Aqueous binder solution for lithium ion batteries, slurry for negative electrodes of lithium ion batteries, negative electrodes for lithium ion batteries, and lithium ion batteries
A water-soluble polymer with (meth)acrylamide and alkoxyalkyl (meth)acrylate monomers addresses flexibility and adhesiveness issues in lithium-ion battery binders, enhancing storage stability and discharge capacity.
Patent Information
- Application Number
- JP2020155058
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2020-09-16
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-09-16
AI Technical Summary
Existing lithium-ion battery binders face issues with reduced flexibility and adhesiveness due to crosslinking agents, leading to reduced discharge capacity retention and poor storage stability of electrodes.
A water-soluble polymer containing a predetermined unsaturated monomer, specifically a lithium ion battery binder aqueous solution with a composition of (meth)acrylamide group-containing compounds and alkoxyalkyl (meth)acrylate, is used to enhance electrode flexibility and adhesion, improving storage stability and discharge capacity.
The solution provides excellent storage stability, flexibility, and adhesion to the electrodes, resulting in improved discharge capacity retention rates.
Smart Images

Figure 0007577950000001 
Figure 0007577950000002 
Figure 0007577950000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an aqueous binder solution for a lithium ion battery, a slurry for a lithium ion battery negative electrode, a lithium ion battery negative electrode, and a lithium ion battery. [Background technology]
[0002] Lithium-ion batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been studied in order to further improve the performance of lithium-ion batteries.
[0003] Both the positive and negative electrodes of a lithium-ion battery are manufactured by dispersing an electrode active material and a binder resin in a solvent to form a slurry, which is applied to both sides of a current collector (e.g., a metal foil), drying and removing the solvent to form an electrode layer, and then compression molding this using a roll press or the like.
[0004] In recent years, various electrode active materials have been proposed for lithium ion battery electrodes in order to increase the battery capacity. However, some electrode active materials tend to expand and contract with charging and discharging. Therefore, lithium ion battery electrodes that tend to expand and contract with charging and discharging undergo volume changes from the beginning of repeated charging and discharging (springback property), and tend to deteriorate the electrical properties such as cycle characteristics of lithium ion batteries using them.
[0005] In this field, therefore, studies have been made to solve the above problems by using binder resins, and it has been proposed, for example, that good charge-discharge characteristics can be obtained by using polyacrylamide as a binder for water-soluble resins (Patent Documents 1 and 2). It has also been proposed to suppress the expansion and contraction that accompanies the charge and discharge of active materials by adding a crosslinking agent to the particulate resin, which is the binder resin (Patent Document 3). The crosslinking agent usually causes a crosslinking reaction during the drying process after the slurry composition is applied to the current collector, forming crosslinks between particles of the particulate resin, etc. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-118908 A [Patent Document 2] JP 2015-106488 A [Patent Document 3] International Publication No. 2015 / 098507 Summary of the Invention [Problem to be solved by the invention]
[0007] However, when crosslinking is performed using a crosslinking agent, the flexibility of the binder resin decreases, which can result in a problem of decreased adhesion to the electrode.
[0008] Therefore, an object of the present invention is to provide a good aqueous binder solution for lithium ion batteries that imparts a good discharge capacity retention rate to a lithium ion battery, imparts good electrode flexibility and electrode adhesion to an electrode, and imparts good storage stability to a slurry. [Means for solving the problem]
[0009] As a result of extensive investigations, the present inventors have found that the above problems can be solved by a water-soluble polymer containing a specific unsaturated monomer as a constituent component.
[0010] The present disclosure provides the following: (Item 1) Relative to 100 mol% of the monomer group, 30 to 95 mol % of a (meth)acrylamide group-containing compound (a), and The aqueous binder solution for lithium ion batteries contains a water-soluble poly(meth)acrylamide (A) which is a polymer of a monomer group containing 5 to 40 mol % of an alkoxyalkyl (meth)acrylate (b) represented by the following general formula (1): CH2 =C(R 1 )-CO-OR 2 -OR 3 (1) (In the formula, R 1 is a hydrogen atom or a methyl group, and R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 is an alkyl group having 1 to 4 carbon atoms. 1 , R 2 , and R 3 The total number of carbon atoms in the groups is 5 or less. (Item 2) A slurry for a lithium ion battery negative electrode, comprising the aqueous binder solution for a lithium ion battery described in the above item and a negative electrode active material. (Item 3) A negative electrode for a lithium ion battery, obtained by applying the slurry for a lithium ion battery negative electrode described in the above item to a current collector, and drying and curing the slurry. (Item 4) A lithium ion battery comprising the lithium ion battery negative electrode described in the above item.
[0011] In the present disclosure, one or more of the above-described features may be provided in further combinations in addition to the combinations explicitly stated. Effect of the Invention
[0012] The aqueous binder solution for lithium ion batteries of the present invention can impart excellent storage stability to a slurry for a lithium ion battery negative electrode. The slurry for a lithium ion battery negative electrode of the present invention has excellent storage stability. Furthermore, the electrode of the present invention has excellent flexibility and adhesion. And the battery of the present invention has an excellent discharge capacity retention rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Throughout this disclosure, the range of the values of the physical properties, contents, etc. may be set as appropriate (for example, by selecting from the upper and lower limit values described in each item below). Specifically, when A4, A3, A2, A1 (where A4>A3>A2>A1) are exemplified as the upper and lower limits of the value α, the range of the value α is exemplified as A4 or less, A3 or less, A2 or less, A1 or more, A2 or more, A3 or more, A1 to A2, A1 to A3, A1 to A4, A2 to A3, A2 to A4, A3 to A4, etc.
[0014] [Aqueous binder solution for lithium-ion battery electrodes: also called aqueous solution] The present disclosure relates to a monomer group having a molecular weight of 100 mol %. 30 to 95 mol % of a (meth)acrylamide group-containing compound (a), and The aqueous binder solution for lithium ion batteries contains a water-soluble poly(meth)acrylamide (A) which is a polymer of a monomer group containing 5 to 40 mol % of an alkoxyalkyl (meth)acrylate (b) represented by the following general formula (1): CH 2 =C(R 1 )-CO-OR 2 -OR 3 (1) (In the formula, R 1 is a hydrogen atom or a methyl group, and R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 is an alkyl group having 1 to 4 carbon atoms. 1 , R 2 , and R 3 The total number of carbon atoms in the groups is 5 or less. to provide.
[0015] <Water-soluble poly(meth)acrylamide: Also referred to as component (A)> In this disclosure, "water-soluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble matter is less than 0.5% by mass (less than 2.5 mg).
[0016] If component (A) is not water-soluble, it will not dissolve in water and will not become an aqueous solution in the first place. As a result, component (A) will not contribute to the dispersion of the slurry. In addition, it will not be possible to impart the viscosity required for coating the current collector to the slurry.
[0017] When 0.5 g of component (A) is dissolved in 100 g of water, the insoluble content of component (A) is, for example, 0.5, 0.4, 0.3, 0.2, less than 0.1 mass %, or 0 mass %.
[0018] In the present disclosure, "poly(meth)acrylamide" refers to a (co)polymer obtained by polymerizing a group of monomers including a (meth)acrylamide group-containing compound.
[0019] In the present disclosure, "(meth)acrylic" means "at least one selected from the group consisting of acrylic and methacrylic". Similarly, "(meth)acrylate" means "at least one selected from the group consisting of acrylate and methacrylate". In addition, "(meth)acryloyl" means "at least one selected from the group consisting of acryloyl and methacryloyl".
[0020] <(Meth)acrylamide group-containing compound (a): also referred to as component (a)> In the present disclosure, the term "(meth)acrylamide group-containing compound" refers to a compound having a (meth)acrylamide group. As the (meth)acrylamide group-containing compound, various known compounds can be used without particular limitation, and they may be used alone or in combination of two or more kinds.
[0021] In one embodiment, the (meth)acrylamide group-containing compound has the following structural formula: [ka] (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 and R 3 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, or an acetyl group; 2and R 3 are groups that together form a ring structure, and R 4 and R 5 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a hydroxyl group, an amino group (-NR a R b (R a and R b are each independently a hydrogen atom or a substituted or unsubstituted alkyl group), and an acetyl group. Examples of the substituent of the substituted alkyl group include a hydroxy group, an amino group, and an acetyl group. 2 and R 3 Examples of the group that combines with each other to form a ring structure include a morpholyl group. It is expressed by:
[0022] Examples of the alkyl group include a straight-chain alkyl group, a branched alkyl group, and a cycloalkyl group.
[0023] A straight chain alkyl group is -C n H 2n+1 (n is an integer of 1 or more). Examples of the straight-chain alkyl group include a methyl group, an ethyl group, a propyl group, a n-butyl group, a n-pentyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, and a n-decamethyl group.
