Hydrolyzate and laminate
A hydrolyzate composed of specific ethylene and vinyl ester copolymers, a compatibilizer, and a crosslinking agent improves adhesion and reduces foreign substances in laminates, enhancing the performance of EVOH-based packaging.
Patent Information
- Application Number
- JP2020055813
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-26
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing laminates using ethylene-vinyl alcohol copolymers (EVOH) face issues with low adhesion to thermoplastic resins due to low affinity, leading to poor adhesive strength and the presence of foreign substances like fish eyes and gel-like substances during repeated kneading.
A hydrolyzate is developed by combining specific ethylene and vinyl ester copolymers, a compatibilizer, a crosslinking agent, and a thermoplastic resin, which are melt-kneaded and then hydrolyzed to improve adhesion and reduce foreign substances.
The hydrolyzate exhibits excellent adhesion to both thermoplastic resins with few polar groups and EVOH, reducing fish eyes and gel-like substances, and is suitable for food and sanitary packaging applications.
Smart Images

Figure 0007577925000001 
Figure 0007577925000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrolysate that has excellent adhesion to both a thermoplastic resin having few polar groups and EVOH, and has excellent appearance with few foreign matters such as fish eyes and gel-like substances, and to a laminate that includes the hydrolysate as an intermediate layer. [Background technology]
[0002] Ethylene-vinyl alcohol copolymer (hereinafter referred to as "EVOH") has excellent gas barrier properties, aroma retention, and solvent resistance, and is therefore used as a packaging material for foods, beverages, medicines, etc. to prevent the contents from deteriorating. EVOH is hydrophilic and its gas barrier properties, etc. deteriorate when it absorbs moisture, so it is generally used as an intermediate layer in laminates made of thermoplastic resins with excellent water resistance, such as polyethylene and polypropylene.
[0003] However, since EVOH has many hydroxyl groups in the molecule, its affinity with thermoplastic resins that do not have polar groups is extremely low, and the two generally do not adhere to each other. For this reason, it is known to insert, as an intermediate layer between the EVOH and the thermoplastic resin, a laminate using a graft-modified ethylene-based resin composition grafted with an unsaturated carboxylic acid or its derivative (Patent Documents 1 and 2), or a composition of an ethylene-vinyl acetate copolymer, a saponified ethylene-vinyl acetate copolymer, and a tackifier (Patent Document 3), and to use the intermediate layer as an adhesive layer.
[0004] The compositions disclosed in Patent Documents 1 and 2 have excellent adhesive properties. However, when the compositions are repeatedly kneaded, the resin remaining in the extruder or die increases in viscosity and becomes discolored and gelled, resulting in the presence of numerous fish eyes and gel-like substances in the product, which poses a problem in appearance. On the other hand, the saponified ethylene-vinyl acetate copolymer disclosed in Patent Document 3 does not discolor or gel when repeatedly kneaded, and furthermore, the addition of an adhesive resin improves adhesion to EVOH. However, the adhesive strength is not sufficient, and peeling often occurs when small impacts or friction are applied during transportation or use, leaving an issue with the adhesive strength.
[0005] As a method to solve the low adhesion problem, a technology has been disclosed that uses a hydrolysate of a resin composition containing ethylene-vinyl acetate copolymers with different vinyl acetate contents and their graft modified products. Although the hydrolysate has good adhesion and exhibits a certain level of performance in terms of appearance, further improvement is desired. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 61-270155 [Patent Document 2] Japanese Patent Publication No. 62-158043 [Patent Document 3] Japanese Patent Application Publication No. 7-108655 [Patent Document 4] Patent Publication No. 2017-210608 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a hydrolysate that has excellent adhesion to both a thermoplastic resin having few polar groups and EVOH, has few foreign matter such as fish eyes and gel-like substances, and has an excellent appearance, and a laminate that includes the hydrolysate as an intermediate layer. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors conducted intensive research to solve the above problems and discovered that a hydrolysate obtained by hydrolyzing a composition containing specific components is free of foreign matter and has excellent adhesion to a layer containing a thermoplastic resin and an EVOH layer, thereby solving the problems of the present invention.
