Toner for developing electrostatic images, electrostatic image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

The toner formulation with balanced Na/Cl ratios and crystalline resin domains addresses the fixing property issues of existing toners, achieving enhanced halftone image adherence and uniform melting.

JP7577954B2Active Publication Date: 2024-11-06FUJIFILM BUSINESS INNOVATION CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020159120
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-23
Publication Date
2024-11-06
Estimated Expiration
2040-09-23

AI Technical Summary

Technical Problem

Existing toners for electrostatic image development do not achieve optimal fixing properties for halftone images, particularly due to imbalances in the ratios of sodium (Na) and chlorine (Cl) intensities, which affect the toner's surface hardness and melting behavior.

Method used

A toner formulation incorporating amorphous and crystalline polyester resins, with controlled ratios of Na and Cl intensities, and specific crystalline resin domain configurations, enhances fixing properties by ensuring uniform heat distribution and surface properties.

Benefits of technology

The toner exhibits superior fixing properties for halftone images by maintaining a balanced Na/Cl ratio and crystalline resin domain arrangement, leading to improved image adherence and uniform melting during fixation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577954000005
    Figure 0007577954000005
  • Figure 0007577954000006
    Figure 0007577954000006
  • Figure 0007577954000007
    Figure 0007577954000007
Patent Text Reader

Abstract

To provide a toner for electrostatic charge image development that is excellent in fixability of a halftone image.SOLUTION: A toner for electrostatic charge image development contains an amorphous polyester resin and a crystalline polyester resin. The Net intensity NNa of a Na element measured by fluorescent X-ray analysis and the Net intensity NCl of a Cl element measured by fluorescent X-ray analysis satisfy the relationship of 2.5≤NCl / NNa≤260.0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge, an image forming apparatus, and an image forming method. [Background technology]

[0002] Patent Document 1 discloses a toner for developing electrostatic images, which contains toner particles containing residual ammonium ions and silica particles containing a chlorine compound as an external additive.

[0003] Patent Document 2 discloses a toner for developing electrostatic images, which contains a binder resin and a colorant, the binder resin being a polyester resin or a polyol resin, the toner particles containing 0.007 to 0.140 mass % of aluminum and 0.002 to 0.412 mass % of chlorine, and the toner particles having an average circularity of 0.94 to 0.99 and an average circle-equivalent diameter of 2.6 to 74 μm.

[0004] Patent Document 3 discloses a toner including toner particles having a toner core containing a melt-kneaded product of a non-crystalline resin and a crystalline resin and a shell layer containing a thermosetting resin, in which the melt-kneaded product contains a plurality of crystalline resin domains, and the proportion of domains among the plurality of crystalline resin domains that satisfy the conditions of a short axis diameter of 50 nm or more and 200 nm or less and an aspect ratio of 4.0 or more and 20.0 or less is 80% or more by number.

[0005] Patent Document 4 discloses a toner having toner particles containing an amorphous polyester resin, a crystalline polyester resin, and a wax, in which wax domains and crystalline polyester resin crystals are present, the area of ​​the toner cross-sectional area occupied by the wax domains is 0.5% or more and 8.0% or less, the area occupied by the crystalline polyester resin crystals is 0.5% or more and 8.0% or less, the number average diameter of the wax domains is 60 nm or more and 240 nm or less, the aspect ratio of the crystalline polyester resin crystals is 5.0 or more and 25.0 or less, and the number average diameter of the major axis length of the crystalline polyester resin crystals is 0.8 times or more and 2.0 times or less the number average diameter of the wax domains. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-068307 A [Patent Document 2] JP 2004-287421 A [Patent Document 3] JP 2019-040024 A [Patent Document 4] JP 2017-003990 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present disclosure relates to a polyester resin composition comprising an amorphous polyester resin and a crystalline polyester resin, and a net intensity N Na and the net intensity N of Cl element measured by X-ray fluorescence analysis. Cl But, 2.5>N Cl / N Na It is an object of the present invention to provide a toner for developing electrostatic images, which has excellent fixing properties for halftone images, compared with toners for developing electrostatic images, which have the above-mentioned relationship. [Means for solving the problem]

[0008] Means for solving the above problems include the following aspects.

[0009] <1> Contains an amorphous polyester resin and a crystalline polyester resin, Net intensity of Na element measured by X-ray fluorescence analysis, N Na and the net intensity N of Cl element measured by X-ray fluorescence analysis. Cl And, 2.5≦N Cl / N Na ≦260.0 <2> The net strength N Na and the net strength N Cl and 4.0≦N Cl / N Na ≦60.0. <1> 2. The toner for developing electrostatic images according to claim 1 . <3> The net strength N Cl is 0.10 kcps or more and 1.30 kcps or less, <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . <4> The net strength N Cl is 0.12 kcps or more and 1.10 kcps or less, <3> 2. The toner for developing electrostatic images according to claim 1 . <5> The net strength N Na is 0.005 kcps or more and 0.040 kcps or less, <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, <6> The net strength N Na is 0.010 kcps or more and 0.030 kcps or less, <5> 2. The toner for developing electrostatic images according to claim 1 . <7> The crystalline polyester resin contains a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol. <1> ~ <6> 10. The toner for developing an electrostatic image according to claim 9, <8> The polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol includes a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol. <7> 2. The toner for developing electrostatic images according to claim 1 . <9> the toner for developing an electrostatic image further contains a release agent, the release agent containing an ester wax; <1> ~ <8> 10. The toner for developing an electrostatic image according to claim 9,

[0010] <10> The toner particles have at least two crystalline resin domains that satisfy the following condition (A), the following condition (B1), the following condition (C), and the following condition (D) when a cross section of the toner particle is observed. <1> ~ <9> 10. The toner for developing an electrostatic image according to claim 9, Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The major axis length of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less. <11> The toner particles have at least two crystalline resin domains that satisfy the following condition (A), the following condition (B2), the following condition (C), and the following condition (D) when a cross section of the toner particle is observed, <1> ~ <9> 10. The toner for developing an electrostatic image according to claim 9, Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two crystalline resin domains, the ratio of the major axis length of the crystalline resin domain to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less. <12> the toner particles contain a release agent, and when a cross section of the toner particles is observed, a domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particles. <10> or <11> 2. The toner for developing electrostatic images according to claim 1 . <13> The content of the toner particles is 40% by number or more of the total toner particles. <10> ~ <12> 10. The toner for developing an electrostatic image according to claim 9, <14> The content of the toner particles is 70% by number or more of the total toner particles. <13> 2. The toner for developing electrostatic images according to claim 1 .

[0011] <15> <1> ~ <14> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <16> <1> ~ <14> The toner for developing an electrostatic image according to any one of the above items is contained in the container. A toner cartridge that is detachably attached to an image forming apparatus. <17> <15> and a developing unit which develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus. <18> An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; <15> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: <19> a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; <15> a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 1; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1, Effect of the Invention

[0012] <1> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a value of less than 2.5. <2> According to the invention, N Cl / N Na The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a toner density of less than 4.0. <3> According to the invention, the net strength N Cl The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a viscosity of less than 0.10 kcps. <4> According to the invention, the net strength N Cl The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a viscosity of less than 0.12 kcps. <5> According to the invention, the net strength N Na The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a viscosity of more than 0.040 kcps. <6> According to the invention, the net strength N Na The present invention provides a toner for developing electrostatic images which is excellent in fixing ability of halftone images, as compared with a toner for developing electrostatic images having a viscosity of more than 0.030 kcps. <7> or <8> According to the present invention, there is provided a toner for developing electrostatic images which is excellent in fixing property of halftone images, compared with a form in which the crystalline polyester resin does not contain a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol. <9> According to the present invention, there is provided a toner for developing electrostatic images which is excellent in fixing ability of halftone images, compared to a toner in which the release agent does not contain an ester wax.

