Toner and Developer

A toner with a controlled binder resin and ester wax ratio and particle size effectively addresses hot offset and replenishment issues, ensuring reliable operation in low-temperature fixing processes.

JP7577928B2Active Publication Date: 2024-11-06RICOH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020071921
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-19
Filing Date
2020-04-13
Publication Date
2024-11-06
Estimated Expiration
2040-04-13

AI Technical Summary

Technical Problem

Toner used for low-temperature fixing tends to adhere to fixing rollers, causing hot offset, and wax oozes out during replenishment with a Mono pump, leading to filming and replenishment failures.

Method used

A toner formulation with a specific ratio of binder resin and ester wax, characterized by a FTIR-ATR mapping wave number ratio of 2850cm to 828cm absorption peaks between 0.10 and 0.19, and a volume average particle diameter of 4.9 to 5.5 μm, which suppresses filming and replenishment failures.

Benefits of technology

The toner achieves excellent low-temperature fixability, hot offset resistance, and prevents filming and replenishment failures when using a Mono pump.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577928000001
    Figure 0007577928000001
  • Figure 0007577928000002
    Figure 0007577928000002
  • Figure 0007577928000003
    Figure 0007577928000003
Patent Text Reader

Abstract

To provide a toner that is excellent in low-temperature fixability and hot offset resistance and can prevent filming and faulty supply during the use of a mohnopump.SOLUTION: A toner contains a binder resin and a mold release agent. In the toner, the average value of the intensity ratios of an absorption spectrum peak at a wave number of 2850 cm-1 to an absorption spectrum peak at a wave number of 828 cm-1, which is obtained by FTIR-ATR mapping, is 0.10 to 0.19. In the toner, the ratio at which the intensity ratio of the absorption spectrum peak at a wave number of 2850 cm-1 to the absorption spectrum peak at a wave number of 828 cm-1 is 0.20 or more, which is obtained by FTIR-ATR mapping, is 5 to 10%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to toners and developers. [Background technology]

[0002] 2. Description of the Related Art In recent years, in the field of electrophotographic image forming technology, competition has intensified to develop color image forming apparatuses capable of forming images at high speed and with low power consumption.

[0003] In order to form images at high speed and with low power consumption, it is necessary to reduce the amount of heat required to fix a toner image.

[0004] Therefore, in order to improve the low-temperature fixing property of the toner, a toner containing a binder resin and a releasing agent is used.

[0005] However, such toner has the problem that it adheres to the fixing roller or fixing belt, causing hot offset.

[0006] Patent Document 1 describes a toner having toner particles containing a binder resin and wax, in which, in a toner cross section observed with a transmission electron microscope, the ratio of the area occupied by the wax in a surface region up to 1.0 μm from the toner surface is defined as As, and the ratio of the area occupied by the wax in an internal region inside the surface region is defined as Ac, as expressed by the formula 18.0%≧As≧1.5% (1) 10.0≧Ac / As≧2.0 (2) A toner that satisfies the above requirements is disclosed. Summary of the Invention [Problem to be solved by the invention]

[0007] However, there is a problem in that the wax adheres to the photoreceptor, causing filming.

[0008] In addition, when toner is replenished using a mono pump, wax seeps out of the toner, causing the toner to adhere to the rotor inside the mono pump. As a result, a gap is created between the rotor and the stator, reducing the differential pressure and resulting in poor toner replenishment.

[0009] Here, the mono pump is a single-shaft eccentric screw pump whose main components are a rotor and a stator. The mono pump requires a high level of sealing between the rotor and the stator due to its structure, so friction between the rotor and the stator generates heat, which causes wax to seep out of the toner.

[0010] An object of one aspect of the present invention is to provide a toner that is excellent in low-temperature fixing property and hot offset resistance, and is capable of suppressing filming and supply failure when using a mono pump. [Means for solving the problem]

[0011] In one embodiment of the present invention, a toner contains a binder resin and a release agent, and is characterized in that the toner has a wavelength of 828 cm by FTIR-ATR mapping. -1 The wavenumber for the absorption spectrum peak at 2850 cm -1 The average intensity ratio of the absorption spectrum peaks in the sample is 0.10 to 0.19, and the proportion of the intensity ratios that are 0.20 or more is 5 to 10%. The volume average particle size is 4.9 to 5.5 μm, and the release agent is an ester wax. do. Effect of the Invention

[0012] According to one aspect of the present invention, it is possible to provide a toner that is excellent in low-temperature fixing property and hot offset resistance, and is capable of suppressing filming and supply failure when using a mono pump. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described.

[0014] (toner) The toner of the present embodiment contains a binder resin and a release agent (wax), and may further contain a colorant, a charge control agent, and the like, as necessary.

[0015] The toner of this embodiment can be used to develop an electrostatic latent image formed on a photoconductor.

[0016] The toner of the present embodiment has a wave number of 828 cm by FTIR-ATR mapping. -1 The wavenumber for the absorption spectrum peak at 2850 cm -1 The intensity ratio of the absorption spectrum peaks (PI 2850 / PI 828 The average value of the PI of the toner is 0.10 to 0.19. 2850 / PI 828 If the average value is less than 0.10, the hot offset resistance of the toner decreases, and if it exceeds 0.19, filming and poor supplying when using a mono pump occur.

[0017] The toner of the present embodiment is PI 2850 / PI 828 The percentage of toner with a PI of 0.2 or more is 5 to 10%. 2850 / PI 828 If the ratio of 0.2 or more is less than 5%, the hot offset resistance of the toner decreases, and if it exceeds 10%, filming and supply failure when using a mono pump occur.

[0018] Here, P.I. 2850 is the intensity of the peak due to the release agent, and PI 828 is the intensity of the peak derived from the binder resin, so PI 2850 / PI 828 is the relative amount of release agent near the surface of the toner.

[0019] PI of the toner of this embodiment 2850 / PI 828 The half-value width of the histogram of the frequency of the toner of the present embodiment is preferably 0.10 to 0.13, and more preferably 0.10 to 0.11. 2850 / PI828 When the half-width of the frequency histogram is 0.10 or more, the hot offset resistance of the toner is further improved, and when it is 0.13 or less, the hot offset resistance of the toner is further improved and filming and supply failure when using a mono pump can be further suppressed.

[0020] The toner of this embodiment has a volume average particle diameter of preferably 4.9 to 5.5 μm, and more preferably 4.9 to 5.2 μm. When the toner of this embodiment has a volume average particle diameter of 4.9 μm or more, filming can be further suppressed, and when the toner has a volume average particle diameter of 5.5 μm or less, the hot offset resistance of the toner is further improved.

[0021] The toner in this embodiment may be either a magnetic toner or a non-magnetic toner.

[0022] (Binding resin) The binder resin can be appropriately selected from known binder resins used in toners.