[0009] That is, the present invention relates to a hydrolysate of a melt-kneaded product containing (A) a copolymer of ethylene and a vinyl ester having a vinyl ester content of 3.5 mol% or more and 7.0 mol% or less, (B) a copolymer of ethylene and a vinyl ester having a vinyl ester content of 17 mol% or more and 75 mol% or less, (C) a compatibilizer, (D) a crosslinking agent, and (E) a thermoplastic resin that satisfies the following requirements (1) and (2): (1) Vinyl ester content is less than 3.5 mol%. (2) The melt mass-flow rate at 190°C under a load of 2.16 kg is higher than the melt mass-flow rate of an ethylene and vinyl ester copolymer (A) having a vinyl ester content of 3.5 mol% or more and 7.0 mol% or less, and the melt mass-flow rate of an ethylene and vinyl ester copolymer (B) having a vinyl ester content of 17 mol% or more and 75 mol% or less. Effect of the Invention
[0010] According to the present invention, it is possible to provide a hydrolysate that has excellent adhesion to thermoplastic resins with few polar groups and EVOH, and combines mechanical properties and appearance, and that can be suitably used for food packaging and sanitary packaging, and a laminate including a layer of the hydrolysate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The resin composition according to one embodiment of the present invention will be described in detail below.
[0012] The hydrolysate of the present invention is a hydrolysate of a melt-kneaded product containing (A) a copolymer of ethylene and a vinyl ester having a vinyl ester content of 3.5 mol% or more and 7.0 mol% or less, (B) a copolymer of ethylene and a vinyl ester having a vinyl ester content of 17 mol% or more and 75 mol% or less, (C) a compatibilizer, (D) a crosslinking agent, and (E) a thermoplastic resin that satisfies the following requirements (1) and (2) (hereinafter referred to as "the hydrolysate of the present invention"). (1) Vinyl ester content is less than 3.5 mol%. (2) The melt mass-flow rate at 190°C under a load of 2.16 kg is higher than the melt mass-flow rate of an ethylene and vinyl ester copolymer (A) having a vinyl ester content of 3.5 mol% or more and 7.0 mol% or less, and the melt mass-flow rate of an ethylene and vinyl ester copolymer (B) having a vinyl ester content of 17 mol% or more and 75 mol% or less.
[0013] More specifically, the composition of the present invention is a composition obtained by hydrolysis treatment (hereinafter also referred to as "hydrolysate") containing a graft modified product (hereinafter also referred to as "graft modified product") of a composition of an ethylene and vinyl ester copolymer (A) having a vinyl ester content of 3.5 mol% or more and 7.0 mol% or less, an ethylene and vinyl ester copolymer (B) having a vinyl ester content of 17 mol% or more and 75 mol% or less, a compatibilizer (C), and a specific thermoplastic resin (E). The graft modified product can be, for example, a product obtained by crosslinking the compositions (A), (B), (C), and (E) above. Examples of the crosslinking treatment include a method in which a crosslinking agent such as a peroxide is added to the composition and the composition is melt-kneaded, and a method using electron beam irradiation. The graft modified product is preferably a product that has been crosslinked by the melt-kneading method.
[0014] The ethylene and vinyl ester copolymer (A) (hereinafter referred to as component (A)) in the present invention having a vinyl ester content of 3.5 mol % or more and 7.0 mol % or less is specifically a copolymer having ethylene residue units and vinyl ester residue units.
[0015] Examples of the vinyl ester in component (A) include aliphatic vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, and vinyl stearate, and aromatic vinyl esters such as vinyl benzoate, etc. From the viewpoint of cost, component (A) is preferably an ethylene-vinyl acetate copolymer.
[0016] The vinyl ester content of component (A) is from 3.5 mol % to 7.0 mol %, and most preferably from 4.5 mol % to 6.5 mol %, from the viewpoint of adhesion to a thermoplastic resin layer when laminated.
[0017] Here, when the components (B), (C), and (E) described below are copolymers of ethylene and vinyl ester, the component (A) is different from the other components in at least one of the vinyl ester content, the melt mass flow rate, and the density. The vinyl ester content of the component (A) is less than that of the component (B). It is also preferable that the vinyl ester content of the component (A) is less than that of the component (C) and more than that of the component (E).