[0024] A branched alkyl group is a group in which at least one hydrogen atom of a linear alkyl group is replaced by an alkyl group. Examples of branched alkyl groups include an i-propyl group, an i-butyl group, an s-butyl group, a t-butyl group, a diethylpentyl group, a trimethylbutyl group, a trimethylpentyl group, and a trimethylhexyl group.
[0025] Examples of the cycloalkyl group include a monocyclic cycloalkyl group, a bridged ring cycloalkyl group, and a condensed ring cycloalkyl group.
[0026] In the present disclosure, a monocyclic ring refers to a ring structure formed by a carbon covalent bond and having no internal bridge structure. A fused ring refers to a ring structure in which two or more monocyclic rings share two atoms (i.e., each ring shares only one side (fused) with each other). A bridged ring refers to a ring structure in which two or more monocyclic rings share three or more atoms.
[0027] Examples of the monocyclic cycloalkyl group include a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclodecyl group, and a 3,5,5-trimethylcyclohexyl group.
[0028] Examples of the bridged ring cycloalkyl group include a tricyclodecyl group, an adamantyl group, and a norbornyl group.
[0029] The condensed ring cycloalkyl group is exemplified by a bicyclodecyl group.
[0030] Examples of the (meth)acrylamide group-containing compound (a) include (meth)acrylamide, N-isopropyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dimethylaminopropyl(meth)acrylamide, N-methylol(meth)acrylamide, diacetone(meth)acrylamide, maleic acid amide, (meth)acrylamide t-butylsulfonic acid, (meth)acryloylmorpholine, hydroxyethyl(meth)acrylamide, and salts thereof, and examples of the salts include dimethylaminopropyl(meth)acrylamide methyl chloride quaternary salt, dimethylaminoethyl(meth)acrylate benzyl chloride quaternary salt, etc. Among these, when (meth)acrylamide, particularly acrylamide, is used, it is possible to prepare a binder that is highly water-soluble, has a high interaction with the electrode active material, and has high dispersibility in the slurry and high binding ability between the electrode active materials inside the electrode.
[0031] The upper and lower limits of the content of the (meth)acrylamide group-containing compound relative to 100 mol % of the monomer group are, for example, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30 mol %, etc. In one embodiment, the content is preferably in the range of 30 to 95 mol %.
[0032] The upper and lower limits of the content of the (meth)acrylamide group-containing compound relative to 100% by mass of the monomer group are 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20% by mass, etc. In one embodiment, the content of the (meth)acrylamide group-containing compound relative to 100% by mass of the monomer group is preferably 20 to 95% by mass.
[0033] <Alkoxyalkyl (meth)acrylate (b): Also referred to as component (b)> The component (b) is represented by the following general formula (1): CH 2 =C(R 1 )-CO-OR 2 -OR 3 (1) (In the formula, R 1 is a hydrogen atom or a methyl group, and R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 is an alkyl group having 1 to 4 carbon atoms. 1 , R 2 , and R 3 The total number of carbon atoms in the groups is 5 or less. As the alkoxyalkyl (meth)acrylate, various known compounds can be used without particular limitation, and they may be used alone or in combination of two or more kinds.
[0034] R 1 , R 2 , and R 3 The upper and lower limits of the total number of carbon atoms in the group are 5, 4, 3, 2, etc. 1 , R 2 , and R 3The total number of carbon atoms in the groups is specified to be 5 or less from the viewpoints of ensuring the water solubility of component (A) and easy availability. If the total number of carbon atoms exceeds 5, the water solubility of the alkoxyalkyl (meth)acrylate decreases, making it difficult to ensure the water solubility of component (A). In addition, from the viewpoints of further improving the storage stability of the negative electrode slurry, the flexibility and adhesion of the negative electrode, and the discharge capacity retention rate of the lithium ion battery, the above carbon number is more preferably 4 or less. In addition, from the same viewpoint, R 3 The carbon number of is preferably 1.
[0035] In the general formula (1), R 1 , R 2 , and R 3 The reason why the storage stability of the negative electrode slurry, the flexibility and adhesion of the negative electrode, and the discharge capacity retention rate of the lithium ion battery are improved by making the total number of carbon atoms in the groups 5 or less is as follows. Note that the following is merely one theory, and it is not intended that the present invention be limited thereto. In the general formula (1), R 1 , R 2 , and R 3 A monomer having a total carbon number of the groups exceeding 5 is a hydrophobic monomer. When component (A) is produced using such a hydrophobic monomer, the water solubility of component (A) decreases. Therefore, the surface tension of an aqueous solution containing component (A) decreases. As a result, bubbles are likely to be generated when a slurry is produced using an aqueous solution containing component (A). The generation of bubbles leads to the following problems. (1) When producing a slurry, the blades of the disperser collide with the bubbles, preventing the slurry from being dispersed, resulting in poor storage stability. (2) When a bubble-containing slurry is applied to a current collector to manufacture an electrode, the dried and hardened electrode will have holes due to the bubbles. These holes can cause cracks and peeling, resulting in a decrease in the electrode flexibility and adhesion. From the above, if the water solubility of component (A) is improved, that is, R 1 , R 2 , and R 3It is believed that, when the total number of carbon atoms in the groups is 5 or less, the storage stability of the negative electrode slurry, the flexibility and adhesion of the negative electrode, and the discharge capacity retention rate of the lithium ion battery are improved.
[0036] R 1 , R 2 , and R 3 Examples of the combination of groups are as follows. [Table 1-1] [Table 1-2] Me: Methyl group (-CH 3 ) R 2 The left side is the ester bond side and the right side is the alkoxy group side.
[0037] The alkoxyalkyl (meth)acrylate may be methoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 1-methoxyethyl (meth)acrylate, Examples include 3-methoxypropyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, 1-methoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methoxybutyl (meth)acrylate, 1-methoxybutyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 1-ethoxyethyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 2-ethoxypropyl (meth)acrylate, 1-ethoxypropyl (meth)acrylate, propoxymethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 1-propoxyethyl (meth)acrylate, butoxymethyl (meth)acrylate, and the like.
[0038] The upper and lower limits of the content of the alkoxyalkyl (meth)acrylate relative to 100 mol % of the monomer group are, for example, 40, 35, 30, 25, 20, 15, 10, 9, 5 mol %, etc. In one embodiment, the content is preferably in the range of 5 to 40 mol %.
[0039] The upper and lower limits of the content of the alkoxyalkyl (meth)acrylate relative to 100% by mass of the monomer group are, for example, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5% by mass, etc. In one embodiment, the content of the alkoxyalkyl (meth)acrylate relative to 100% by mass of the monomer group is preferably 5 to 60% by mass.
[0040] <Unsaturated organic acid or its salt (c): Also referred to as component (c)> In the present disclosure, the unsaturated organic acid refers to a compound having an acidic group and a polymerizable unsaturated bond. The unsaturated organic acid may be used alone or in combination of two or more kinds.
[0041] The salt of an unsaturated organic acid means a salt of the above-mentioned unsaturated organic acid. The salt of an unsaturated organic acid may be used alone or in combination of two or more kinds.
[0042] Examples of the unsaturated organic acid include unsaturated carboxylic acids, unsaturated sulfonic acids, and unsaturated phosphoric acids.
[0043] Examples of the unsaturated carboxylic acid include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid.
[0044] Examples of unsaturated sulfonic acids include α,β-ethylenically unsaturated sulfonic acids such as vinyl sulfonic acid, styrene sulfonic acid, and (meth)allyl sulfonic acid; (meth)acrylamide t-butyl sulfonic acid, 2-(meth)acrylamide-2-methylpropane sulfonic acid, 2-(meth)acrylamide-2-hydroxypropane sulfonic acid, 3-sulfopropane (meth)acrylic acid ester, and bis-(3-sulfopropyl)itaconic acid ester.
[0045] Examples of unsaturated phosphoric acids include vinylphosphonic acid, vinyl phosphate, bis((meth)acryloxyethyl)phosphate, diphenyl-2-(meth)acryloyloxyethyl phosphate, dibutyl-2-(meth)acryloyloxyethyl phosphate, dioctyl-2-(meth)acryloyloxyethyl phosphate, monomethyl-2-(meth)acryloyloxyethyl phosphate, and 3-(meth)acryloxy-2-hydroxypropane phosphoric acid.
[0046] In the present disclosure, a compound that corresponds to both a (meth)acrylamide group-containing compound and an unsaturated organic acid is considered to be an unsaturated organic acid.
[0047] The salt of the unsaturated organic acid is exemplified by an inorganic salt of the unsaturated organic acid. The inorganic salt of the unsaturated organic acid is a salt in which the cationic portion is a metal cation. Examples of the inorganic salt include an alkali metal salt and an alkaline earth metal salt.
[0048] Examples of the alkali metal include lithium, sodium, and potassium.
[0049] Examples of alkaline earth metals include magnesium and calcium.
