Toner for developing electrostatic images, electrostatic image developer, toner cartridge, process cartridge and image forming apparatus
A toner composition with a core and amorphous polyester coating layer addresses the issue of adhesion to fixing members during low-density imaging, ensuring clear images by optimizing release agent domains and particle size distribution.
Patent Information
- Application Number
- JP2021087061
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-05-24
AI Technical Summary
Existing toners with small particle sizes used for improved image resolution tend to adhere to fixing members when forming images with low image densities, causing defects such as blurred images.
The toner composition includes a core with a binder resin and a release agent having a melting temperature of 80°C or less, covered by a coating layer containing an amorphous polyester resin, with specific domain and thickness ratios, and optimized particle size distribution to minimize adhesion during fixing.
The toner effectively suppresses adhesion to fixing members during low-density image formation, ensuring clear and defect-free images by enhancing the release properties and fixing performance.
Smart Images

Figure 0007578067000003 
Figure 0007578067000004 
Figure 0007578067000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge and an image forming apparatus. [Background technology]
[0002] Patent Document 1 proposes "a toner for developing electrostatic images, comprising a binder resin, a colorant, a release agent and an external additive, the toner having a volume average particle size of 5.0 to 7.0 μm, a content of toner particles having a particle size of 5.08 μm or less being 16 to 50% by number, a content of toner particles having a particle size of 5.08 to 7.92 μm being 50 to 80% by number, a content of toner particles having a particle size of 15.4 μm or more being 0.1% by volume or less, and a ratio (N / V) of the number percentage (N) of toner particles having a particle size of 5.08 μm or less to the volume percentage (V) of toner particles having a particle size of 5.08 μm or less being 1.2 to 3.0."
[0003] Patent Document 2 proposes "a toner for developing electrostatic images having a core-shell structure having a core layer containing a non-crystalline resin and a colorant and a shell layer covering the core layer, the shell layer being made from composite resin particles containing a crystalline polyester resin and a non-crystalline resin."
[0004] Patent Document 3 proposes "an electrostatic image developing toner comprising toner particles having a core-shell structure in which the surfaces of core particles are coated with a shell layer, the core particles containing a crystalline polyester resin, the shell layer containing a vinyl resin and a release agent, and a mass ratio of the crystalline polyester resin to the vinyl resin of 95:5 to 60:40." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2003-084478 A [Patent Document 2] JP 2011-149986 A [Patent Document 3] JP 2015-011304 A Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a toner for developing electrostatic images, which has toner particles constituted of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer containing an amorphous polyester resin coating the core, and the toner particles have a volume average particle size of 4.2 μm to 5.8 μm, and which can suppress adhesion of the toner to a fixing member (non-visual offset) when an image with a low image density is formed, compared with a case in which, when a cross-section of the toner particle is observed, the core portion has zero or more than three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm, or a case in which, when a cross-section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is less than 1% or more than 25%. [Means for solving the problem]
[0007] The above problems are solved by the following means: <1> The toner particles are composed of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer that coats the core and contains an amorphous polyester resin, when a cross section of the toner particle is observed, one to three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm are present in the core portion, The toner particles have a volume average particle size of 4.2 μm or more and 5.8 μm or less, The toner for developing electrostatic images, wherein when a cross section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is 1% or more and 25% or less. <2> The binder resin contains a styrene acrylic resin, a crystalline polyester resin, and an amorphous polyester resin. <1> 2. The toner for developing electrostatic images according to claim 1 . <3> the content of the styrene-acrylic resin relative to the total amount of the toner particles is 50% by mass or more and 90% by mass or less, the content of the crystalline polyester resin relative to the total amount of the toner particles is 9.5% by mass or more and 40% by mass or less, the total content of the amorphous polyester resin of the core and the amorphous polyester resin of the coating layer is 0.5% by mass or more and 5% by mass or less with respect to the entire toner particles; <2> 2. The toner for developing electrostatic images according to claim 1 . <4> the toner particles contain a colorant; The content of the colorant in the toner particles is 5% by mass or more and 12% by mass or less. <1> ~ <3> 10. The toner for developing an electrostatic image according to claim 9, <5> The net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles is measured by fluorescent X-ray analysis. A is 0.10 kcps or more and 0.40 kcps or less. <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, <6> The net strength N A is the net intensity of Na element, N N , Net intensity of Mg element N M , or the net strength of Ca element N C The above <5> 2. The toner for developing electrostatic images according to claim 1 . <7> The net strength N A However, the net intensity N of Mg element measured by X-ray fluorescence analysis M The above <5> 2. The toner for developing electrostatic images according to claim 1 . <8> The present invention has an external additive containing fatty acid metal salt particles, The ratio (DT / DS) of the volume average particle diameter DT of the toner particles to the volume average particle diameter DS of the fatty acid metal salt particles is 1.9 or more. <1> ~ <7> 10. The toner for developing an electrostatic image according to claim 9, <9> The toner particles have a small diameter volume particle size distribution index (lower GSDv) of 1.15 or more and 1.30 or less. <1> ~ <8> 10. The toner for developing an electrostatic image according to claim 9, <10> The above <1> ~ <9> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <11> The above <1> ~ <9> 13. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 12 and is detachably mountable to an image forming apparatus. <12> The above <10> and a developing means for developing an electrostatic image formed on a surface of an image carrier by using the electrostatic image developer into a toner image. <13> An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; The above <10> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: Effect of the Invention
[0008] <1> According to the invention, there is provided a toner for developing electrostatic images, which has toner particles composed of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer containing an amorphous polyester resin coating the core, and the volume average particle size of the toner particles is 4.2 μm to 5.8 μm. When the cross section of the toner particle is observed, the core portion contains zero or more than three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm, or when the cross section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is less than 1% or more than 25%, and when an image with a low image density is formed, the toner for developing electrostatic images is suppressed from adhering to a fixing member. <2> According to the present invention, there is provided a toner for developing electrostatic images, which can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared to a case in which the binder resin contains only a styrene-acrylic resin. <3> According to the invention, there is provided a toner for developing electrostatic images, which can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared to when the content of the styrene acrylic resin is less than 50% by mass or more than 90% by mass, the content of the crystalline polyester resin is less than 9.5% by mass or more than 40% by mass, or the total content of the amorphous polyester resin in the core and the amorphous polyester resin in the coating layer is less than 0.5% by mass or more than 5% by mass, relative to the entire toner particles.
[0009] <4> According to the present invention, there is provided a toner for developing electrostatic images, which, when the toner particles contain a colorant, can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared to when the content of the colorant relative to the entire toner particles is less than 5 mass % or more than 12 mass %. <5> According to the present invention, the net intensity N of the total of the alkali metal element and the alkaline earth metal element in the toner particles measured by fluorescent X-ray analysis AIn comparison with a toner having a density of less than 0.10 kcps or more than 0.40 kcps, the toner for developing electrostatic images can be prevented from adhering to a fixing member when an image with a low image density is formed. <6> According to the invention, the net strength N A is provided, which can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared with the case where the net strength N of the sum of alkali metal elements and alkaline earth metal elements other than Na, Mg, and Ca elements is measured by X-ray fluorescence analysis. <7> According to the invention, the net strength N A is the net intensity of Na element, N N , or the net strength of Ca element N C The present invention provides a toner for developing electrostatic images, which can suppress adhesion of the toner to a fixing member when an image with a low image density is formed, as compared with the case where the toner is not attached to a fixing member.
[0010] <8> According to the invention, there is provided a toner for developing electrostatic images having an external additive containing fatty acid metal salt particles, which can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared to a case in which the ratio (DT / DS) of the volume average particle diameter of the toner particles to the volume average particle diameter DS of the fatty acid metal salt particles is less than 1.9. <9> According to the present invention, there is provided a toner for developing electrostatic images, which can suppress adhesion of the toner to a fixing member when an image with low image density is formed, compared to when the small diameter side volume particle size distribution index (lower GSDv) of the toner particles is less than 1.15 or exceeds 1.30.
[0011] <10> ~ <13> According to the invention, there is provided an electrostatic image developer, a toner cartridge, a process cartridge and an image forming apparatus, which are provided with an electrostatic image developing toner that has toner particles composed of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer that coats the core and contains an amorphous polyester resin, and the toner particles have a volume average particle size of 4.2 μm to 5.8 μm, in which, when a cross-section of the toner particle is observed, the core portion has zero or more than three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm, or when a cross-section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is less than 1% or more than 25%, and which is capable of suppressing adhesion of the toner to a fixing member when an image with a low image density is formed. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail. In addition, in numerical ranges described in stages, the upper limit or lower limit value described in a certain numerical range may be replaced with the upper limit or lower limit value of another numerical range described in stages. In addition, in a numerical range, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. When a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0014] "Alkali metal element" refers to Li, Na, K, Rb, Cs, and Fr. "Alkaline earth metal elements" refers to Be, Mg, Ca, Sr, Ba, and Ra.