[0018] The melt mass flow rate (hereinafter referred to as "MFR") of component (A) at 190°C under a load of 2.16 kg is preferably 0.5 g / 10 min or more and 40 g / 10 min or less, and most preferably 3 g / 10 min or more and 35 g / 10 min or less.
[0019] The method for producing the ethylene-vinyl acetate copolymer in component (A) is not particularly limited as long as it allows the production of an ethylene-vinyl acetate copolymer, and examples of the method include known production methods such as high-pressure radical polymerization, solution polymerization, and latex polymerization. Such resins can be conveniently selected from commercially available products, and are commercially available from Tosoh Corporation under the trade name Ultrathene.
[0020] In the present invention, examples of the copolymer (B) of ethylene and a vinyl ester having a vinyl ester content of 17 mol % or more and 75 mol % or less (hereinafter referred to as component (B)) include aliphatic vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, and vinyl stearate, and aromatic vinyl esters such as vinyl benzoate, among which ethylene-vinyl acetate copolymers are preferred from the viewpoint of cost.
[0021] The vinyl ester content of component (B) is from 17 mol % to 75 mol %, and most preferably from 17 mol % to 40 mol %, in order to further improve the adhesion between the hydrolysate of the present invention and EVOH.
[0022] The MFR of component (B) at 190° C. under a load of 2.16 kg is preferably 0.5 g / 10 min or more and less than 75 g / 10 min.
[0023] The method for producing the ethylene-vinyl acetate copolymer in component (B) is not particularly limited as long as it allows production of the ethylene-vinyl acetate copolymer, and examples of such methods include known production methods such as high-pressure radical polymerization, solution polymerization, and latex polymerization. Such resins can be conveniently selected from commercially available products, and are commercially available under the trade names Ultrathene from Tosoh Corporation and Levaprene and Levamelt from Lanxess KK, respectively.
[0024] The graft modified product of the present invention before the hydrolysis treatment of the hydrolyzate further contains a compatibilizer (C) (hereinafter referred to as "component (C)") in addition to components (A) and (B). Component (C) is added to enhance the dispersibility of components (A) and (B).
[0025] Component (C) is preferably a copolymer of ethylene and a vinyl ester, in which case component (C) has a higher vinyl ester content than component (A) and a lower vinyl ester content than component (B). The vinyl ester content of component (C) is preferably in the range of 7.5 mol % or more and 16 mol % or less.
[0026] Examples of the vinyl ester of component (C) include aliphatic vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, and vinyl stearate; and aromatic vinyl esters such as vinyl benzoate.
[0027] When component (C) contains a copolymer of ethylene and a vinyl ester, the polymer may be used alone or in a composition containing two or more types of copolymers, but it is preferable to use two or more types of copolymers of ethylene and a vinyl ester, which improves the dispersibility of components (A) and (B), improves the adhesion of the hydrolyzate of the present invention to thermoplastic resins and EVOH, and contributes to reducing fish eyes and gels.
[0028] When component (C) is a composition containing at least two types of ethylene and vinyl ester copolymers, the components of the composition are different in at least one of the vinyl ester content, melt mass flow rate, and density, and preferably the vinyl ester content of each component of the composition is different.
[0029] When two or more types of copolymers of ethylene and vinyl ester are used as the compatibilizer (C), the difference in the content of each vinyl ester is preferably within 8 mol %, and most preferably within 5 mol %.
[0030] A suitable blending ratio of components (A), (B), and (C) in the saponified product is, in order to reduce foreign matter such as fish eyes and gels and to improve adhesion to the thermoplastic resin and EVOH of the present application, 4 to 95 parts by weight of component (A), 4 to 95 parts by weight of component (B), and 1 to 50 parts by weight of component (C) (the total of (A), (B), and (C) is 100 parts by weight), more preferably 15 to 90 parts by weight of component (A), 5 to 75 parts by weight of component (B), and 5 to 45 parts by weight of component (C), and even more preferably 15 to 80 parts by weight of component (A), 15 to 50 parts by weight of component (B), and 5 to 40 parts by weight of component (C).