[0013] <10> According to the present invention, there is provided a toner for developing electrostatic images, which has excellent fixing properties for halftone images, compared with a toner for developing electrostatic images that does not have toner particles that satisfy conditions (A), (B1), (C), and (D). <11> According to the present invention, there is provided a toner for developing electrostatic images, which has excellent fixing properties for halftone images, compared with a toner for developing electrostatic images that does not have toner particles that satisfy conditions (A), (B2), (C), and (D). <12> According to the present invention, there is provided a toner for developing electrostatic images which has excellent fixing properties for halftone images compared to a toner for developing electrostatic images in which the domain of the release agent is present in a surface layer less than 50 nm deep from the surface of the toner particle. <13> According to the invention, there is provided a toner for developing electrostatic images which is excellent in fixing property of halftone images, compared with a toner for developing electrostatic images in which the content of toner particles satisfying conditions (A), (B1), (C), and (D) is less than 40% by number of all toner particles, or compared with a toner for developing electrostatic images in which the content of toner particles satisfying conditions (A), (B2), (C), and (D) is less than 40% by number of all toner particles. <14> According to the invention, there is provided a toner for developing electrostatic images which is excellent in fixing property of halftone images, compared with a toner for developing electrostatic images in which the content of toner particles satisfying conditions (A), (B1), (C), and (D) is less than 70% by number of all toner particles, or compared with a toner for developing electrostatic images in which the content of toner particles satisfying conditions (A), (B2), (C), and (D) is less than 70% by number of all toner particles.

[0014] <15> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The present invention provides an electrostatic image developer which is excellent in fixing ability of halftone images, as compared with an electrostatic image developer containing a toner for developing electrostatic images having a toner density of less than 2.5. <16> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The toner cartridge is superior in fixing ability of half-tone images as compared with a toner cartridge containing a toner for developing electrostatic images having a toner density of less than 2.5. <17> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The present invention provides a process cartridge which is superior in fixing ability of halftone images as compared with a process cartridge which accommodates an electrostatic image developer containing a toner for developing electrostatic images having a toner density of less than 2.5. <18> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The present invention provides an image forming apparatus having excellent fixability of halftone images, as compared with an image forming apparatus in which an electrostatic image developer containing an electrostatic image developing toner having a toner density of less than 2.5 is accommodated in a developing means. <19> According to the present invention, a polyester resin composition containing an amorphous polyester resin and a crystalline polyester resin is provided. Cl / N Na The present invention provides an image forming method which is superior in fixability of halftone images as compared with an image forming method which uses, in a developing step, an electrostatic image developer containing a toner for developing electrostatic images having a toner density of less than 2.5. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge that is detachably mounted to the image forming apparatus according to the present embodiment. [Diagram 3] 2 is a schematic diagram showing a cross section of a toner particle in the electrostatic image developing toner according to the exemplary embodiment; FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0017] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0018] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved.

[0019] When an embodiment of the present disclosure is described with reference to the drawings, the configuration of the embodiment is not limited to the configuration shown in the drawings. In addition, the size of the members in each drawing is conceptual, and the relative relationship between the sizes of the members is not limited to this.

[0020] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.

[0021] In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0022] In this disclosure, the "toner for developing electrostatic images" is also referred to simply as "toner", and the "electrostatic image developer" is also referred to simply as "developer".

[0023] <Toner for developing electrostatic images> The toner according to the present embodiment contains an amorphous polyester resin and a crystalline polyester resin, and has a net intensity N Na and the net intensity N of Cl element measured by X-ray fluorescence analysis. Cl And, 2.5≦N Cl / N Na The relationship is satisfied: ≦260.0.

[0024] The toner according to the present embodiment has excellent fixing properties for halftone images on a recording medium, and the mechanism behind this is presumed to be as follows.

[0025] The toner may contain Na ions. The Na ions are derived from, for example, a colorant, a dispersant used in producing toner particles by a wet process, etc. It is presumed that the Na ions form ionic bridges with the binder resin on the toner surface to harden the toner surface, and toner with a hardened surface tends to have a lower melting property when heat is applied. As a result, the fixability of the toner image to the recording medium decreases, and in particular, the fixability of a halftone image decreases. In contrast, when a toner contains Cl ions, the Cl ions form salts with Na ions, which inhibits the Na ions from forming ionic bridges with the binder resin, and is believed to inhibit hardening of the toner surface. As a result, it is believed that images formed with a toner containing Cl ions exhibit the expected melting properties when heat is applied, and that the fixation of halftone images to recording media is excellent. Net intensity of Na element N NaNet intensity N of Cl element against Cl The ratio of N Cl / N Na In a toner having a ratio of less than 2.5, the action of Cl ions on Na ions is insufficient, and the fixing property of halftone images is poor. Cl / N Na is 2.5 or more, preferably 3.0 or more, and more preferably 4.0 or more. Net intensity of Na element N Na Net intensity N of Cl element against Cl The ratio of N Cl / N Na In the case of a toner having a Cr content of more than 260.0, secondary transfer defects may occur due to the influence of Cl ions. Cl / N Na is 260.0 or less, preferably 150.0 or less, and more preferably 60.0 or less.

[0026] Net intensity of Na element N Na and the net intensity of Cl element N Cl The measurement method is as follows. Approximately 200 mg of toner (toner containing external additives is the additive-inclusive type) is compressed with a compression molding machine under a load of 10 t for 60 seconds to produce a disk with a diameter of 10 mm and a thickness of 2 mm. This disk is used as a sample and a total element analysis is performed using a scanning X-ray fluorescence analyzer (Rigaku ZSX PrimusII) under measurement conditions of a tube voltage of 40 kV and a tube current of 70 mA to determine the net strength (unit: kilo counts per second, kcps) of each of the Na and Cl elements.

[0027] The incorporation of Cl ions into the toner can be achieved, for example, by using a chloride salt when producing the toner particles. Examples of the chloride salt include ammonium chloride.

[0028] In the toner according to the present embodiment, the net intensity N ClFrom the viewpoint of excellent fixing ability of halftone images and suppression of secondary transfer defects, the viscosity is preferably from 0.10 kcps to 1.30 kcps, more preferably from 0.11 kcps to 1.20 kcps, and even more preferably from 0.12 kcps to 1.10 kcps.

[0029] In the toner according to the present embodiment, the net intensity N Na is not particularly limited, but is preferably 0.005 kcps or more and 0.040 kcps or less, more preferably 0.007 kcps or more and 0.035 kcps or less, and even more preferably 0.010 kcps or more and 0.030 kcps or less.

[0030] The toner according to this embodiment will be described in detail below.

[0031] The toner according to the present embodiment is configured to contain toner particles and, if necessary, an external additive.

[0032] [Toner particles] The toner particles are configured to contain, for example, a binder resin, and, if necessary, a colorant, a release agent, and other additives.

[0033] -Binding resin- The binder resin contains at least an amorphous polyester resin and a crystalline polyester resin. In the present disclosure, a crystalline polyester resin refers to a polyester resin that has a clear endothermic peak rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC), specifically, a polyester resin whose half-value width of the endothermic peak is within 10°C when measured at a heating rate of 10°C / min. In the present disclosure, the term "amorphous polyester resin" refers to a polyester resin having an endothermic peak with a half-width exceeding 10°C when measured at a heating rate of 10°C / min, a polyester resin that shows a stepwise change in endothermic amount, or a polyester resin in which no clear endothermic peak is observed.

[0034] Amorphous polyester resin The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. As the amorphous polyester resin, a commercially available product or a synthesized product may be used.

[0035] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferred as the polyvalent carboxylic acid. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0036] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, aromatic diols and alicyclic diols are preferred as polyhydric alcohols, and aromatic diols are more preferred. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0037] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature of the amorphous polyester resin is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0038] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5000 to 1,000,000, more preferably 7000 to 500,000. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2000 to 100,000. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 to 100, more preferably 2 to 60. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.

[0039] The amorphous polyester resin is obtained by a known manufacturing method. Specifically, for example, the polymerization temperature is set to 180°C or more and 230°C or less, the reaction system is depressurized as necessary, and the reaction is carried out while removing water and alcohol generated during condensation. If the raw material monomer is not dissolved or compatible at the reaction temperature, a high-boiling point solvent may be added as a dissolution aid to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the dissolution aid. If a monomer with poor compatibility is present in the copolymerization reaction, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed with the monomer and then polycondensed with the main component.