[0015] <Toner for developing electrostatic images> The toner for developing electrostatic images (hereinafter also referred to as "toner") according to this embodiment has toner particles containing a binder resin and a release agent having a melting temperature Tm of 80°C or less, and the toner particles are composed of a core and a coating layer that coats the core and contains an amorphous polyester resin. When a cross section of the toner particle is observed, one to three domains of the release agent having a circle-equivalent diameter of 1 μm to 3 μm are present in the core portion, the volume average particle diameter of the toner particle is 4.2 μm to 5.8 μm, and when a cross section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is 1% to 25%.
[0016] The toner according to the present embodiment, due to the above-mentioned constitution, suppresses adhesion of the toner to the fixing member when an image with a low image density (for example, an image density of 20% or less) is formed. The reason for this is presumed to be as follows.
[0017] In recent years, there has been a demand for improved image resolution, and toners with small particle sizes (for example, toner particles with a volume average particle size of 4.2 μm or more and 5.8 μm or less) are sometimes used to meet this demand. However, when a toner with small particle size is used to form an image with low image density, the toner is likely to adhere to the fixing member, which can easily cause image defects such as blurred images. When an image with low image density is formed, a toner with small particle size may have a large amount of isolated toner when transferred to a recording medium. Then, in the subsequent fixing process, the isolated toner tends to be less likely to be fixed on the recording medium compared to toners that are adjacent to other toners, and therefore the toner is likely to adhere to the fixing member side. Then, image defects such as blurred images can easily occur.
[0018] The toner according to the present embodiment is composed of a core and a coating layer that contains an amorphous polyester resin and covers the core. When the cross section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is 1% or more and 25% or less. The melting temperature of the amorphous polyester resin tends to be low. When the thickness of the coating layer containing the amorphous polyester resin is within the above range, the toner is easily melted during fixing and easily permeates into the recording medium. In addition, the toner according to the present embodiment contains a release agent having a melting temperature Tm of 80° C. or less in the core of the toner particle. The core of the toner particle has one to three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm. By making the domain of the release agent in the core of the toner particle as described above, the release agent is more likely to seep out during fixing to a recording medium, and adhesion of the toner to the fixing member is suppressed. By having a release agent having the above melting temperature, the plasticity of the release agent is improved, and the release agent is more likely to spread on the surface of the fixing member during fixing. Therefore, adhesion of the toner to the fixing member is further suppressed.
[0019] From the above, it is presumed that the toner according to this embodiment can suppress adhesion of the toner to the fixing member when an image with a low image density is formed.
[0020] (Toner particles) The toner particles contain a binder resin and a release agent having a melting temperature Tm of 80° C. or lower. The toner particles are composed of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer that coats the core and contains an amorphous polyester resin.
[0021] -Core- The core contains a binder resin, a release agent having a melting temperature Tm of 80° C. or less, and, if necessary, a colorant and other additives.
[0022] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0023] Examples of the binder resin include non-crystalline (also called "non-crystalline") resins and crystalline resins. The "crystalline" nature of a resin refers to the presence of a clear endothermic peak rather than a stepwise change in the amount of endothermic heat in differential scanning calorimetry (DSC); specifically, the half-width of the endothermic peak is within 15°C when measured at a heating rate of 10 (°C / min). On the other hand, the term "amorphous" for a resin refers to a half-width exceeding 15° C., a stepwise change in endothermic heat quantity, or no clear endothermic peak being observed.
[0024] The amorphous resin will now be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene-acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, amorphous polyester resin and amorphous vinyl resin (particularly styrene-acrylic resin) are preferred, and amorphous polyester resin is more preferred. In addition, it is also a preferred embodiment to use an amorphous polyester resin and a styrene-acrylic resin in combination as the amorphous resin. It is also a preferred embodiment to use an amorphous resin having an amorphous polyester resin segment and a styrene-acrylic resin segment (hereinafter also referred to as a "hybrid amorphous resin") as the amorphous resin.
[0025] The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.
[0026] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0027] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a trihydric or higher polyhydric alcohol having a crosslinked or branched structure may be used in combination with the diol. Examples of the trihydric or higher polyhydric alcohol include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0028] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0029] Here, the amorphous polyester resin may be a modified amorphous polyester resin in addition to the unmodified amorphous polyester resin described above. The modified amorphous polyester resin is an amorphous polyester resin having a bond group other than an ester bond, or an amorphous polyester resin having a resin component different from the amorphous polyester resin component bonded by a covalent bond or an ionic bond. The modified amorphous polyester resin may be, for example, an amorphous polyester resin having a functional group such as an isocyanate group that reacts with an acid group or a hydroxyl group at the end introduced therein, and a resin having a modified end that is reacted with an active hydrogen compound.
[0030] The styrene-acrylic resin is a copolymer obtained by copolymerizing at least a styrene-based monomer (a monomer having a styrene skeleton) and a (meth)acrylic-based monomer (a monomer having a (meth)acrylic group, preferably a monomer having a (meth)acryloxy group). The styrene-acrylic resin includes, for example, a copolymer of a styrene monomer and a (meth)acrylic acid ester monomer. The acrylic resin portion of the styrene-acrylic resin is a partial structure formed by polymerizing either an acrylic monomer or a methacrylic monomer, or both. In addition, the term "(meth)acrylic" includes both "acrylic" and "methacrylic".
[0031] Specific examples of styrene-based monomers include styrene, alkyl-substituted styrenes (e.g., α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, etc.), halogen-substituted styrenes (e.g., 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, etc.), vinylnaphthalene, etc. The styrene-based monomers may be used alone or in combination of two or more. Of these, as the styrene-based monomer, styrene is preferred from the viewpoints of ease of reaction, ease of reaction control, and availability.
[0032] Specific examples of the (meth)acrylic monomer include (meth)acrylic acid and (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include (meth)acrylic acid alkyl esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, and (meth) Examples of the (meth)acrylic acid monomer include neopentyl acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, etc.), aryl (meth)acrylate esters (e.g., phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, etc.), dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, β-carboxyethyl (meth)acrylate, and (meth)acrylamide. The (meth)acrylic acid monomer may be used alone or in combination of two or more. Among these (meth)acrylic esters among the (meth)acrylic monomers, from the viewpoint of fixation, (meth)acrylic acid esters having an alkyl group having 2 to 14 carbon atoms (preferably 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms) are preferred. Of these, n-butyl (meth)acrylate is preferred, and n-butyl acrylate is particularly preferred.
[0033] The copolymerization ratio of the styrene monomer to the (meth)acrylic monomer (mass basis, styrene monomer / (meth)acrylic monomer) is not particularly limited, but is preferably 85 / 15 to 70 / 30.
[0034] The styrene-acrylic resin may have a crosslinked structure. A preferred example of the styrene-acrylic resin having a crosslinked structure is a copolymer of at least a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinkable monomer.
[0035] The crosslinkable monomer may, for example, be a bifunctional or higher functional crosslinking agent. Examples of bifunctional crosslinking agents include divinylbenzene, divinylnaphthalene, di(meth)acrylate compounds (e.g., diethylene glycol di(meth)acrylate, methylene bis(meth)acrylamide, decanediol diacrylate, glycidyl (meth)acrylate, etc.), polyester type di(meth)acrylate, 2-([1'-methylpropylideneamino]carboxyamino)ethyl methacrylate, etc. Examples of polyfunctional crosslinking agents include tri(meth)acrylate compounds (e.g., pentaerythritol tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.), tetra(meth)acrylate compounds (e.g., pentaerythritol tetra(meth)acrylate, oligoester (meth)acrylate, etc.), 2,2-bis(4-methacryloxy, polyethoxyphenyl)propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diaryl chlorendate, etc. Among these, as the crosslinkable monomer, from the viewpoints of suppressing the occurrence of a decrease in image density and suppressing the occurrence of uneven image density, and of fixability, a bifunctional or higher (meth)acrylate compound is preferred, a bifunctional (meth)acrylate compound is more preferred, a bifunctional (meth)acrylate compound having an alkylene group with 6 to 20 carbon atoms is further preferred, and a bifunctional (meth)acrylate compound having a linear alkylene group with 6 to 20 carbon atoms is particularly preferred.
[0036] The copolymerization ratio of the crosslinkable monomer to the total monomers (mass basis, crosslinkable monomer / total monomers) is not particularly limited, but is preferably 2 / 1,000 to 20 / 1,000.