[0031] The graft-modified product of the hydrolyzate of the present invention before the hydrolysis treatment further contains a thermoplastic resin (E) (hereinafter referred to as "component (E)") in addition to components (A), (B), and (C).
[0032] Examples of component (E) include polyolefins, and more specifically, examples thereof include homopolymers of α-olefins having 2 to 12 carbon atoms, such as ethylene, propylene, and 1-butene, copolymers of such olefins, ethylene-vinyl ester copolymers, and ethylene-acrylic acid ester copolymers.
[0033] Component (E) is preferably a copolymer of ethylene and vinyl ester. When the above-mentioned components (A), (B), and (C) are copolymers of ethylene and vinyl ester, component (E) is different from the other components in at least one of the vinyl ester content, melt mass flow rate, and density. Preferably, the vinyl ester content of component (E) is different from the vinyl ester content of the other components, and the vinyl ester content of component (E) is preferably lower than the vinyl ester content of any of components (A), (B), and (C).
[0034] Specifically, the vinyl ester content in component (E) is preferably in the range of 0.1 mol % or more and 3.4 mol % or less.
[0035] Furthermore, the MFR of component (E) at 190° C. under a load of 2.16 kg is higher than the MFRs of both components (A) and (B). The MFR of component (E) is preferably 75 g / 10 min or more.
[0036] Examples of the component (E) include ethylene polymers such as high-pressure low-density polyethylene, high-density polyethylene, medium-density polyethylene, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid ester copolymer, polypropylene, propylene-ethylene copolymer, propylene-1-butene copolymer, poly-1-butene, poly-1-hexene, and poly-4-methyl-1-pentene. The thermoplastic resin (E) may be used alone or in combination of two or more.
[0037] Among these, from the viewpoints of adhesion of the hydrolysate of the present invention to thermoplastic resins such as polyethylene and polypropylene, and cost, at least one of the group consisting of high-pressure low-density polyethylene, high-density polyethylene, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-vinyl acetate copolymer, and polypropylene is most preferred.
[0038] The method for producing high-pressure low-density polyethylene can be exemplified by high-pressure radical polymerization, and such resins can be conveniently selected from commercially available products, for example, those available from Tosoh Corporation under the trade name Petrocene. The method for producing high-density polyethylene, ethylene-1-butene copolymer, and ethylene-1-hexene copolymer is not particularly limited, and examples thereof include high-, medium-, and low-pressure ionic polymerization methods using Ziegler-Natta catalysts, Phillips catalysts, and metallocene catalysts, and such resins can be conveniently selected from commercially available products, for example, those available from Tosoh Corporation under the trade names Nipolon Hard, Nipolon-L, and Nipolon-Z.
[0039] The method for producing ethylene-vinyl acetate copolymer is not particularly limited as long as it is possible to produce a copolymer of ethylene and vinyl ester, but examples thereof include the well-known high-pressure radical polymerization method and ionic polymerization method. An ethylene-vinyl acetate copolymer produced by high-pressure radical polymerization method is commercially available from Tosoh Corporation under the trade name Ultrathene.
[0040] The method for producing polypropylene is not particularly limited, but for example, it can be obtained by polymerizing propylene or copolymerizing propylene and one or more other α-olefins in the presence of a single-site catalyst, typically a catalyst formed from a solid titanium catalyst component and an organometallic compound catalyst component, or a catalyst formed from both of these components and an electron donor, or a metallocene catalyst. Such resins can be conveniently selected from commercially available products. For example, they are commercially available from Japan Polypropylene Corporation under the trade names Novatec and Wintech, respectively.
[0041] The amount of component (E) added is preferably 0.1 to 40 parts by weight per 100 parts by weight of the total of components (A), (B) and (C).
[0042] The hydrolyzate of the present invention is obtained by hydrolyzing a graft modified product obtained by crosslinking the composition (A), (B), (C), and (E). Here, the crosslinking treatment can be exemplified by a method of adding a crosslinking agent such as a peroxide to the composition and melt-kneading the composition, or a method of irradiating the composition with an electron beam, and the graft modified product is preferably treated by the melt-kneading method. When using the melt-kneading method, it is preferable to include a crosslinking agent (hereinafter referred to as component (D)).