[0023] Examples of the binder resin include polyester, polystyrene, poly(p-chlorostyrene), polyvinyltoluene, and other styrene homopolymers or derivatives thereof; styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, and styrene-α-chloromethyl methacrylate copolymers. Examples of the copolymers include styrene copolymers such as acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, and aromatic petroleum resins, and two or more of them may be used in combination. Among these, polyester is preferred in terms of low-temperature fixing property and gloss of full-color images.

[0024] Examples of polyester include unmodified polyester (hereinafter referred to as unmodified polyester), urea-modified polyester, and the like.

[0025] The unmodified polyester can be synthesized, for example, by polycondensing a polyhydric alcohol and a polycarboxylic acid at 120 to 230° C. in an inert gas atmosphere, if necessary, using a known esterification catalyst.

[0026] The polyhydric alcohol can be appropriately selected from known polyhydric alcohols used in the synthesis of unmodified polyesters.

[0027] Examples of polyhydric alcohols include alkylene glycols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol; polyalkylene glycols such as diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polybutylene glycol; alicyclic dialcohols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alkylene oxide adducts of alicyclic dialcohols obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to alicyclic dialcohols; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to bisphenols. Two or more of these may be used in combination. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols and mixtures of alkylene oxide adducts of bisphenols and alkylene glycols having 2 to 12 carbon atoms are particularly preferred.

[0028] The polybasic carboxylic acid can be appropriately selected from known polybasic carboxylic acids used in the synthesis of unmodified polyesters.

[0029] As the polyvalent carboxylic acid, a divalent carboxylic acid, a trivalent or higher carboxylic acid, a mixture of a divalent carboxylic acid and a trivalent or higher carboxylic acid, etc. Among these, a divalent carboxylic acid or a mixture of a divalent carboxylic acid and a trivalent or higher carboxylic acid is preferred.

[0030] Examples of the divalent carboxylic acid include alkylene dicarboxylic acids such as succinic acid, adipic acid, and sebacic acid, alkenylene dicarboxylic acids such as maleic acid and fumaric acid, and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalene dicarboxylic acid, and two or more of these may be used in combination. Among these, alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred.

[0031] Examples of trivalent or higher carboxylic acids include trivalent or higher aromatic carboxylic acids such as trimellitic acid and pyromellitic acid, and two or more of them may be used in combination. Among these, trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms are preferred.

[0032] Instead of the polycarboxylic acid, anhydrides or lower alkyl esters of the polycarboxylic acid may also be used.

[0033] Examples of lower alkyl esters include methyl esters, ethyl esters, and isopropyl esters.

[0034] Examples of the esterification catalyst include organotin compounds such as dibutyltin oxide, organotitanium compounds, and organozirconium compounds.

[0035] In addition, when synthesizing the unmodified polyester, after polycondensation of a diol and a dicarboxylic acid, a trivalent or higher alcohol and / or a trivalent or higher carboxylic acid may be added and polycondensed.

[0036] The glass transition temperature of the unmodified polyester is preferably 30 to 80° C., and more preferably 40 to 65° C. When the glass transition temperature of the binder resin is 30° C. or higher, the heat-resistant storage stability of the toner is improved, and when it is 80° C. or lower, the low-temperature fixing property of the toner is improved.

[0037] The weight average molecular weight of the unmodified polyester is preferably 2,000 to 90,000, and more preferably 2,500 to 30,000. When the weight average molecular weight of the binder resin is 2,000 or more, the heat resistant storage stability of the toner is improved, and when it is 90,000 or less, the low temperature fixing property of the toner is improved.

[0038] The urea-modified polyester is produced, for example, as described below, by reacting a polyester prepolymer having an isocyanate group with an amine during the production of the toner.

[0039] The polyester prepolymer having an isocyanate group can be synthesized by reacting an unmodified polyester having a hydroxyl group with a polyisocyanate.

[0040] The polyhydric alcohols and polybasic carboxylic acids used in synthesizing the unmodified polyester having a hydroxyl group are the same as the polyhydric alcohols and polybasic carboxylic acids described above.

[0041] The polyisocyanate can be appropriately selected from known polyisocyanates used in the synthesis of polyester prepolymers having an isocyanate group.

[0042] Examples of the polyisocyanate include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, 2,6-diisocyanatomethyl caproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and cyclohexylmethane diisocyanate; tolylene diisocyanate and diphenylmethane diisocyanate; Examples of the isocyanurates include aromatic diisocyanates such as 1,5-naphthylene diisocyanate, diphenylene-4,4'-diisocyanate, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 3-methyldiphenylmethane-4,4'-diisocyanate, and diphenylether-4,4'-diisocyanate; aromatic aliphatic diisocyanates such as α,α,α',α'-tetramethylxylylene diisocyanate; and isocyanurates such as tris(isocyanatoalkyl)isocyanurate and triisocyanatocycloalkylisocyanurate, and two or more of them may be used in combination. Among these, isophorone diisocyanate is preferred from the viewpoint of toner quality.

[0043] The amines can be appropriately selected from known amines used in the synthesis of urea-modified polyesters.

[0044] Examples of the amines include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, etc., and two or more of them may be used in combination. Among these, diamines and mixtures of diamines and small amounts of trivalent or higher amines are preferred.

[0045] Examples of diamines include aromatic diamines such as phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane; alicyclic diamines such as 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine; and aliphatic diamines such as ethylenediamine, tetramethylenediamine, and hexamethylenediamine.

[0046] Examples of the trivalent or higher amine include diethylenetriamine and triethylenetetramine.

[0047] Examples of amino alcohols include ethanolamine and hydroxyethylaniline.

[0048] Examples of amino mercaptans include aminoethyl mercaptan and aminopropyl mercaptan.

[0049] Examples of the amino acid include aminopropionic acid and aminocaproic acid.

[0050] The amino group of the amines may be protected with a protecting group.

[0051] (Release agent) The release agent can be appropriately selected from known release agents used in toners.

[0052] Examples of the release agent include polyolefin waxes such as polyethylene wax, polypropylene wax, and modified polyethylene wax, synthetic waxes such as Fischer-Tropsch wax, petroleum waxes such as ester wax, paraffin wax, and microcrystalline wax, and vegetable waxes such as carnauba wax, candelilla wax, rice wax, and hydrogenated castor oil, and two or more of these may be used in combination. Among these, ester waxes are preferred from the viewpoint of hot offset resistance of the toner.

[0053] Commercially available ester wax products include the WEP series (manufactured by NOF Corp.).

[0054] Commercially available paraffin wax products include the HNP series (manufactured by Nippon Seiro Co., Ltd.).

[0055] The melting point of the ester wax is preferably 70 to 80° C., and more preferably 70 to 75° C. When the melting point of the ester wax is 70° C. or higher, filming and supply failure when using a mono pump can be further suppressed, and when the melting point is 80° C. or lower, the hot offset resistance of the toner is further improved.