[0037] The method for producing the styrene-acrylic resin is not particularly limited, and various polymerization methods (e.g., solution polymerization, precipitation polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc.) are applied. In addition, the polymerization reaction is carried out by a known operation (e.g., batchwise, semi-continuous, continuous, etc.).
[0038] Hybrid amorphous resin The hybrid amorphous resin is an amorphous resin in which an amorphous polyester resin segment and a styrene-acrylic resin segment are chemically bonded to each other. Examples of the hybrid amorphous resin include a resin having a main chain made of a polyester resin and a side chain made of a styrene-acrylic resin chemically bonded to the main chain; a resin having a main chain made of a styrene-acrylic resin and a side chain made of a polyester resin chemically bonded to the main chain; a resin having a main chain formed by chemically bonding a polyester resin and a styrene-acrylic resin; a resin having a main chain formed by chemically bonding a polyester resin and a styrene-acrylic resin, and at least one of a side chain made of a polyester resin chemically bonded to the main chain and a side chain made of a styrene-acrylic resin chemically bonded to the main chain; and the like.
[0039] The amorphous polyester resin and the styrene-acrylic resin in each segment are as described above, and therefore the description will be omitted.
[0040] The total amount of the polyester resin segment and the styrene-acrylic resin segment in the entire hybrid amorphous resin is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass%.
[0041] In the hybrid amorphous resin, the proportion of the styrene-acrylic resin segment in the total amount of the polyester resin segment and the styrene-acrylic resin segment is preferably 20% by mass or more and 60% by mass or less, more preferably 25% by mass or more and 55% by mass or less, and even more preferably 30% by mass or more and 50% by mass or less.
[0042] The hybrid amorphous resin is preferably produced by any one of the following methods (i) to (iii). (i) After preparing a polyester resin segment by condensation polymerization of a polyhydric alcohol and a polycarboxylic acid, a monomer constituting a styrene-acrylic resin segment is addition-polymerized. (ii) A styrene-acrylic resin segment is prepared by addition polymerization of an addition-polymerizable monomer, and then a polyhydric alcohol and a polycarboxylic acid are condensation-polymerized. (iii) Polycondensation of a polyhydric alcohol and a polycarboxylic acid and addition polymerization of an addition-polymerizable monomer are carried out in parallel.
[0043] The proportion of the hybrid amorphous resin in the total binder resin is preferably 60% by mass or more and 98% by mass or less, more preferably 65% by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 90% by mass or less.
[0044] The glass transition temperature (Tg) of the amorphous resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0045] The weight average molecular weight (Mw) of the amorphous resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0046] The crystalline resin will now be described. Examples of the crystalline resin include known crystalline resins such as crystalline polyester resins, crystalline vinyl resins (e.g., polyalkylene resins, long-chain alkyl (meth)acrylate resins, etc.) Among these, crystalline polyester resins are preferred.
[0047] The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.
[0048] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0049] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0050] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0051] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.
[0052] The melting temperature of the crystalline resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0053] The weight average molecular weight (Mw) of the crystalline resin is preferably 6,000 or more and 35,000 or less.
[0054] The crystalline polyester resin is preferably a polymer of a linear α,ω-aliphatic dicarboxylic acid and a linear α,ω-aliphatic diol.
[0055] The α,ω-linear aliphatic dicarboxylic acid is preferably an α,ω-linear aliphatic dicarboxylic acid in which the alkylene group connecting the two carboxy groups has 3 or more and 14 or less carbon atoms, more preferably the alkylene group has 4 or more and 12 or less carbon atoms, and even more preferably the alkylene group has 6 or more and 10 or less carbon atoms. Examples of α,ω-linear aliphatic dicarboxylic acids include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid (commonly known as suberic acid), 1,7-heptanedicarboxylic acid (commonly known as azelaic acid), 1,8-octanedicarboxylic acid (commonly known as sebacic acid), 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Of these, 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, and 1,10-decanedicarboxylic acid are preferred. The α,ω-linear aliphatic dicarboxylic acids may be used alone or in combination of two or more kinds.
[0056] The α,ω-linear aliphatic diol is preferably an α,ω-linear aliphatic diol in which the alkylene group connecting the two hydroxy groups has 3 to 14 carbon atoms, more preferably the alkylene group has 4 to 12 carbon atoms, and further preferably the alkylene group has 6 to 10 carbon atoms. Examples of the α,ω-linear aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,18-octadecanediol. Of these, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred. The α,ω-linear aliphatic diols may be used alone or in combination of two or more kinds.
[0057] As the polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol, a polymer of at least one selected from the group consisting of 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, 1,9-nonanedicarboxylic acid, and 1,10-decanedicarboxylic acid and at least one selected from the group consisting of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol is preferred, and among these, a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol is more preferred.
[0058] The binder resin preferably contains a styrene-acrylic resin, a crystalline polyester resin, and an amorphous polyester resin. By including the above-mentioned resin in the binder resin, the phenomenon in which the viscoelasticity of the toner becomes too high or too low during toner fixing is easily suppressed, so that the toner is more easily fixed to the recording medium during toner fixing, and adhesion of the toner to the fixing member is more effectively suppressed.
[0059] Here, it is preferable that the binder resin of the entire toner particles contains the styrene acrylic resin, the crystalline polyester resin and the amorphous polyester resin in the following amounts. Styrene acrylic resin: the content relative to the entire toner particles is preferably from 50% by mass to 90% by mass, more preferably from 55% by mass to 85% by mass, and even more preferably from 60% by mass to 70% by mass. Crystalline polyester resin: the content relative to the entire toner particles is preferably from 9.5% by mass to 40% by mass, more preferably from 15% by mass to 35% by mass, and even more preferably from 20% by mass to 30% by mass. Amorphous polyester resin in the core and amorphous polyester resin in the coating layer: the content relative to the entire toner particles is preferably from 0.5% by mass to 5% by mass, more preferably from 1.5% by mass to 4% by mass, and even more preferably from 2.0% by mass to 3% by mass.
[0060] By setting the content of the resin in the binder resin within the above range, the phenomenon in which the viscoelasticity of the toner becomes too high or too low during toner fixing can be further suppressed, so that the toner is more easily fixed to the recording medium during toner fixing, and adhesion of the toner to the fixing member is further suppressed.
[0061] The content of the binder resin contained in the core is, for example, preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the entire toner particles.
[0062] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, and tetrahydrofuran. Examples of the dyes include various pigments such as phosphorus blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate, and various dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.
[0063] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.
[0064] The content of the colorant is, for example, preferably from 1% by mass to 30% by mass, more preferably from 3% by mass to 15% by mass, even more preferably from 5% by mass to 12% by mass, and most preferably from 7% by mass to 10% by mass, based on the total amount of the toner particles. By setting the colorant content to 12% by mass or less, the toner loading amount increases even when an image with low image density is formed, and the amount of toner that is isolated during transfer to a recording medium is easily reduced. Therefore, in the fixing process, the toner is easily fixed onto the recording medium, and adhesion of the toner to the fixing member is suppressed. Furthermore, if the amount of applied toner becomes too large, the toner will adhere to the fixing member, but by setting the content of the colorant to 5% by mass or more, the amount of applied toner can be prevented from becoming too large.
[0065] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0066] The melting temperature Tm of the release agent is 80° C. or lower. From the viewpoint of further suppressing adhesion of the toner to the fixing member, the melting temperature Tm is preferably 20°C or higher and 75°C or lower, and more preferably 30°C or higher and 70°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."
[0067] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.
[0068] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, and inorganic powders. Further, other additives include, for example, an alkali metal element source, an alkaline earth metal element source, and the like. These additives are contained in the toner particles as internal additives.
[0069] -Source of alkali metal elements- The alkali metal element supply source may be an additive containing an alkali metal element (such as a surfactant or a flocculant). Specifically, the additive containing an alkali metal element may be, for example, a salt containing an alkali metal element. Examples of salts containing an alkali metal element include salts containing lithium element, such as lithium chloride, lithium sulfate, lithium nitrate, etc.; salts containing sodium element, such as sodium chloride, sodium sulfate, sodium nitrate, etc.; salts containing potassium element, such as potassium chloride, potassium sulfate, potassium nitrate, etc.; salts containing rubidium element, such as rubidium chloride, rubidium sulfate, rubidium nitrate, etc.; salts containing cesium element, such as cesium chloride, cesium sulfate, cesium nitrate, etc.; and salts containing francium element, such as francium chloride, francium sulfate, francium nitrate, etc. Examples of the salt containing an alkali metal element include salts containing an alkali metal element sulfonate (eg, sodium alkylbenzenesulfonate such as sodium dodecylbenzenesulfonate).
