Coating agent for forming hydrous gel sheet and hydrous gel sheet

The coating agent with specific polymer, crosslinking agent, and emulsion components addresses rapid gelation issues, ensuring extended pot life and strong adhesion in hydrogel sheet manufacturing, enhancing production efficiency and substrate adherence.

JP7577994B2Active Publication Date: 2024-11-06TOYO INK MFG CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020209850
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-18
Publication Date
2024-11-06
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

Existing hydrogel sheet manufacturing processes face challenges with rapid gelation during coating, leading to reduced pot life, difficulty in coating on supports, and inadequate adhesion to substrates, especially when using transfer coating methods.

Method used

A coating agent comprising an unneutralized water-soluble carboxyl group-containing polymer, a crosslinking agent that ionically bonds with the polymer, and an acrylic emulsion with a pH of 1.0 to 10.5, along with optional additives, is used to create a hydrogel sheet with a pH of 1.0 or more and less than 3.0, ensuring sufficient pot life, excellent wettability, and strong adhesion.

Benefits of technology

The solution provides a hydrogel sheet laminate with extended pot life, uniform coating on release sheets, and strong adhesion to substrates, enabling efficient production and improved productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577994000001
    Figure 0007577994000001
  • Figure 0007577994000002
    Figure 0007577994000002
Patent Text Reader

Abstract

To provide coating agents that can form a water-containing gel sheet having sufficient pot life at the time of painting, excellent wettability to a peeling film, and sufficient adhesion to a bonded substrate.SOLUTION: Provided is a coating agent for forming a water-containing gel sheet, which is obtained by mixing an unneutralized water-soluble carboxyl group-containing polymer (A), a crosslinking agent (B) ionically bonding with the polymer (A), and an acrylic emulsion (C) with pH 1.0 to 10.5, in which a completely or partially neutralized water-soluble carboxyl group-containing polymer is not mixed, and a desiccant may be contained. The coating agent for forming a water-containing gel sheet has a pH of 1.0 or more and less than 3.0. Also provided is a water-containing gel sheet containing 10 to 95 mass% of a drying conditioner in the total amount excluding water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating agent for forming a hydrous gel sheet and a hydrous gel sheet. [Background technology]

[0002] Hydrous gel sheets, which have appropriate adhesive strength and low skin irritation, are used in the form of hydrous gel sheet laminates laminated on a substrate as medical poultices, medical electrode fixing materials, sheet-like skin cooling materials, wound dressings, and sheet-like cosmetic packs.

[0003] The hydrogel sheet is a hydrophilic polymer that has been crosslinked or insolubilized and swollen with water, and there are various types of hydrophilic polymers depending on the type of hydrophilic polymer and the method of crosslinking or insolubilization. As the polymer used in the hydrogel sheet, non-crosslinked polyacrylic acid or its salt, crosslinked polyacrylic acid or its salt, carboxyl group-containing polymer such as carboxymethylcellulose or its salt, etc. As a method for crosslinking a carboxyl group-containing polymer, a method of forming an ionic bond complex with a polyvalent metal cation such as aluminum hydroxide or aluminum sulfate is known, and this method is widely used industrially.

[0004] However, when the above-mentioned polyvalent metal cations, which have been conventionally used, are mixed into an aqueous solution of a carboxyl group-containing polymer, a crosslinking reaction proceeds rapidly at room temperature to produce a gel, and the period during which the mixture for forming a hydrogel sheet containing the polyvalent metal cations and the carboxyl group-containing polymer (hereinafter referred to as a coating agent) can be stored in a fluid state (hereinafter referred to as a pot life) is shortened. Therefore, even if the coating agent is applied to a support in a sheet form using a roll coater or the like, there is a problem that the coating cannot be applied because the crosslinking reaction has already proceeded and the fluidity has disappeared.