[0056] (Coloring agent) The colorant can be appropriately selected from known dyes and pigments used in toners, and examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazanone, and the like. Yellow BGL, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachloroorthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lu Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples of the pigments include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone, and two or more of them may be used in combination.

[0057] The content of the colorant in the toner is preferably from 1 to 15% by mass, and more preferably from 3 to 10% by mass.

[0058] The colorant may also be used as a master batch in which the colorant is combined with a binder resin.

[0059] Here, the binder resin constituting the master batch is the same as the binder resin described above.

[0060] The master batch can be produced by applying a shear force to the binder resin and the colorant to mix and knead them. In this case, an organic solvent can be used to improve the interaction between the colorant and the binder resin. In addition, a method called a flushing method is also used in which an aqueous paste of the colorant is mixed and kneaded with a resin and an organic solvent, the colorant is transferred to the binder resin, and the water and the organic solvent are removed. In this case, the wet cake of the colorant can be used as it is, so there is no need to dry the wet cake of the colorant.

[0061] When mixing and kneading the binder resin and the colorant, it is preferable to use a high shear dispersion device such as a three-roll mill.

[0062] (Charge control agent) The charge control agent can be appropriately selected from known charge control agents used in toners.

[0063] Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdate chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substances or compounds, tungsten simple substances or compounds, fluorine-based surfactants, metal salts of salicylic acid or derivatives thereof, copper phthalocyanine, perylene, quinacridone, azo pigments, sulfonic acid groups, carboxyl groups, polymeric compounds having quaternary ammonium bases, etc., and two or more of these may be used in combination.

[0064] Commercially available charge control agents include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (both manufactured by Hodogaya Chemical Industry Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX VP434 (all manufactured by Hoechst), and the boron complex LR-147 (manufactured by Nippon Carlit).

[0065] The mass ratio of the charge control agent to the binder resin is preferably 0.1 to 10%, and more preferably 0.2 to 5%.

[0066] The charge control agent may be used as a master batch in which it is combined with a binder resin, or may be fixed to the surface of base particles.

[0067] Here, the binder resin constituting the master batch is the same as the binder resin described above.

[0068] (Organically modified layered inorganic minerals) The toner of the present embodiment preferably further contains an organically modified layered inorganic mineral, which makes it possible to control the shape of the toner of the present embodiment and to finely disperse components such as a colorant and a release agent in the base particles.

[0069] In the organically modified layered inorganic mineral, at least a part of the ions present between the layers of the layered inorganic mineral is modified with an organic ion. The layered inorganic mineral is an inorganic mineral formed by overlapping layers having a thickness of several nm.

[0070] Here, "at least a part of the ions present between the layers of the layered inorganic mineral are modified with organic ions" means that organic ions are introduced as at least a part of the ions present between the layers of the layered inorganic mineral. In addition, the introduction of organic ions also includes, in a broad sense, the intercalation of organic ions.

[0071] Examples of layered inorganic minerals include smectite clay minerals (montmorillonite, saponite, hectorite, etc.), kaolin clay minerals (kaolinite, etc.), bentonite, attapulgite, magadiite, kanemite, etc., and two or more of them may be used in combination. Among these, smectite clay minerals are preferred, and montmorillonite is particularly preferred.

[0072] Examples of organic ions include quaternary alkylammonium ions, phosphonium ions, imidazolium ions, branched, unbranched or cyclic alkyl groups having 1 to 44 carbon atoms, branched, unbranched or cyclic alkenyl groups having 1 to 22 carbon atoms, branched, unbranched or cyclic alkoxy groups having 8 to 32 carbon atoms, branched, unbranched or cyclic hydroxyalkyl groups having 2 to 22 carbon atoms, sulfate ions having a skeleton such as ethylene oxide or propylene oxide, sulfonate ions having the above skeletons, carboxylate ions having the above skeletons, and phosphate ions having the above skeletons, and two or more of these may be used in combination. Among these, quaternary alkylammonium ions and carboxylate ions having an ethylene oxide skeleton are preferred, and quaternary alkylammonium ions are particularly preferred.

[0073] Examples of the quaternary alkyl ammonium ion include trimethylstearyl ammonium ion, dimethylstearylbenzyl ammonium ion, dimethyloctadecyl ammonium ion, and oleylbis(2-hydroxyethyl)methyl ammonium ion.

[0074] It can be confirmed by gas chromatography mass spectrometry (GCMS) that at least some of the ions present between the layers of the layered inorganic mineral are modified with organic ions. For example, after filtering a liquid in which a binder resin is dissolved by mixing a toner with a solvent, the filtered material is pyrolyzed at 550°C using a pyrolysis apparatus Py-2020D (manufactured by Frontier Labs), and the organic ions are identified using a GCMS apparatus QP5000 (manufactured by Shimadzu Corporation).

[0075] An organically modified layered inorganic mineral can be synthesized, for example, by replacing some of the divalent metals constituting the layered inorganic mineral with trivalent metals to introduce metal anions, and then modifying at least some of the metal anions with organic anions.

[0076] Examples of commercially available organically modified layered inorganic minerals include quaternium-18 bentonites such as Bentone 3, Bentone 38, Bentone 38V (all manufactured by Elementis Specialties), Thixogel VP (manufactured by United Catalyst), Clayton 34, Clayton 40, and Clayton XL (manufactured by Southern Clay); stearalkonium bentonites such as Bentone 27 (manufactured by Rheox), Thixogel LG (manufactured by BYK Additives & Instruments), Clayton AF, and Clayton APA (manufactured by BYK Additives & Instruments); quaternium-18 / benzalkonium bentonites such as Clayton HT and Clayton PS (manufactured by Southern Clay); organically modified montmorillonites such as Clayton HY (manufactured by Southern Clay); and organically modified squemetites such as Lucentite SPN (manufactured by Co-op Chemical). Among these, Clayton AF and Clayton APA are preferred.

[0077] The organically modified layered inorganic mineral is, for example, DHT-4A (manufactured by Kyowa Chemical Industry Co., Ltd.) having the general formula R1(OR2) n OSO3M···(1) (wherein R1 is an alkyl group having 1 to 3 carbon atoms, R2 is an alkylene group having 2 to 6 carbon atoms, n is an integer of 2 to 10, and M is a monovalent metal cation.) It is preferable to synthesize the compound by modifying the compound with a compound represented by the formula:

[0078] An example of the compound represented by the general formula (1) is Hitenol 330T (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).

[0079] The organically modified layered inorganic mineral may be used as a master batch in which it is composited with a binder resin.

[0080] Here, the binder resin constituting the master batch is the same as the binder resin described above.