[0043] The component (D) is not particularly limited as long as it is an organic peroxide, and examples thereof include dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,3-di-(t-butylperoxy)-diisopropylbenzene, n-butyl-4,4-bis(t-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, t-butylperoxybenzoate, t-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and t-butylcumyl peroxide. These can be used alone or in combination of two or more kinds. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 1,1-di(t-butylperoxy)cyclohexane are preferably used from the viewpoint of reactivity, and such crosslinking agents (D) can be conveniently selected from commercially available products, and are commercially available from NOF Corporation under the trade names Perhexa 25B and Perhexa C, respectively.
[0044] In order to improve the dispersibility of the crosslinking agent during melt kneading, any one of components (A), (B) and (C) may be impregnated with the crosslinking agent (D).
[0045] Furthermore, together with the crosslinking agent (D), a crosslinking assistant such as triallyl isocyanurate or divinylbenzene may be used, if necessary. The amount of the crosslinking agent (D) is preferably in the range of 0.005 to 1 part by weight based on 100 parts by weight of the total of the components (A), (B) and (C), which is preferable from the viewpoint of moldability and improves the adhesion of the hydrolyzate of the present invention to EVOH.
[0046] In the present invention, a specific example of a production process for obtaining a melt-kneaded product containing a graft modified product is as follows.
[0047] The dry blend of the components (A) to (E) is charged into a hopper of an extruder. At this time, at least a part of the components (A) to (E) may be added from a side feeder or the like. Furthermore, two or more extruders may be used to sequentially melt-knead the components (A) to (E) in a stepwise manner. A Henschel mixer, a V blender, a ribbon blender, a tumbler, or the like may be used to dry-blend the components (A) to (E).
[0048] In addition to the above-mentioned components, additives such as crosslinking aids, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, etc., which are usually used in polyolefins such as polyethylene and polypropylene, may be added as necessary.
[0049] The method of melt-kneading the components (A) to (E) is not particularly limited as long as the melt-kneading device can uniformly disperse each component, and production can be performed using a commonly used resin mixing device. Examples of melt-kneading devices include single-screw extruders, multi-screw extruders, Banbury mixers, pressure kneaders, and rotating rolls. Among them, twin-screw extruders, which have a high degree of kneading and can be operated continuously, are preferred because they can achieve a fine and uniform dispersion state. The melting temperature is preferably in the range of the melting point of component (A) to about 260°C. By melt-kneading at the above temperature, a melt-kneaded product containing a graft modified product can be obtained.
[0050] The hydrolysis method for obtaining the hydrolysate of the present invention is preferably a method of directly hydrolyzing pellets or powder of the melt-kneaded product containing the graft modified product in an alkali from the viewpoint of productivity. As the alkali, an alcohol solution in which sodium hydroxide is dissolved is preferably used. As the alcohol, it is preferable to use methanol, which is excellent in terms of cost, and the concentration of sodium hydroxide is preferably adjusted in the range of 0.1 to 10% by weight. The temperature of the hydrolysis treatment is appropriately set depending on the desired saponification degree, and when methanol is used as the alcohol, it is preferably adjusted in the range of 30 to 65°C under normal pressure conditions. If the hydrolysis does not proceed easily under normal pressure conditions, it may be performed under pressurized conditions.
[0051] The degree of saponification can be determined from the difference in vinyl ester content between the molten kneaded product and the hydrolyzate, and the vinyl ester content can be measured in accordance with JIS K7192 (1999).
[0052] In the hydrolysate of the present invention, the vinyl ester component of the melt-kneaded product containing the components (A) to (E) preferably has a degree of saponification of 10% by weight or more. If the degree of saponification is 10% by weight or more, the adhesion to EVOH is sufficient.
[0053] The hydrolysate of the present invention can be used in any form, such as pellets or powder.
[0054] The laminate according to one embodiment of the present invention will be described in detail below.
[0055] The hydrolysate of the present invention may be used as a laminate comprising a layer of the hydrolysate and at least one layer of another material (hereinafter referred to as "the laminate of the present invention").