[0005] To solve this problem, a chelating agent such as ethylenediaminetetraacetic acid (EDTA) or its sodium salt has been added to the coating agent as a gelation rate regulator. The gelation reaction of a coating agent to which a gelation rate regulator has been added is delayed, and the coating agent has sufficient fluidity at the time of coating, making it possible to coat the coating agent on a support using a roll coater or the like. However, since the gelation reaction delay effect remains even after coating, there is a problem in that the coated product needs to be kept for a long time without being deformed (hereinafter referred to as seasoning). Therefore, when applying a coating agent to a sheet of support, there is a problem that production equipment is required to wait for the completion of the crosslinking reaction without deforming the coated sheet of the hydrogel sheet laminate. When the coating agent is applied to a long support in the form of a web, rather than a sheet, there is a problem that a large-scale special production facility is required to wait for the completion of the crosslinking reaction without rolling up the long hydrous gel sheet laminate after coating as it is, without deforming it. If an attempt is made to roll up the long hydrous gel sheet laminate after coating in a state in which crosslinking is not complete, there is also a problem that the hydrous gel sheet protrudes from the end of the roll-shaped laminate due to the pressure during rolling. If it becomes possible to wind up a web-like long hydrous gel sheet laminate into a roll without seasoning, the laminate can be transported in roll form to the next processing step such as slitting or punching, simplifying the manufacturing process and enabling the product to be supplied in roll form, thereby dramatically improving productivity compared to the case of a single-leaf hydrous gel sheet laminate.

[0006] Patent Document 1 discloses a hydrous gel sheet that has a sufficient pot life during coating to provide excellent productivity, and does not transfer to an adherend due to sufficient gelation, and has good conformability to the adherend. The hydrous gel sheet is characterized by containing a carboxyl group-containing polymer and a crosslinking agent that forms an ionic bond with the carboxyl group-containing polymer, having a pH of 1 or more and less than 3, and having a moisture content of 1 to 30 mass%. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6593566 Summary of the Invention [Problem to be solved by the invention]

[0008] Meanwhile, there are two methods for obtaining a hydrous gel sheet laminate by applying a coating agent onto a support, heating the support, and volatilizing and removing a portion of the moisture, as follows. (1) Direct coating: A method in which a coating agent is applied onto a support such as a resin film, and after a drying process, a release sheet with a release-treated surface is attached as necessary to protect the formed hydrous gel sheet. (2) Transfer coating: A method in which a coating agent is applied onto a release sheet, which serves as a support during coating, and after a drying process, a substrate such as a resin film is laminated onto the surface to integrate the formed hydrous gel sheet with the substrate.

[0009] The transfer coating method (2) above does not apply heat to the substrate, and does not subject the substrate to strong tension resulting from the structure of the coating machine. Therefore, it is widely used in the manufacture of products that use thermoplastic, highly elastic substrates, such as polyurethane and nonwoven fabrics.

[0010] The coating agent described in Patent Document 1 has a problem that, in transfer coating, when the coating agent is applied onto a release sheet such as a PET (polyethylene terephthalate) film with a release-treated surface, repelling occurs, making it difficult to obtain a uniform gel sheet. Furthermore, when a substrate such as a resin film is laminated after coating to integrate the hydrous gel sheet with the substrate, sufficient adhesion to the substrate is not obtained.

[0011] The problem to be solved by the present invention is to provide a coating agent capable of forming a hydrogel sheet laminate having a sufficient pot life during coating, excellent wettability to a release sheet, and a good degree of gelation while having sufficient adhesion to a substrate. [Means for solving the problem]

[0012] Means for Solving the Problems The present inventors have conducted extensive research to find a solution to the above problems, and have completed the present invention.

[0013] That is, the present invention relates to a coating agent for forming a hydrous gel sheet, which comprises a mixture of an unneutralized water-soluble carboxyl group-containing polymer (A), a crosslinking agent (B) that forms an ionic bond with the polymer (A), and an acrylic emulsion (C) having a pH of 1.0 to 10.5, in which no completely or partially neutralized water-soluble carboxyl group-containing polymer is mixed, the coating agent may contain a drying regulator, and the coating agent has a pH of 1.0 or more and less than 3.0.

[0014] The present invention also relates to the above coating agent for forming a hydrogel sheet, in which the viscosity increase rate after mixing the polymer (A), the crosslinking agent (B) and the acrylic emulsion (C) at 25°C for 24 hours is 20% or less.