[0081] The content of the organic modified layered inorganic mineral in the toner of this embodiment is preferably 0.1 to 3.0% by mass, more preferably 0.3 to 1.5% by mass. When the content of the organic modified layered inorganic mineral in the toner of this embodiment is 0.1% by mass or more, the effect of the organic modified layered inorganic mineral is easily exhibited, and when it is 3.0% by mass or less, the low temperature fixability of the toner of this embodiment is improved.

[0082] (Toner manufacturing method) The method for producing the toner of the present embodiment can be appropriately selected from known methods for producing toner, and examples of such methods include a pulverization method and a dissolution suspension method. 2850 / PI 828 The dissolution suspension method is preferred because it is easy to control the amount of the solution.

[0083] An example of a method for producing a toner using a pulverization method will be described below.

[0084] First, a toner composition containing unmodified polyester, a release agent, a colorant, a polyester prepolymer having an isocyanate group, amines, and an organically modified layered inorganic mineral is melt-kneaded using a kneader to prepare a kneaded toner composition.

[0085] Examples of the kneader include a closed type kneader and an open roll type kneader. 2850 / PI 828 Since it is easy to control the mixing ratio, an open roll type kneader is preferred.

[0086] Next, the kneaded mixture of the toner composition is pulverized using a pulverizer to prepare base particles.

[0087] Examples of the pulverizer include an airflow pulverizer (jet mill) and a mechanical pulverizer (turbo mill).

[0088] Next, inorganic fine particles are externally added to the base particles to prepare a toner.

[0089] The inorganic fine particles can be appropriately selected from known inorganic fine particles for toner, and examples thereof include silica fine particles and titanium oxide fine particles.

[0090] The device used for externally adding inorganic fine particles to the base particles can be appropriately selected from known devices, and examples thereof include a mixer.

[0091] An example of a method for producing a toner using the solution suspension method will be described below.

[0092] First, a toner composition containing unmodified polyester, a release agent, a colorant, a polyester prepolymer having an isocyanate group, amines, and an organically modified layered inorganic mineral is dispersed in an organic solvent to prepare a first liquid.

[0093] The organic solvent can be appropriately selected from known organic solvents used in the dissolution suspension method, and examples thereof include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc., and two or more of them may be used in combination. Among these, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, etc. are preferred, and ethyl acetate is particularly preferred.

[0094] The boiling point of the organic solvent is preferably less than 150° C. This makes it easier to remove the organic solvent after the base particles are formed.

[0095] The mass ratio of the organic solvent to the toner composition is preferably from 0.4 to 3, more preferably from 0.6 to 1.4, and further preferably from 0.80 to 1.2.

[0096] The dispersing machine used when dispersing the toner composition in the organic solvent is not particularly limited, but a high-speed shear type dispersing machine or a media type dispersing machine is preferred because they are capable of finely dispersing the toner composition.

[0097] The high-speed shear type disperser can finely disperse the toner composition by pulverizing the toner composition with a high shear force generated in a narrow gap between a rotor and a stator.

[0098] An example of a high-speed shear type dispersing machine is a Milder emulsifying dispersing machine.

[0099] The media type disperser can finely disperse the toner composition by filling a vessel with media such as zirconia beads and rotating the vessel, and pulverizing the toner composition through collisions between the media or between the media and the vessel.

[0100] An example of the media type dispersing machine is a bead mill.

[0101] The media type disperser is effective for pulverizing materials exceeding 1 μm. On the other hand, the high-speed shear type disperser is effective for pulverizing materials of the submicron order. The media type disperser and the high-speed shear type disperser differ in the size of the main object to be pulverized. For this reason, it is preferable to use the media type disperser and the high-speed shear type disperser in combination to improve the uniformity of the material. The order in which the media type disperser and the high-speed shear type disperser are used in combination is not particularly limited.

[0102] The peripheral speed of the rotor of the high-speed shear disperser is preferably more than 12 m / s, which allows the material to be pulverized efficiently.

[0103] The peripheral speed of the disk of the media type dispersing machine is preferably 6 m / s or more, and more preferably 10 to 12 m / s. When the peripheral speed of the disk of the media type dispersing machine is 6 m / s or more, the material can be efficiently pulverized.

[0104] The diameter of the media in the media-type dispersing machine is preferably 0.5 mm or less, and more preferably 0.3 mm or less. When the diameter of the media in the media-type dispersing machine is 0.5 mm or less, the material can be efficiently pulverized.

[0105] Here, since the toner composition contains an organically modified layered inorganic mineral having a higher hardness than an organic compound, it is possible to reduce base particles having a non-uniform composition.

[0106] This is because, in addition to collisions between the media and between the media and the vessel, collisions also occur between the media and the organically modified layered inorganic mineral, and between the vessel and the organically modified layered inorganic mineral, making it possible to efficiently grind organic compounds with low hardness.

[0107] The content of the organically modified layered inorganic mineral in the toner composition is preferably 0.2 to 2.0% by mass, and more preferably 0.7 to 1.5% by mass. When the content of the organically modified layered inorganic mineral in the toner composition is 0.2% by mass or more and 2.0% by mass or less, the amount of base particles having a non-uniform composition can be reduced.

[0108] Next, the first liquid is dispersed in an aqueous medium to prepare a second liquid.

[0109] The mass ratio of the aqueous medium to the first liquid is preferably 0.5 to 20, and more preferably 1 to 10. When the mass ratio of the aqueous medium to the first liquid is 0.5 or more, the dispersibility of the second liquid is improved, and when it is 20 or less, it is economical.

[0110] The aqueous medium contains water and may further contain an organic solvent, if necessary.

[0111] The organic solvent can be appropriately selected from known organic solvents that are miscible with water, and examples thereof include alcohols (methanol, isopropyl alcohol, ethylene glycol, etc.), dimethylformamide, tetrahydrofuran, cellosolves (methyl cellosolve, etc.), lower ketones (acetone, methyl ethyl ketone, etc.), etc.

[0112] The aqueous medium preferably further contains a dispersant such as a surfactant, resin fine particles, or an inorganic compound dispersant.

[0113] The surfactant can be appropriately selected from known surfactants, and examples thereof include anionic surfactants such as alkylbenzenesulfonates, α-olefinsulfonates, and phosphates; amine salt-type cationic surfactants such as alkylamine salts, aminoalcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazolines; quaternary ammonium salt-type cationic surfactants such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, and benzethonium chloride; nonionic surfactants such as fatty acid amide derivatives and polyhydric alcohol derivatives; and amphoteric surfactants such as alanine, dodecylbis(aminoethyl)glycine, bis(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine.

[0114] Moreover, as the surfactant, a surfactant having a fluoroalkyl group may be used.

[0115] The resin constituting the resin particles may be either a thermoplastic resin or a thermosetting resin.