[0040] The amorphous polyester resin may be a modified amorphous polyester resin in addition to an unmodified amorphous polyester resin. The modified amorphous polyester resin is an amorphous polyester resin having a bond group other than an ester bond, or an amorphous polyester resin having a resin component different from polyester bonded by a covalent bond or an ionic bond. The modified amorphous polyester resin may be, for example, a resin modified at the end by reacting an amorphous polyester resin having a functional group such as an isocyanate group introduced at the end with an active hydrogen compound.

[0041] The proportion of the amorphous polyester resin in the total binder resin is preferably 60% by mass or more and 98% by mass or less, more preferably 65% ​​by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 90% by mass or less.

[0042] Crystalline polyester resin The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. As the crystalline polyester resin, a commercially available product or a synthesized product may be used. Since the crystalline polyester resin easily forms a crystalline structure, a polycondensation product using a straight-chain aliphatic polymerizable monomer is preferable to a polymerizable monomer having an aromatic ring.

[0043] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower (e.g., carbon number 1 to 5) alkyl esters. As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0044] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0045] The polyhydric alcohol may have an aliphatic diol content of 80 mol % or more, and preferably 90 mol % or more.

[0046] The melting temperature of the crystalline polyester resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature of the crystalline polyester resin is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0047] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more and 35,000 or less.

[0048] The crystalline polyester resin can be obtained, for example, by a known production method, like the amorphous polyester resin.

[0049] As the crystalline polyester resin, a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol is preferred from the viewpoint of easily forming a crystal structure and having good compatibility with the amorphous polyester resin, thereby improving the fixability of halftone images.

[0050] The α,ω-linear aliphatic dicarboxylic acid is preferably an α,ω-linear aliphatic dicarboxylic acid in which the alkylene group connecting the two carboxy groups has 3 or more and 14 or less carbon atoms, more preferably the alkylene group has 4 or more and 12 or less carbon atoms, and even more preferably the alkylene group has 6 or more and 10 or less carbon atoms. Examples of α,ω-linear aliphatic dicarboxylic acids include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid (commonly known as suberic acid), 1,7-heptanedicarboxylic acid (commonly known as azelaic acid), 1,8-octanedicarboxylic acid (commonly known as sebacic acid), 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Of these, 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, and 1,10-decanedicarboxylic acid are preferred. The α,ω-linear aliphatic dicarboxylic acids may be used alone or in combination of two or more kinds.

[0051] The α,ω-linear aliphatic diol is preferably an α,ω-linear aliphatic diol in which the alkylene group connecting the two hydroxy groups has 3 to 14 carbon atoms, more preferably the alkylene group has 4 to 12 carbon atoms, and further preferably the alkylene group has 6 to 10 carbon atoms. Examples of the α,ω-linear aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,18-octadecanediol. Of these, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred. The α,ω-linear aliphatic diols may be used alone or in combination of two or more kinds.

[0052] As the polymer of an α,ω-straight-chain aliphatic dicarboxylic acid and an α,ω-straight-chain aliphatic diol, from the viewpoint of easily forming a crystal structure and having good compatibility with an amorphous polyester resin, thereby improving the fixing property of a halftone image, a polymer of at least one selected from the group consisting of 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, 1,9-nonanedicarboxylic acid, and 1,10-decanedicarboxylic acid and at least one selected from the group consisting of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol is preferred, and among these, a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol is more preferred.

[0053] The proportion of the crystalline polyester resin in the total binder resin is preferably from 1% by mass to 20% by mass, more preferably from 2% by mass to 15% by mass, and even more preferably from 3% by mass to 10% by mass.

[0054] Styrene acrylic resin The binder resin may be a styrene-acrylic resin, which is preferably an amorphous resin.

[0055] Examples of styrene-based monomers constituting the styrene-acrylic resin include styrene, α-methylstyrene, metachlorostyrene, parachlorostyrene, parafluorostyrene, paramethoxystyrene, meta-tert-butoxystyrene, para-tert-butoxystyrene, paravinylbenzoic acid, paramethyl-α-methylstyrene, etc. The styrene-based monomers may be used alone or in combination of two or more.

[0056] Examples of (meth)acrylic monomers constituting the styrene acrylic resin include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)methacrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The (meth)acrylic monomers may be used alone or in combination of two or more. In the present disclosure, "(meth)acrylic" refers to both "acrylic" and "methacrylic".

[0057] The polymerization ratio of the styrene-based monomer to the (meth)acrylic monomer is preferably styrene-based monomer:(meth)acrylic monomer=70:30 to 95:5 on a mass basis.

[0058] The styrene-acrylic resin may have a crosslinked structure. The styrene-acrylic resin having a crosslinked structure can be produced, for example, by copolymerizing a styrene-based monomer, a (meth)acrylic monomer, and a crosslinkable monomer. The crosslinkable monomer is not particularly limited, but is preferably a bifunctional or higher (meth)acrylate compound.

[0059] The method for producing the styrene-acrylic resin is not particularly limited, and for example, solution polymerization, precipitation polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. The polymerization reaction is carried out by a known operation (for example, a batch system, a semi-continuous system, a continuous system, etc.).

[0060] The proportion of the styrene-acrylic resin in the total binder resin is preferably from 0% to 20% by mass, more preferably from 1% to 15% by mass, and even more preferably from 2% to 10% by mass.

[0061] Other binder resins Further examples of the binder resin include homopolymers of monomers such as ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), and copolymers of two or more of these monomers. Other examples of the binder resin include non-vinyl resins such as epoxy resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.

[0062] The content of the binder resin is preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total mass of the toner particles.

[0063] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, Examples of the dyes include pigments such as ultramarine blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate; and dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.

[0064] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.

[0065] The content of the colorant is preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.

[0066] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.

[0067] As the release agent, from the viewpoint of having good compatibility with the amorphous polyester resin and, as a result, improving the fixation of halftone images, an ester wax is preferred, and an ester wax of a higher fatty acid having from 10 to 30 carbon atoms and a monovalent or polyvalent alcohol having from 1 to 30 carbon atoms is more preferred.

[0068] Examples of ester waxes include ester compounds of higher fatty acids having 10 or more carbon atoms and monovalent or polyvalent aliphatic alcohols having 8 or more carbon atoms, and having a melting temperature of 60°C or higher and 110°C or lower (preferably 65°C or higher and 100°C or lower, more preferably 70°C or higher and 95°C or lower). Examples of ester waxes include ester compounds of higher fatty acids (caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, oleic acid, etc.) and alcohols (monohydric alcohols such as methanol, ethanol, propanol, isopropanol, butanol, capryl alcohol, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, oleyl alcohol, etc.; polyhydric alcohols such as glycerin, ethylene glycol, propylene glycol, sorbitol, pentaerythritol, etc.). Specific examples include carnauba wax, rice wax, candelilla wax, jojoba oil, Japan wax, beeswax, privet wax, lanolin, and montanic acid ester wax.

[0069] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature of the release agent is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0070] The content of the release agent is preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total mass of the toner particles.

[0071] -Other additives- Examples of other additives include known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.

[0072] -Characteristics of toner particles- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. The toner particles having a core-shell structure may be composed of, for example, a core containing a binder resin and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing the binder resin.

[0073] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm.

[0074] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5 mass % aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the small diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:

[0075] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.

[0076] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. The toner particles to be measured are sucked and collected, flattened, and instantly strobed to capture a still image of the particles, which is then analyzed by a flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation). The number of samples to be taken when calculating the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.

[0077] The toner particles are preferably any of the first toner particles and the second toner particles described below.

[0078] First toner particles Toner particles in which, when a cross section of the toner particle is observed, at least two crystalline resin domains satisfy the conditions (A), (B1), (C) and (D). Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The major axis length of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.

[0079] Second toner particles Toner particles in which, when a cross section of the toner particle is observed, at least two crystalline resin domains satisfy the conditions (A), (B2), (C) and (D). Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two crystalline resin domains, the ratio of the major axis length of the crystalline resin domain to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): The angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.

[0080] The first toner particles may or may not be the second toner particles, and preferably are the second toner particles. The second toner particles may or may not be the first toner particles, and preferably are the first toner particles.