[0015] The present invention further relates to a hydrogel sheet formed from the above-mentioned coating agent for forming a hydrogel sheet, characterized in that the hydrogel sheet has a pH of 1.0 or more and less than 3.0 and a moisture content of 1 to 30% by mass.

[0016] Furthermore, the present invention relates to the above hydrogel sheet, which contains a dryness adjusting agent in an amount of 10 to 95% by mass based on the total amount excluding water. Effect of the Invention

[0017] The present invention has made it possible to provide a coating agent capable of forming a hydrogel sheet laminate having a sufficient pot life during coating, excellent wettability to a release sheet, and a good degree of gelation while having sufficient adhesion to a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail.

[0019] The coating agent for forming a hydrous gel sheet of the present invention (hereinafter, sometimes referred to as the coating agent) is a mixture of an unneutralized water-soluble carboxyl group-containing polymer (A), a crosslinking agent (B) that forms an ionic bond with the polymer (A), and an acrylic emulsion (C) having a pH of 1.0 to 10.5, in which no completely or partially neutralized water-soluble carboxyl group-containing polymer is mixed, the coating agent may contain a drying regulator, and has a pH of 1.0 or more and less than 3.0.

[0020] The unneutralized water-soluble carboxyl group-containing polymer (A) used in the present invention is a polymer having a carboxyl group and is water-soluble, that is, an unneutralized polymer that dissolves in water. A water-soluble polymer is an expression used for a polymer that swells or disperses in water, and is transparent when the solution is 10% by mass at 23°C. A water-swellable or dispersible polymer is one that is cloudy when the solution is 10% by mass at 23°C. A concentration of 10% by mass refers to when 10 parts by mass of polymer are added to 90 parts by mass of water. Cloudy refers to a haze of 50% or more when measured using a cell with an optical path length of 10 mm.

[0021] The non-neutralized water-soluble carboxyl group-containing polymer (A) used in the present invention includes synthetic polymers such as homopolymers and copolymers of (meth)acrylic acid, polysaccharides such as hyaluronic acid, xanthan gum, gellan gum, pectin, and carrageenan, and proteins such as glycinin (soybean protein). One or more kinds of carboxyl group-containing polymers can be used. Among them, polyacrylic acid is preferably used.

[0022] The mass average molecular weight of the water-soluble carboxyl group-containing polymer is preferably 20,000 or more, more preferably 150,000 or more. The upper limit of the mass average molecular weight is not particularly limited, but is generally 5,000,000 or less. By using an unneutralized water-soluble carboxyl group-containing polymer with a mass average molecular weight of 20,000 or more, the gel strength required for sheet formation can be obtained.

[0023] Examples of the crosslinking agent (B) that forms an ionic bond with the unneutralized water-soluble carboxyl group-containing polymer (A) include inorganic compounds that generate polyvalent metal cations, such as aluminum chloride, zirconium chloride, magnesium chloride, calcium chloride, and titanium chloride, and organic compounds that generate polyvalent cations, such as 1,3-diaminoethane, 4,4'-diaminodiphenylmethane, and melamine. The crosslinking agent (B) can be one or more components. Among them, alum, which is an aluminum salt, is preferably used.

[0024] The crosslinking agent (B) can be used in any amount, but is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 50 parts by mass, relative to 100 parts by mass of the unneutralized water-soluble carboxyl group-containing polymer (A). When the amount of crosslinking agent (B) added is 0.1 part by mass or more, gelation proceeds quickly as the moisture content of the coating agent decreases, and when the amount is 50 parts by mass or less, a gel sheet with high transparency and excellent appearance can be produced.