[0116] The resin constituting the resin microparticles can be appropriately selected from known resins capable of forming an aqueous dispersion, and examples thereof include vinyl resins, polyurethanes, epoxy resins, polyesters, polyamides, polyimides, silicon resins, phenol resins, melamine resins, urea resins, aniline resins, ionomer resins, polycarbonates, etc., and two or more of them may be used in combination. Among these, vinyl resins, polyurethanes, epoxy resins, and polyesters are preferred because they are easy to obtain an aqueous dispersion of fine, spherical resin microparticles.

[0117] Specific examples of vinyl resins include styrene-(meth)acrylic acid ester copolymers, styrene-butadiene copolymers, (meth)acrylic acid-acrylic acid ester polymers, styrene-acrylonitrile copolymers, styrene-maleic anhydride copolymers, and styrene-(meth)acrylic acid copolymers.

[0118] The volume average particle size of the resin fine particles is preferably from 5 to 200 nm, and more preferably from 20 to 300 nm.

[0119] Examples of inorganic compound dispersants include tricalcium phosphate, calcium carbonate, titanium oxide, colloidal silica, and hydroxyapatite.

[0120] The dispersion stability of the second liquid may be improved by using resin fine particles, an inorganic compound dispersant, and a polymer protective colloid in combination.

[0121] Examples of the polymeric compounds constituting the polymeric protective colloid include monomers having a carboxyl group (e.g., acrylic acid, methacrylic acid, α-cyanoacrylic acid, α-cyanomethacrylic acid, itaconic acid, crotonic acid, fumaric acid, maleic acid, or maleic anhydride), (meth)acrylic monomers containing a hydroxyl group (e.g., β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, γ-hydroxypropyl acrylate, γ-hydroxypropyl methacrylate, 3-chloro-2-hydroxypropyl acrylate, 3-chloro-2-hydroxypropyl methacrylate, diethylene glycol mono ... Examples of the vinyl ester include homopolymers or copolymers of monomethacrylates, glycerin monoacrylates, glycerin monomethacrylates, N-methylol acrylamide, N-methylol methacrylamide, vinyl alcohol, vinyl alkyl ethers (e.g., vinyl methyl ether, vinyl ethyl ether, vinyl propyl ether), vinyl carboxylates (e.g., vinyl acetate, vinyl propionate, vinyl butyrate), acrylamide, methacrylamide, diacetone acrylamide, or methylol derivatives thereof, acid chlorides (e.g., acrylic acid chloride, methacrylic acid chloride), and nitrogen-containing compounds (e.g., vinyl pyridine, vinyl pyrrolidone, vinyl imidazole, ethylene imine).

[0122] Examples of polymer compounds constituting the polymer protective colloid other than those mentioned above include polyoxyethylene compounds such as polyoxyethylene, polyoxypropylene, polyoxyethylene alkylamines, polyoxypropylene alkylamines, polyoxyethylene alkylamides, polyoxypropylene alkylamides, polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl phenyl ether, polyoxyethylene stearyl phenyl ester, and polyoxyethylene nonylphenyl ester; and celluloses such as methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.

[0123] The dispersing machine used when dispersing the first liquid in the aqueous medium can be appropriately selected from known dispersing machines, and examples thereof include a low-speed shearing dispersing machine, a high-speed shearing dispersing machine, a friction dispersing machine, a high-pressure jet dispersing machine, an ultrasonic dispersing machine, etc. Among these, a high-speed shearing dispersing machine is preferred because it can set the particle size of the second liquid to 2 to 20 μm.

[0124] When a high-speed shear type disperser is used, the rotation speed is preferably from 1,000 to 30,000 rpm, and more preferably from 5,000 to 20,000 rpm.

[0125] When a high-speed shear type disperser is used, the dispersion time is preferably 0.1 to 5 minutes in the case of a batch system.

[0126] When a high-speed shear type disperser is used, the temperature is preferably 0 to 150°C (under pressure), and more preferably 40 to 98°C.

[0127] Next, the organic solvent is removed from the second liquid to form base particles, thereby producing a third liquid.

[0128] For example, the temperature of the entire system is gradually increased while stirring the laminar flow, and then vigorously stirred at a certain temperature range to react the polyester prepolymer having an isocyanate group with the amines, and the solvent is then removed to form spindle-shaped base particles.

[0129] Next, the base particles contained in the third liquid are washed and dried.

[0130] Here, when tricalcium phosphate is used as the acid- or alkali-soluble inorganic compound dispersant, the tricalcium phosphate can be dissolved with an acid such as hydrochloric acid, and then washed with water to remove the tricalcium phosphate from the base particles.

[0131] Alternatively, the dispersant can be removed by a procedure such as decomposition with an enzyme.

[0132] Next, inorganic fine particles are externally added to the base particles to prepare a toner.

[0133] The inorganic fine particles can be appropriately selected from known inorganic fine particles for toner, and examples thereof include silica fine particles and titanium oxide fine particles.

[0134] The device used for externally adding inorganic fine particles to the base particles can be appropriately selected from known devices, and examples thereof include a mixer.

[0135] (Developer) The developer of the present embodiment contains the toner of the present embodiment and a carrier.

[0136] (Career) The carrier can be appropriately selected from known carriers for developers, and examples thereof include carriers having a coating film formed on a core material.

[0137] The core material can be appropriately selected from known core materials for carriers, and examples thereof include ferrite containing a divalent metal such as iron, manganese, zinc, or copper.

[0138] The resin constituting the coating film can be appropriately selected from resins constituting known coating films on carriers, and examples thereof include silicone resins, styrene-acrylic resins, fluororesins, and olefin resins.

[0139] The thickness of the coating film is preferably 0.05 to 10 μm, and more preferably 0.3 to 4 μm.

[0140] The method for forming the coating film can be appropriately selected from known methods for forming coating films on carriers, and examples thereof include a method in which a resin solution is sprayed onto a fluidized bed of a core material, and a method in which resin fine particles are electrostatically attached to a core material and then thermally melted.

[0141] The weight average particle diameter of the carrier is preferably 20 to 100 μm. If the weight average particle diameter of the carrier is 20 μm or more, the carrier is less likely to adhere to the photoreceptor during development, and if it is 100 μm or less, the toner is less likely to suffer from poor charging during continuous use. EXAMPLES

[0142] Examples of the present invention will be described below. Note that the present invention is not limited to the Examples. Furthermore, parts means parts by mass unless otherwise specified.

[0143] [Method of measuring wax characteristics] [1] Melting point The DSC curve was measured using TA-60WS and DSC-60 (manufactured by Shimadzu Corporation) under the measurement conditions shown below, and then analyzed using data analysis software TA-60, version 1.52 (manufactured by Shimadzu Corporation) to determine the melting point.

