LAMINATE AND METHOD FOR MANUFACTURING LAMINATE
The laminate structure with controlled cracks and voids in the colloidal crystal layer, combined with a resin layer, addresses the challenge of achieving both color development and adhesion, enhancing the laminate's durability and color retention.
Patent Information
- Application Number
- JP2022200986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Conventional colloidal crystals face challenges in achieving both excellent color development and adhesion due to the presence of voids between particles or between particles and substrates, leading to poor abrasion resistance and loss of color.
A laminate structure comprising a base material, a colloidal crystal layer with controlled cracks and voids, and a resin layer in contact within the cracks, utilizing core-shell type resin particles for improved adhesion.
The laminate achieves both vivid color development and enhanced adhesion by leveraging cracks and voids in the colloidal crystal layer, ensuring the resin layer contacts within these features for improved bonding.
Smart Images

Figure 0007578130000007 
Figure 0007578130000008 
Figure 0007578130000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having a colloidal crystal layer and a method for producing the laminate, and more particularly to a laminate having a colloidal crystal layer that is excellent in color development and adhesion, and a method for producing the laminate. [Background technology]
[0002] Photonic crystals are nano-periodic structures in which materials with different refractive indices are arranged at intervals equivalent to the wavelength of light. Photonic crystals are currently the subject of active research because the refractive index changes periodically within them, resulting in a variety of interesting optical properties, such as the reflection of light of a specific wavelength known as Bragg reflection, light trapping using photonic bandgaps, and high demultiplexing properties. Colloidal crystals, a type of photonic crystal, have a structure in which submicron-order resin particles or silica particles are regularly arranged, and can be formed by applying a particle suspension to a substrate, etc., and then drying it. Colloidal crystals have a structure in which particles are regularly packed closely together, and the structural color is expressed by Bragg reflection caused by the refractive index difference between the particles and the gaps between the particles. The greater the refractive index difference between the particles and the gaps between the particles, the stronger the Bragg reflection. Therefore, except for inverse opal colloidal crystals, the best coloring is obtained when the gaps between the particles are air. However, such colloidal crystals with excellent coloring have poor abrasion resistance and substrate adhesion due to the presence of gaps between the particles or between the particles and the substrate. Furthermore, there was a problem that the coloring of the colloidal crystals was easily lost when the gaps between the particles were filled, because the refractive index difference became small.
[0003] Patent Documents 1 and 2 disclose compositions for colloidal crystals that contain core-shell type microparticles consisting of a core and a shell. Because the glass transition point of the core is high and the glass transition point of the shell is low, the shell flows when heated, resulting in a colloidal crystal in which the core is regularly arranged in the shell. In addition, the shell easily flows when heated, so that the shell adheres to the substrate and polymer chains become entangled between the particles, resulting in a colloidal crystal with excellent abrasion resistance and substrate adhesion.
[0004] Patent Document 3 discloses a colloidal crystal laminate having cracks. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-047231 A [Patent Document 2] JP 2009-249527 A [Patent Document 3] JP 2006-208453 A
[0006] However, the colloidal crystals of Patent Documents 1 and 2 are designed so that the shell portion completely fills the gaps between particles in the core portion, which reduces the difference in refractive index between the particles and the gaps between them, resulting in a problem that the colloidal crystals formed do not have excellent color development properties.
[0007] Furthermore, the colloidal crystals of Patent Document 3 are essentially just particles arranged on a substrate, and have the problem of poor adhesion. As described above, it has been difficult for conventional laminates including colloidal crystals to achieve both color development and adhesion. Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, an object of the present invention is to provide a laminate including colloidal crystals that exhibit both color development and adhesion. [Means for solving the problem]
[0009] That is, the present invention relates to a laminate comprising a substrate, a colloidal crystal layer that develops color through the interference of light, and a resin layer, arranged in that order, and which satisfies the following conditions (1) to (4). (1) Cracks are formed in the colloidal crystal layer (2) The area ratio of the cracks in the colloidal crystal layer is 0.1 to 30%. (3) There are voids between the particles that make up the colloidal crystal layer. (4) The colloidal crystal layer and the resin layer are in contact inside the crack.
[0010] The present invention also relates to the above laminate, which further comprises a primer layer between the substrate and the colloidal crystal layer.
[0011] The present invention also relates to the above laminate, wherein the particles constituting the colloidal crystal layer are core-shell type resin fine particles.
[0012] The present invention also relates to a method for producing the above laminate, which comprises the following steps 1 to 3, and further comprises step 3 during or after step 1. (Step 1) Forming a colloidal crystal layer on a substrate (Step 2) A step of forming a resin layer on the colloidal crystal layer formed in step 1. (Step 3) Heating to 70℃ or higher Effect of the Invention
[0013] According to the present invention, it is possible to provide a laminate including a colloidal crystal layer that exhibits both color development and adhesion. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic cross-sectional view of a laminate of the present invention. [Diagram 2]1 is a SEM photograph of a crack according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Laminate> The laminate of the present invention is a laminate comprising a base material, a colloidal crystal layer that develops color due to the interference of light, and a resin layer, arranged in that order, and is characterized in that it satisfies all of the following conditions (1) to (4): (1) Cracks are formed in the colloidal crystal layer (2) The area ratio of the cracks in the colloidal crystal layer is 0.1 to 30%. (3) There are voids between the particles that make up the colloidal crystal layer. (4) The colloidal crystal layer and the resin layer are in contact inside the crack.