[0025] The acrylic emulsion (C) used in the present invention may be any acrylic emulsion having a pH of 1.0 to 10.5, but in view of safety, an acrylic emulsion that has a proven track record of use on human skin is preferred. For example, in a dispersion medium mainly composed of water, an alkyl (meth)acrylate such as n-butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate is used as a main monomer, and a carboxyl group-containing monomer such as (meth)acrylic acid ("acrylic acid" and "methacrylic acid" are collectively referred to as "(meth)acrylic acid", the same applies below.) copolymerizable with the main monomer, a hydroxyl group-containing monomer such as 2-hydroxyethyl (meth)acrylate, an amide group-containing monomer such as dimethylacrylamide, or the like is used as a sub-monomer, and the main monomer is subjected to emulsion polymerization alone or the main monomer and the sub-monomer are subjected to emulsion polymerization in a conventional manner. The pH of the acrylic emulsion (C) and the pH of the coating agent for forming the hydrogel sheet can be measured using a pH meter having a sensor of any shape, such as a probe, dome, or flat surface. Commercially available devices can be used, such as LAQUAtwin. <ph-22b>(Horiba, Ltd.) can be used.

[0026] More specifically, examples of the acrylic emulsion (C) include methyl acrylate-2-ethylhexyl acrylate copolymer resin emulsion listed in the Pharmaceutical Excipients Standards, alkyl acrylate copolymer emulsion (2) listed in the Quasi-drug Raw Materials Standards, and alkyl acrylate copolymer ammonium, (acrylates / diacetoneacrylamide) copolymer, and (dimethylacrylamide / hydroxyethyl acrylate / methoxyethyl acrylate) copolymer registered in INCI (International Nomenclature of Cosmetic Ingredients), among which methyl acrylate-2-ethylhexyl acrylate copolymer resin emulsion and alkyl acrylate copolymer emulsion (2) are particularly preferred.

[0027] The acrylic emulsion (C) can be used in any amount, but is preferably 10 to 2000 parts by mass, more preferably 50 to 2000 parts by mass, calculated as solid content, per 100 parts by mass of the unneutralized water-soluble carboxyl group-containing polymer (A). When the amount is 10 parts by mass or more, wettability to the release sheet during transfer coating and sufficient adhesion to the substrate can be ensured, and when the amount is 2000 parts by mass or less, a hydrous gel sheet having a sufficient gel feel can be formed.

[0028] The coating agent may further contain a hydrophilic polymer other than the components (A) to (C) and other additives, if necessary.

[0029] Examples of hydrophilic polymers include synthetic polymers such as polyvinyl alcohol, polyvinylpyrrolidone, polyallylamine or a salt thereof, polyethyleneimine or a salt thereof, polyacrylamide or a salt thereof, polydiallyldimethylammonium, and polyvinylpyridine, and polysaccharides such as starch, locust bean gum, guar gum, tamarind seed gum, chitosan, carboxymethylcellulose, alginic acid, and karaya gum. These hydrophilic polymers can adjust the rheology of the coating agent and the physical properties such as the gel strength and adhesive strength of the obtained hydrous gel sheet depending on the type and amount of the polymer added.

[0030] Other additives include drying regulators, pH regulators, antioxidants, preservatives, UV absorbers, lubricants, colorants (dyes or pigments), drugs, fillers (particulate or fibrous), and conductivity imparting agents.

[0031] As the drying regulator, a hydrophilic compound with a mass average molecular weight of 10,000 or less that has little effect on the viscosity of the coating agent can be used. Examples include compounds that are liquid at room temperature, such as glycerin and polyethylene glycol, and sugars. By using the drying regulator, it is possible to suppress the deterioration of the usability of the hydrous gel sheet due to excessive evaporation of water during the drying process, and further to suppress the change in moisture content after the hydrous gel sheet is produced.

[0032] The amount of the dryness adjusting agent added is preferably 10 to 95% by mass, more preferably 15 to 92% by mass, based on the total amount of the formed hydrogel sheet excluding water. When the amount is 10% by mass or more, excessive drying can be prevented, and when the amount is 95% by mass or less, a hydrogel sheet having sufficient strength can be obtained. In other words, the dryness adjusting agent can be included in an amount of 10 to 95% by mass based on 100% by mass of the total amount of the components other than water contained in the coating agent.

[0033] As the pH adjuster, in addition to strong acids such as sulfuric acid, weak acids such as phosphoric acid having a pKa capable of lowering the pH of the coating agent or the formed hydrous gel sheet to less than 3.0 can be used. The pH adjuster can be added in any amount.