[0144] Sample container: Aluminum sample pan (with lid) Sample size: 5mg Reference: Aluminum sample pan (alumina 10 mg) Atmosphere: Nitrogen (Flow rate: 50ml / min) Starting temperature: 20℃ Heating rate: 10℃ / min End temperature: 150℃ Hold Time: None Cooling rate: 10℃ / min End temperature: 20℃ Hold Time: None Heating rate: 10℃ / min End temperature: 150℃ [Method of measuring toner characteristics] [1]PI 2850 / PI 828 Using a Spotlight 400 infrared imaging system (Perkin Elmer), a toner pellet with a diameter of 40 mm and a thickness of approximately 2 mm was subjected to FTIR-ATR mapping under the conditions of a measurement range of 50 μm × 50 μm and a pixel size of 1.56 μm × 1.56 μm (1024 divisions). 2850 / PI 828 Average value of PI 2850 / PI 828 The proportion of cases where PI is 0.20 or more 2850 / PI 828 The half-width of the frequency histogram was calculated.

[0145] The toner pellets were prepared by pressing 3 g of toner for 1 minute under a load of 6 t using an automatic pellet molding machine Type M No. 50 BRP-E (manufactured by MAEKAWA TESTING MACHINE).

[0146] [2] Volume average particle size First, 0.1 to 5 ml of surfactant alkylbenzene sulfonate was added to 100 to 150 ml of electrolyte ISOTON-II (manufactured by Coulter), then 2 to 20 mg of toner was added and dispersed for about 1 to 3 minutes using an ultrasonic disperser. Next, the volume average particle size of the toner was determined using a 100 μm aperture in a precision particle size distribution measuring device Multisizer II (manufactured by Coulter). Here, 13 channels were used: 2.00 μm or more and less than 2.52 μm; 2.52 μm or more and less than 3.17 μm; 3.17 μm or more and less than 4.00 μm; 4.00 μm or more and less than 5.04 μm; 5.04 μm or more and less than 6.35 μm; 6.35 μm or more and less than 8.00 μm; 8.00 μm or more and less than 10.08 μm; 10.08 μm or more and less than 12.70 μm; 12.70 μm or more and less than 16.00 μm; 16.00 μm or more and less than 20.20 μm; 20.20 μm or more and less than 25.40 μm; 25.40 μm or more and less than 32.00 μm; and 32.00 μm or more and less than 40.30 μm, and particles with particle sizes of 2.00 μm or more and less than 40.30 μm were measured.

[0147] [Toner evaluation method] [1] Hot offset resistance A Teflon (registered trademark) roller was used as the fixing roller, and a copying test was carried out by filling a developer into a copying machine MF2200 (manufactured by Ricoh) with a modified fixing section, setting type 6200 paper (manufactured by Ricoh), and setting it. At this time, the fixing temperature was changed to determine the hot offset occurrence temperature (upper fixing temperature limit) and evaluating the hot offset resistance. The evaluation conditions for hot offset resistance were a paper feed linear speed of 50 mm / s and a surface pressure of 2.0 kgf / cm. 2 The nip width was set to 4.5 mm.

[0148] The criteria for hot offset resistance are as follows.

[0149] ◎: When the maximum fixing temperature is 195℃ or higher ○: When the maximum fixing temperature is 190℃ or higher and lower than 195℃ △: When the upper fixing temperature is 180℃ or higher and less than 190℃ ×: When the upper fixing temperature limit is less than 180°C [2] Low-temperature fixability A Teflon (registered trademark) roller was used as the fixing roller, and a copying test was carried out by loading a developer into a copying machine MF2200 (manufactured by Ricoh) with a modified fixing section, setting type 6200 paper (manufactured by Ricoh), and then loading the developer into the copying machine. At this time, the fixing temperature was changed to determine the temperature at which cold offset occurred (lowest limit fixing temperature), and the low-temperature fixing property was evaluated. The evaluation conditions for low-temperature fixing property were a paper feed linear speed of 120 to 150 mm / s, and a surface pressure of 1.2 kgf / cm. 2 The nip width was set to 3 mm.

[0150] The criteria for judging the low-temperature fixability are as follows.

[0151] ◎: When the minimum fixing temperature is less than 140℃ ○: When the minimum fixing temperature is 140℃ or higher and lower than 150℃ △: When the minimum fixing temperature is 150℃ or higher and lower than 160℃ ×: When the minimum fixing temperature is 160°C or higher [3] Filming The developer was filled into a copy machine MP9001 (manufactured by Ricoh) and the basis weight was 67 g / m 2 After printing 100 sheets of A4 size plain paper was repeated 50 times, the photoconductor was visually observed and filming was evaluated.

[0152] The criteria for judging filming are as follows:

[0153] ◎: When filming does not occur on the photoconductor ○: Filming occurs slightly on the photoconductor △: Filming occurs only on a part of the photoconductor ×: Filming occurs over the entire surface of the photoconductor. [4] Poor supply when using the mono pump The operation conditions were 0.2 seconds ON / 0.5 seconds OFF, and the Mono Pump (manufactured by Ricoh) was operated to repeatedly replenish toner. At this time, the number of sheets that would cause a toner replenishment failure was calculated, assuming that the state in which toner replenishment was repeated for 17 hours was equivalent to 500,000 sheets, and the replenishment failure when using the Mono Pump was evaluated.

[0154] The criteria for determining whether a supply failure occurs when using a mono pump are as follows:

[0155] ◎: When the number of sheets that cause toner supply failure is equivalent to 3 million sheets or more ○: When the number of sheets that cause toner supply failure is between 2.5 million and 3 million sheets. △: When the number of sheets that cause toner supply failure is between 2 million and 2.5 million sheets. ×: When the number of sheets that cause toner supply failure is less than 2 million sheets. [5] Overall Judgment The evaluation was made as follows: if all of the evaluation results of [1] to [4] were △ or higher, it was judged as O; if at least one of the evaluation results of [1] to [4] was ×, it was judged as ×.

[0156] [Synthesis of unmodified polyester] Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 229 parts of bisphenol A ethylene oxide 2 mol adduct, 529 parts of bisphenol A propylene oxide 3 mol adduct, 208 parts of terephthalic acid, 46 parts of adipic acid, and 2 parts of dibutyltin oxide were added, and reacted at normal pressure and 230° C. for 8 hours. Next, after reacting for 5 hours under a reduced pressure of 10 to 15 mmHg, 44 parts of trimellitic anhydride were added to the reaction vessel, and reacted at normal pressure and 180° C. for 2 hours to obtain an unmodified polyester.

[0157] The unmodified polyester had a number average molecular weight of 2700, a weight average molecular weight of 6900, a glass transition temperature of 45.1° C., and an acid value of 22 mgKOH / g.

[0158] [Masterbatch production] Using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), 1200 parts of water, 540 parts of carbon black Printex35 (manufactured by Dexa Co., Ltd.) with a DBP oil absorption of 42 ml / 100 mg and a pH of 9.5, and 1200 parts of unmodified polyester were mixed, and then kneaded using a two-roll mill at 150° C. for 30 minutes. Next, the kneaded product was rolled and cooled, and then pulverized using a pulverizer (manufactured by Hosokawa Micron Co., Ltd.) to obtain a master batch.