[0016] The laminate of the present invention exhibits excellent adhesion because the resin layer is partially formed perpendicular to the film surface of the laminate due to the formation of cracks in the colloidal crystal layer. In addition, the surface area ratio of the cracks is a predetermined ratio, so that both the adhesion and color development of the laminate are good. In addition, the color development of the laminate is excellent because the gaps between the particles constituting the colloidal crystal are maintained. In addition, the contact between the colloidal crystal layer and the resin layer inside the cracks improves the adhesion between the colloidal crystal layer and the resin layer, improving the adhesion of the laminate. The elements constituting the present invention will now be described in detail.
[0017] <Colloidal crystal layer> As shown in Figures 1 and 2, the colloidal crystal layer has a densely packed structure in which fine particles are regularly arranged, with gaps existing between the particles. In addition, cracks exist between the crystal domains. The laminate of the present invention exhibits vivid structural colors due to Bragg reflection caused by the difference in refractive index between the densely packed particles and the air existing between the particles. The colloidal crystal layer can be formed by applying a composition for colloidal crystals containing fine particles (A) and water, which will be described later, onto a substrate.
[0018] <Crack> The colloidal crystal layer has cracks. In the present invention, cracks refer to minute gaps present in the colloidal crystal layer, and include those that do not penetrate the colloidal crystal layer in the thickness direction and those that penetrate the colloidal crystal layer. The width of the crack is preferably 500 nm or more, and more preferably 1 μm or more. Here, the width of the crack is measured in the horizontal direction on the surface where the colloidal crystal layer contacts the resin layer. The depth of the crack is preferably 25% or more, and more preferably 50% or more, of the thickness of the colloidal crystal layer, where the depth of the crack is measured in a cross section perpendicular to the surface of the laminate in a direction horizontal to the cross section.
[0019] It is important that the area ratio of the cracks is 0.1 to 30%. The area ratio is preferably 1 to 20%. When the area ratio of the cracks is 0.1% or more, the contact between the resin layer and the colloidal crystal layer inside the cracks increases, and the adhesion of the laminate becomes good. In addition, when the area ratio of the cracks is 30% or less, the laminate has excellent color development properties.
[0020] Here, the crack area ratio refers to the ratio of the total crack area contained in any 200 μm × 300 μm area expressed as a percentage. In the present invention, the surface of the laminate was observed with an optical microscope, and the ratio of the total crack area contained in a 200 μm × 300 μm area was expressed as a percentage using image analysis software WinROOF manufactured by Mitani Shoji Co., Ltd. The colloidal crystals are formed as the solvent dries, and the width of the cracks can be controlled by the drying conditions, the type of solvent, the particle size of the particles that form the colloidal crystals, and the like.
[0021] <Void> It is important that the colloidal crystal layer has voids between the particles that make up the colloidal crystal layer. Here, the voids refer to the gaps between particles that contain air. The presence of air in the gaps between particles increases the difference in refractive index between the particles and the gaps between the particles, resulting in good color development of the laminate. In the present invention, the voids and cracks between particles are different in size. When voids with a mode pore size of 10 to 200 nm are detected in the colloidal crystal layer by the nitrogen adsorption method, it can be determined that the voids between particles in the colloidal crystal layer are air. The mode pore size can be determined by the peak top of the nitrogen adsorption isotherm on the adsorption side obtained by analysis based on the Barrett-Joyner-Halenda method (BJH method). In the BJH method, the standard t curve is calculated using the Harkins-Jura type equation and analyzed based on the volume frequency distribution. In the present invention, the measurement was performed using an apparatus named BELSORP-maxII manufactured by Microtrack Bell Co., Ltd.
[0022] <Fine particles (A)> Examples of the fine particles (A) that constitute the colloidal crystal layer include resin fine particles made of a polymer of an ethylenically unsaturated monomer and inorganic fine particles such as silica or titanium dioxide. Resin fine particles are preferred because they can easily introduce reactive groups that can form crosslinks between adjacent particles in the colloidal crystal layer or between the colloidal crystal layer and a resin layer or substrate that is adjacent to the colloidal crystal layer, and more preferably resin fine particles made of an acrylic resin or a styrene-acrylic resin. Moreover, the resin microparticles preferably have a core-shell structure including a core (inner layer) and a shell (outer layer) structure in which the core and shell are water-insoluble polymers and are incompatible with each other. The core functions to maintain the spherical shape, and the shell has fluidity and functions as a binding site. By applying a composition containing core-shell type resin microparticles (hereinafter also referred to as a composition for colloidal crystal layer) to a substrate, and forming a colloidal crystal layer in which the core-shell type resin microparticles are advected and accumulated to be regularly arranged, the shells of adjacent core-shell type resin microparticles and the shells of the core-shell type resin microparticles and the substrate layer are easily bound to each other, and the laminate exhibits excellent adhesion. When the resin fine particles constituting the colloidal crystal layer are made of a polymer of an ethylenically unsaturated monomer, the target resin can be obtained by emulsion polymerization of the ethylenically unsaturated monomer.