[0034] The pH of the coating agent for forming a hydrogel sheet of the present invention is 1.0 or more and less than 3.0. By keeping the pH less than 3.0, the generation of ionic carboxyl groups that contribute to the crosslinking reaction is suppressed, and the pot life of the coating agent can be ensured. Specifically, after mixing the polymer (A), the crosslinking agent (B), and the acrylic emulsion (C), the viscosity increase rate after 24 hours at 25°C is 20% or less, and the coatability can be maintained in the production of a hydrogel sheet. The viscosity increase rate is ([viscosity after 24 hours]-[initial viscosity])÷[initial viscosity]×100(%). For example, when the initial viscosity is 10 Pa·s and the viscosity after 24 hours is 12 Pa·s, the viscosity increase rate is 20%. Furthermore, a pH of 1.0 or higher ensures the presence of ionic carboxyl groups necessary for gelation, making it unnecessary to add excess acid.

[0035] The coating agent for forming a hydrous gel sheet of the present invention can be diluted with water, but the nonvolatile content (concentration) is preferably 20 to 80 mass %, and the viscosity at 23°C when the polymer (A), the crosslinking agent (B), and the acrylic emulsion (C) are mixed is preferably 0.1 Pa s or more and 30 Pa s or less, more preferably 0.2 Pa s or more and 20 Pa s or less. If the viscosity is too low, there is a risk of repelling when applied to a release sheet, whereas if the viscosity is too high, stirring becomes difficult and problems such as reduced liquid transportability and roughness of the coated surface occur during application. In the present invention, the viscosity of the coating agent for forming a hydrous gel sheet, the polymer (A), the acrylic emulsion (C), etc. can be measured using a B-type viscometer. A commercially available device can be used, for example, a TVB10 viscometer (manufactured by Toki Sangyo Co., Ltd.). The measurement conditions are 25°C, and the rotation speed and rotor are set to be suitable for the viscosity of the object to be measured. For example, when measuring a coating agent with a viscosity of 10 Pa s, a rotation speed of 12 rpm and an M3 rotor can be used.

[0036] The coating agent of the present invention is applied onto a support (substrate or release sheet) by the above-mentioned direct coating or transfer coating, and then dried to volatilize and remove a portion of the moisture, thereby obtaining a hydrous gel sheet laminate in which a hydrous gel sheet is provided on a substrate.

[0037] The pH of the hydrogel sheet is 1.0 or more and less than 3.0. The pH of the hydrogel sheet reflects the pH of the coating agent that forms the sheet. The pH of the hydrogel sheet can be measured using a pH meter with a flat sensor. Commercially available devices can be used, such as LAQUAtwin. <ph-22b>(Horiba, Ltd.) can be used.

[0038] The moisture content of the hydrous gel sheet formed by the coating agent is 1 to 30% by mass, and more preferably 2 to 25% by mass. When the moisture content of the hydrous gel sheet is 1% by mass or more, the flexibility of the hydrous gel sheet can be ensured. Furthermore, when the moisture content is 30% by mass or less, gelation proceeds quickly. The moisture content of the hydrous gel sheet can be measured using a Karl Fischer moisture meter. A commercially available device can be used, for example, a coulometric Karl Fischer moisture meter CA-200 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.).

[0039] The hydrogel sheet of the present invention can be obtained by direct coating or transfer coating using a coating agent. As the substrate, a resin film, a cloth or knit made of natural fiber, semi-synthetic fiber, synthetic fiber, or composite fiber thereof, a nonwoven fabric, paper, synthetic paper, etc. can be used. These substrates may be surface-treated with a primer or a water-repellent / hydrophilic treatment, and may be composited with the same or different substrates. Among them, polyurethane, nonwoven fabric, and composite substrates thereof are preferably used because they have good adhesion to the hydrogel sheet formed by the coating agent, but as described above, when these are used as the substrate, transfer coating is preferable. The type of release sheet is not particularly limited, and a sheet whose surface has been subjected to release treatment with silicone resin etc. is usable. The thickness of the substrate and the release sheet is not particularly limited, but is preferably 5 to 3000 μm.