[0070] -Source of alkaline earth metal elements- The alkaline earth metal element supply source may be an additive containing an alkaline earth metal element (such as a surfactant or a flocculant). Specifically, the additive containing an alkaline earth metal element may be, for example, a salt containing an alkaline earth metal element. Specific examples of salts containing alkaline earth metal elements include salts containing beryllium element, such as beryllium chloride, beryllium sulfate, and beryllium nitrate; salts containing magnesium element, such as magnesium chloride, magnesium sulfate, and magnesium nitrate; salts containing calcium element, such as calcium chloride, calcium sulfate, and calcium nitrate; salts containing strontium element, such as strontium chloride, strontium sulfate, and strontium nitrate; salts containing barium element, such as barium chloride, barium sulfate, and barium nitrate; and salts containing radium element, such as radium chloride, radium sulfate, and radium nitrate. Examples of salts containing an alkaline earth metal element include salts containing an alkaline earth metal element sulfonate (calcium alkylbenzenesulfonate such as calcium dodecylbenzenesulfonate) and metal sulfides (calcium polysulfide).
[0071] The salt containing an alkali metal element is preferably a salt containing a sodium element, such as sodium chloride, sodium sulfate, or sodium nitrate. The salt containing an alkaline earth metal element is preferably a salt containing magnesium element such as magnesium chloride, magnesium sulfate, magnesium nitrate, etc.; and a salt containing calcium element such as calcium chloride, calcium sulfate, calcium nitrate, etc.; and more preferably a salt containing magnesium element such as magnesium chloride, magnesium sulfate, magnesium nitrate, etc.
[0072] The total content of the alkali metal element source and the alkaline earth metal element source in the toner particles is the net strength N A It is preferable to add it so that the viscosity becomes 0.10 kcps or more and 0.40 kcps or less.
[0073] -Coating layer- The coating layer contains an amorphous polyester resin as a binder resin. Here, the amorphous polyester resin contained in the coating layer is the same as the amorphous polyester resin contained in the core portion (core particle).
[0074] The coating layer may contain a resin other than the amorphous polyester resin. Examples of other resins contained in the coating layer include vinyl resins consisting of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Other resins contained in the coating layer include, for example, non-vinyl resins such as epoxy resins, crystalline polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. Furthermore, the core may contain the binder resin described above.
[0075] The content of the amorphous polyester resin in the binder resin contained in the coating layer is, for example, preferably 80% by mass or more and 100% by mass or less, more preferably 85% by mass or more and 99% by mass or less, and even more preferably 90% by mass or more and 98% by mass or less, based on the entire binder resin contained in the coating layer.
[0076] The content of the binder resin in the coating layer is, for example, preferably from 80% by mass to 100% by mass, more preferably from 85% by mass to 99% by mass, and even more preferably from 90% by mass to 98% by mass, based on the entire coating layer.
[0077] The coating layer may contain a release agent, a colorant, and other additives, as necessary. The release agent, colorant, and other additives may be the same as those contained in the core.
[0078] (Characteristics of toner particles) -Release Agent Domain- In the toner according to the present embodiment, when a cross section of a toner particle is observed, one to three domains of the release agent having a circle-equivalent diameter of 1 μm to 3 μm exist in the core portion.
[0079] From the viewpoint of further improving the ease of exudation of the release agent during fixing, the equivalent circle diameter of the domain of the release agent is more preferably 1.2 μm or more and 2.8 μm or less, and further preferably 1.4 μm or more and 2.6 μm or less.
[0080] The circle equivalent diameter of the domains of the release agent and the number of the domains are measured by the following method. Toner particles (or toner) are mixed and embedded in epoxy resin, and the epoxy resin is solidified. The solidified product is cut using an ultramicrotome (Ultracut UCT manufactured by Leica) to prepare a thin section sample with a thickness of 80 nm to 130 nm. Next, the obtained thin section sample is stained with ruthenium tetroxide for 3 hours in a desiccator at 30°C. Then, an SEM image of the stained thin section sample is obtained using an ultra-high resolution field emission scanning electron microscope (FE-SEM, S-4800 manufactured by Hitachi High-Technologies Corporation). In the cross section of the toner particle, the colorant domain is smaller than the release agent domain, and therefore can be distinguished by size. The colorant domain can also be distinguished by the shade of dye in the release agent domain. In the cross section of the toner particle, the core and the coating layer can also be distinguished by the shade of dye. In the SEM image, 30 toner particle cross sections in which the diameter of the toner particle cross section is 85% or more of the volume average particle diameter of the toner particle are selected, and the circle-equivalent diameter of the domain of the dyed release agent present in the core is measured. Then, the number of domains in which the circle-equivalent diameter of the domain is 1 μm or more and 3 μm or less is counted. Then, the total number of domains in which the circle-equivalent diameter of the domain present in the 30 selected toner particle cross sections is 1 μm or more and 3 μm or less is calculated, and the total number is divided by 30 to calculate the number of domains of the release agent present in the core.
[0081] -Volume average particle size and circularity- The toner according to this embodiment has a volume average particle size of 4.2 μm or more and 5.8 μm or less. The volume average particle size of the toner particles may be 4.4 μm or more and 5.6 μm or less, or may be 4.6 μm or more and 5.4 μm or less.
[0082] In the toner according to the present embodiment, the smaller diameter volume particle size distribution index (lower GSDv) of the toner particles is preferably 1.15 or more and 1.30 or less. By setting the small diameter volume particle size distribution index of the toner particles within the above range, the proportion of fine toner particles is reduced, and scattering of toner during development and transfer is suppressed. As a result, the proportion of isolated toner particles on the recording medium is further reduced, and adhesion of toner to the fixing member is further suppressed.
[0083] The smaller diameter volume particle size distribution index (lower GSDv) of the toner particles is more preferably 1.18 or more and 1.28 or less, and further preferably 1.20 or more and 1.26 or less.
[0084] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as: Using these, the small diameter volume particle size distribution index (lower GSDv) is (D50v / D16v) 1 / 2 It is calculated as:
[0085] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.
[0086] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.
[0087] -Coating layer thickness ratio- In the toner according to the present embodiment, when a cross section of a toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is 1% or more and 25% or less. From the viewpoint of further improving the penetration of the toner into the recording medium during fixing, the ratio of the thickness of the coating layer to the maximum diameter of the toner particles is preferably 3% or more and 22% or less, more preferably 6% or more and 19% or less, and even more preferably 9% or more and 16% or less.
[0088] The ratio of the thickness of the coating layer to the maximum diameter of the toner particles is calculated as follows. Toner particles (or toner) are mixed and embedded in epoxy resin, and the epoxy resin is solidified. The solidified product is cut using an ultramicrotome (Ultracut UCT manufactured by Leica) to prepare a thin section sample with a thickness of 80 nm to 130 nm. Next, the obtained thin section sample is stained with ruthenium tetroxide for 3 hours in a desiccator at 30°C. Then, an SEM image of the stained thin section sample is obtained using an ultra-high resolution field emission scanning electron microscope (FE-SEM, S-4800 manufactured by Hitachi High-Technologies Corporation). In addition, in the cross section of a toner particle, the core and the coating layer can be distinguished from each other by the shade of the dye. Then, 10 toner particle cross sections in which the diameter of the toner particle cross section is 85% or more of the volume average particle diameter of the toner particle are selected from the SEM image. The arithmetic average of the diameters of the selected toner particle cross sections is defined as the "maximum diameter of the toner particle." Here, the diameter of the toner particle cross section refers to the maximum length of a straight line drawn between any two points on the contour line of the toner particle cross section (so-called major axis). Next, in the SEM image of the cross section of the selected toner particle, the longest straight line is drawn between any two points on the contour line of the cross section of the toner particle. The length between point A where the straight line intersects with the contour line of the cross section of the toner particle and point B (located immediately adjacent to point A) where the straight line intersects with the boundary line between the core and the coating layer is calculated. The arithmetic average of the lengths between points A and B calculated from the cross sections of each toner particle is defined as the "thickness of the coating layer." The ratio of the "maximum diameter of the toner particles" to the "thickness of the coating layer" taken as 100 is defined as the "ratio of the thickness of the coating layer to the maximum diameter of the toner particles."
[0089] -Net strength- Net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by X-ray fluorescence analysis A is preferably 0.10 kcps or more and 0.40 kcps or less.