[0050] The upper and lower limits of the content of the unsaturated organic acid or a salt thereof relative to 100 mol% of the monomer group are, for example, 40, 35, 30, 25, 20, 15, 10, 5, 0 mol%, etc. In one embodiment, the content is preferably 0 to 40 mol%, and from the viewpoint of improving the water solubility and slurry dispersibility of the (A) component, the content is more preferably 10 to 40 mol%.
[0051] The upper and lower limits of the content of the unsaturated organic acid or a salt thereof relative to 100% by mass of the monomer group are, for example, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 0% by mass, etc. In one embodiment, the content of the unsaturated organic acid or a salt thereof relative to 100% by mass of the monomer group is preferably 0 to 50% by mass.
[0052] <Hydroxyalkyl (meth)acrylate (d) having a hydroxyalkyl group having 2 to 4 carbon atoms: Also referred to as component (d)> As the component (d), various known substances can be used without particular limitation, and they may be used alone or in combination of two or more kinds.
[0053] In the present disclosure, a "hydroxyalkyl group having 2 to 4 carbon atoms" refers to a group in which one of the hydrogen atoms constituting an alkyl group having 2 to 4 carbon atoms has been substituted with a hydroxy group.
[0054] Hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 2 to 4 carbon atoms include 1-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-1-methylethyl (meth)acrylate, 1-hydroxy-2-methylethyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-hydroxypropyl (meth)acrylate. Examples include butyl, 4-hydroxybutyl (meth)acrylate, 1-hydroxy-1-methyl-propyl (meth)acrylate, 2-hydroxy-1-methyl-propyl (meth)acrylate, 3-hydroxy-1-methyl-propyl (meth)acrylate, 1-ethyl-2-hydroxyethyl (meth)acrylate, 1-hydroxy-2-methyl-propyl (meth)acrylate, 2-hydroxy-2-methyl-propyl (meth)acrylate, 3-hydroxy-2-methyl-propyl (meth)acrylate, and 1,1-dimethyl-2-hydroxyethyl (meth)acrylate.
[0055] The upper and lower limits of the content of the hydroxyalkyl (meth)acrylate having a hydroxyalkyl group having 2 to 4 carbon atoms relative to 100 mol % of the monomer group are, for example, 40, 35, 30, 25, 20, 15, 10, 5, 0 mol %, etc. In one embodiment, the content is preferably 0 to 40 mol %, and from the viewpoint of improving the water solubility of the (A) component and the flexibility of the electrode, the content is more preferably 5 to 40 mol %.
[0056] The upper and lower limits of the content of the hydroxyalkyl (meth)acrylate having a hydroxyalkyl group having 2 to 4 carbon atoms relative to 100% by mass of the monomer group are, for example, 40, 35, 30, 25, 20, 15, 10, 5, 0% by mass, etc. In one embodiment, the content of the hydroxyalkyl (meth)acrylate (d) having a hydroxyalkyl group having 2 to 4 carbon atoms relative to 100% by mass of the monomer group is preferably 0 to 40% by mass.
[0057] <α,β-unsaturated nitrile (e): also called component (e)> The α,β-unsaturated nitrile may be used alone or in combination of two or more. The α,β-unsaturated nitrile is preferably used for the purpose of imparting flexibility to the electrode. Examples of the α,β-unsaturated nitrile include (meth)acrylonitrile, α-chloro(meth)acrylonitrile, α-ethyl(meth)acrylonitrile, vinylidene cyanide, and the like. Among these, (meth)acrylonitrile is preferred, and acrylonitrile is particularly preferred.
[0058] The upper and lower limits of the content of the α,β-unsaturated nitrile relative to 100 mol% of the monomer group are, for example, 40, 35, 30, 25, 20, 15, 10, 5, 0 mol%, etc. In one embodiment, the content is preferably 0 to 40 mol%, and from the viewpoint of improving the flexibility of the electrode, the content is more preferably 5 to 40 mol%.
[0059] The upper and lower limits of the content of the α,β-unsaturated nitrile relative to 100% by mass of the monomer group are, for example, 30, 25, 20, 15, 10, 5, 0% by mass, etc. In one embodiment, the content of the α,β-unsaturated nitrile (e) relative to 100% by mass of the monomer group is preferably 0 to 30% by mass.
[0060] <Relative ratio of monomer components> The upper and lower limits of the molar ratio of the (b) component to the (a) component in the monomer group [substance amount of the (b) component / substance amount of the (a) component] are exemplified as 1.3, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, etc. In one embodiment, the molar ratio is preferably 0.05 to 1.3.
[0061] The upper and lower limits of the molar ratio of any one of the components (c) to (e) contained in the monomer group to the component (a) [substance amount of any one of the components (c) to (e) / substance amount of the component (a)] are, for example, 1.3, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the molar ratio is preferably 0 to 1.3.
[0062] The upper and lower limits of the molar ratio of any one of the components (c) to (e) contained in the monomer group to the component (b) [substance amount of any one of the components (c) to (e) / substance amount of the component (b)] are, for example, 8, 7, 6, 5, 4, 3, 2, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the molar ratio is preferably 0 to 8.
[0063] The upper and lower limits of the mass ratio of the component (b) to the component (a) contained in the monomer group [mass of the component (b) / mass of the component (a)] are, for example, 3, 2.5, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, etc. In one embodiment, the mass ratio is preferably 0.05 to 3.
[0064] The upper and lower limits of the mass ratio of the component (c) to the component (a) contained in the monomer group [mass of component (c) / mass of component (a)] are, for example, 2.5, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the above mass ratio is preferably 0 to 2.5.
[0065] The upper and lower limits of the mass ratio of the component (d) to the component (a) contained in the monomer group [mass of the component (d) / mass of the component (a)] are, for example, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the above mass ratio is preferably 0 to 2.
[0066] The upper and lower limits of the mass ratio of the component (e) to the component (a) contained in the monomer group [mass of component (e) / mass of component (a)] are, for example, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the above mass ratio is preferably 0 to 1.5.
[0067] The upper and lower limits of the mass ratio of the component (c) to the component (b) contained in the monomer group [mass of the component (c) / mass of the component (b)] are, for example, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the above mass ratio is preferably 0 to 10.
[0068] The upper and lower limits of the mass ratio of the component (d) to the component (b) contained in the monomer group [mass of component (d) / mass of component (b)] are, for example, 8, 7, 6, 5, 4, 3, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the mass ratio is preferably 0 to 8.
[0069] The upper and lower limits of the mass ratio of the component (e) to the component (b) contained in the monomer group [mass of the component (e) / mass of the component (b)] are, for example, 6, 5, 4, 3, 2, 1.5, 1, 0.9, 0.5, 0.2, 0.1, 0.09, 0.05, 0, etc. In one embodiment, the mass ratio is preferably 0 to 6.
[0070] <Monomers other than components (a) to (e): Also called "other components"> In the above monomer group, a monomer other than any of the components (a) to (e) (other component) can be used as long as it does not impair the desired effects of the present invention. As the other component, various known ones may be used alone or two or more kinds may be used in combination.
[0071] Examples of other components include non-hydroxyl group-containing unsaturated carboxylic acid esters, conjugated dienes, aromatic vinyl compounds, and the like.
[0072] The hydroxyl-free unsaturated carboxylic acid ester is preferably a hydroxyl-free (meth)acrylic acid ester. Examples of the hydroxyl-free (meth)acrylic acid ester include a hydroxyl-free linear (meth)acrylic acid ester, a hydroxyl-free branched (meth)acrylic acid ester, a hydroxyl-free alicyclic (meth)acrylic acid ester, and a hydroxyl-free substituted (meth)acrylic acid ester.
[0073] Examples of non-hydroxyl group-containing linear (meth)acrylate esters include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-amyl (meth)acrylate, hexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, and decyl (meth)acrylate.
[0074] Examples of non-hydroxyl group-containing branched (meth)acrylic esters include i-propyl (meth)acrylate, i-butyl (meth)acrylate, i-amyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.
[0075] Examples of the non-hydroxyl group-containing alicyclic (meth)acrylic acid ester include cyclohexyl (meth)acrylate.
[0076] Examples of non-hydroxyl group-containing substituted (meth)acrylic acid esters include glycidyl (meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate.
[0077] The non-hydroxyl group-containing substituted (meth)acrylic ester also includes alkoxyalkyl (meth)acrylates other than the alkoxyalkyl (meth)acrylate represented by the general formula (1) above.
[0078] The non-hydroxyl group-containing unsaturated carboxylic acid ester is preferably used for the purpose of imparting flexibility to the electrode. From the above viewpoint, the content of the non-hydroxyl group-containing unsaturated carboxylic acid ester relative to 100 mol % of the monomer group is preferably less than 40 mol % (e.g., 30, 20, 19, 15, 10, 5, less than 1 mol %, or 0 mol %).
[0079] The content of the non-hydroxyl-containing unsaturated carboxylic acid ester relative to 100% by mass of the above monomer group is preferably 40% by mass or less (for example, less than 30, 20, 19, 15, 10, 5, or 1% by mass, or 0% by mass).