[0081] FIG. 3 shows a schematic cross section of a toner particle. The symbols in FIG. 3 are TN: toner particle, Amo: amorphous resin, Cry: crystalline resin, L cry : Long axis length of the crystalline resin domain, L T : Maximum diameter of toner particles, θ A θ is the angle between the extension of the long axis of the crystalline resin domain and the tangent at the contact point where the extension touches the surface of the toner particle. B : The crossing angle between the extension lines of the long axes of the domains of the two crystalline resins, respectively.

[0082] The first toner particles or the second toner particles improve the fixability of a halftone image to a recording medium, and the reason for this is presumed to be as follows. The first toner particles and the second toner particles have at least two domains of crystalline resin that are elliptical or needle-shaped with a large aspect ratio and long axis length, which are arranged to extend from the surface side of the toner particles toward the inside and intersect with each other (see FIG. 3). When a toner image having these toner particles is fixed, it is presumed that when heat is applied to the toner particles, the elliptical or needle-shaped crystalline resin melts and heat is rapidly transferred from the surface to the inside of the toner particles. As a result, heat is transferred almost uniformly to the entire toner particles, and the entire toner particles melt in an almost uniform state, improving the fixability of the halftone image to the recording medium.

[0083] In the first toner particle, when a cross section of the toner particle is observed, at least two crystalline resin domains (preferably at least three crystalline resin domains) satisfy the conditions (A), (B1), (C) and (D). From the viewpoint of fixability of a halftone image to a recording medium, the first toner particles are preferably 40% by number or more, more preferably 70% by number or more, even more preferably 80% by number or more, and particularly preferably 90% by number or more, based on the total toner particles. Ideally, the ratio of the first toner particles to the total toner particles is 100% by number.

[0084] In the second toner particle, when a cross section of the toner particle is observed, at least two crystalline resin domains (preferably at least three crystalline resin domains) satisfy the conditions (A), (B2), (C) and (D). From the viewpoint of fixability of a halftone image to a recording medium, the proportion of the second toner particles is preferably 40% by number or more, more preferably 70% by number or more, even more preferably 80% by number or more, and particularly preferably 90% by number or more, based on the total toner particles. Ideally, the proportion of the second toner particles is 100% by number based on the total toner particles.

[0085] Each of the conditions (A), (B1), (B2), (C) and (D) has a preferred range.

[0086] Condition (A) From the viewpoint of fixability of a halftone image to a recording medium, the aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less, and preferably 10 or more and 40 or less. The aspect ratio of a crystalline resin domain means the ratio of the long axis length to the short axis length (long axis length / short axis length) in a crystalline resin domain. The long axis length of a crystalline resin domain means the maximum length of the crystalline resin domain. The short axis length of a crystalline resin domain means the maximum length among the lengths in the direction perpendicular to the extension line of the long axis length of the crystalline resin domain.

[0087] ·Conditions (B1) From the viewpoint of the fixation of halftone images to recording media, the long axis length of the domain of the crystalline resin (L in Fig. 3) cry ) is 0.5 μm or more and 1.5 μm or less, and preferably 0.8 μm or more and 1.5 μm or less.

[0088] ·Conditions (B2) From the viewpoint of the fixation of halftone images to recording media, the long axis length of the crystalline resin domain (L in Fig. 3) relative to the maximum diameter of the toner particles (Lt in Fig. 3) is cry The proportion of ) is 10% or more and 30% or less, preferably 13% or more and 30% or less, and more preferably 17% or more and 30% or less. The maximum diameter of a toner particle means the maximum length of a straight line drawn between any two points on the contour line of the cross section of a toner particle (so-called major axis).

[0089] ·Condition (C) From the viewpoint of the fixation of a halftone image to a recording medium, the angle between the extension line of the long axis of the crystalline resin domain and the tangent line at the contact point where the extension line touches the surface of the toner particle (i.e., the outer edge of the toner particle) (θ in FIG. 3) is A ) is 60 degrees or more and 90 degrees or less, and preferably 75 degrees or more and 90 degrees or less.

[0090] Condition (D) From the viewpoint of the fixation of the halftone image to the recording medium, the crossing angle of the extension lines of the long axes of the two crystalline resin domains (θ B ) is 45 degrees or more and 90 degrees or less, and preferably 60 degrees or more and 90 degrees or less.

[0091] - Method for observing the cross section of a toner particle Toner particles (or toner particles with external additives) are mixed and embedded in epoxy resin, and the epoxy resin is solidified. The solidified product is cut using an ultramicrotome device (Ultracut UCT manufactured by Leica) to prepare a thin section sample with a thickness of 80 nm to 130 nm. The thin section sample is stained with ruthenium tetroxide for 3 hours in a desiccator at 30°C. Then, an STEM observation image (acceleration voltage: 30 kV, magnification: 20,000 times) of the stained thin section sample in transmission image mode is obtained using an ultra-high resolution field emission scanning electron microscope (FE-SEM, S-4800 manufactured by Hitachi High-Technologies Corporation). The image includes cross sections of toner particles of various sizes, and a cross section of a toner particle whose diameter is 85% or more of the volume average particle diameter of the toner particle is selected and observed. Here, the diameter of the toner particle cross section refers to the maximum length (so-called major axis) of a straight line drawn between any two points on the contour line of the toner particle cross section. In the image, the amorphous resin, the crystalline resin, and the release agent are distinguished based on the contrast and shape. With ruthenium staining, the amorphous resin (e.g., amorphous polyester resin) is stained the darkest, followed by the crystalline resin (e.g., crystalline polyester resin), and the release agent is stained the lightest. By adjusting the contrast, the amorphous resin is observed to be black, the crystalline resin to be light gray, and the release agent to be white. The domains of the crystalline resin are subjected to image analysis to determine whether the toner particles satisfy the conditions (A), (B1), (B2), (C), and (D). When determining the proportion of the first toner particles or the second toner particles, 100 toner particles are observed, and the proportion of the number of the first toner particles or the second toner particles is calculated.

[0092] From the viewpoint of the fixability of a halftone image to a recording medium, the first toner particles and the second toner particles preferably satisfy the following condition (E).

[0093] Condition (E): When the cross section of a toner particle is observed, the domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle. In other words, when the cross section of a toner particle is observed, the shortest distance between the domain of the release agent present in the toner particle and the surface (i.e., the outer edge) of the toner particle is 50 nm or more.

[0094] Condition (E) means that the domain of the release agent is not exposed on the surface of the toner particle. If the domain of the release agent is exposed on the surface of the toner particle, the external additive will be unevenly distributed and adhere to the exposed part of the release agent. However, if the domain of the release agent is present at a depth of 50 nm or more from the surface of the toner particle, the external additive will adhere to the surface of the toner particle in a nearly uniform state. As a result, uneven melting of the toner particles during fixing is suppressed, and the fixability of the halftone image to the recording medium is improved.

[0095] The condition (E) is confirmed by the above-mentioned method of observing the cross section of the toner particle.

[0096] From the viewpoint of fixability of a halftone image to a recording medium, the proportion of the first toner particles satisfying condition (E) is preferably 40% by number or more, more preferably 70% by number or more, even more preferably 80% by number or more, particularly preferably 90% by number or more, and ideally 100% by number, relative to the total toner particles.

[0097] From the viewpoint of fixability of a halftone image to a recording medium, the proportion of second toner particles satisfying condition (E) is preferably 40% by number or more, more preferably 70% by number or more, even more preferably 80% by number or more, particularly preferably 90% by number or more, and ideally 100% by number, relative to all toner particles.

[0098] [External additives] Examples of the external additive include inorganic particles. Examples of inorganic particles include SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, and K2O·(TiO2). n , Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, MgSO4, etc.

[0099] The surface of the inorganic particles as an external additive may be hydrophobized. The hydrophobization may be performed, for example, by immersing the inorganic particles in a hydrophobizing agent. The hydrophobizing agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 to 10 parts by mass relative to 100 parts by mass of the inorganic particles.

[0100] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate, and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.

[0101] The amount of the external additive is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.

[0102] [Toner manufacturing method] The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles.