[0090] The alkali metal elements and alkaline earth metal elements act as cross-linking agents for the binder resin. A By setting the value of the toner particle diameter to within the above range, the above elements are appropriately contained in the toner particles, and the phenomenon in which the viscoelasticity of the toner becomes too high or too low during toner fixing is more easily suppressed. Therefore, the toner is more easily fixed to the recording medium during toner fixing, and adhesion of the toner to the fixing member is more effectively suppressed.
[0091] From the viewpoint of suppressing adhesion of toner to the fixing member, the net strength N A is more preferably 0.20 kcps or more and 0.60 kcps or less, and further preferably 0.40 kcps or more and 0.50 kcps or less.
[0092] Net strength N of alkali metal elements and alkaline earth metal elements A is calculated by measuring the net strength of alkali metal elements and the net strength of alkaline earth metal elements by the following method and adding up these measured values.
[0093] The method for measuring the net strength of alkali metal elements and the net strength of alkaline earth metal elements is as follows. Approximately 0.12 g of toner particles (or toner having toner particles and external additives) is compressed with a compression molding machine under a load of 6 t for 60 seconds to produce a disk with a diameter of 50 mm and a thickness of 2 mm. This disk is used as a sample and qualitative and quantitative elemental analysis is performed under the following conditions using a scanning X-ray fluorescence analyzer (Rigaku ZSX PrimusII) to determine the net intensity (unit: kilo counts per second, kcps) of each of the alkali metal elements and alkaline earth metal elements. The net intensity of the alkali metal elements and the net intensity of the alkaline earth metal elements are then summed to obtain the net intensity N A Calculate. Tube voltage: 40kV ·Tube current: 70mA ·Anti-cathode: Rhodium Measurement time: 15 minutes ·Analysis diameter: 10mm in diameter
[0094] The net strength N A is the net intensity of Na element, N N , Net intensity of Mg element N M , or the net strength of Ca element N C It is preferable that: That is, the toner according to the present embodiment has a "Net intensity N N "The net intensity N of Mg element measured by X-ray fluorescence analysis is 0.10 kcps or more and 0.40 kcps or less." M "The net strength N of Ca element measured by X-ray fluorescence analysis is 0.10 kcps or more and 0.40 kcps or less" C is preferably 0.10 kcps or more and 0.40 kcps or less.
[0095] Among the alkali metal elements and alkaline earth metal elements, Na, Mg, and Ca tend to be more effective as crosslinking agents, and therefore, by incorporating these elements in the toner particles so that the net strength of these elements falls within the above range, adhesion of the toner to the fixing member is further suppressed.
[0096] Since Mg element has a tendency to have a higher effect as a crosslinking agent, from the viewpoint of suppressing adhesion of the toner to the fixing member, the net strength N A However, the net intensity N of Mg element measured by X-ray fluorescence analysis M It is preferable that: That is, the toner according to the present embodiment has a net intensity N M is preferably 0.10 kcps or more and 1.20 kcps or less.
[0097] Here, the net strength of Na element N N , Net intensity of Mg element N M , and the net intensity of Ca element N C The measurement is the net intensity N of Na element during qualitative and quantitative elemental analysis. N , Net intensity of Mg element N M , and the net intensity of Ca element N C The measurement is performed in the same manner as the measurement of the net strength of alkali metal elements and the net strength of alkaline earth metal elements, except that the above is determined.
[0098] In order to set each Net within the above range, for example, it is preferable to incorporate an alkali metal element source or an alkaline earth metal element source into the toner particles.
[0099] (External additives) Examples of the external additive include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.
[0100] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0101] Examples of the external additive include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, fatty acid metal salt particles, and fluorine-based polymer particles), and the like.
[0102] The toner in the present embodiment preferably contains fatty acid metal salt particles as an external additive. It is preferable that the external additive contains fatty acid metal salt particles, since adhesion of the toner to the fixing member is further suppressed.
[0103] The fatty acid metal salt particles are particles of a salt formed from a fatty acid and a metal. The fatty acid may be either a saturated fatty acid or an unsaturated fatty acid. The number of carbon atoms of the fatty acid may be from 10 to 25 (preferably from 12 to 22). The number of carbon atoms of the fatty acid includes the carbon of the carboxyl group. Specific examples of fatty acids include saturated fatty acids such as behenic acid, stearic acid, palmitic acid, myristic acid, and lauric acid; and unsaturated fatty acids such as oleic acid, linoleic acid, and ricinoleic acid. Among these fatty acids, stearic acid and lauric acid are preferred, and stearic acid is more preferred. It is preferable to use a divalent metal as the metal. Specific examples of the metal include magnesium, calcium, aluminum, barium, and zinc. Among these, zinc is preferable.
[0104] Specific examples of fatty acid metal salt particles include metal salts of stearic acid such as aluminum stearate, calcium stearate, potassium stearate, magnesium stearate, barium stearate, lithium stearate, zinc stearate, copper stearate, lead stearate, nickel stearate, strontium stearate, cobalt stearate, and sodium stearate; and zinc palmitate, cobalt palmitate, copper palmitate, magnesium palmitate, aluminum palmitate, and calcium palmitate. Examples of particles include metal salts of palmitic acid; metal salts of lauric acid, such as zinc laurate, manganese laurate, calcium laurate, iron laurate, magnesium laurate, and aluminum laurate; metal salts of oleic acid, such as zinc oleate, manganese oleate, iron oleate, aluminum oleate, copper oleate, magnesium oleate, and calcium oleate; metal salts of linoleic acid, such as zinc linoleate, cobalt linoleate, and calcium linoleate; and metal salts of ricinoleic acid, such as zinc ricinoleate and aluminum ricinoleate.
[0105] Among these, as the fatty acid metal salt particles, from the viewpoints of cleaning properties and material availability, particles of a metal salt of stearic acid or a metal salt of lauric acid are preferred, particles of zinc stearate or zinc laurate are more preferred, and zinc stearate particles are even more preferred.
[0106] -Volume average particle size of fatty acid metal salt particles- The volume average particle size of the fatty acid metal salt particles is preferably from 0.1 μm to 10 μm, and more preferably from 0.5 μm to 3 μm.
[0107] The volume average particle size of the fatty acid metal salt particles can be measured, for example, by the following method. 1g of the toner to be measured is placed in a 1L beaker, and 500g of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) is added. Ultrasonic waves are applied to remove the external additives from the toner particles, and then centrifugation is performed. Since the density of fatty acid metal salt particles is less than 1, and that of toner is usually more than 1, the fatty acid metal salt particles are contained in the supernatant after centrifugation. 2ml of this supernatant is added to 100ml to 150ml of electrolyte (ISOTON-II, manufactured by Beckman Coulter, Inc.), and the measurement sample is prepared by dispersing the particles for 1 minute using an ultrasonic disperser. Using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc., aperture diameter 100μm), the particle diameter of 50,000 particles between 2μm and 60μm is measured, and the cumulative volume distribution is drawn from the small diameter side, and the particle diameter at which the cumulative 50% is reached is taken as the volume average particle diameter (D50v).
[0108] - Particle size ratio of toner particles to fatty acid metal salt particles (DT / DS) - In the toner of this embodiment, when the volume average particle diameter of the toner particles is DT and the volume average particle diameter of the fatty acid metal salt particles is DS, it is preferable that the ratio of the volume average particle diameter of the toner particles DT to the volume average particle diameter of the fatty acid metal salt particles DS (DT / DS) is 1.9 or more.
[0109] By setting the ratio (DT / DS) of the volume average particle diameter DT of the toner particles to the volume average particle diameter DS of the fatty acid metal salt particles within the above range, the fatty acid metal salt particles are easily physically adsorbed to the toner particles, and therefore the proportion of the toner having fatty acid metal salt particles on the surface of the toner particles increases, so that the adhesion of the toner to the fixing member is further suppressed.
[0110] The above ratio (DT / DS) is more preferably 2.3 or more and 5.0 or less, and further preferably 2.6 or more and 4.7 or less.
[0111] The amount of the external additive added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.
[0112] -Characteristics of toner- In the toner according to this embodiment, the maximum endothermic peak temperature during the first temperature rise measured by a differential scanning calorimeter (DSC) is preferably 58° C. or more and 75° C. or less. By setting the maximum endothermic peak temperature of the toner to 58° C. or more and 75° C. or less, the low-temperature fixability of the toner is improved.
[0113] The maximum endothermic peak temperature during the first temperature rise of the toner is measured by a differential scanning calorimeter (DSC) as follows. A PerkinElmer DSC-7 differential scanning calorimeter is used, and the melting points of indium and zinc are used to correct the temperature of the detector, and the heat of fusion of indium is used to correct the amount of heat. An aluminum pan is used for the sample, and an empty pan is set as a control, and the temperature is raised from room temperature to 150°C at a rate of 10°C / min. Then, the temperature at which the maximum endothermic peak is obtained in the obtained endothermic curve is determined.