[0080] Examples of conjugated dienes include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, and substituted and side-chain conjugated hexadienes.
[0081] The content of the conjugated diene relative to 100 mol % of the monomer group is preferably less than 10 mol %, more preferably 0 mol %, from the viewpoint of the cycle characteristics of a lithium ion battery.
[0082] The upper and lower limits of the content of the conjugated diene relative to 100% by mass of the monomer group are, for example, 30, 20, 10, 5, 1, 0% by mass, etc. In one embodiment, the content is preferably 0 to 30% by mass.
[0083] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, and divinylbenzene.
[0084] The content of the aromatic vinyl compound relative to 100 mol % of the above monomer group is preferably less than 10 mol %, more preferably 0 mol %, from the viewpoint of the cycle characteristics of the lithium ion battery.
[0085] The upper and lower limits of the content of the aromatic vinyl compound relative to 100% by mass of the monomer group are, for example, 30, 20, 10, 5, 1, 0% by mass, etc. In one embodiment, the content is preferably 0 to 30% by mass.
[0086] The proportion of other components other than the hydroxyl group-free unsaturated carboxylic acid ester, the conjugated diene, and the aromatic vinyl compound in the monomer group is, relative to 100 mol% of the monomer group, exemplified by less than 10 mol%, less than 5 mol%, less than 2 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol%, 0 mol%, etc. Furthermore, relative to 100 mass% of the monomer group, exemplified by less than 10 mass%, less than 9 mass%, less than 7 mass%, less than 5 mass%, less than 4 mass%, less than 2 mass%, less than 1 mass%, less than 0.9 mass%, less than 0.5 mass%, less than 0.3 mass%, less than 0.1 mass%, less than 0.05 mass%, less than 0.01 mass%, 0 mass%, etc.
[0087] <Method of manufacturing component (A)> The component (A) can be synthesized by various known polymerization methods, preferably radical polymerization methods. Specifically, it is preferable to add a radical polymerization initiator and, if necessary, a chain transfer agent to a monomer mixture containing the above components, and carry out a polymerization reaction at a reaction temperature of 50 to 100° C. while stirring. The reaction time is not particularly limited, and is preferably 1 to 10 hours.
[0088] As the radical polymerization initiator, various known ones can be used without any particular limitation. Examples of the radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate; redox-based polymerization initiators combining the above-mentioned persulfates with a reducing agent such as sodium hydrogen sulfite; and azo-based initiators such as 2,2'-azobis-2-amidinopropane dihydrochloride. The amount of the radical polymerization initiator used is not particularly limited, but is preferably 0.05 to 5.0% by mass, more preferably 0.1 to 3.0% by mass, based on 100% by mass of the monomer group that gives the component (A).
[0089] For the purpose of improving production stability, before the radical polymerization reaction and / or when the obtained component (A) is dissolved in water, the pH of the reaction solution may be adjusted with a common neutralizing agent such as ammonia, organic amine, potassium hydroxide, sodium hydroxide, lithium hydroxide, etc. In this case, the pH is preferably 2 to 11. For the same purpose, it is also possible to use a metal ion-sequestering agent such as ethylenediaminetetraacetic acid (EDTA) or a salt thereof.
[0090] When the (A) component has an acid group, the neutralization rate can be adjusted appropriately according to the application (a neutralization rate of 100% indicates that the acid component contained in the (A) component is neutralized with the same number of moles of alkali. A neutralization rate of 50% indicates that the acid component contained in the (A) component is neutralized with half the number of moles of alkali). The neutralization rate when dispersing the electrode active material is not particularly limited. In one embodiment, the neutralization rate is preferably 95 to 100% after the formation of a coating layer or the like. From the viewpoint of preventing a decrease in the initial capacity, 95% or more is preferable, and from the viewpoint of preventing hydrolysis, 100% or less is preferable. Examples of neutralization salts include Li salts, Na salts, K salts, ammonium salts, Mg salts, Ca salts, Zn salts, and Al salts.
[0091] In one embodiment, the component (A) is preferably an inorganic salt. The inorganic salt of the component (A) refers to a salt in which the cationic moiety is a metal cation. Examples of the inorganic salt include those mentioned above.
[0092] <Physical properties of component (A)> Examples of upper and lower limits of the glass transition temperature of the component (A) are 160, 155, 150, 145, 140, 135, 130, 125, 120, 115, 110, 105, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, and 0° C. In one embodiment, 0° C. or higher is preferable, and from the viewpoint of mechanical strength and heat resistance, 30° C. or higher is more preferable.
[0093] The glass transition temperature of component (A) can be adjusted by the combination of monomers. The glass transition temperature of component (A) can be calculated from the glass transition temperature (Tg) (absolute temperature: K) of the homopolymer of the monomers and their mass fractions based on the Fox formula shown below. 1 / Tg=(W 1 / Tg 1 )+(W 2 / Tg 2 )+(W 3 / Tg 3 )+···+(W n / Tg n ) [Wherein, Tg is the glass transition temperature (K) of the polymer to be determined, W 1 ~W n is the mass fraction of each monomer, Tg 1 ~Tg n indicates the glass transition temperature (K) of the homopolymer of each monomer.
[0094] For example, the glass transition temperature is 165°C for homopolymer of acrylamide, 106°C for homopolymer of acrylic acid, -15°C for homopolymer of hydroxyethyl acrylate, and 105°C for homopolymer of acrylonitrile. The monomer composition constituting component (A) can be determined so as to obtain a component having a desired glass transition temperature. The glass transition temperature of the homopolymer of the monomer can be measured, for example, under conditions of heating from -100°C to 300°C (heating rate 10°C / min.) using a DSC (differential scanning calorimeter), DTA (differential thermal analyzer), TMA (thermomechanical analyzer), or the like. Values described in literature can also be used. Examples of literature include "Chemical Handbook Basics II Edited by the Chemical Society of Japan (Revised 5th Edition)", p. 325, and the like.
[0095] The weight average molecular weight (Mw) of the (A) component is not particularly limited, but examples of the upper and lower limits include 7 million, 6.5 million, 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 350,000, 300,000, 250,000, 200,000, 150,000, and 100,000. In one embodiment, from the viewpoint of dispersion stability of the slurry, it is preferably 100,000 to 7 million, and more preferably 350,000 to 6 million.
[0096] The number average molecular weight (Mn) of the component (A) is not particularly limited, but examples of the upper and lower limits include 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 300,000, 200,000, 100,000, 50,000, 10,000, etc. In one embodiment, the number average molecular weight (Mn) of the component (A) is preferably 10,000 or more.
[0097] The weight average molecular weight and number average molecular weight can be determined, for example, as a polyacrylic acid equivalent value measured in an appropriate solvent by gel permeation chromatography (GPC).
[0098] Examples of the upper and lower limits of the molecular weight distribution (Mw / Mn) of the component (A) are 15, 14, 13, 11, 10, 9, 7.5, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) of the component (A) is preferably 1.1 to 15.
[0099] The B-type viscosity of an aqueous solution containing 13% by mass of component (A) is not particularly limited, but examples of the upper and lower limits include 100,000, 90,000, 80,000, 70,000, 60,000, 50,000, 45,000, 40,000, 30,000, 20,000, 10,000, 900, 700, 500, 300, 200, 1000, 900, 700, 500, 300, 200, 100 mPa s, etc. In one embodiment, the B-type viscosity is preferably in the range of 100 to 100,000 mPa s.
[0100] The Brookfield viscosity is measured using a Brookfield viscometer such as the "Brookfield Viscometer Model BM" manufactured by Toki Sangyo Co., Ltd.
[0101] Examples of the upper and lower limits of the pH of the aqueous binder solution for lithium ion batteries are 9, 8.9, 8.5, 8, 7.9, 7.5, 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, 5, and 4. In one embodiment, the pH of the aqueous binder solution for lithium ion batteries is preferably pH 4 to 9, and more preferably pH 4 to 7, from the viewpoint of solution stability.
[0102] The pH can be measured at 25° C. using a glass electrode pH meter (for example, product name "pH Meter D-52" manufactured by Horiba, Ltd.).
[0103] The upper and lower limits of the content of the component (A) relative to 100% by mass of the aqueous binder solution for lithium ion batteries are, for example, 20, 19, 15, 14, 12, 10, 9, 7, 6, 5% by mass, etc. In one embodiment, the content of the component (A) relative to 100% by mass of the aqueous binder solution for lithium ion batteries is preferably 5 to 20% by mass.
[0104] The upper and lower limits of the water content relative to 100% by mass of the aqueous binder solution for lithium ion batteries are, for example, 95, 90, 85, 80% by mass, etc. In one embodiment, the water content relative to 100% by mass of the aqueous binder solution for lithium ion batteries is preferably 80 to 95% by mass.