[0103] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). There is no particular limitation on these production methods, and any known production method may be used. Among these, it is preferable to obtain the toner particles by the aggregation and coalescence method.

[0104] Specifically, when the toner particles are produced by the aggregation and coalescence method, A step of preparing an amorphous resin particle dispersion liquid in which amorphous resin particles are dispersed, and a crystalline resin particle dispersion liquid in which crystalline resin particles are dispersed (a resin particle dispersion liquid preparation step); a step of aggregating the amorphous resin particles (and other particles as necessary) in an amorphous resin particle dispersion (in a dispersion after mixing other particle dispersions as necessary) to form first aggregated particles (first aggregated particle forming step); a step of mixing the aggregated particle dispersion in which the first aggregated particles are dispersed with an amorphous resin particle dispersion and a crystalline resin particle dispersion (or mixing the aggregated particle dispersion in which the first aggregated particles are dispersed with a mixed liquid of the amorphous resin particle dispersion and the crystalline resin particle dispersion), and aggregating the first aggregated particles so that the amorphous resin particles and the crystalline resin particles are further attached to the surfaces of the first aggregated particles, repeating this operation two or more times to form second aggregated particles (second aggregated particle forming step); a step of mixing the aggregated particle dispersion liquid in which the second aggregated particles are dispersed with the amorphous resin particle dispersion liquid, and aggregating the second aggregated particles so that the amorphous resin particles are attached to the surfaces of the second aggregated particles to form third aggregated particles (third aggregated particle forming step); a step of heating the aggregated particle dispersion liquid in which the third aggregated particles are dispersed to fuse and coalesce the aggregated particles to form toner particles (a fusion and coalescence step); The toner particles are produced through the above steps.

[0105] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described. The colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.

[0106] -Resin particle dispersion preparation process- An amorphous resin particle dispersion liquid in which amorphous resin particles are dispersed, and a crystalline resin particle dispersion liquid in which crystalline resin particles are dispersed are prepared.

[0107] The resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.

[0108] Examples of the dispersion medium used in the resin particle dispersion liquid include aqueous media. Examples of the aqueous media include water such as distilled water and ion-exchanged water, and alcohols. These may be used alone or in combination of two or more.

[0109] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactants may be used alone or in combination of two or more.

[0110] In the resin particle dispersion, the resin particles are dispersed in the dispersion medium by a general dispersion method such as a rotary shear type homogenizer, a ball mill with media, a sand mill, or a dyno mill. Depending on the type of resin particles, the resin particles may be dispersed in the dispersion medium by a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to invert the phase from W / O to O / W, thereby dispersing the resin in the aqueous medium in the form of particles.

[0111] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (for example, LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are measured in the same manner.

[0112] The content of the resin particles in the resin particle dispersion is preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.

[0113] In the same manner as the resin particle dispersion liquid, for example, a colorant particle dispersion liquid and a release agent particle dispersion liquid are also prepared. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion liquid are the same for the colorant particles dispersed in the colorant particle dispersion liquid and the release agent particles dispersed in the release agent particle dispersion liquid.

[0114] -First agglomerated particle formation process- A non-crystalline resin particle dispersion, a colorant particle dispersion, and a release agent particle dispersion are mixed together, and in the mixed dispersion, the non-crystalline resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form first aggregate particles containing the non-crystalline resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.

[0115] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature close to the glass transition temperature of the resin particles (specifically, for example, the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form first aggregated particles. In the first aggregate particle formation step, for example, the mixed dispersion may be stirred with a rotary shear homogenizer, an aggregating agent may be added at room temperature (e.g., 25°C), the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), a dispersion stabilizer may be added as necessary, and then the mixture may be heated.

[0116] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant contained in the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. When a metal complex is used as the flocculant, the amount of the surfactant used is reduced, and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ion of the flocculant may be used together with the flocculant. As this additive, a chelating agent is preferably used.

[0117] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate; and inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, for example, oxycarboxylic acid such as tartaric acid, citric acid, gluconic acid, etc., aminocarboxylic acid such as iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, based on 100 parts by mass of the resin particles.

[0118] -Second agglomerated particle formation process- The aggregated particle dispersion in which the first aggregated particles are dispersed is mixed with an amorphous resin particle dispersion and a crystalline resin particle dispersion. The aggregated particle dispersion in which the first aggregated particles are dispersed may be mixed with a mixed liquid of an amorphous resin particle dispersion and a crystalline resin particle dispersion. Then, in the dispersion in which the first aggregated particles, the amorphous resin particles, and the crystalline resin particles are dispersed, the amorphous resin particles and the crystalline resin particles are aggregated on the surfaces of the first aggregated particles.

[0119] Specifically, for example, in the first aggregated particle forming step, when the first aggregated particles reach a target particle size, a non-crystalline resin particle dispersion and a crystalline resin particle dispersion are added, and heating is performed at a temperature equal to or lower than the glass transition temperature of the non-crystalline resin particles. This aggregation operation is repeated two or more times to form second aggregated particles.

[0120] In the second aggregate particle forming step, it is preferable to add a chloride (for example, ammonium chloride) to the dispersion liquid and blend Cl ions in the surface layer of the toner particles.

[0121] -Third agglomerated particle formation process- The aggregated particle dispersion in which the second aggregated particles are dispersed is mixed with an amorphous resin particle dispersion, and the amorphous resin particles are aggregated on the surfaces of the second aggregated particles in the dispersion in which the second aggregated particles and the amorphous resin particles are dispersed.

[0122] Specifically, for example, when the second aggregated particles reach a target particle size in the second aggregated particle formation step, a non-crystalline resin particle dispersion is added, heating is performed at a temperature equal to or lower than the glass transition temperature of the non-crystalline resin particles, and the pH of the dispersion is adjusted to stop the progress of aggregation.

[0123] In the third aggregate particle forming step, it is preferable to add a chloride (for example, ammonium chloride) to the dispersion liquid and blend Cl ions in the surface layer of the toner particles.

[0124] -Fusion / unification process- The aggregated particle dispersion liquid in which the third aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the amorphous resin particles (for example, a temperature 10° C. to 30° C. higher than the glass transition temperature of the amorphous resin particles) to fuse and coalesce the aggregated particles to form toner particles.

[0125] After heating for fusion and coalescence, it is advisable to cool to 30° C. at a cooling rate of 5° C. / min to 40° C. / min. This rapid cooling makes it easier for the toner particle surface to shrink, which is presumably why cracks tend to form from the inside of the toner particle toward the toner surface. Next, the temperature is raised again at a rate of 0.1°C / min to 2°C / min, and the temperature is maintained at a temperature equal to or higher than the melting temperature of the crystalline resin minus 5°C for 10 minutes or more. After that, the temperature is gradually cooled at a rate of 0.1°C / min to 1°C / min, whereby the domains of the crystalline resin grow in the crack direction, and grow from the inside of the toner particle toward the surface, so that the domains of the crystalline resin satisfy the above conditions. In addition, for example, when the temperature is increased again, if the temperature is increased to the melting temperature of the release agent or higher, the domain of the release agent is likely to grow to the vicinity of the surface of the toner particles. Therefore, the heating temperature after the temperature is increased again is preferably set to a temperature higher than the melting temperature of the crystalline resin minus 5°C or higher and lower than the melting temperature of the release agent.

[0126] After the fusion and coalescence process is completed, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain dried toner particles. From the viewpoint of chargeability, the washing process is preferably performed by sufficient substitution washing with ion-exchanged water. From the viewpoint of productivity, the solid-liquid separation process is preferably performed by suction filtration, pressure filtration, etc. From the viewpoint of productivity, the drying process is preferably performed by freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc.

[0127] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.

[0128] <Electrostatic image developer> The electrostatic image developer according to the present embodiment includes at least the toner according to the present embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer including only the toner according to the present embodiment, or may be a two-component developer including the toner and a carrier.

[0129] The carrier is not particularly limited, and may be a known carrier. For example, the carrier may be a coated carrier in which the surface of a core material made of magnetic powder is coated with a resin; a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin; or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material, and the surface of the core material is coated with a resin.