[0056] The laminate of the present invention is preferably a laminate having a layer made of the hydrolyzate and at least one layer of a thermoplastic resin group such as polyolefins such as polyethylene and polypropylene, polyesters such as polylactic acid and polybutylene terephthalate, polyamides such as nylon, and EVOH. It may also have a laminate structure having a combination of two or more of these or a combination of various resin layers. In particular, from the viewpoints of cost and moldability, those having a thermoplastic resin with few polar groups such as polyethylene or polypropylene, and EVOH are preferred.
[0057] The laminate is preferably an outer layer made of a thermoplastic resin having few polar groups / a layer of the hydrolyzate of the present invention / an EVOH layer laminated in this order, and more preferably an outer layer made of a thermoplastic resin having few polar groups / a layer of the hydrolyzate of the present invention / an EVOH layer / a layer of the hydrolyzate of the present invention / an inner layer made of a thermoplastic resin having few polar groups. The laminate of the present invention can be molded using a normal molding device, and examples of the molding method include any method such as extrusion molding, blow molding, sheet molding, injection molding, compression molding, calendar molding, and vacuum molding, and can be molded into a sheet, film, pipe, block, or other arbitrary shape. By adopting a laminate structure with other materials, it is possible to impart the properties of the other materials, such as gas barrier properties, mechanical properties, oil resistance, and weather resistance, to the laminate.
[0058] The laminate of the present invention can be used as a packaging material or container made of a thermoplastic resin for foods, beverages, medicines, etc., which require these properties. EXAMPLES
[0059] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0060] [Melt Mass Flow Rate (MFR)] Measurements were performed in accordance with JIS K6922-1 (1997). [Saponification degree] Each of the hydrolysates obtained in the examples was measured in accordance with JIS K7192 (1999). [Film appearance] A monolayer film having a thickness of 50 μm was produced using each hydrolyzate obtained in the examples. The monolayer film was produced using a monolayer cast film molding machine (manufactured by Sumiju Modern Co., Ltd.) at a set temperature of 200° C. The obtained monolayer film was cut into a 10 cm × 10 cm piece, and the presence or absence of fisheyes of 0.3 mm or more in the film was observed. If there were 100 or more fisheyes (foreign matter) of 0.3 mm or more, the film was marked with "X", if there were 50 or more but less than 100, the film was marked with "△", and if there were less than 50, the film was marked with "O". [Interlaminar adhesion strength (peel strength)] Using each hydrolyzate obtained in the examples, a three-kind five-layer film including a thermoplastic resin layer (polyethylene) and an ethylene-vinyl alcohol layer was produced. The three-kind five-layer film was produced using a multilayer cast film molding machine (manufactured by Plastics Engineering Research Institute Co., Ltd.) at a set temperature of 200°C, and the film structure was a thermoplastic resin layer / hydrolyzate layer / ethylene-vinyl alcohol copolymer layer / hydrolyzate layer / thermoplastic resin layer, with thicknesses of 20μm / 10μm / 10μm / 10μm / 20μm, respectively. The interlayer adhesive strength (peel strength) between the thermoplastic resin layer / hydrolyzate layer or between the hydrolyzate layer / ethylene-vinyl alcohol copolymer layer of the three-kind five-layer film was measured using a tensile tester (300mm / min, T-type peel) after peeling a part of the interlayer at the end of the three-kind five-layer film, cutting out the film at intervals of 15mm in the direction of resin flow (MD direction). If peeling between layers is difficult, it is possible to peel relatively easily by immersing the end of the three-kind five-layer film in a methanol solution for 1 to 2 minutes.