[0105] The upper and lower limits of the mass ratio of the component (A) to water contained in the aqueous binder solution for lithium ion batteries are, for example, 0.25, 0.2, 0.15, 0.1, 0.05, etc. In one embodiment, the mass ratio of the component (A) to water contained in the aqueous binder solution for lithium ion batteries is preferably 0.05 to 0.25.
[0106] <Dispersion (emulsion)> In one embodiment, the aqueous binder solution for a lithium ion battery includes a dispersion (emulsion).
[0107] Dispersions (emulsions) include styrene-butadiene copolymer latex, polystyrene polymer latex, polybutadiene polymer latex, acrylonitrile-butadiene copolymer latex, polyurethane polymer latex, polymethyl methacrylate polymer latex, methyl methacrylate-butadiene copolymer latex, polyacrylate polymer latex, vinyl chloride polymer latex, vinyl acetate polymer emulsion, vinyl acetate-ethylene copolymer emulsion, polyethylene emulsion, carboxy-modified styrene butadiene copolymer latex, poly ... Examples include diene copolymer resin emulsion, acrylic resin emulsion, polyethylene, polypropylene, polyethylene terephthalate, polyamide (PA), polyimide (PI), polyamideimide (PAI), aromatic polyamide, alginic acid and its salts, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), and the like.
[0108] Examples of upper and lower limits of the content of the dispersion (emulsion) relative to 100 mass% of the component (A) are 50, 45, 40, 35, 30, 25, 20, 19, 17, 15, 13, 10, 9, 7, 5, 4, 2, 1, 0 mass%, etc. In one embodiment, from the viewpoints of springback resistance and discharge capacity retention rate, the amount of the dispersion (emulsion) added relative to 100 mass% of the component (A) is preferably 0 to 50 mass%.
[0109] <Additives> The aqueous binder solution for lithium ion batteries may contain, as an additive, something that does not fall under any of the component (A), water, and a dispersion (emulsion).
[0110] Examples of the additives include dispersants, leveling agents, antioxidants, thickeners, and the like.
[0111] The content of the additives relative to 100% by mass of the component (A) is, for example, 0 to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, 0% by mass, etc. In one embodiment, the content of the additives relative to 100% by mass of the component (A) is preferably 5% by mass or less, from the viewpoint that haze occurs in the binder when the content exceeds 5% by mass.
[0112] Further, examples of the amount are 0 to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, 0% by mass, and the like, relative to 100% by mass of the aqueous solution.
[0113] Examples of the dispersant include anionic dispersants, cationic dispersants, nonionic dispersants, and polymer dispersants.
[0114] Examples of the leveling agent include surfactants such as alkyl surfactants, silicon surfactants, fluorine surfactants, and metal surfactants. The use of a surfactant can prevent repellency during coating and improve the smoothness of the slurry layer (coating layer).
[0115] Examples of the antioxidant include phenol compounds, hydroquinone compounds, organic phosphorus compounds, sulfur compounds, phenylenediamine compounds, and polymeric phenol compounds. The polymeric phenol compounds are polymers having a phenol structure in the molecule. The weight average molecular weight of the polymeric phenol compounds is preferably 200 to 1000, and more preferably 600 to 700.
[0116] Examples of thickeners include cellulose-based polymers such as carboxymethyl cellulose, methyl cellulose, and hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; (modified) poly(meth)acrylic acid and their ammonium salts and alkali metal salts; (modified) polyvinyl alcohols such as copolymers of acrylic acid or acrylates and vinyl alcohol, and copolymers of maleic anhydride or maleic acid or fumaric acid and vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinylpyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, and hydrogenated acrylonitrile-butadiene copolymers.
[0117] The aqueous binder solution for lithium ion batteries can be used as an aqueous binder solution for lithium ion battery electrodes and an aqueous binder solution for lithium ion battery negative electrodes.
[0118] [Lithium-ion battery negative electrode slurry: also called slurry] The present disclosure provides a slurry for a lithium ion battery negative electrode, comprising the above-mentioned aqueous binder solution for a lithium ion battery electrode and a negative electrode active material (B).
[0119] In this disclosure, "slurry" means a suspension of liquid and solid particles.
[0120] The upper and lower limits of the content of the component (A) relative to 100% by mass of the slurry are 99.9, 95, 90, 80, 70, 60, 50, 40, 30, 20, 10, 5, 1, 0.5, 0.2, 0.1% by mass, etc. In one embodiment, the component (A) is contained in an amount of 0.1 to 99.9% by mass relative to 100% by mass of the slurry.
[0121] Examples of water include ultrapure water, pure water, distilled water, ion-exchanged water, and tap water.
[0122] The upper and lower limits of the water content relative to 100% by mass of the slurry are exemplified as 70, 65, 60, 55, 50, 45, 40, 35, 30% by mass, etc. In one embodiment, the water content relative to 100% by mass of the slurry is preferably 30 to 70% by mass.
[0123] <Negative electrode active material (B): Also called component (B)> The negative electrode active materials may be used alone or in combination of two or more kinds.
[0124] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium, and an appropriate material can be selected depending on the type of the target lithium ion battery, and may be used alone or in combination of two or more. Examples of the negative electrode active material include carbon materials, silicon materials, oxides containing lithium atoms, lead compounds, tin compounds, arsenic compounds, antimony compounds, and aluminum compounds that are alloyed with lithium.
[0125] Examples of the carbon material include highly crystalline carbon such as graphite (also called graphite, and examples of which include natural graphite and artificial graphite), low crystalline carbon (soft carbon, hard carbon), carbon black (ketjen black, acetylene black, channel black, lamp black, oil furnace black, thermal black, etc.), fullerene, carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon fibrils, mesocarbon microbeads (MCMB), and pitch-based carbon fibers.
[0126] In addition to silicon, silicon oxide, and silicon alloys, the silicon material includes SiC, SiO x C y (0 < x ≤ 3, 0 < y ≤ 5), Si 3 N 4 Si 2 N 2 O, SiO x (0 < x ≤ 2) silicon oxide composites (such as the materials described in JP-A-2004-185810 and JP-A-2005-259697), and silicon materials described in JP-A-2004-185810 are exemplified. Further, the silicon materials described in Patent No. 5390336 and Patent No. 5903761 may also be used.
[0127] The silicon oxide is preferably silicon oxide represented by the compositional formula SiO x (0 < x < 2, preferably 0.1 ≤ x ≤ 1).
[0128] The silicon alloy is preferably an alloy of silicon and at least one transition metal selected from the group consisting of titanium, zirconium, nickel, copper, iron, and molybdenum. These transition metal silicon alloys are preferred because they have high electron conductivity and high strength. The silicon alloy is more preferably a silicon-nickel alloy or a silicon-titanium alloy, and particularly preferably a silicon-titanium alloy. The content ratio of silicon in the silicon alloy is preferably 10 mol% or more, more preferably 20 to 70 mol%, based on 100 mol% of the metal elements in the silicon alloy. The silicon material may be any of single crystal, polycrystal, and amorphous.
[0129] When a silicon material is used as the negative electrode active material, a negative electrode active material other than the silicon material may be used in combination. Such negative electrode active materials include the above carbon materials; conductive polymers such as polyacene; A X B Y O Z(A is an alkali metal or a transition metal, B is at least one selected from transition metals such as cobalt, nickel, aluminum, tin, manganese, etc., O represents an oxygen atom, and X, Y, and Z are numbers in the ranges of 0.05 < X < 1.10, 0.85 < Y < 4.00, and 1.5 < Z < 5.00, respectively.) Composite metal oxides represented by the formula, and other metal oxides, etc. are exemplified. When a silicon material is used as the negative electrode active material, since the volume change accompanying the absorption and release of lithium is small, it is preferable to use a carbon material in combination.
[0130] The above-mentioned oxides containing lithium atoms include lithium nickel cobalt manganese oxide, lithium-manganese composite oxide (LiMn 2 O 4 etc.), lithium-nickel composite oxide (LiNiO 2 etc.), lithium-cobalt composite oxide (LiCoO 2 etc.), lithium-iron composite oxide (LiFeO 2 etc.), lithium-nickel-manganese composite oxide (LiNi 0.5 Mn 0.5 O 2 etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2 O 2 etc.), lithium-transition metal phosphate compound (LiFePO 4 etc.), and lithium-transition metal sulfate compound (Li x Fe 2 (SO 4 ) 3 ), lithium-titanium composite oxide (lithium titanate: Li 4 Ti 5 O 12 ), etc. lithium-transition metal composite oxides, and other conventionally known negative electrode active materials, etc. are exemplified.
[0131] From the viewpoint that the effects of the present invention are significantly exhibited, a carbon material and / or a material that alloyizes with lithium are preferably contained in the negative electrode active material in an amount of 50% by mass or more, more preferably 80% by mass or more, still more preferably 90% by mass or more, and particularly preferably 100% by mass.
[0132] In one embodiment, the negative electrode active material (B) is preferably a negative electrode active material containing 1 mass % or more (2, 5, 10, 25, 50, 75, 90 mass % or more, 100 mass %) of silicon and / or silicon oxide covered with a carbon layer.