[0114] (Toner manufacturing method) The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles.
[0115] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). There is no particular limitation on these production methods, and any known production method may be used. Among these, it is preferable to obtain the toner particles by the aggregation and coalescence method.
[0116] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, The toner particles are manufactured through a process including a step of preparing a resin particle dispersion in which resin particles to be a binder resin are dispersed (resin particle dispersion preparation process), a step of aggregating the resin particles (or other particles, if necessary) in the resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation process), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, fusing and coalescing the aggregated particles, and forming toner particles (fusion and coalescence process).
[0117] Here, in order to set the net intensity of each of the above elements in the toner particles within the above range, a supply source of each of the above elements may be added during the production process of the toner particles.
[0118] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0119] -Resin particle dispersion preparation process- First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, as well as a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared.
[0120] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.
[0121] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0122] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.
[0123] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0124] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.
[0125] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.
[0126] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.
[0127] -First agglomerated particle formation process- Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.
[0128] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0129] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.
[0130] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, such as oxycarboxylic acid (e.g., tartaric acid, citric acid, gluconic acid, etc.), iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.
[0131] -Second agglomerated particle formation process- After obtaining the aggregated particle dispersion, the aggregated particle dispersion is further mixed with a resin particle dispersion in which resin particles are dispersed, and the aggregated particles are aggregated so that the resin particles are further attached to the surfaces of the aggregated particles, thereby forming second aggregated particles.
[0132] -Fusion / unification process- Next, the second aggregate particle dispersion liquid in which the second aggregate particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregate particles to form toner particles.
[0133] Through the above steps, toner particles are obtained.
[0134] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.
[0135] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0136] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer containing only the toner according to the present embodiment, or may be a two-component developer in which the toner is mixed with a carrier.
[0137] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0138] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.
[0139] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.
[0140] Here, the method of coating the surface of the core material with the coating resin includes a method of coating with a solution for forming a coating layer in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent, etc. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.
[0141] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.
[0142] <Image forming device / image forming method> An image forming apparatus / image forming method according to this embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.
[0143] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.
[0144] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is then secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder before charging after the transfer of the toner image; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it before charging after the transfer of the toner image. In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.
[0145] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including a developing means that contains the electrostatic image developer according to the present embodiment is preferably used.
[0146] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0147] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K (image forming means) that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.
[0148] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices (developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.
[0149] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.
[0150] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer means) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning means) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).
[0151] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.
[0152] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.
[0153] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.
[0154] When the yellow toner image on the photoreceptor 1Y is transported to the primary transfer, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoreceptor 1Y toward the primary transfer roll 5Y acts on the toner image, and the toner image on the photoreceptor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.
[0155] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of the respective colors are transferred in a superimposed manner.
[0156] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.
[0157] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P, forming a fixed image.
[0158] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, etc. are preferably used.
[0159] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.
[0160] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus.
[0161] In addition, the process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing device and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.
[0162] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.
[0163] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming means), 112 denotes a transfer device (an example of a transfer means), 115 denotes a fixing device (an example of a fixing means), and 300 denotes recording paper (an example of a recording medium).
[0164] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus.
[0165] 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8M, 8C, and 8K can be attached and detached, and the developing devices 4Y, 4M, 4C, and 4K are connected to the toner cartridges corresponding to the respective developing devices (colors) through toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. EXAMPLES
[0166] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass. Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are based on mass.
[0167] (Synthesis of amorphous polyester resin (A)) Terephthalic acid: 68 parts Fumaric acid: 32 parts Ethylene glycol: 42 parts 1,5-Pentanediol: 47 parts The above materials were placed in a flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under a nitrogen gas flow, and 1 part of titanium tetraethoxide was added for a total of 100 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (A) with a weight average molecular weight of 97,000 and a glass transition temperature of 60°C was obtained.
[0168] (Preparation of amorphous polyester resin particle dispersion (A1)) In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of amorphous polyester resin (A) were gradually added and dissolved, and 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped into the mixed liquid while stirring, to perform emulsification. After the dropwise addition, the emulsion was returned to 25°C, and a resin particle dispersion in which resin particles with a volume average particle size of 195 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (A1) was obtained.
[0169] (Preparation of Crystalline Polyester Resin Particle Dispersion (B1)) 1,10-Decanedicarboxylic acid: 260 parts 1,6-Hexanediol: 167 parts Dibutyltin oxide (catalyst): 0.3 parts The above materials were placed in a heated and dried three-necked flask, the air in the three-necked flask was replaced with nitrogen gas to create an inert atmosphere, and the mixture was stirred and refluxed at 180°C for 5 hours by mechanical stirring. Next, the temperature was gradually raised to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Thus, a crystalline polyester resin with a weight average molecular weight of 12500 and a melting temperature of 73°C was obtained. 90 parts of the crystalline polyester resin, 1.8 parts of anionic surfactant (TaycaPower, manufactured by Tayca Co., Ltd., solid content 12%, sodium dodecylbenzenesulfonate) and 210 parts of ion-exchanged water were mixed, heated to 120°C, and dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA Co., Ltd.), and then dispersed for 1 hour using a pressure discharge type Gaulin homogenizer to obtain a resin particle dispersion in which resin particles with a volume average particle size of 195 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, thereby obtaining a crystalline polyester resin particle dispersion (B1).
[0170] (Preparation of styrene acrylic resin particle dispersion (S1)) Styrene: 375 parts n-Butyl acrylate: 25 parts Acrylic acid: 2 parts Dodecanethiol: 24 parts Carbon tetrabromide: 4 parts The mixture obtained by mixing and dissolving the above materials was dispersed and emulsified in a flask in a surfactant solution in which 6 parts of a nonionic surfactant (manufactured by Sanyo Chemical Industries, Nonipol 400) and 10 parts of an anionic surfactant (manufactured by TaycaPower, Tayca Co., Ltd., solid content 12%, sodium dodecylbenzenesulfonate) were dissolved in 550 parts of ion-exchanged water. Next, an aqueous solution in which 4 parts of ammonium persulfate were dissolved in 50 parts of ion-exchanged water was added over a period of 20 minutes while stirring the flask. Next, after nitrogen replacement, the flask was heated in an oil bath while stirring the contents until the temperature reached 70°C, and the emulsion polymerization was continued by maintaining the temperature at 70°C for 5 hours. In this way, a resin particle dispersion in which resin particles having a volume average particle size of 150 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a styrene acrylic resin particle dispersion (S1) was obtained.
[0171] (Preparation of colorant particle dispersion (Ku1)) Carbon black (Cabot, Regal 330): 50 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation) 5 parts Ion-exchanged water: 193 parts The above materials were mixed and dispersed for 10 minutes at 240 MPa using an Ultimizer (manufactured by Sugino Machine Co., Ltd.), and ion-exchanged water was added to obtain a colorant particle dispersion (Ku1) with a solid content of 20%.
[0172] (Preparation of release agent particle dispersion (W1)) Ester wax (Nippon Oil & Fats Co., Ltd., WEP-8, melting temperature 79°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 1000 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W1).
[0173] (Preparation of release agent particle dispersion (W2)) Ester wax (Nippon Oil & Fats Co., Ltd., WEP-5, melting temperature 82°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 220 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W2).
[0174] (Preparation of release agent particle dispersion (W3)) Ester wax (Nippon Oil & Fats Co., Ltd., WEP-8, melting temperature 79°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 2000 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W3).
[0175] (Preparation of release agent particle dispersion (W4)) Ester wax (Nippon Oil & Fats Co., Ltd., WEP-8, melting temperature 79°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 500 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, to obtain release agent particle dispersion (W3).
[0176] (Preparation of release agent particle dispersion (W5)) Ester wax (Nippon Oil & Fats Co., Ltd., WEP-5, melting temperature 82°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 100 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W5).
[0177] <Example 1> [Preparation of toner particles] (Preparation of toner particles (K1)) -First agglomerated particle formation process- - Ion-exchanged water: 200 parts Colorant particle dispersion (Ku1): 15 parts Release agent particle dispersion (W1): 10 parts Styrene acrylic resin particle dispersion (S1): 144 parts Crystalline polyester resin particle dispersion (B1): 26 parts Amorphous polyester resin (A): 5 parts The above materials were placed in a round stainless steel flask, and 0.1N (0.1mol / L) nitric acid was added to adjust the pH to 3.5, after which an aqueous magnesium chloride solution in which 6 parts of magnesium chloride were dissolved in 30 parts of ion-exchanged water was added. The materials were dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50), and then heated to 45°C in a heating oil bath and maintained until the volume average particle size reached 4.5μm.