[0061] The interlayer adhesive strength measurement was repeated 3 to 5 times for the same sample. Adhesive strength less than 2.5 N / 15 mm was considered to be poor adhesion, and 2.5 N / 15 mm or more was considered to be good adhesion. The thermoplastic resin (polyethylene) and EVOH used in film molding were as follows. (1) Polyethylene: Melt mass flow rate 2g / 10min, density 923kg / m 3High-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 226) (2) EVOH: Ethylene-vinyl alcohol copolymer with a melt mass flow rate of 1.7 g / 10 min and an ethylene content of 32 mol% (Kuraray Co., Ltd., product name EVAL F171B)
[0062] [Example 1] Component (A) has a MFR of 14g / 10min and a density of 935kg / m 3 45 parts by weight of an ethylene-vinyl acetate copolymer having a vinyl acetate content of 5.4 mol% (15% by weight) (manufactured by Tosoh Corporation, trade name Ultrathene 625) (hereinafter sometimes abbreviated as component (A-1)), Component (B) has a MFR of 70g / 10min and a density of 968kg / m 3 45 parts by weight of an ethylene-vinyl acetate copolymer having a vinyl acetate content of 19 mol% (42% by weight) (manufactured by Tosoh Corporation, trade name Ultrathene 760, hereinafter sometimes abbreviated as component (B-1)), 10 parts by weight of the following component (C-1) as a compatibilizer (C), [Component (C-1)] A dry blend of the following three types of ethylene-vinyl acetate copolymers, each at 3.3 parts by weight: ·MFR20g / 10min, density 940kg / m 3 , an ethylene-vinyl acetate copolymer with a vinyl acetate content of 20% by weight (manufactured by Tosoh Corporation, product name Ultrathene 633) ·MFR18g / 10min, density 949kg / m 3 , an ethylene-vinyl acetate copolymer with a vinyl acetate content of 28% by weight (manufactured by Tosoh Corporation, trade name Ultrathene 710) ·MFR30g / 10min, density 954kg / m 3 , an ethylene-vinyl acetate copolymer with a vinyl acetate content of 32% by weight (manufactured by Tosoh Corporation, product name Ultrathene 750) 0.02 parts by weight of an organic peroxide (manufactured by NOF Corp., trade name Perhexa 25B, hereinafter sometimes abbreviated as component (D-1)) as a crosslinking agent (D); Component (E) has a MFR of 75g / 10min and a density of 923kg / m 35 parts by weight of an ethylene-vinyl acetate copolymer having a vinyl acetate content of 2.0 mol% (6 wt%) (manufactured by Tosoh Corporation, trade name Ultrathene 530) (hereinafter sometimes abbreviated as component (E-1)), The mixture was dry-blended in a ratio of 1:1 and melt-kneaded in a twin-screw extruder at a set temperature of 190°C to obtain a pellet-shaped melt-kneaded product containing the graft-modified product. The resulting melt-kneaded product containing the graft-modified product was then hydrolyzed in a 2% by weight solution of sodium hydroxide in methanol at 55°C to obtain a hydrolyzate. The obtained hydrolyzate was used to evaluate the film appearance and adhesion, and the results are shown in Table 1. In Table 1, the numerical values for each component represent parts by weight.
[0063] [Example 2] Instead of component (E-1), MFR 145g / 10min, density 915kg / m 3 A hydrolyzate was obtained in the same manner as in Example 1, except that 5 parts by weight of high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 353) (hereinafter sometimes abbreviated as component (E-2)) was added. The obtained hydrolyzate was used to evaluate the film appearance and adhesion, and the results are shown in Table 1.
[0064] [Example 3] A hydrolysate was obtained in the same manner as in Example 1, except that the amount of component (A-1) was changed to 70 parts by weight, and 20 parts by weight of an ethylene-vinyl acetate copolymer (manufactured by LANXESS KK, trade name Levaprene 500, hereinafter sometimes abbreviated as component (B-2)) with MFR of 5 g / 10 min and vinyl acetate content of 57 mol % (50 wt %) was added instead of component (B-1). The obtained hydrolysate was used to evaluate the film appearance and adhesion, and the results are shown in Table 1.
[0065] [Example 4] Except for changing the amount of component (E-1) to 0.5 parts by weight, a hydrolysate was obtained in the same manner as in Example 1. The obtained hydrolysate was used to evaluate the film appearance and adhesiveness, and the results are shown in Table 1.
[0066] [Example 5] Except for changing the amount of component (E-1) to 30 parts by weight, a hydrolysate was obtained in the same manner as in Example 1. The obtained hydrolysate was used to evaluate the film appearance and adhesion, and the results are shown in Table 1.
[0067] [Example 6] Except for changing the amount of component (E-1) to 40 parts by weight, a hydrolysate was obtained in the same manner as in Example 1. The obtained hydrolysate was used to evaluate the film appearance and adhesion, and the results are shown in Table 1.