[0040] The method for applying the coating agent to the substrate or release sheet is not particularly limited as long as it is a method capable of applying a material having fluidity, and examples thereof include methods using a roll coater, knife coater, gravure coater, bar coater, die coater, etc. The amount of the coating agent applied is not particularly limited, and is preferably 10 to 2000 g / m 2 It is preferable that: The atmospheric temperature in the heating step is not particularly limited, but is preferably 50° C. to 200° C., and more preferably 80° C. to 120° C. When the atmospheric temperature in the heating step is 50° C. or higher, the coating agent can be dried efficiently in terms of time, and when the atmospheric temperature is 200° C. or lower, a sudden change in moisture content can be suppressed, and poor appearance due to the generation of bubbles and non-uniformity of the gel can be prevented.

[0041] A release sheet is attached to the coating film that has been applied and has had some of the moisture removed by heating and drying in the case of direct coating, or a substrate is attached in the case of transfer coating, to obtain a laminate of hydrous gel sheets, which can be wound into a roll as necessary. A normal winder can be used for winding. EXAMPLES

[0042] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. <Raw materials> The raw materials of the coating agents used in the examples and comparative examples shown in Tables 1 and 2 are as follows. <<Water-soluble polymer with carboxyl groups>> Julimer AC-10SH: Non-crosslinked polyacrylic acid, weight average molecular weight 1 million, aqueous solution with non-volatile content of 10% by weight, manufactured by Toagosei Co., Ltd. Julimer AC-10L: Non-crosslinked polyacrylic acid, weight average molecular weight 25,000, non-volatile content 40% by weight aqueous solution, manufactured by Toagosei Co., Ltd. -Jurimer AC-10H: (non-crosslinked polyacrylic acid, weight average molecular weight 150,000, non-volatile content concentration 20% by weight in aqueous solution, manufactured by Toagosei Co., Ltd.) AQUALIC AS58: Non-crosslinked polyacrylic acid, weight average molecular weight 800,000, manufactured by Nippon Shokubai Co., Ltd. AQUALIC HL-415: Non-crosslinked polyacrylic acid, weight average molecular weight 10,000, manufactured by Nippon Shokubai Co., Ltd. Aronvis SX: Non-crosslinked sodium polyacrylate, mass average molecular weight 4.5 million, manufactured by Toagosei Co., Ltd.

[0043] <<Acrylic emulsion>> Nikasol TS-620 (methyl acrylate-2-ethylhexyl acrylate copolymer resin emulsion, non-volatile content 60% by mass, pH 2.5), manufactured by Nippon Carbide Industries Co., Ltd. · BPW HW-2 (methyl acrylate-2-ethylhexyl acrylate copolymer resin emulsion, non-volatile content 60% by mass, pH 2.4), manufactured by Toyochem Co., Ltd. TOCRYL FSK-6649T (alkyl acrylate copolymer emulsion, non-volatile content 58% by mass, pH 7.1), manufactured by Toyochem Co., Ltd.

[0044] <<Drying agent>> Macrogol 400: Polyethylene glycol, weight average molecular weight 400, Sanyo Chemical Industries, Ltd. <<Hydrophilic polymer>> Gohsenol EG-40: polyvinyl alcohol, viscosity 43 mPa s, non-volatile component concentration 4% by mass, 20°C, manufactured by Nippon Synthetic Chemical Industry Co., Ltd. PAA-HCL-10L: Polyallylamine hydrochloride, weight average molecular weight 150,000, non-volatile content 40% by weight, pH 2.5 as a 5% by weight aqueous solution, manufactured by Nittobo Medical Co., Ltd.

[0045] [Example 1] 50 parts of Julimer AC-10SH (including 5 parts of non-volatile matter), 12.5 parts of Julimer AC-10L (including 5 parts of non-volatile matter), 1 part of potassium aluminum sulfate 12-hydrate, 17 parts of Nikasol TS-620 (including 10 parts of non-volatile matter), 60 parts of glycerin, and water were mixed to obtain a coating agent with a viscosity of 10 Pa s, and the pot life was evaluated according to the method described below. The obtained coating agent was applied to a silicone release-treated polyethylene terephthalate (PET) film as a release sheet in an amount of about 200 g / m 2 The coating was performed using a knife coater so that the coating composition was 10%. The coating composition was then dried by heating to obtain a gel sheet with a moisture content of 10%. Coating properties were evaluated according to the method described below. The sheet was laminated to the following two types of substrates to obtain two types of hydrogel sheet laminates, which were then wound into rolls. The adhesion of the hydrogel sheet to the substrates was evaluated according to the method described below. Substrate 1: DN-11U: Polyurethane film, average thickness 11 μm, manufactured by Nippon Shizai Co., Ltd. Substrate 2: Sontara: nonwoven fabric, average thickness 180 μm, manufactured by Teijin DuPont Co., Ltd.