[0178] -Second agglomerated particle formation process- Next, 30 parts of the amorphous polyester resin particle dispersion (A1) and 15 parts of the crystalline polyester resin particle dispersion (B1) were added and held for 30 minutes. These two dispersions were added at 30 minute intervals a total of four times. Next, 40 parts of the amorphous polyester resin particle dispersion (A1) was added, and the pH was adjusted to 9.0 with a 1N aqueous sodium hydroxide solution.
[0179] -Fusion / coalescence process- Next, while continuing stirring, the temperature was increased to 85°C at a rate of 0.05°C / min, and after being held at 85°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min (first cooling). Next, it was heated to 85°C at a rate of 0.2°C / min (reheating), held for 30 minutes, and then cooled to 30°C at a rate of 0.5°C / min (second cooling). Next, the solid content was filtered off, washed with ion-exchanged water, and dried to obtain black toner particles (K1) having a volume average particle size of 4.7 μm.
[0180] [External addition of additives] 100 parts of black toner particles (K1) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with 45 μm openings to obtain black toner (KT1).
[0181] [Creating the carrier] After 500 parts of spherical magnetite powder particles (volume average particle diameter 0.55 μm) were stirred with a Henschel mixer, 5 parts of a titanate-based coupling agent were added, and the mixture was heated to 100 ° C and stirred for 30 minutes. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of magnetite particles treated with a titanate-based coupling agent, 6.25 parts of 25% ammonia water, and 425 parts of water were added to a four-neck flask and stirred, and reacted at 85 ° C for 120 minutes while stirring. Next, the mixture was cooled to 25 ° C, 500 parts of water were added, and the supernatant liquid was removed and the precipitate was washed with water. The washed precipitate was heated and dried under reduced pressure to obtain a carrier (CA) with an average particle size of 35 μm.
[0182] [Mixing toner and carrier] Black toner (KT1) and carrier (CA) were placed in a V blender in a ratio of black toner (KT1):carrier (CA) = 5:95 (mass ratio) and stirred for 20 minutes to obtain black developer (KD1).
[0183] <Example 2> A black toner (KT2) and a black developer (KD2) were obtained in the same manner as in Example 1, except that the release agent particle dispersion (W1) was changed to the release agent particle dispersion (W3).
[0184] <Example 3> A black toner (KT3) and a black developer (KD3) were obtained in the same manner as in Example 1, except that the release agent particle dispersion (W1) was changed to the release agent particle dispersion (W4).
[0185] <Example 4> A black toner (KT4) and a black developer (KD4) were obtained in the same manner as in Example 1, except that the amounts of the amorphous polyester resin particle dispersion (A1) and the crystalline polyester resin particle dispersion (B1), which were added a total of four times in the second aggregate particle formation process, were changed to 3 parts and 1.5 parts, respectively.
[0186] <Example 5> A black toner (KT5) and a black developer (KD5) were obtained in the same manner as in Example 1, except that the amounts of the amorphous polyester resin particle dispersion (A1) and the crystalline polyester resin particle dispersion (B1), which were added a total of four times in the second aggregate particle formation process, were changed to 75 parts and 37.5 parts, respectively.
[0187] <Example 6> A black toner (KT6) and a black developer (KD6) were obtained in the same manner as in Example 1, except that the styrene-acrylic resin particle dispersion (S1) was not added when preparing the toner particles.
[0188] <Example 7> A black toner (KT7) and a black developer (KD7) were obtained in the same manner as in Example 1, except that the amounts of the styrene acrylic resin particle dispersion (S1), the crystalline polyester resin particle dispersion (B1), and the amorphous polyester resin (A) added in the first aggregate particle formation process were changed to 85.8 parts, 26.2 parts, and 63 parts, respectively.
[0189] <Example 8> A black toner (KT8) and a black developer (KD8) were obtained in the same manner as in Example 1, except that the amount of Ku1 added was changed to 7.5 parts.
[0190] <Example 9> A black toner (KT9) and a black developer (KD9) were obtained in the same manner as in Example 1, except that the amount of Ku1 added was changed to 9.4 parts.
[0191] <Example 10> A black toner (KT10) and a black developer (KD10) were obtained in the same manner as in Example 1, except that the amount of Ku1 added was changed to 22.5 parts.
[0192] <Example 11> A black toner (KT11) and a black developer (KD11) were obtained in the same manner as in Example 1, except that the amount of Ku1 added was changed to 24.4 parts.
[0193] <Example 12> A black toner (KT12) and a black developer (KD12) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution of 1.3 parts of sodium chloride, 0.6 parts of magnesium chloride, and 0.7 parts of calcium chloride dissolved in 30 parts of ion-exchanged water.
[0194] <Example 13> A black toner (KT13) and a black developer (KD13) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution of 1.3 parts of sodium chloride, 0.6 parts of magnesium chloride, 0.7 parts of calcium chloride, and 3.3 parts of potassium chloride dissolved in 30 parts of ion-exchanged water.
[0195] <Example 14> A black toner (KT14) and a black developer (KD14) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution of 1.3 parts of sodium chloride, 0.6 parts of magnesium chloride, 0.7 parts of calcium chloride, and 28.2 parts of potassium chloride dissolved in 30 parts of ion-exchanged water.
[0196] <Example 15> A black toner (KT15) and a black developer (KD15) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution of 1.3 parts of sodium chloride, 0.6 parts of magnesium chloride, 0.7 parts of calcium chloride, and 36.5 parts of potassium chloride dissolved in 30 parts of ion-exchanged water.
[0197] <Example 16> A black toner (KT16) and a black developer (KD16) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution in which 4.3 parts of sodium chloride was dissolved in 30 parts of ion-exchanged water.
[0198] <Example 17> A black toner (KT17) and a black developer (KD17) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution in which 6.3 parts of sodium chloride was dissolved in 30 parts of ion-exchanged water.
[0199] <Example 18> A black toner (KT18) and a black developer (KD18) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution in which 18.9 parts of sodium chloride was dissolved in 30 parts of ion-exchanged water.
[0200] <Example 19> A black toner (KT19) and a black developer (KD19) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to a mixed solution in which 19.3 parts of sodium chloride was dissolved in 30 parts of ion-exchanged water.
[0201] <Example 20> A black toner (KT20) and a black developer (KD20) were obtained in the same manner as in Example 1, except that the amount of magnesium chloride added when preparing the aqueous magnesium chloride solution was changed to 22.2 parts.
[0202] <Example 21> A black toner (KT21) and a black developer (KD21) were obtained in the same manner as in Example 1, except that the amount of magnesium chloride added when preparing the aqueous magnesium chloride solution was changed to 3.2 parts.
[0203] <Example 22> A black toner (KT22) and a black developer (KD22) were obtained in the same manner as in Example 1, except that the amount of magnesium chloride added when preparing the aqueous magnesium chloride solution was changed to 9.6 parts.
[0204] <Example 23> A black toner (KT23) and a black developer (KD23) were obtained in the same manner as in Example 1, except that the amount of magnesium chloride added when preparing the aqueous magnesium chloride solution was changed to 9.8 parts.
[0205] <Example 24> A black toner (KT24) and a black developer (KD24) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous calcium chloride solution prepared by dissolving 2.6 parts of calcium chloride in 30 parts of ion-exchanged water.
[0206] <Example 25> A black toner (KT25) and a black developer (KD25) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous calcium chloride solution prepared by dissolving 3.7 parts of calcium chloride in 30 parts of ion-exchanged water.
[0207] <Example 26> A black toner (KT26) and a black developer (KD26) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous calcium chloride solution prepared by dissolving 11.2 parts of calcium chloride in 30 parts of ion-exchanged water.
[0208] <Example 27> A black toner (KT27) and a black developer (KD27) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous calcium chloride solution prepared by dissolving 11.4 parts of calcium chloride in 30 parts of ion-exchanged water.
[0209] <Example 28> A black toner (KT28) and a black developer (KD28) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous potassium chloride solution in which 8.3 parts of potassium chloride were dissolved in 30 parts of ion-exchanged water.
[0210] <Example 29> A black toner (KT29) and a black developer (KD29) were obtained in the same manner as in Example 1, except that the magnesium chloride aqueous solution was changed to an aqueous potassium chloride solution prepared by dissolving 33.2 parts of potassium chloride in 30 parts of ion-exchanged water.