[0133] The shape of the negative electrode active material is not particularly limited, and may be any shape such as fine particles or thin film, but fine particles are preferred. The average particle size of the negative electrode active material is not particularly limited, but the upper and lower limits are 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 4, 3, 2.9, 2, 1, 0.5, 0.1 μm, etc. In one embodiment, from the viewpoint of forming a uniform and thin coating film, more specifically, if it is 0.1 μm or more, the handling property is good, and if it is 50 μm or less, the application of the electrode is easy, so that the average particle size of the negative electrode active material is preferably 0.1 to 50 μm, more preferably 0.1 to 45 μm, even more preferably 1 to 10 μm, and particularly preferably 5 μm.
[0134] In this disclosure, the term "particle size" refers to the maximum distance between any two points on the contour of a particle (hereinafter the same). In addition, in this disclosure, the term "average particle size" refers to a value calculated as the average particle size of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM) unless otherwise specified (hereinafter the same).
[0135] The upper and lower limits of the content of the component (A) relative to 100% by mass of the negative electrode active material (B) in the slurry are, for example, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1.5, 1, 0.5% by mass, etc. In one embodiment, the content is preferably 0.5 to 15% by mass.
[0136] <Conductive assistant> In one embodiment, a conductive assistant may be included in the slurry. Examples of the conductive assistant include fibrous carbon such as vapor grown carbon fiber (VGCF), carbon nanotube (CNT), and carbon nanofiber (CNF), graphite particles, carbon black such as acetylene black, ketjen black, and furnace black, and fine powder of Cu, Ni, Al, Si, or alloys thereof having an average particle size of 10 μm or less. The content of the conductive assistant is not particularly limited, but is preferably 0 to 10 mass %, and more preferably 0.5 to 6 mass %, based on the negative electrode active material components.
[0137] <Slurry viscosity adjusting solvent> The slurry viscosity adjusting solvent is not particularly limited, and may include a non-aqueous medium having a normal boiling point of 80 to 350° C. The slurry viscosity adjusting solvent may be used alone or in combination of two or more kinds. Examples of the slurry viscosity adjusting solvent include amide solvents such as N-methylpyrrolidone, dimethylformamide, and N,N-dimethylacetamide; hydrocarbon solvents such as toluene, xylene, n-dodecane, and tetralin; alcohol solvents such as methanol, ethanol, 2-propanol, isopropyl alcohol, 2-ethyl-1-hexanol, 1-nonanol, and lauryl alcohol; ketone solvents such as acetone, methyl ethyl ketone, cyclohexanone, phorone, acetophenone, and isophorone; ether solvents such as dioxane and tetrahydrofuran (THF); ester solvents such as benzyl acetate, isopentyl butyrate, methyl lactate, ethyl lactate, and butyl lactate; amine solvents such as o-toluidine, m-toluidine, and p-toluidine; lactones such as γ-butyrolactone and δ-butyrolactone; sulfoxide and sulfone solvents such as dimethyl sulfoxide and sulfolane; and water. Among these, N-methylpyrrolidone is preferred from the viewpoint of coating workability. The content of the non-aqueous medium is not particularly limited, but is preferably 0 to 10% by mass relative to 100% by mass of the slurry.
[0138] The above-mentioned slurry may contain, as an additive, an additive other than the (A) component, the (B) component, water, a conductive assistant, or a slurry viscosity adjusting solvent, within a range that does not impair the effects of the present invention. Examples of the additive include those mentioned above.
[0139] The content of the additives is, for example, 0 to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, 0% by mass, etc., relative to 100% by mass of the component (A).
[0140] The content of the additive relative to 100% by mass of the component (B) is, for example, 0 to 5% by mass, less than 1% by mass, less than 0.1% by mass, less than 0.01% by mass, or 0% by mass.
[0141] The dispersion (emulsion) may be contained in a larger amount than the additives described above. The upper and lower limits of the content of the dispersion (emulsion) relative to 100% by mass of the slurry for the lithium ion battery negative electrode are 20, 19, 17, 15, 13, 10, 9, 7, 5, 4, 2, 1, and 0% by mass. In one embodiment, from the viewpoint of springback resistance and discharge capacity retention rate, the amount of the dispersion (emulsion) added relative to 100% by mass of the aqueous solution or the slurry for the lithium ion battery negative electrode is preferably less than 5% by mass.
[0142] The above slurry is produced by mixing the component (A), the component (B), and water, and, if necessary, a conductive assistant and a slurry viscosity adjusting solvent.
[0143] Examples of means for mixing the slurry include a ball mill, a sand mill, a pigment disperser, a crusher, an ultrasonic disperser, a homogenizer, a planetary mixer, and a Hobart mixer.
[0144] [Lithium-ion battery negative electrode] The present disclosure provides a lithium ion battery negative electrode obtained by applying the above-mentioned slurry for lithium ion battery negative electrodes to a current collector, followed by drying and curing. The lithium ion battery negative electrode has a cured product of the above-mentioned slurry for lithium ion battery negative electrodes on a current collector surface.
[0145] The current collector may be any of various known current collectors without any particular limitation. The material of the current collector is not particularly limited, and examples thereof include metal materials such as copper, iron, aluminum, nickel, stainless steel, and nickel-plated steel, and carbon materials such as carbon cloth and carbon paper. The form of the current collector is also not particularly limited, and examples of metal materials include metal foil, metal cylinder, metal coil, and metal plate, and examples of carbon materials include carbon plate, carbon thin film, and carbon cylinder. Among them, when the electrode active material is used for the negative electrode, copper foil is preferred as the current collector because it is currently used in industrialized products.
[0146] The coating means is not particularly limited, and examples thereof include conventionally known coating devices such as a comma coater, a gravure coater, a microgravure coater, a die coater, and a bar coater.
[0147] The drying means is not particularly limited, and the temperature is preferably 60 to 200° C., more preferably 100 to 195° C. The atmosphere may be dry air or an inert atmosphere.
[0148] The thickness of the negative electrode (cured product) is not particularly limited, but is preferably 5 to 300 μm, and more preferably 10 to 250 μm. By setting the thickness within the above range, it may become easier to obtain a sufficient Li absorption / release function for a high-density current value.
[0149] [Lithium-ion battery] The present disclosure provides a lithium ion battery including the above-mentioned negative electrode for lithium ion batteries. In one embodiment, the battery includes an electrolyte solution, a separator, a positive electrode, and the like. These are not particularly limited.
[0150] The electrolyte solution may be, for example, a non-aqueous electrolyte solution in which a supporting electrolyte is dissolved in a non-aqueous solvent, etc. The non-aqueous electrolyte solution may also contain a film-forming agent.
[0151] As the non-aqueous solvent, various known solvents can be used without any particular limitation, and may be used alone or in combination of two or more. Examples of the non-aqueous solvent include chain carbonate solvents such as diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate; cyclic carbonate solvents such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain ether solvents such as 1,2-dimethoxyethane; cyclic ether solvents such as tetrahydrofuran, 2-methyltetrahydrofuran, sulfolane, and 1,3-dioxolane; chain ester solvents such as methyl formate, methyl acetate, and methyl propionate; cyclic ester solvents such as γ-butyrolactone and γ-valerolactone; and acetonitrile. Among these, a combination of a mixed solvent containing a cyclic carbonate and a chain carbonate is preferred.
[0152] The supporting electrolyte is a lithium salt. Various known lithium salts can be used without particular limitation, and may be used alone or in combination of two or more kinds. The supporting electrolyte is LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C. 4 F 9 SO 3 Li, C.F. 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF, which is easily soluble in solvents and has a high degree of dissociation, is the most popular. 6 , LiClO 4 , C.F. 3 SO 3 Li is preferred. The higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity. Therefore, the lithium ion conductivity can be adjusted by the type of supporting electrolyte.
[0153] The coating agent may be any of various known agents without particular limitation, and may be used alone or in combination of two or more. Examples of the coating agent include carbonate compounds such as vinylene carbonate, vinyl ethylene carbonate, vinyl ethyl carbonate, methyl phenyl carbonate, fluoroethylene carbonate, and difluoroethylene carbonate; alkene sulfides such as ethylene sulfide and propylene sulfide; sultone compounds such as 1,3-propane sultone and 1,4-butane sultone; and acid anhydrides such as maleic anhydride and succinic anhydride. The content of the coating agent in the electrolyte solution is not particularly limited, but is preferably 10% by mass or less, 8% by mass or less, 5% by mass or less, and 2% by mass or less in that order. By setting the content to 10% by mass or less, it becomes easier to obtain the advantages of the coating agent, such as suppression of initial irreversible capacity and improvement of low-temperature characteristics and rate characteristics.