[0046] [Examples 2 to 3] As shown in Table 1, a coating agent having a viscosity of 10 Pa s was obtained in the same manner as in Example 1, except that BPW HW-2 and TOCRYL FSK-6649T were used as acrylic emulsions in place of Nikasol TS-620 so as to contain 10 parts of nonvolatile matter, respectively. The heating and drying conditions were appropriately changed to obtain gel sheet laminates having a moisture content of 10%, which were then evaluated in the same manner.

[0047] [Comparative Example 1] As shown in Table 1, a coating agent having a viscosity of 10 Pa·s and a hydrous gel sheet laminate having a water content of 10% were obtained in the same manner as in Example 1, except that Nikasol TS-620 was not mixed, and these were similarly evaluated.

[0048] [Comparative Example 2] As shown in Table 1, a coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10% were obtained and evaluated in the same manner as in Example 3, except that 10 parts of ARONBIS SX, a sodium neutralized product, was mixed instead of the unneutralized water-soluble carboxyl group-containing polymer. If a uniform coating agent was not obtained due to gelation, it was determined that coating was not possible because it was not possible to prepare a hydrous gel sheet laminate. [Comparative Examples 3 to 5] As shown in Table 1, a coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10% were obtained and evaluated in the same manner as in Example 3, except that an unneutralized water-soluble carboxyl group-containing polymer and a sodium neutralized product were mixed with an acrylic emulsion, etc. If a uniform coating agent was not obtained due to gelation, it was determined that coating was not possible because a hydrous gel sheet laminate could not be produced.

[0049] [Comparative Examples 6 and 7] A coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10% were obtained and evaluated in the same manner as in Example 3, except that an aqueous solution of sodium hydroxide dissolved in water was used instead of the water used in Example 3, as shown in Table 1. If a uniform coating agent was not obtained by gelation, it was determined that coating was not possible because a hydrous gel sheet laminate could not be produced.

[0050] [Examples 4 to 10] Using the composition of Example 3 as a reference, a coating agent having a viscosity of 10 Pa s and a hydrous gel sheet laminate having a water content of 10% were obtained in the same manner as in Example 3, except that the amount of acrylic emulsion mixed was changed as shown in Table 1, and these were evaluated in the same manner.

[0051] [Examples 11 to 18] As shown in Table 2, unneutralized water-soluble carboxyl group-containing polymers (AQUALIC AS58:AQUALIC HL-415) were mixed with different amounts and types of crosslinking agent and acrylic emulsion in a ratio of 8:2 on a non-volatile basis to obtain a coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10%, which were then evaluated in the same manner.

[0052] [Examples 19 to 26] Using the composition of Example 14 as a reference, a coating agent having a viscosity of 10 Pa s and a hydrous gel sheet laminate having a moisture content of 10% were obtained in the same manner as in Example 14, except that the amount and type of the dryness adjusting agent were changed as shown in Table 2, and these were similarly evaluated.

[0053] [Examples 27 to 31] As shown in Table 2, the type of unneutralized water-soluble carboxyl group-containing polymer was changed, and a hydrophilic polymer was further mixed in, to obtain a coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10%, which were then evaluated in the same manner.

[0054] [Comparative Example 8] A coating agent having a viscosity of 10 Pa·s and a hydrous gel sheet laminate having a water content of 10% were obtained in the same manner as in Example 13, except that the acrylic emulsion was not mixed, based on the composition of Example 13, and were similarly evaluated. [Comparative Example 9] A coating agent with a viscosity of 10 Pa s and a hydrous gel sheet laminate with a water content of 10% were obtained in the same manner as in Example 27, except that the acrylic emulsion was not mixed, based on the composition of Example 27, and were evaluated in the same manner.