[0159] [Synthesis of polyesters having hydroxyl groups] Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 682 parts of bisphenol A ethylene oxide 2 mol adduct, 81 parts of bisphenol A propylene oxide 2 mol adduct, 283 parts of terephthalic acid, 22 parts of trimellitic anhydride, and 2 parts of dibutyltin oxide were charged and reacted at normal pressure and 230°C for 8 hours. Next, the mixture was reacted under reduced pressure of 10 to 15 mHg for 5 hours to obtain a polyester having hydroxyl groups.

[0160] The polyester having hydroxyl groups had a number average molecular weight of 2100, a weight average molecular weight of 9500, a glass transition temperature of 55° C., an acid value of 0.5 mgKOH / g, and a hydroxyl value of 51 mgKOH / g.

[0161] [Synthesis of polyester prepolymer having isocyanate groups] Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 410 parts of a polyester having a hydroxyl group, 89 parts of isophorone diisocyanate, and 500 parts of ethyl acetate were added, and the mixture was reacted at 100°C for 5 hours to obtain a polyester prepolymer having an isocyanate group.

[0162] The polyester prepolymer having an isocyanate group had a free isocyanate content of 1.53% by mass.

[0163] [Synthesis of ketimines] In a reaction vessel equipped with a stirring bar and a thermometer, 170 parts of isophoronediamine and 75 parts of methyl ethyl ketone were charged, and the mixture was reacted at 50° C. for 5 hours to obtain ketimine.

[0164] The ketimine had an amine value of 418 mg KOH / g.

[0165] [Preparation of dispersion of resin particles] In a reaction tank equipped with a stirring rod and a thermometer, 683 parts of water, 11 parts of a reactive emulsifier (sodium salt of sulfate of ethylene oxide adduct of methacrylic acid) Eleminol RS-30 (manufactured by Sanyo Chemical Industries), 83 parts of styrene, 83 parts of methacrylic acid, 110 parts of butyl acrylate, and 1 part of ammonium persulfate were added and stirred at 400 rpm for 15 minutes. Next, the temperature was raised to 75°C and reacted for 5 hours, after which 30 parts of a 1% by mass aqueous solution of ammonium persulfate was added and aged at 75°C for 5 hours to obtain a dispersion of resin fine particles.

[0166] The volume average particle diameter of the dispersion of resin particles was measured using a Nanotrac particle size distribution analyzer UPA-EX150 (manufactured by Nikkiso Co., Ltd.) and found to be 105 nm. In addition, a part of the dispersion of resin particles was dried to isolate the resin, and the glass transition temperature and weight average molecular weight of the resin were measured and found to be 59°C and 150,000, respectively.

[0167] [Synthesis of ester wax] In a four-neck flask equipped with a Dimroth reflux and a Dean-Stark water separator, 1740 parts of benzene, 1300 parts of a mixture of behenic acid and stearic acid as a long-chain alkyl carboxylic acid component, 1200 parts of a mixture of behenyl alcohol and stearyl alcohol as a long-chain alkyl alcohol component, and 120 parts of p-toluenesulfonic acid were added, and then thoroughly stirred to dissolve. Next, after refluxing for 5 hours, the valve of the water separator was opened and azeotropic distillation was performed. Next, the mixture was thoroughly washed with sodium bicarbonate, dried, and benzene was distilled off. The resulting product was recrystallized, washed, and purified to obtain an ester wax.

[0168] Here, the compositions and amounts of the long-chain alkyl carboxylic acid component and the long-chain alkyl alcohol component were appropriately adjusted to control the melting points of Waxes 1 to 3, 5, and 6 to 60 to 85° C. (see Table 1).

[0169] [Example 1] (Preparation of the first liquid) 378 parts of unmodified polyester, 120 parts of wax 1, and 947 parts of ethyl acetate were added to a reaction tank equipped with a stirring rod and a thermometer, and the temperature was then raised to 80° C. under stirring. The mixture was then held at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, 500 parts of master batch, 25 parts of organically modified montmorillonite CLAYTONE (manufactured by BYK), and 500 parts of ethyl acetate were added to the reaction tank, and mixed for 1 hour to obtain a toner material liquid.

[0170] After transferring 1324 parts of the toner material liquid to the reaction tank, a bead mill, Ultraviscomill (manufactured by Imex), was used to obtain a dispersion liquid (A) of the toner material, with 80% by volume of zirconia beads of 0.5 mm in diameter, and three passes were made under the conditions of a liquid feed rate of 1 kg / h and a disk peripheral speed of 6 m / s. Next, 1324 parts of a 65% by mass ethyl acetate solution of unmodified polyester was put into the reaction tank, and one pass was made using a bead mill under the same conditions as above to obtain a dispersion liquid (B) of the toner material. Next, 200 parts of the dispersion liquid (B) of the toner material was stirred at 8000 rpm for 20 minutes using a TK Homo Disper (manufactured by Tokushu Kika Kogyo), to obtain a dispersion liquid (C) of the toner material.

[0171] 749 parts of the dispersion liquid (C) of the toner materials, 115 parts of a polyester prepolymer having an isocyanate group, and 2.9 parts of ketimine were added to a reaction tank, and then mixed at 5,000 rpm for 1 minute using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to obtain a first liquid.

[0172] (Preparation of aqueous medium) 990 parts of water, 83 parts of a dispersion of resin fine particles, 37 parts of Eleminol MON-7 (manufactured by Sanyo Chemical Industries, Ltd.), a 48.5% by mass aqueous solution of sodium dodecyl diphenyl ether disulfonate, 135 parts of Cellogen BS-H-3 (manufactured by Dai-ichi Kogyo Seiyaku, Ltd.), a 1% by mass aqueous solution of sodium carboxymethyl cellulose, a polymeric protective colloid, and 90 parts of ethyl acetate were mixed and stirred to obtain an aqueous medium.

[0173] (Preparation of the second liquid) 867 parts of the first liquid were added to 1200 parts of the aqueous medium, and then mixed for 20 minutes at 13000 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to obtain a second liquid.

[0174] (Preparation of the third liquid) The second liquid was charged into a reaction vessel equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours, followed by maturing at 45° C. for 4 hours to form base particles, thereby obtaining a third liquid.

[0175] (Washing and drying of base particles) 100 parts by mass of the third liquid was filtered under reduced pressure. 100 parts of ion-exchanged water was added to the obtained filter cake, and the mixture was mixed at 12,000 rpm for 10 minutes using a TK homomixer, and then filtered.

[0176] A 10% by mass aqueous phosphoric acid solution was added to the obtained filter cake to adjust the pH to 3.7, and the mixture was mixed at 12,000 rpm for 10 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), and then filtered.