[0130] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt; magnetic oxides such as ferrite and magnetite; and the like.

[0131] Examples of the resin and matrix resin for coating include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin or its modified product containing organosiloxane bonds, fluororesin, polyester, polycarbonate, phenolic resin, epoxy resin, etc. The resin and matrix resin for coating may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, potassium titanate, etc.

[0132] Examples of methods for coating the surface of the core material with a resin include a method using a coating layer forming solution in which the coating resin and various additives (used as necessary) are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the type of resin used, coating suitability, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer; a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material; a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air; and a kneader coater method in which the carrier core material and the solution for forming a coating layer are mixed in a kneader coater and then the solvent is removed.

[0133] The mixture ratio (mass ratio) of the toner and the carrier in the two-component developer is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.

[0134] <Image forming device, image forming method> An image forming apparatus and an image forming method according to the present embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.

[0135] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.

[0136] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder after the transfer of the toner image and before charging; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it after the transfer of the toner image and before charging it. When the image forming apparatus according to the present embodiment is an intermediate transfer type apparatus, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0137] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge that contains the electrostatic charge image developer according to the present embodiment and has the developing means is preferably used.

[0138] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this example. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted.

[0139] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth image forming units 10Y, 10M, 10C, and 10K (image forming means) of an electrophotographic type that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachably attached to the image forming apparatus.

[0140] Above each of the units 10Y, 10M, 10C, and 10K, an intermediate transfer belt (one example of an intermediate transfer body) 20 is provided, which extends through each unit. The intermediate transfer belt 20 is provided wrapped around a drive roll 22 and a support roll 24, and runs in a direction from the first unit 10Y toward the fourth unit 10K. A force is applied to the support roll 24 by a spring (not shown) or the like in a direction away from the drive roll 22, and tension is applied to the intermediate transfer belt 20 wrapped around them. An intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. The developing devices (an example of developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with yellow, magenta, cyan, and black toners contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.

[0141] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration and operation, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative.

[0142] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer means) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning means) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20, and is provided at a position facing the photoconductor 1Y. A bias power supply (not shown) that applies a primary transfer bias is connected to the primary transfer rolls 5Y, 5M, 5C, and 5K of each unit. Each bias power supply changes the value of the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).

[0143] Hereinafter, the operation of forming a yellow image in the first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity of 1×10 at 20° C. -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam, the resistivity of the portion irradiated with the laser beam changes. Therefore, the exposed surface of the charged photoreceptor 1Y is irradiated with a laser beam 3Y from the exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). As a result, an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.

[0144] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y rotates to a predetermined developing position as the photoconductor 1Y travels. At this developing position, the electrostatic image on the photoconductor 1Y is developed into a toner image by the developing device 4Y and made visible.

[0145] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.

[0146] When the yellow toner image on the photoreceptor 1Y is transported to the primary transfer position, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoreceptor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoreceptor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and is controlled to, for example, +10 μA by a control unit (not shown) in the first unit 10Y. On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.

[0147] The primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of each color are transferred and superimposed.

[0148] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, and the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.

[0149] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P, forming a fixed image.

[0150] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets and the like. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with a resin or the like, art paper for printing, etc. are preferably used.

[0151] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.

[0152] <Process cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus.

[0153] The process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing means and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.

[0154] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. In the following description, the main parts shown in the drawings will be described, and the description of the rest will be omitted.

[0155] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming means), 112 denotes a transfer device (an example of a transfer means), 115 denotes a fixing device (an example of a fixing means), and 300 denotes a recording paper (an example of a recording medium). EXAMPLES

[0156] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are based on mass.

[0157] <Preparation of amorphous polyester resin particle dispersion (A1)> Terephthalic acid: 70 parts Fumaric acid: 30 parts Ethylene glycol: 41 parts 1,5-Pentanediol: 48 parts The above materials were placed in a flask equipped with a stirrer, nitrogen inlet tube, temperature sensor, and distillation column, and the temperature was raised to 220°C over 1 hour under nitrogen gas flow, and 1 part of titanium tetraethoxide was added for a total of 100 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin with a weight average molecular weight of 96,000 and a glass transition temperature of 61°C was obtained.

[0158] In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of amorphous polyester resin were gradually added and dissolved, and 10% aqueous ammonia solution (equivalent to 3 times the amount by molar ratio relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was added dropwise while stirring the mixed liquid, to perform emulsification. After the dropwise addition was completed, the emulsion was returned to 25°C to obtain a resin particle dispersion in which resin particles with a volume average particle size of 190 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (A1) was obtained.

[0159] <Preparation of Crystalline Polyester Resin Particle Dispersion (B1)> 1,10-Decanedicarboxylic acid: 265 parts 1,6-Hexanediol: 168 parts Dibutyltin oxide (catalyst): 0.3 parts The above materials were placed in a heated and dried three-necked flask, the air in the flask was replaced with nitrogen gas to create an inert atmosphere, and the mixture was stirred and refluxed at 180°C for 5 hours using mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Thus, a crystalline polyester resin with a weight average molecular weight of 12700 and a melting temperature of 73°C was obtained.

[0160] 90 parts of crystalline polyester resin, 1.8 parts of anionic surfactant (TaycaPower, manufactured by Tayca Corporation) and 210 parts of ion-exchanged water were mixed, heated to 120°C, dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA Corporation), and then dispersed for 1 hour using a pressure discharge type Gaulin homogenizer to obtain a resin particle dispersion in which resin particles having a volume average particle size of 190 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a crystalline polyester resin particle dispersion (B1) was obtained.

[0161] <Preparation of styrene acrylic resin particle dispersion (C1)> Styrene: 370 parts n-Butyl acrylate: 30 parts Acrylic acid: 2 parts Dodecanethiol: 24 parts Carbon tetrabromide: 4 parts The mixture obtained by mixing and dissolving the above materials was dispersed and emulsified in a flask in a surfactant solution in which 6 parts of a nonionic surfactant (manufactured by Sanyo Chemical Industries, Nonipol 400) and 10 parts of an anionic surfactant (manufactured by Tayca Power, Tayca Co., Ltd.) were dissolved in 550 parts of ion-exchanged water. Next, an aqueous solution in which 4 parts of ammonium persulfate were dissolved in 50 parts of ion-exchanged water was added over a period of 20 minutes while stirring the flask. Next, after nitrogen replacement, the flask was heated in an oil bath while stirring the contents until the temperature reached 70°C, and the temperature was maintained at 70°C for 5 hours to continue emulsion polymerization. Thus, a resin particle dispersion in which resin particles having a volume average particle size of 140 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a styrene acrylic resin particle dispersion (C1) was obtained.

[0162] <Preparation of release agent particle dispersion (W1)> Ester wax (Nippon Oil & Fats Co., Ltd., WEP-8, melting temperature 79°C): 100 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 1 part Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 220 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W1).

[0163] <Preparation of colorant particle dispersion (K1)> Carbon black (Cabot, Regal 330): 50 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 5 parts Ion-exchanged water: 193 parts The above materials were mixed and dispersed for 10 minutes at 240 MPa using an Ultimizer (manufactured by Sugino Machine Co., Ltd.), and ion-exchanged water was added to obtain a colorant particle dispersion (K1) with a solid content of 20%.

[0164] <Example 1> [Preparation of toner particles] Ion-exchanged water: 200 parts Amorphous polyester resin particle dispersion (A1): 130 parts Styrene acrylic resin particle dispersion (C1): 30 parts Release agent particle dispersion (W1): 10 parts Colorant particle dispersion (K1): 15 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 2.8 parts The above materials were placed in a round stainless steel flask, and 0.1N (0.1mol / L) nitric acid was added to adjust the pH to 3.5, after which an aqueous solution of 2.5 parts of aluminum sulfate dissolved in 30 parts of ion-exchanged water was added. The materials were dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50), and then heated to 45°C in a heating oil bath and maintained until the volume average particle size reached 4.5μm.