[0154] The separator is an article interposed between the positive electrode and the negative electrode, and is used to prevent short circuit between the electrodes. Specifically, a porous separator such as a porous membrane or a nonwoven fabric can be preferably used, and is used by impregnating the nonaqueous electrolyte solution. The separator is made of a polyolefin such as polyethylene or polypropylene, or polyethersulfone, and is preferably made of polyolefin.
[0155] The positive electrode may be any of various known positive electrodes without any particular limitations. Examples of the positive electrode include a positive electrode obtained by mixing a positive electrode active material, a conductive assistant, and a positive electrode binder with an organic solvent to prepare a slurry, and applying the prepared slurry to a positive electrode current collector, drying, and pressing the slurry.
[0156] The positive electrode active material is exemplified by inorganic positive electrode active materials and organic positive electrode active materials. Examples of the inorganic positive electrode active material include transition metal oxides, composite oxides of lithium and transition metals, transition metal sulfides, etc. Examples of the transition metals include Fe, Co, Ni, Mn, Al, etc. Inorganic compounds used for the positive electrode active material include LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2O 4 , LiFePO 4 , LiNi 1 / 2 Mn 3 / 2 O 4 , LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li[Li 0.1 Al 0.1 Mn 1.8 ]O 4 , LifeVO 4 Lithium-containing complex metal oxides such as TiS 2 , TiS 3 , amorphous MoS 2 Transition metal sulfides such as Cu 2 V 2 O 3 , amorphous V 2 OP 2 O 5 , MoO 3 , V 2 O 5 , V 6 O 13 Examples of the organic positive electrode active material include conductive polymers such as polyacetylene and poly-p-phenylene. Iron-based oxides, which have poor electrical conductivity, may be used as an electrode active material covered with a carbon material by making a carbon source material present during reduction and firing. These compounds may also be partially substituted with elements. Among these, LiCoO is particularly preferred in terms of practicality, electrical properties, and long life. 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , LiFePO 4 , LiNi 1 / 2 Mn 3 / 2 O 4 , LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O 2 , Li[Li 0.1 Al 0.1 Mn 1.8 ]O 4 is preferred.
[0157] Examples of the conductive assistant include fibrous carbon such as vapor grown carbon fiber (VGCF), carbon nanotube (CNT), and carbon nanofiber (CNF), graphite particles, carbon black such as acetylene black, ketjen black, and furnace black, and fine powders of Cu, Ni, Al, Si, or alloys thereof having an average particle size of 10 μm or less.
[0158] The positive electrode binder may be any of various known binders without particular limitation, and may be used alone or in combination of two or more. Examples of the positive electrode binder include fluorine-based resins (polyvinylidene fluoride, polytetrafluoroethylene, etc.), polyolefins (polyethylene, polypropylene, etc.), polymers having unsaturated bonds (styrene-butadiene rubber, isoprene rubber, butadiene rubber, etc.), and acrylic acid-based polymers (acrylic acid copolymers, methacrylic acid copolymers, etc.).
[0159] The positive electrode current collector is exemplified by an aluminum foil, a stainless steel foil, and the like.
[0160] The shape of the lithium ion battery is not particularly limited. Examples of the shape of the lithium ion battery include a cylinder type in which a sheet electrode and a separator are spirally wound, a cylinder type with an inside-out structure in which a pellet electrode and a separator are combined, and a coin type in which a pellet electrode and a separator are laminated. In addition, by housing a battery of these shapes in an arbitrary exterior case, it can be used in an arbitrary shape such as a coin type, a cylindrical type, or a square type.
[0161] The method for manufacturing the lithium ion battery is not particularly limited, and the battery may be assembled in an appropriate procedure according to the structure of the battery. The lithium ion battery may be manufactured, for example, by the method described in JP 2013-089437 A. The battery can be manufactured by placing a negative electrode on an exterior case, providing an electrolyte and a separator thereon, placing a positive electrode facing the negative electrode, and fixing them with a gasket and a sealing plate. EXAMPLES
[0162] The present invention will be specifically described below through examples and comparative examples. However, the above-mentioned description of the preferred embodiment and the following examples are provided for illustrative purposes only and are not provided for the purpose of limiting the present invention. Therefore, the scope of the present invention is not limited to the embodiments or examples specifically described in this specification, but is limited only by the claims. In each example and comparative example, unless otherwise specified, numerical values such as parts and % are based on mass.
[0163] (A) Manufacturing of ingredients Manufacturing Example 1 In a reaction apparatus equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, 1240g of ion-exchanged water, 350g (2.46mol) of 50% acrylamide aqueous solution, 56.6g (0.43mol) of 2-methoxyethyl acrylate, and 0.23g (0.0014mol) of sodium methallylsulfonate were placed, and oxygen in the reaction system was removed by passing nitrogen gas through it, after which the temperature was raised to 55°C. 2.1g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 20g of ion-exchanged water were placed therein, and the temperature was raised to 80°C and the reaction was carried out for 3 hours. Ion-exchanged water was added so that the solid concentration was 13%, and an aqueous binder solution containing water-soluble poly(meth)acrylamide was obtained. The B-type viscosity of this solution at 25°C was 10,000mPa·s.
[0164] In Production Examples 2 to 4, aqueous binder solutions containing water-soluble poly(meth)acrylamide were prepared in the same manner as in Production Example 1, except that the monomer compositions were changed to those shown in the table below.
[0165] Production Example 5 In a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube, 1170g of ion-exchanged water, 120g (0.84mol) of 50% acrylamide aqueous solution, 12g (0.12mol) of N,N-dimethylacrylamide, 62.8g (0.48mol) of 2-methoxyethyl acrylate, 87g (0.96mol) of 80% acrylic acid, and 0.19g (0.0012mol) of sodium methallylsulfonate were placed, and oxygen in the reaction system was removed by passing nitrogen gas through it, and the temperature was raised to 55°C. 1.8g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 20g of ion-exchanged water were placed therein, and the temperature was raised to 80°C and the reaction was carried out for 3 hours. Then, 64.4 g (0.77 mol) of 48% sodium hydroxide solution was added as a neutralizing agent and stirred, and ion-exchanged water was added to make the solids concentration 13%, to obtain an aqueous binder solution containing water-soluble poly(meth)acrylamide. The Brookfield viscosity of this solution at 25°C was 12,000 mPa s.
[0166] In Production Examples 6 and 7, aqueous binder solutions containing water-soluble poly(meth)acrylamide were prepared in the same manner as in Production Example 5, except that the monomer composition and the amount of neutralizing agent were changed as shown in the table below.
[0167] Comparative Manufacturing Example 1 In a reactor equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet, 1280g of ion-exchanged water, 500g (3.52mol) of 50% acrylamide aqueous solution, and 0.28g (0.0018mol) of sodium methallylsulfonate were placed, and oxygen in the reaction system was removed by passing nitrogen gas through it, after which the temperature was raised to 55°C. 2.3g of 2,2'-azobis-2-amidinopropane dihydrochloride (manufactured by Nippoh Chemical Co., Ltd., product name "NC-32") and 20g of ion-exchanged water were added, and the temperature was raised to 80°C and the reaction was carried out for 3 hours. After that, ion-exchanged water was added so that the solid concentration was 13%, and an aqueous binder solution containing water-soluble poly(meth)acrylamide was obtained. The B-type viscosity of this solution at 25°C was 15,000mPa·s.
[0168] In the comparative production examples other than the above-mentioned Comparative Production Example 1, aqueous solutions containing water-soluble poly(meth)acrylamide were prepared in the same manner as in the above-mentioned Comparative Production Example 1, except that the monomer composition and the like in the above-mentioned Comparative Production Example 1 were changed to those shown in the table below.
[0169] B type viscosity The viscosity of each aqueous binder solution was measured at 25° C. under the following conditions using a Brookfield viscometer (manufactured by Toki Sangyo Co., Ltd., product name: Brookfield viscometer model BM). Uses No.3 rotor, rotation speed 6 rpm.