[0055] (Pot life of coating agent) After preparation, the coating agent was left to stand at 25° C. for 24 hours and the viscosity increase rate was evaluated according to the following criteria. ◎: Increase rate is 10% or less. (Very good) ○: The increase rate is greater than 10% and less than 20%. (Good) ×: The rate of increase is more than 20%, or the coating is impossible due to gelation (poor).

[0056] (Coating ability of coating agent on release-treated PET film) The coating properties of the coating agent applied to the release-treated PET film were visually observed and evaluated according to the following criteria: ◎: No repelling or ridges are observed in the center or edges, and the thickness of the film is uniform throughout. (Very good) ○: The edges are slightly thick, but the rest of the coated surface is uniform in thickness. (Good) △: The edge is clearly high, but most of the film maintains the expected film thickness and is within the allowable range (lower practical limit). ×: Cracks spread over the entire coating film, resulting in uneven thickness, or random circular cracks are formed (poor).

[0057] (Adhesion to substrate in hydrogel sheet laminate) The adhesion between the formed hydrogel sheet and the polyurethane film or nonwoven fabric used as the substrate was evaluated. After the release sheet was peeled off, the evaluation was carried out according to the following criteria. ◎: The hydrogel sheet surface does not peel off from the base material even when rubbed with a finger. (Very good) ○: When the surface of the hydrogel sheet is rubbed with a finger, the base material and the gel sheet peel off at the interface, but when the sheet is applied to the skin and then peeled off, no gel remains on the skin. (Good) ×: When the hydrogel sheet surface is applied to the skin and then peeled off, the gel remains on the skin. Or, when the release sheet is peeled off, a part or the whole of the hydrogel sheet is peeled off from the base material and remains on the release sheet. (Poor)

[0058] [Table 1]

[0059] [Table 2]

[0060] In the tables, the blended parts of the carboxyl group-containing polymer and acrylic emulsion are shown as the number of parts of the resin (parts by mass). In addition, in Table 1, "%" represents "mass %."

[0061] In all of Examples 1 to 30, the pot life of the coating agent was sufficiently long, there was no coating defect on the release sheet during the coating process, and a hydrogel sheet that was sufficiently adherent to the substrate could be produced. On the other hand, in Comparative Examples 1 to 9, defects were observed in either the pot life of the coating agent, the coatability on the release sheet, or the adhesion to the substrate.

Claims

1. A coating agent for forming a hydrous gel sheet, which is obtained by mixing an unneutralized water-soluble carboxyl group-containing polymer (A), a crosslinking agent (B) which forms an ionically bond with the polymer (A), and an acrylic emulsion (C) having a pH of 1.0 to 10.5, does not contain a completely or partially neutralized water-soluble carboxyl group-containing polymer, and may contain a dryness adjusting agent, and has a pH of 1.0 or more and less than 3.0, wherein the coating agent has a nonvolatile content (concentration) of 20 to 80% by mass, and has a viscosity of 0.1 Pa s or more and 30 Pa s or less at 23°C when the polymer (A), the crosslinking agent (B), and the acrylic emulsion (C) are mixed.

2. 2. The coating agent for forming a hydrogel sheet according to claim 1, wherein after mixing the polymer (A), the crosslinking agent (B) and the acrylic emulsion (C), the viscosity increase rate after 24 hours at 25°C is 20% or less.

3. 3. A hydrogel sheet formed from the coating agent for forming a hydrogel sheet according to claim 1 or 2, characterized in that the hydrogel sheet has a pH of 1.0 or more and less than 3.0 and a moisture content of 1 to 30% by mass.

4. The hydrogel sheet according to claim 3, comprising a dryness adjusting agent in an amount of 10 to 95% by mass based on the total amount excluding water.

Citation Information

Patent Citations

  • Water-containing patch

    JP2014156497A

  • Patch

    JP2020164471A

  • Hydrous gel sheet

    JP2020179605A

  • Hydrated gel sheet

    JP6593566B1