[0165] Next, 30 parts of the amorphous polyester resin particle dispersion (A1) and 15 parts of the crystalline polyester resin particle dispersion (B1) were added and held for 30 minutes. The addition of these two components was repeated a total of four times at 30 minute intervals. Next, 40 parts of the amorphous polyester resin particle dispersion (A1) and 4 parts of an aqueous ammonium chloride solution prepared by dissolving 20 parts of ammonium chloride in 80 parts of ion-exchanged water were added, and the pH was adjusted to 9.0 using a 1N aqueous sodium hydroxide solution. Next, while continuing stirring, the temperature was increased to 85°C at a rate of 0.05°C / min, and after being held at 85°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min (first cooling). Next, it was heated to 85°C at a rate of 0.2°C / min (reheating), held for 30 minutes, and then cooled to 30°C at a rate of 0.5°C / min (second cooling). Next, the solid content was filtered off, washed with ion-exchanged water, and dried to obtain toner particles (1) having a volume average particle size of 5.9 μm.

[0166] [External addition of additives] 100 parts of toner particles (1) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with an opening of 45 μm to obtain toner (1). The volume average particle diameter of toner (1) was 5.9 μm.

[0167] [Net strength N Na and Net strength N Cl Measurement of The toner (1) was used as a sample and subjected to total elemental analysis using an X-ray analyzer (ZSX PrimusII manufactured by Rigaku Corporation) to determine the net intensity (unit: kcps) of each of the Na element and the Cl element.

[0168] [Measurement of domains in toner particles] The domains in the toner particles were measured according to the method described above. The toner of Example 1 contained toner particles satisfying all of the conditions (A), (B1), (B2), (C), (D) and (E), and these toner particles accounted for 70% or more by number of all the toner particles.

[0169] [Creating the carrier] After 500 parts of spherical magnetite powder particles (volume average particle diameter 0.55 μm) were stirred with a Henschel mixer, 5 parts of a titanate-based coupling agent were added, and the mixture was heated to 100 ° C and stirred for 30 minutes. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of magnetite particles treated with a titanate-based coupling agent, 6.25 parts of 25% ammonia water, and 425 parts of water were added to a four-neck flask and stirred, and reacted at 85 ° C for 120 minutes while stirring. Next, the mixture was cooled to 25 ° C, 500 parts of water were added, and the supernatant liquid was removed and the precipitate was washed with water. The washed precipitate was heated and dried under reduced pressure to obtain a carrier (M) with an average particle size of 35 μm.

[0170] [Mixing toner and carrier] The toner (1) and the carrier (M) were placed in a V blender in a ratio of toner (1):carrier (M)=5:95 (mass ratio) and stirred for 20 minutes to obtain a developer (1).

[0171] <Examples 2 to 6> Toner particles (2) to (6) were prepared in the same manner as in the preparation of toner particles (1), except that the amount of the aqueous ammonium chloride solution added was increased. Toners (2) to (6) and developers (2) to (6) were prepared in the same manner as in the preparation of toner (1) and developer (1), except that one of toner particles (2) to (6) was used in place of toner particle (1).

[0172] <Comparative Examples 1 to 2> Toner particles (C1) to (C2) were prepared in the same manner as in the preparation of toner particles (1), except that the amount of the aqueous ammonium chloride solution added was increased or decreased. Toners (C1) to (C2) and developers (C1) to (C2) were prepared in the same manner as in the preparation of toner (1) and developer (1), except that one of toner particles (C1) to (C2) was used in place of toner particle (1).

[0173] <Example 7> [Preparation of toner particles] Ion-exchanged water: 200 parts Amorphous polyester resin particle dispersion (A1): 130 parts Crystalline polyester resin particle dispersion (B1): 60 parts Styrene acrylic resin particle dispersion (C1): 30 parts Release agent particle dispersion (W1): 10 parts Colorant particle dispersion (K1): 15 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 2.8 parts The above materials were placed in a round stainless steel flask, and 0.1N (0.1mol / L) nitric acid was added to adjust the pH to 3.5, after which an aqueous solution of 2.5 parts of aluminum sulfate dissolved in 30 parts of ion-exchanged water was added. The materials were dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50), and then heated to 45°C in a heating oil bath and maintained until the volume average particle size reached 5.0μm.

[0174] Next, 160 parts of the amorphous polyester resin particle dispersion (A1) was added, and 20 parts of an aqueous ammonium chloride solution prepared by dissolving 20 parts of ammonium chloride in 80 parts of ion-exchanged water was added. Then, the pH was adjusted to 9.0 using a 1N aqueous sodium hydroxide solution. Next, while continuing stirring, the temperature was raised to 85°C at a rate of 0.05°C / min, and the mixture was kept at 85°C for 3 hours, and then cooled to 30°C at a rate of 0.5°C / min. Next, the solid content was filtered, washed with ion-exchanged water, and dried to obtain toner particles (7) having a volume average particle size of 5.9 μm.

[0175] [External addition of additives] 100 parts of toner particles (7) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with an opening of 45 μm to obtain toner (7). The volume average particle diameter of toner (7) was 5.9 μm.

[0176] [Net strength N Na and Net strength N Cl Measurement of The toner (7) was used as a sample and subjected to total elemental analysis using an X-ray analyzer (ZSX PrimusII manufactured by Rigaku Corporation) to determine the net intensity (unit: kcps) of each of the Na element and the Cl element.

[0177] [Measurement of domains in toner particles] The domains in the toner particles were measured according to the method previously described.The toner of Example 7 did not contain either the first toner particles or the second toner particles.

[0178] [Mixing toner and carrier] The toner (7) and the carrier (M) were placed in a V blender in a ratio of toner (7):carrier (M) = 5:95 (mass ratio) and stirred for 20 minutes to obtain a developer (7).

[0179] <Developer performance evaluation> [Halftone image fixation] A modified image forming device "ApeosPortIV C5575" manufactured by Fuji Xerox Co., Ltd. was prepared, and the developer was placed in the developing device. After leaving the image forming device for one day in an environment with a temperature of 25°C and a relative humidity of 15%, 100 halftone images with an image density of 5% were printed on "P paper" manufactured by Fuji Xerox Co., Ltd. under the same environment. The weights of the first and 100th sheets were weighed, the halftone image was rubbed with Kimwipe (manufactured by Nippon Paper Crecia Co., Ltd.), and the weight was measured again. The weight retention rate (weight after rubbing ÷ weight before rubbing × 100, unit: %) was calculated from the weights before and after rubbing. In addition, the difference in concentration before and after rubbing was visually observed. The weight retention rate and the difference in concentration were classified as follows:

[0180] G1: The weight retention rate for both the 1st and 100th sheets was 99.5% or more, and no difference in concentration was observed before and after rubbing. G2: The weight retention rate for both the 1st and 100th sheets was 99.5% or more, and only a slight difference in concentration was observed before and after rubbing. G3: The weight retention rate for both the 1st and 100th sheets was between 98.0% and 99.5%, and a difference in concentration was observed before and after rubbing. G4: The weight retention rate for both the 1st and 100th sheets was between 97.0% and 98.0%, and a difference in concentration was observed before and after rubbing. G5: The weight retention rate was less than 97.0% for both the 1st and 100th sheets, and a difference in concentration was observed before and after rubbing.

[0181] [Secondary transfer efficiency] A modified Fuji Xerox image forming apparatus "ApeosPortIV C5575" was prepared, and the developer was placed in the developing device. After leaving the image forming apparatus for one day in an environment with a temperature of 30°C and a relative humidity of 85%, 10,000 images with an image density of 1% were output on Fuji Xerox "P paper" in the same environment. Next, a 3cm x 4cm solid patch was developed and transferred, and the transferred toner image on the intermediate transfer belt was collected using the adhesiveness of the adhesive tape surface, and the weight W1 of the transferred toner image was measured. Next, a 3cm x 4cm solid patch was image-formed on P paper, and the weight W2 of the image was measured. From these weights, the transfer efficiency (W2÷W1×100, unit: %) was calculated, and the transfer efficiency was classified as follows.

