface of the solid electrolyte layer. Note that no firing was performed on No. 1.
[0050] The obtained electrode was subjected to Raman spectroscopy to confirm the presence or absence of fluorescence. Specifically, a laser Raman microscope (RAMAN touch, manufactured by Nanophoton Corporation, laser light source 532 nm, 1500 mW) was used to irradiate the center of the electrode with laser light at a laser power of 10 6 W / cm 2 and wavelength 51~2630cm -1 Measurements were carried out in the range of
[0051] In addition, the mass reduction rate of the obtained electrode was calculated by the following formula when the electrode was heat-treated at the decomposition temperature of the organic binder + 50°C.
[0052] Mass reduction rate = ((mass of electrode before firing - mass of electrode after firing) / mass of electrode before firing) x 100 (%)
[0053] Furthermore, the obtained electrode was subjected to DTA measurement to confirm the presence or absence of an exothermic peak and an endothermic peak in the range from the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100°C.
[0054] Next, a current collector made of a gold electrode with a thickness of 300 nm was formed on the surface of the electrode layer using a sputtering device (SC-701AT manufactured by Sanyu Electronics Co., Ltd.) Then, in an argon atmosphere with a dew point of -60°C or less, metallic sodium as a counter electrode was pressed onto the other surface of the solid electrolyte layer, and placed on the bottom lid of a coin cell, followed by covering with the top lid to prepare a CR2032 test battery.
[0055] A charge / discharge test was performed using the obtained test battery, and the initial charge / discharge capacity and average discharge voltage were measured. The results are shown in Table 1. The initial charge / discharge curve of No. 4 is shown in Figure 1. The charge / discharge test was performed by CC (constant current) charging (sodium ion absorption into the negative electrode active material) from the open circuit voltage (OCV) to 0.001V, and CC discharging (sodium ion release from the negative electrode active material) from 0.001V to 2.5V. The C rate was set to 0.1C, and the test was performed at 60°C. The charge / discharge capacity was the amount of electricity charged and discharged per unit mass of the negative electrode active material contained in the negative electrode layer.
[0056] (No.9) A test battery was prepared in the same manner as in No. 4, except that 20% cross-linked polyacrylic acid (20CLPAH manufactured by Wako Pure Chemical Industries, Ltd.) was used as the organic binder, and a charge-discharge test was carried out. The results are shown in Table 2.
[0057] (No.10) A test battery was fabricated in the same manner as No. 4, except that 100% cross-linked polyacrylic acid (100CLPAH manufactured by Wako Pure Chemical Industries, Ltd.) was used as the organic binder and the amount of N-methylpyrrolidone added was doubled, and a charge-discharge test was performed. The results are shown in Table 2.
[0058] (No.11) A test battery was prepared in the same manner as in No. 4, except that polyvinylidene fluoride (PVdF) was used as the organic binder, and a charge-discharge test was carried out. The results are shown in Table 2.
[0059] (No.12, 13) Test batteries were prepared in the same manner as No. 4, except that sodium methylcellulose (Daicel FineChem Corporation No. 1350 or No. 2200 (referred to as CMC1350 or CMC2200 in the table)) was used as the organic binder and pure water was used instead of N-methylpyrrolidone, and a charge-discharge test was performed. The results are shown in Table 2.
[0060] (No.14) A test battery was prepared in the same manner as in No. 4, except that the firing atmosphere was N2 gas, and a charge-discharge test was carried out. The results are shown in Table 2.
[0061] (No.15~19) Test batteries were prepared in the same manner as in No. 4, except that the negative electrode active materials were those shown in Table 3, and a charge-discharge test was carried out. The results are shown in Table 3.
[0062] (No.20, 21) A test battery was prepared in the same manner as No. 4, except that the positive electrode active material shown in Table 3 was used as the electrode active material. A charge / discharge test was performed on the prepared test battery. In the charge / discharge test, CC (constant current) charging (sodium ion release from the positive electrode active material) was performed from the open circuit voltage (OCV) to 4.5 V, and CC discharging (sodium ion absorption into the positive electrode active material) was performed from 4.5 V to 2.0 V. The C rate was set to 0.1 C, and the test was performed at 60°C. The charge / discharge capacity was the amount of electricity charged and discharged per unit mass of the positive electrode active material contained in the positive electrode layer.
[0063] (No.22) Graphite powder (Hitachi Chemical Co., Ltd., MAGD) was used as the electrode active material (negative electrode active material), and LLZ (Ga-doped Li7La3Zr2O 12 A test battery was fabricated in the same manner as No. 4, except that a 0.5 mm thick battery (manufactured by Toshima Manufacturing Co., Ltd.) and metallic lithium were used as the counter electrode, and a charge-discharge test was carried out. The results are shown in Table 3.
[0064] (No.23) Test batteries were prepared in the same manner as in No. 4, except that raw materials containing, by mass%, 70% hard carbon powder as the negative electrode active material, 5% acetylene black as the conductive additive, 15% polyacrylic acid as the binder, and 10% β-alumina as the solid electrolyte powder were used, and a charge-discharge test was performed. The results are shown in Table 4.
[0065] As shown in Table 1, in the examples Nos. 3 to 6, the electrode layer was subjected to Raman spectroscopy at a wavelength of 532 nm, and fluorescence was confirmed, the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50° C. was less than 0.1%, and in the DTA measurement, neither an exothermic peak nor an endothermic peak appeared between the decomposition temperature of the organic binder and the decomposition temperature of the organic binder + 100° C. Therefore, Nos. 3 to 6 were excellent in each characteristic, with an average discharge voltage of 0.07 to 0.2 V, an initial charge capacity of 102 to 483 mAh / g, and an initial discharge capacity of 19 to 290 mAh / g.