[0170] Weight average molecular weight The weight average molecular weight was determined as a polyacrylic acid equivalent value measured by gel permeation chromatography (GPC) in a 0.2 M phosphate buffer / acetonitrile solution (90 / 10, pH 8.0). The GPC apparatus used was HLC-8220 (manufactured by Tosoh Corporation), and the column used was SB-806M-HQ (manufactured by SHODEX). [Table 2] AM: Acrylamide (Mitsubishi Chemical Corporation "50% Acrylamide") ·DMAA: N,N-Dimethylacrylamide ("DMAA" manufactured by KJ Chemicals Co., Ltd.) MEA: 2-Methoxyethyl acrylate (Osaka Organic Chemical Industry Ltd. "2-MTA") MMEA: 2-Methoxyethyl Methacrylate (Tokyo Chemical Industry Co., Ltd. "2-Methoxyethyl Methacrylate") · MEEA: 2-ethoxyethyl methacrylate (Tokyo Chemical Industry Co., Ltd. "2-Ethoxyethyl Methacrylate") AA: Acrylic acid (Osaka Organic Chemical Industry Co., Ltd. "80% acrylic acid") ·HEA: 2-hydroxyethyl acrylate ("HEA" manufactured by Osaka Organic Chemical Industry Ltd.) AN: Acrylonitrile (Mitsubishi Chemical Corporation "Acrylonitrile") ·BA: Butyl acrylate (manufactured by Toagosei Co., Ltd. "Butyl acrylate") ·SMAS: Sodium methallyl sulfonate NaOH: Sodium hydroxide (Kanto Chemical Co., Ltd. "48% sodium hydroxide solution")
[0171] Slurry production, cell construction and evaluation Example 1 <Production of electrode slurry> A slurry was prepared using a commercially available homodisper ("Homodisper 2.5 type" manufactured by Primix Corporation). 5 parts by mass of the aqueous binder solution for lithium ion batteries containing the water-soluble poly(meth)acrylamide (A) obtained in Production Example 1, calculated as solid content, 20 parts by mass of silicon monoxide particles ("CC Powder" manufactured by Osaka Titanium Technologies Co., Ltd.) with a D50 (median diameter) of 5 μm, 80 parts by mass of artificial graphite ("G1-A♯" manufactured by Jiangxi Zishen Technology Co., Ltd.) with a D50 (median diameter) of 20 μm, and 1 part by mass of a conductive assistant ("Super C65" manufactured by Imerys GC Japan Co., Ltd.) were mixed in a mayonnaise bottle as a container. Ion-exchanged water was added thereto so that the solid content concentration was 47%, and the container was set in the homodisper. Then, the mixture was kneaded at 3,000 rpm for 10 minutes. Thereafter, the mixture was defoamed for 1 minute using a planetary centrifugal mixer (Thinky Corporation's "Awatori Rentaro") to obtain a slurry for electrodes.
[0172] In the examples and comparative examples other than Example 1, slurries were prepared in the same manner as in Example 1 above, except that the composition in Example 1 was changed to that shown in the table below.
[0173] <Storage stability test of electrode slurry> The storage stability of the electrode slurry was evaluated as follows. The viscosity of the electrode slurry (unit: mPa s) was measured using a Brookfield viscometer, and then it was stored in an oven heated to 40°C for three days. After storage, the viscosity was measured again using the Brookfield viscometer, and the change in viscosity was calculated using the following formula and evaluated according to the following criteria. Viscosity change (%) = {(viscosity of electrode slurry after storage) / (viscosity of electrode slurry before storage)} × 100 A: Less than 110% B: 110% or more but less than 120% C: 120% or more but less than 130% D: 130% or more
[0174] <Electrode flexibility evaluation> The electrode flexibility was evaluated as follows. The above-mentioned lithium ion battery slurry was uniformly applied to the surface of a copper foil current collector (20 μm) by a doctor blade method so that the film thickness after drying would be 170 μm, and the coating was heated and dried for 15 minutes at 150° C. to obtain an electrode. The obtained electrode was cut to a width of 10 mm and a length of 70 mm, and wrapped around a Teflon (registered trademark) rod with a diameter of 30 mm with the active material layer facing outward. The surface condition of the active material layer was observed and evaluated according to the following criteria. A: The active material layer bonded to the current collector had no cracks or peeling whatsoever. B: Cracks are observed in the active material layer bonded to the current collector, but no peeling is observed. C: Cracks and peeling were observed in the active material layer bonded to the current collector.
[0175] <Electrode Adhesion Evaluation> The electrode adhesion was evaluated as follows. The above-mentioned slurry for lithium ion batteries was uniformly applied to the surface of a current collector (20 μm) made of copper foil by a doctor blade method so that the film thickness after drying would be 170 μm, and after drying at 150° C. for 30 minutes, it was heat-treated at 150° C. / vacuum for 120 minutes. After that, the density of the film (electrode active material layer) was 1.5 g / cm 3The electrode was obtained by pressing the electrode with a roll press machine so that the electrode was in a shape of 2 cm wide x 10 cm long. A test piece with a width of 2 cm x length of 10 cm was cut out from the obtained electrode and fixed with the coating surface facing up. Next, a 15 mm wide adhesive tape ("Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.) (specified in JIS Z1522) was applied to the surface of the active material layer of the test piece while pressing it, and then the stress was measured when the adhesive tape was peeled off from one end of the test piece in the 180° direction at a speed of 30 mm / min using a tensile tester ("Tensilon RTM-100" manufactured by A&D Co., Ltd.) under a condition of 25°C. The measurement was performed twice, and the value was converted to a value per 15 mm width, and the average value was calculated as the peel strength. The higher the peel strength, the higher the adhesion strength between the current collector and the active material layer or the binding strength between the active materials, and the more difficult it is to peel off the active material layer or the active materials from the current collector.
[0176] The electrode adhesion was evaluated according to the following criteria and is shown in the table. AA:41N / m or more A: 30~40N / m B: 20~30N / m C: Less than 20N / m
[0177] <Assembling lithium half-cells> The above-mentioned slurry for lithium ion batteries was uniformly applied to the surface of a current collector (20 μm) made of copper foil by a doctor blade method so that the film thickness after drying would be 170 μm, and after drying at 150° C. for 30 minutes, it was heat-treated at 150° C. / vacuum for 120 minutes. After that, the density of the film (electrode active material layer) was 1.5 g / cm 3 The electrode was obtained by pressing the electrode sheet with a roll press machine so that the electrode sheet had a thickness of 100 mm. In a glove box substituted with argon, the above electrode was punched out to a diameter of 16 mm and placed inside the packing on the aluminum bottom cover of a test cell (manufactured by Nippon Tomcell Co., Ltd.). Next, a separator made of a polypropylene porous film punched out to a diameter of 24 mm (manufactured by CS TECH CO., LTD, "Selion P2010") was placed, and 500 μL of electrolyte was poured in so as to prevent air from entering. Then, a commercially available metallic lithium foil punched out to a diameter of 16 mm was placed on the separator, and the exterior body of the test cell was screwed down and sealed to assemble a lithium half cell. The electrolyte used here was LiPF 6 This is a solution in which the above is dissolved at a concentration of 1 mol / L.
[0178] <Charge / discharge measurement> The lithium half-cell was placed in a thermostatic chamber at 25° C., and charging was started at a constant current (0.1 C), and charging was completed (cut off) when the voltage reached 0.01 V. Next, discharging was started at a constant current (0.1 C), and charging and discharging was repeated 30 times, with discharging completed (cut off) when the voltage reached 1.0 V. In the above measurement conditions, "1C" refers to the current value at which a cell with a certain capacity is discharged at a constant current and the discharge is completed in 1 hour. For example, "0.1C" refers to the current value at which the discharge is completed in 10 hours, and "10C" refers to the current value at which the discharge is completed in 0.1 hour.
[0179] <Discharge capacity maintenance rate> The discharge capacity retention rate was calculated according to the following formula. Discharge capacity retention rate = {(discharge capacity at 30th cycle) / (discharge capacity at 1st cycle)} x 100 (%)
[0180] The discharge capacity retention rate was evaluated according to the following criteria and is shown in the table. AA: 90% or more A: 80~89% B: 70~79% C: Less than 70%
[0181]
Table 3
Claims
1. Relative to 100 mol % of the monomer group, 30 to 95 mol % of a (meth)acrylamide group-containing compound (a), and The present invention relates to a polymerizable composition comprising a non-crosslinkable water-soluble poly(meth)acrylamide (A) which is a polymer of a monomer group containing 5 to 40 mol % of an alkoxyalkyl (meth)acrylate (b) represented by the following general formula (1): Aqueous binder solution for lithium-ion batteries. CH 2 =C(R 1 )-CO-O-R 2 -O-R 3 (1) (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 is an alkylene group having 1 to 4 carbon atoms, R 3 is an alkyl group having 1 to 4 carbon atoms. 1 , R 2 , and R 3 The total number of carbon atoms in the groups is 5 or less.
2. A slurry for a lithium ion battery negative electrode, comprising the aqueous binder solution for a lithium ion battery according to claim 1 and a negative electrode active material.
3. A negative electrode for a lithium ion battery, obtained by applying the slurry for a lithium ion battery negative electrode according to claim 2 to a current collector, followed by drying and curing.
4. A lithium ion battery comprising the negative electrode for a lithium ion battery according to claim 3.
Citation Information
Patent Citations
Method for producing organic-inorganic composite gel in slurry state and organic-inorganic composite gel coating film
JP2012241085A
Slurry for electricity storage device negative electrode and electricity storage device negative electrode, slurry for electricity storage device positive electrode and electricity storage device positive electrode, and electricity storage device
JP2015106488A
Binder composition for electricity storage device, slurry for electricity storage device, electricity storage device electrode, separator, and electricity storage device
JP2015118908A
Positive electrode for battery, method for manufacturing the same, and battery
JP2018170219A
Organic-inorganic composite gel, secondary battery electrolyte gel, and secondary battery, and manufacturing method therefor
WO2012144332A1