[0182] A: Transfer efficiency is 90% or more B: Transfer efficiency is between 80% and 90% C: Transfer efficiency is less than 80%

[0183] [Table 1]

[0184] <Examples 101 to 129> Toner particles (101) to (129) were produced in the same manner as in the production of toner particles (1), except that the type of release agent, the amount of resin particle dispersion used in the second aggregated particle formation step, the amount of resin particle dispersion used in the third aggregated particle formation step, and the fusion and coalescence step were adjusted so that the crystalline resin domains and release agent domains in the toner particles had the properties shown in Tables 3 and 4. The cooling rate in the first cooling step, the holding temperature after re-heating, and the cooling rate in the second cooling step in the fusion and coalescence steps were as shown in Table 2.

[0185] Toners (101) to (129) and developers (101) to (129) were prepared in the same manner as in the preparation of toner (1) and developer (1), except that one of toner particles (101) to (129) was used in place of toner particle (1).

[0186] The toners (101) to (129) were used as samples and subjected to total element analysis using an X-ray analyzer (Rigaku Corporation ZSX Primus II) to determine the net intensity (unit: kcps) of each of the Na element and the Cl element. As a result, the toners of Examples 101 to 129 each had a net intensity of Na element N Na and the net intensity of Cl element N Cl and 2.5≦N Cl / N Na The relationship was satisfied: ≦260.0.

[0187] [Table 2]

[0188] [Table 3]

[0189] [Table 4]

[0190] The symbols in Tables 3 and 4 have the following meanings: First toner particles A: toner particles satisfying the conditions (A), (B1), (C) and (D). First toner particles B: toner particles satisfying the conditions (A'), (B1'), (C') and (D'). Condition (A'): The aspect ratio of the domain of the crystalline resin is 10 or more and 40 or less. Condition (B1'): The major axis length of the domain of the crystalline resin is 0.8 μm or more and 1.5 μm or less. Condition (C'): The angle between the extension line of the long axis of the crystalline resin domain and the tangent line at the point where the extension line contacts the surface of the toner particle is 75 degrees or more and 90 degrees or less. Condition (D'): The crossing angle between the extension lines of the long axes of the two crystalline resin domains is 60 degrees or more and 90 degrees or less. Second toner particles A: toner particles satisfying the conditions (A), (B2), (C) and (D). Second toner particles B: toner particles satisfying the conditions (A'), (B2'), (C') and (D'). Condition (A'): The aspect ratio of the domain of the crystalline resin is 10 or more and 40 or less. Condition (B2'): The ratio of the major axis length of the crystalline resin domain to the maximum diameter of the toner particle is 13% or more and 30% or less. Condition (C'): The angle between the extension line of the long axis of the crystalline resin domain and the tangent line at the point where the extension line contacts the surface of the toner particle is 75 degrees or more and 90 degrees or less. Condition (D'): The crossing angle between the extension lines of the long axes of the two crystalline resin domains is 60 degrees or more and 90 degrees or less. · AR: Aspect ratio of the domains of the crystalline resin. ·Lcry: The long axis length of the domain of the crystalline resin. ·θA: the angle between the extension of the long axis of the crystalline resin domain and the tangent at the point where the extension touches the surface of the toner particle. ·θB: The crossing angle between the extension lines of the long axes of the two crystalline resin domains. · Shortest distance: The shortest distance between the release agent domain and the surface (i.e., outer edge) of a toner particle. Ester wax: WEP-5 manufactured by NOF Corporation, melting temperature 85℃. Paraffin wax: HNP-0190 manufactured by Nippon Seiro Co., Ltd., melting temperature 89°C. ·Polyethylene wax: melting temperature 89°C. [Explanation of symbols]

[0191] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K Photoconductor cleaning device (an example of a cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 28 Fixing device (an example of a fixing means) 30 Intermediate transfer body cleaning device P Recording paper (an example of a recording medium) 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium)

Claims

1. Contains an amorphous polyester resin and a crystalline polyester resin, Net intensity N of Na element measured by X-ray fluorescence analysis Na and the net intensity N of Cl element measured by X-ray fluorescence analysis. Cl And, 2.5≦N Cl / N Na ≦260.0, the net strength N Na is 0.005 kcps or more and 0.040 kcps or less, the net strength N Cl is 0.10 kcps or more and 1.30 kcps or less, The toner particles have at least two crystalline resin domains that satisfy the following conditions (A), (B1), (C), and (D) when a cross section of the toner particle is observed: Toner for developing electrostatic images. Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B1): The length of the major axis of the domain of the crystalline resin is 0.5 μm or more and 1.5 μm or less. Condition (C): the angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.

2. Contains an amorphous polyester resin and a crystalline polyester resin, Net intensity N of Na element measured by X-ray fluorescence analysis Na and the net intensity N of Cl element measured by X-ray fluorescence analysis. Cl And, 2.5≦N Cl / N Na ≦260.0, the net strength N Na is 0.005 kcps or more and 0.040 kcps or less, the net strength N Cl is 0.10 kcps or more and 1.30 kcps or less, The toner particles have at least two crystalline resin domains that satisfy the following conditions (A), (B2), (C), and (D) when a cross section of the toner particle is observed: Toner for developing electrostatic images. Condition (A): The aspect ratio of the domain of the crystalline resin is 5 or more and 40 or less. Condition (B2): In at least one of the two crystalline resin domains, the ratio of the major axis length of the crystalline resin domain to the maximum diameter of the toner particle is 10% or more and 30% or less. Condition (C): the angle between an extension line of the long axis of the crystalline resin domain and a tangent line at the contact point where the extension line contacts the surface of the toner particle is 60 degrees or more and 90 degrees or less. Condition (D): The crossing angle between the extensions of the long axes of the two crystalline resin domains is 45 degrees or more and 90 degrees or less.

3. The net strength N Na and the net strength N Cl and 4.0≦N Cl / N Na 3. The toner for developing electrostatic images according to claim 1, which satisfies the relationship: ≦60.

0.

4. The net strength N Cl The toner for developing electrostatic images according to any one of claims 1 to 3, wherein the viscosity is from 0.12 kcps to 1.10 kcps.

5. The net strength N Na The toner for developing electrostatic images according to any one of claims 1 to 4, wherein the viscosity is from 0.010 kcps to 0.030 kcps.

6. 6. The toner for developing electrostatic images according to claim 1, wherein the crystalline polyester resin contains a polymer of a linear α,ω-aliphatic dicarboxylic acid and a linear α,ω-aliphatic diol.

7. 7. The toner for developing electrostatic images according to claim 6, wherein the polymer of an α,ω-straight-chain aliphatic dicarboxylic acid and an α,ω-straight-chain aliphatic diol includes a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol.

8. 8. The toner for developing an electrostatic image according to claim 1, further comprising a release agent, the release agent including an ester wax.

9. The toner for developing an electrostatic image according to any one of claims 1 to 8, wherein the toner particles contain a release agent, and when a cross section of the toner particles is observed, a domain of the release agent is present inside the toner particles to a depth of 50 nm or more from a surface of the toner particles.

10. The toner for developing electrostatic images according to any one of claims 1 to 9, wherein the content of the toner particles is 40% by number or more based on the total number of toner particles.

11. 11. The toner for developing electrostatic images according to claim 10, wherein the content of the toner particles is 70% by number or more based on the total number of toner particles.

12. 12. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1.

13. The toner for developing an electrostatic image according to any one of claims 1 to 11 is contained in the container, A toner cartridge that is detachably attached to an image forming apparatus.

14. a developing unit that contains the electrostatic image developer according to claim 12 and develops an electrostatic image formed on a surface of an image carrier into a toner image by using the electrostatic image developer, A process cartridge that is detachably attached to an image forming apparatus.

15. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 12 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:

16. a charging step of charging the surface of the image carrier; an electrostatic image forming step of forming an electrostatic image on the charged surface of the image carrier; a developing step of developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer according to claim 12; a transfer step of transferring the toner image formed on the surface of the image carrier onto a surface of a recording medium; a fixing step of fixing the toner image transferred onto the surface of the recording medium; The image forming method according to claim 1,

Citation Information

Patent Citations

  • Electrostatic charge image developing toner and method for manufacturing same

    JP2004287421A

  • Toner for electrostatic charge image development and method for producing the same

    JP2011043540A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2012068307A

  • Image forming method

    JP2015206876A

  • Toner and production method of toner

    JP2017003990A