[0211] <Example 30> A black toner (KT30) and a black developer (KD30) were obtained in the same manner as in Example 1, except that fatty acid metal salt particles (F1) (zinc stearate particles (manufactured by NOF Corporation, product name: Zinc Stearate GF-200) were crushed in a mixer to have an average particle size of 2.4 μm) were also added externally together with the hydrophobic silica when the external additives were added.
[0212] <Example 31> A black toner (KT31) and a black developer (KD31) were obtained in the same manner as in Example 1, except that fatty acid metal salt particles (F2) (zinc stearate particles (manufactured by NOF Corporation, product name: Zinc Stearate GF-200) were crushed in a mixer to have an average particle size of 2.3 μm) were also added externally together with the hydrophobic silica when the external additives were added.
[0213] <Example 32> A black toner (KT32) and a black developer (KD32) were obtained in the same manner as in Example 1, except that the retention time in the second aggregate particle formation step was changed to 60 minutes.
[0214] <Example 33> A black toner (KT33) and a black developer (KD33) were obtained in the same manner as in Example 1, except that the retention time in the second aggregate particle formation step was changed to 45 minutes.
[0215] <Example 34> A black toner (KT34) and a black developer (KD34) were obtained in the same manner as in Example 1, except that the retention time in the second aggregate particle formation step was changed to 20 minutes.
[0216] <Example 35> A black toner (KT35) and a black developer (KD35) were obtained in the same manner as in Example 1, except that the retention time in the second aggregate particle formation step was changed to 10 minutes.
[0217] <Comparative Example 1> A black toner (KC1) and a black developer (KC1) were obtained in the same manner as in Example 1, except that the release agent particle dispersion (W1) was changed to the release agent particle dispersion (W2).
[0218] <Comparative Example 2> A black toner (KCT2) and a black developer (KCD2) were obtained in the same manner as in Example 1, except that the release agent dispersion was not added.
[0219] <Comparative Example 3> A black toner (KCT3) and a black developer (KCD3) were obtained in the same manner as in Example 1, except that the release agent particle dispersion (W1) was changed to the release agent particle dispersion (W5).
[0220] <Comparative Example 4> A black toner (KCT4) and a black developer (KCD4) were obtained in the same manner as in Example 1, except that in the first aggregated particle formation process, the retention time was extended until the particle size of the aggregated particles reached 4.7 μm, and in the second aggregated particle formation process, the amorphous polyester resin particle dispersion (A1) and the crystalline polyester resin particle dispersion (B1) were not added, and the pH was adjusted to 9.0 using a 1 N aqueous sodium hydroxide solution.
[0221] <Comparative Example 5> A black toner (KCT5) and a black developer (KCD5) were obtained in the same manner as in Example 1, except that the amounts of the amorphous polyester resin particle dispersion (A1) and the crystalline polyester resin particle dispersion (B1), which were added a total of four times in the second aggregate particle formation process, were changed to 78 parts and 39 parts, respectively.
[0222] [Measurement of net intensity of each element] For the toner particles of each example, the net intensities of the following elements were measured according to the methods described above. The results are shown in Tables 1 and 2. ·Net strength N of alkali metal elements and alkaline earth metal elements A (In the table, "ALKALI(N A ) 」 (denoted as) Net strength of Na element N N (In the table, “Na(N N )" Net strength of Mg element N M (In the table, “Mg(N M )" Net strength of Ca element N C (In the table, “Ca(N C )" ·Net strength N of alkali metal elements and alkaline earth metal elements other than Na, Mg, and Ca A-NMC ((In the table, “ALKALI-(Na+Mg+Ca)(N A-NMC )"
[0223] <Offset evaluation> The developer set of each example was placed in a developing device of a modified DocuCentreColor400 (manufactured by Fuji Xerox Co., Ltd.). Using this modified machine, 10,000 images with an image density of 20% were output on A4 size J paper (manufactured by Fuji Xerox Co., Ltd.) in an environment of 28°C and 85% RH. The 10,000th image was visually confirmed and evaluated for the presence or absence of offset. Evaluation was performed according to the following evaluation criteria. Note that A to C were considered to be within the acceptable range. -Evaluation criteria- A: It cannot be confirmed. B: There is an offset of less than 1% of the image area. C: There is an offset of 1% or more but less than 10% of the image area. D: There is an offset of 10% or more but less than 15% of the image area. E: There is an offset of 15% or more of the image area.
[0224] The abbreviations in the table are as follows. St: styrene acrylic resin ·Cry: Crystalline polyester resin Amo: Amorphous polyester resin
[0225] In the table, "binder resin content (St / Cry / Amo)" indicates the content of styrene acrylic resin, the content of crystalline polyester resin, and the total content of amorphous polyester resin in the core and amorphous polyester resin in the coating layer relative to the entire toner particle. In the table, "Ratio (%) of thickness of coating layer" indicates the ratio of the thickness of the coating layer to the maximum diameter of the toner particle. In the table, the "particle size (μm)" of the toner particles indicates the volume average particle size of the toner particles.
[0226] [Table 1]
[0227] [Table 2]
[0228] From the above results, it is understood that the toner for developing electrostatic images of this embodiment can suppress adhesion of the toner to the fixing member when an image with a low image density is formed. [Explanation of symbols]
[0229] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K Photoconductor cleaning device (an example of a cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 28 Fixing device (an example of fixing means) 30 Intermediate transfer body cleaning device P Recording paper (an example of a recording medium) 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium)
Claims
1. The toner particles are composed of a core containing a binder resin and a release agent having a melting temperature Tm of 80° C. or less, and a coating layer that coats the core and contains an amorphous polyester resin, when a cross section of the toner particle is observed, one to three domains of the release agent having a circle equivalent diameter of 1 μm to 3 μm are present in the core portion, The toner particles have a volume average particle size of 4.2 μm or more and 5.8 μm or less, The toner for developing electrostatic images, wherein when a cross section of the toner particle is observed, the ratio of the thickness of the coating layer to the maximum diameter of the toner particle is 1% or more and 25% or less.
2. 2. The toner for developing electrostatic images according to claim 1, wherein the binder resin comprises a styrene-acrylic resin, a crystalline polyester resin and an amorphous polyester resin.
3. the content of the styrene-acrylic resin relative to the total amount of the toner particles is 50% by mass or more and 90% by mass or less, the content of the crystalline polyester resin relative to the total amount of the toner particles is 9.5% by mass or more and 40% by mass or less, 3. The toner for developing electrostatic images according to claim 2, wherein the total content of the amorphous polyester resin of the core and the amorphous polyester resin of the coating layer is 0.5% by mass or more and 5% by mass or less with respect to the entire toner particles.
4. the toner particles contain a colorant; 4. The toner for developing electrostatic images according to claim 1, wherein the content of the colorant in the entire toner particles is from 5% by mass to 12% by mass.
5. The net strength N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by fluorescent X-ray analysis A 5. The toner for developing electrostatic images according to claim 1, wherein the viscosity is from 0.10 kcps to 0.40 kcps.
6. The net strength N A is the net intensity N of Na element measured by X-ray fluorescence analysis. N , Net strength of Mg element N M , or the net strength of Ca element N C 6. The toner for developing electrostatic images according to claim 5, wherein
7. The net strength N A is the net intensity N of Mg element measured by X-ray fluorescence analysis. M 6. The toner for developing electrostatic images according to claim 5, wherein
8. The present invention has an external additive containing fatty acid metal salt particles, The toner for developing electrostatic images according to any one of claims 1 to 7, wherein a ratio (DT / DS) of a volume average particle diameter DT of the toner particles to a volume average particle diameter DS of the fatty acid metal salt particles is 1.9 or more.
9. The toner for developing electrostatic images according to any one of claims 1 to 8, wherein the toner particles have a smaller diameter volume particle size distribution index (lower GSDv) of 1.15 or more and 1.30 or less.
10. 10. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1.
11. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 9 and is detachably mountable to an image forming apparatus.
12. 11. A process cartridge detachably mounted to an image forming apparatus, comprising: a developing unit that contains the electrostatic image developer according to claim 10 and develops an electrostatic image formed on a surface of an image carrier by the electrostatic image developer into a toner image.
13. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 10 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:
Citation Information
Patent Citations
Electrostatic charge image developing toner
JP2003084478A
Electrostatic latent image developing toner and its manufacturing method, electrostatic latent image developer and image forming method
JP2004287185A
Toner for electrostatic latent image development, electrostatic latent image developer, toner cartridge, process cartridge, and image forming apparatus
JP2010054674A
Electrostatic charge image developing toner, method for producing the same, electrostatic charge image developer and image forming method
JP2011149986A
Toner for electrostatic charge image development and manufacturing method of the same
JP2015004721A