[0066] On the other hand, in the comparative examples No. 1 and No. 2, the Raman spectroscopy measurement of the electrode layer at a wavelength of 532 nm showed that no fluorescence was observed, the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50 ° C was large at 12.8% or more, and the DTA measurement showed an exothermic or endothermic peak in the range of the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100 ° C. Therefore, No. 1 and No. 2 were inferior in each characteristic, with an average discharge voltage of 0.01 to 0.03 V, an initial charge capacity of 2 to 4 mAh / g, and an initial discharge capacity of 1 to 2 mAh / g. In No. 7, the organic binder was completely decomposed and carbonized by firing, so that no organic binder remained in the electrode. Therefore, the electrode layer peeled off from the solid electrolyte layer, and the battery did not work. In No. 8, the electrode layer was prepared without using an organic binder, so there was no binding force to the solid electrolyte layer, and the electrode layer peeled off from the solid electrolyte layer when dried, and the battery did not work.
[0067] As shown in Tables 2 to 4, Nos. 9 to 13, which were based on No. 4 and had the organic binder changed, No. 14, which had the firing atmosphere changed, Nos. 15 to 22, which had the electrode active material (and solid electrolyte layer, counter electrode) changed, and No. 23, which had a solid electrolyte powder mixed in the electrode, were also subjected to Raman spectroscopy at a wavelength of 532 nm. As a result, fluorescence was confirmed, and the mass loss rate when heat-treated at the decomposition temperature of the organic binder + 50 ° C was less than 0.1%, and in the DTA measurement, neither an exothermic peak nor an endothermic peak appeared in the range from the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100 ° C (partial measurement was not performed for No. 11). Therefore, the average discharge voltage was 0.08 to 3.17 V, the initial charge capacity was 82 to 750 mAh / g, and the initial discharge capacity was 50 to 723 mAh / g, and each characteristic was excellent.
Claims
1. A sodium ion secondary battery having a secondary battery electrode containing an electrode active material powder and an organic binder, and a solid electrolyte layer, the electrode active material powder is a crystal containing Na, M (M is at least one transition metal element selected from Cr, Fe, Mn, Co, and Ni), P, O, hard carbon, titanium oxide, Sn, or Bi; The secondary battery electrode emits fluorescence when measured by Raman spectroscopy at a wavelength of 532 nm, The sodium ion secondary battery is characterized in that the secondary battery electrode is provided in contact with a surface of the solid electrolyte layer.
2. A sodium ion secondary battery having a secondary battery electrode containing an electrode active material powder and an organic binder, and a solid electrolyte layer, the electrode active material powder is a crystal containing Na, M (M is at least one transition metal element selected from Cr, Fe, Mn, Co, and Ni), P, O, hard carbon, titanium oxide, Sn, or Bi; The secondary battery electrode has a mass reduction rate of 5% or less when heat-treated at a temperature equal to or higher than a decomposition temperature of the organic binder +50°C, The sodium ion secondary battery is characterized in that the secondary battery electrode is provided in contact with a surface of the solid electrolyte layer.
3. A sodium ion secondary battery having a secondary battery electrode containing an electrode active material powder and an organic binder, and a solid electrolyte layer, the electrode active material powder is a crystal containing Na, M (M is at least one transition metal element selected from Cr, Fe, Mn, Co, and Ni), P, O, hard carbon, titanium oxide, Sn, or Bi; In the secondary battery electrode, no exothermic peak or endothermic peak appears in the range of the decomposition temperature of the organic binder to the decomposition temperature of the organic binder + 100° C. in a DTA measurement; The sodium ion secondary battery is characterized in that the secondary battery electrode is provided in contact with a surface of the solid electrolyte layer.
4. The sodium ion secondary battery according to any one of claims 1 to 3, characterized in that the secondary battery electrode is made of a sintered material containing an electrode active material powder and an organic binder.
5. The sodium ion secondary battery according to any one of claims 1 to 4, characterized in that the secondary battery electrode contains 0.1 to 30 mass % of an organic binder.
6. The sodium ion secondary battery according to any one of claims 1 to 5, characterized in that the organic binder is at least one selected from the group consisting of polyacrylic acid, sodium polyacrylate, sodium methylcellulose, polyvinylidene fluoride, styrene-butadiene rubber, polyimide and polyethylene oxide.
7. The sodium ion secondary battery according to any one of claims 1 to 6, characterized in that the secondary battery electrode further contains a solid electrolyte powder.
8. 8. The sodium ion secondary battery according to claim 7, wherein the solid electrolyte powder is a sodium ion conductive crystalline powder.
9. The sodium ion secondary battery according to claim 8, characterized in that the sodium ion conductive solid electrolyte powder is at least one selected from β-alumina, β″-alumina and NASICON crystal.
10. A method for producing a sodium ion secondary battery, comprising the steps of: firing a material containing an electrode active material powder, which is Na, M (M is at least one transition metal element selected from Cr, Fe, Mn, Co, and Ni), P, O, hard carbon, titanium oxide, Sn, or Bi, and an organic binder, within a range of −15° C. to +202° C. relative to the decomposition temperature of the organic binder, thereby providing a secondary battery electrode in contact with a surface of a solid electrolyte layer.
Citation Information
Patent Citations
Lithium secondary battery
JP1993205741A
Lithium secondary battery negative electrode, its manufacture, and secondary battery using negative electrode
JP1998172573A
Manufacturing method of negative electrode for non- aqueous electrolytic solution secondary battery
JP2002117839A
Lithium secondary cell and fabrication method thereof
JP2008034352A
All-solid battery
JP2010015782A