[0068] [Comparative Example 1] Instead of component (E-1), MFR 8g / 10min, density 919kg / m 3 A hydrolysate was obtained in the same manner as in Example 1, except that 5 parts by weight of high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 203) (hereinafter sometimes abbreviated as component (E-3)) was added. The obtained hydrolysate was used to evaluate the film appearance and adhesion to LDPE and EVOH, and the results are shown in Table 2. In Table 2, the value of each component represents parts by weight. The obtained film had poor appearance.
[0069] [Comparative Example 2] A hydrolysate was obtained in the same manner as in Example 1, except that component (C) was not added. The obtained hydrolysate was used to evaluate the film appearance and adhesion to LDPE and EVOH, and the results are shown in Table 2. The obtained film had poor adhesion to the EVOH layer.
[0070] [Comparative Example 3] A hydrolysate was obtained in the same manner as in Example 1, except that component (D) was not added. The obtained hydrolysate was used to evaluate the film appearance and adhesion to LDPE and EVOH, and the results are shown in Table 2. The obtained film had poor adhesion to the EVOH layer.
[0071] [Comparative Example 4] A hydrolysate was obtained in the same manner as in Example 1, except that component (E) was not added. The obtained hydrolysate was used to evaluate the film appearance and adhesion to LDPE and EVOH, and the results are shown in Table 2. The obtained film had poor appearance.
[0072] [Comparative Example 5] A melt-kneaded product containing a graft modified product was obtained in the same manner as in Example 1, except that no hydrolysis treatment was performed. The obtained melt-kneaded product containing a graft modified product was used to evaluate the film appearance and adhesion to LDPE and EVOH, and the results are shown in Table 2. The obtained film had poor adhesion to the EVOH layer.
[0073] [Table 1]
[0074] [Table 2]
Claims
1. Ethylene and vinyl ester having a vinyl ester content of 3.5 mol % or more and 7.0 mol % or less A copolymer (A) of a vinyl ester and an ethylene glycol having a vinyl ester content of 17 mol % or more and 75 mol % or less. (B) a copolymer of ethylene and vinyl ester, (C) a compatibilizer, (D) a crosslinking agent, and A hydrolysate of a melt-kneaded product containing a thermoplastic resin (E) that satisfies the requirements (1) and (2). (1) At least one member selected from the group consisting of homopolymers of α-olefins having 2 to 12 carbon atoms, copolymers thereof, and copolymers of ethylene and vinyl esters having a vinyl ester content of 0.1 mol % or more and 3.4 mol % or less. (2) The melt mass flow rate at 190°C under a load of 2.16 kg is vinyl ester. A copolymer of ethylene and a vinyl ester having a ter content of 3.5 mol % or more and 7.0 mol % or less. The melt mass flow rate of the polymer (A) and the vinyl ester content are 17 mol% or more. Melt mass flow rate of 5 mol % or less of ethylene and vinyl ester copolymer (B) Higher than
2. The compatibilizer (C) is a copolymer of ethylene and vinyl ester, and the vinyl ester content is 7. . At least 5 mol % to 16 mol % of ethylene and vinyl ester copolymer The hydrolysate according to claim 1 , further comprising one kind of
3. Ethylene and vinyl ester having a vinyl ester content of 3.5 mol % or more and 7.0 mol % or less (A) a copolymer with ethyl acetate having a vinyl ester content of 17 mol % or more and 75 mol % or less; For a total of 100 parts by weight of the copolymer of ethylene and vinyl ester (B) and the compatibilizer (C), 3. The composition according to claim 1 or 2, further comprising 0.1 parts by weight or more and 40 parts by weight or less of a thermoplastic resin (E). The hydrolysate described.
4. A laminate comprising a layer made of the hydrolysate according to any one of claims 1 to 3.
5. A layer containing a thermoplastic resin / a layer containing the hydrolysate according to any one of claims 1 to 3 / A laminate in which layers containing ethylene-vinyl alcohol copolymers are laminated in order.
Citation Information
Patent Citations
Laminated structure
JP1986270155A
laminate
JP1987158043A
Thermoplastic resin composition
JP1993070635A
Laminate having gas barrier properties
JP1995108655A
Adhesive and laminate containing the same
JP2017210608A