[0177] To the obtained filter cake, 300 parts of ion-exchanged water was added, and the mixture was mixed at 12,000 rpm for 10 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), and then filtered. This operation was repeated twice.

[0178] The obtained filter cake was dried at 45° C. for 48 hours using a circulating air dryer, and then sieved through a mesh with 75 μm openings to obtain base particles.

[0179] (Toner Production) Using a Henschel Mixer 20A (manufactured by Mitsui Mining), 100 parts of base particles, 1.5 parts of hydrophobic silica, and 0.5 parts of titanium oxide were mixed for 10 minutes at a mixer temperature of 35 to 40°C and a peripheral speed of 35 m / s, and then sieved through a 500 mesh screen to obtain a toner.

[0180] [Example 2] A toner was obtained in the same manner as in Example 1, except that in the preparation of the first liquid, the amount of wax 1 added was changed to 110 parts.

[0181] [Example 3] A toner was obtained in the same manner as in Example 1, except that in (Preparation of the first liquid), four passes were performed when preparing the dispersion liquid (A) of the toner materials.

[0182] [Example 4] In (Preparation of the first liquid), a toner was obtained in the same manner as in Example 1, except that five passes were performed when preparing the dispersion liquid (A) of the toner materials.

[0183] [Example 5] A toner was obtained in the same manner as in Example 1, except that Wax 2 was used instead of Wax 1 in (Preparation of the first liquid).

[0184] [Example 6] A toner was obtained in the same manner as in Example 1, except that Wax 3 was used instead of Wax 1 in (Preparation of the first liquid).

[0185] [Example 7] A toner was obtained in the same manner as in Example 4, except that Wax 3 was used instead of Wax 1 in (Preparation of the first liquid).

[0186] [Example 8] A toner was obtained in the same manner as in Example 7, except that in (preparation of the second liquid), mixing was performed at 13,000 rpm for 15 minutes.

[0187] [Example 9] A toner was obtained in the same manner as in Example 7, except that in (preparation of the second liquid), mixing was performed at 13,000 rpm for 25 minutes.

[0188] [Example 10] A toner was obtained in the same manner as in Example 7, except that in (preparation of the first liquid), paraffin wax HNP-9 (manufactured by Nippon Seiro Co., Ltd.) having a melting point of 75° C. (hereinafter referred to as wax 4) was used instead of wax 1.

[0189] [Example 11] A toner was obtained in the same manner as in Example 7, except that Wax 5 was used instead of Wax 1 in (Preparation of the first liquid).

[0190] [Example 12] A toner was obtained in the same manner as in Example 7, except that Wax 6 was used instead of Wax 1 in (Preparation of the first liquid).

[0191] [Example 13] A toner was obtained in the same manner as in Example 7, except that in (Preparation of the first liquid), the amount of wax 1 added was changed to 100 parts, and two passes were performed when preparing the dispersion liquid (A) of the toner materials.

[0192] [Comparative Example 1] A toner was obtained in the same manner as in Example 1, except that in (Preparation of the first liquid), the dispersion liquid (A) of the toner materials was prepared by two passes.

[0193] [Comparative Example 2] In (Preparation of the first liquid), a toner was obtained in the same manner as in Example 1, except that five passes were performed when preparing the dispersion liquid (A) of the toner materials.

[0194] [Comparative Example 3] A toner was obtained in the same manner as in Example 1, except that in (preparation of the first liquid), the amount of wax 1 added was changed to 100 parts.

[0195] [Creating the carrier] Using a homomixer, 21.0 parts of an acrylic resin solution with a solid content of 50% by mass, 6.4 parts of a guanamine solution with a solid content of 70% by mass, 7.6 parts of alumina particles with an average particle size of 0.3 μm and a volume resistivity of 1 × 1014 Ω·cm, 65.0 parts of a silicone resin solution SR2410 (manufactured by Toray Dow Corning Silicones) with a solid content of 23% by mass, 1.0 part of aminosilane SH6020 (manufactured by Toray Dow Corning Silicones), 60 parts of toluene, and 60 parts of butyl cellosolve were dispersed for 10 minutes to obtain a coating solution.

[0196] Using a Spiracoater (manufactured by Okada Seiko), a coating solution was applied to a core material of sintered ferrite powder (MgO)1.8 (MnO)49.5 (Fe2O3)48.0 with an average particle size of 25 μm, so that the average thickness of the coating film was 0.15 μm, and then the core material was dried to obtain a ferrite powder with a coating film. Next, the ferrite powder with a coating film was sintered at 150°C for 1 hour using an electric furnace, cooled, and then crushed using a sieve with 106 μm openings to obtain a carrier with a weight average particle size of 35 μm.

[0197] The thickness of the coating film can be determined by observing a cross section of the carrier using a transmission electron microscope.

[0198] [Preparation of developer] Using a turbula mixer of the type that stirs by rolling a container, 100 parts of the carrier and 7 parts of the toner were mixed uniformly and charged to obtain a developer.

[0199] Table 1 shows the measurement results of the wax properties.

[0200] [Table 1] Table 2 shows the measurement results of the toner properties.

[0201] [Table 2] Table 3 shows the evaluation results of the toner.

[0202] [Table 3] From Table 3, it is understood that the toners of Examples 1 to 13 are excellent in low-temperature fixing property and hot offset resistance, and can suppress filming and supply failure when using a mono pump.

[0203] In contrast, the toner of Comparative Example 1 had a PI 2850 / PI 828Since the ratio of those with a value of 0.2 or more is 11%, filming and poor supply when using a mono pump are likely to occur.

[0204] The toner of Comparative Example 2 is PI 2850 / PI 828 Since the ratio of those having a value of 0.2 or more is 4%, the hot offset resistance is poor.

[0205] The toner of Comparative Example 3 is PI 2850 / PI 828 Since the average value is 0.09, the hot offset resistance is poor. [Prior art documents] [Patent documents]

[0206] [Patent Document 1] JP 2017-102399 A

Claims

1. Contains a binder resin and a release agent, FTIR-ATR mapping, wave number 828 cm -1 The wave number for the absorption spectrum peak at 2850 cm -1 the ratio of those having an intensity ratio of 0.20 or more being 5 to 10%; the volume average particle size being 4.9 to 5.5 μm; and the release agent being an ester wax, the ester wax having a melting point of 70 to 80° C.

2. 2. The toner according to claim 1, wherein the intensity ratio has a half-width of a frequency histogram of 0.10 to 0.

13.

3. A developer comprising the toner according to claim 1 and a carrier.

Citation Information

Patent Citations

  • Toner for developing electrostatic charge image, its manufacturing method, image forming apparatus, and processing cartridge

    JP2007249082A

  • Toner for forming image, developer, and process cartridge

    JP2009134109A

  • Toner and manufacturing method of toner

    JP2017102399A