[0023] <Ethylenically unsaturated monomer> Examples of the ethylenically unsaturated monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, vinylnaphthalene, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxytetraethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenyl(meth)acrylate, aromatic ethylenically unsaturated compounds such as acrylate; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, thiazolinone, tetrahydrofuran ... linear or branched alkyl group-containing ethylenically unsaturated monomers such as tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; Alicyclic alkyl group-containing ethylenically unsaturated monomers such as adamantyl (meth)acrylate; fluorinated alkyl group-containing ethylenically unsaturated monomers such as trifluoroethyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate; carboxy group-containing ethylenically unsaturated monomers such as (anhydrous) maleic acid, fumaric acid, itaconic acid, citraconic acid, or alkyl or alkenyl monoesters thereof, succinic acid β-(meth)acryloxyethyl monoester, acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, etc.Sulfo group-containing ethylenically unsaturated monomers such as 2-acrylamido 2-methylpropanesulfonate sodium, methallylsulfonic acid, methallylsulfonic acid, sodium methallylsulfonate, allylsulfonic acid, sodium allylsulfonate, ammonium allylsulfonate, and vinylsulfonic acid; (meth)acrylamide, N-methoxymethyl-(meth)acrylamide, N-ethoxymethyl-(meth)acrylamide, N-propoxymethyl-(meth)acrylamide, N-butoxymethyl-(meth)acrylamide, N-pentoxymethyl-(meth)acrylamide, N,N-di(methoxymethyl)acrylamide, N-ethoxymethyl-N-methoxymethylmethacrylamide, N,N-di(ethoxymethyl)acrylamide, N-ethoxymethyl-N-propoxymethylmethacrylamide, N,N-di(propoxymethyl)acrylamide, N-butoxymethyl-N-(propoxymethyl)methacrylamide, N,N-di(butoxymethyl)acrylamide, ethylenically unsaturated monomers containing an amide group, such as N-butyl-N-(methoxymethyl)acrylamide, N,N-di(pentoxymethyl)acrylamide, N-methoxymethyl-N-(pentoxymethyl)methacrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylaminopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and diacetone acrylamide; ethylenically unsaturated monomers containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 1-ethynyl-1-cyclohexanol, and allyl alcohol; ethylenically unsaturated monomers containing a polyoxyethylene group, such as methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; Amino group-containing ethylenically unsaturated monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, and diethylaminostyrene; epoxy group-containing ethylenically unsaturated monomers such as glycidyl (meth)acrylate and 3,4-epoxycyclohexyl (meth)acrylate; diacetone (meth)acrylamide, acetoacetoxy (meth)acrylate, and 2-acetoacetoxyethyl (meth)acrylate. ethylenically unsaturated monomers containing a ketone group, such as allyl (meth)acrylate, 1-methylallyl (meth)acrylate, 2-methylallyl (meth)acrylate, 1-butenyl (meth)acrylate, 2-butenyl (meth)acrylate, 3-butenyl (meth)acrylate, 1,3-methyl-3-butenyl (meth)acrylate, 2-chloroallyl (meth)acrylate, 3-chloroallyl (meth)acrylate, o-allylphenyl (meth)acrylate, 2-(allyloxy)ethyl (meth)acrylate, acrylate, allyl lactyl (meth)acrylate, citronellyl (meth)acrylate, geranyl (meth)acrylate, rosinyl (meth)acrylate, cinnamyl (meth)acrylate, diallyl maleate, diaryl itaconic acid, vinyl (meth)acrylate, vinyl crotonate, vinyl oleate, vinyl linoleate, 2-(2'-vinyloxyethoxy)ethyl (meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol (meth)acrylate, tetraethylene glycol Ethylenically unsaturated monomers having two or more ethylenically unsaturated groups, such as cholesteryl (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, 1,1,1-trishydroxymethylethane diacrylate, 1,1,1-trishydroxymethylethane triacrylate, 1,1,1-trishydroxymethylpropane triacrylate, divinylbenzene, divinyl adipate, diallyl isophthalate, diallyl phthalate, and diallyl maleate;Examples of the ethylenically unsaturated monomers include alkoxysilyl groups, such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltributoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropyltriethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-methacryloxymethyltrimethoxysilane, γ-acryloxymethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltributoxysilane, and vinylmethyldimethoxysilane; and ethylenically unsaturated monomers containing methylol groups, such as N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide, and alkyl etherified N-methylol(meth)acrylamide. These monomers may be used alone or in combination of two or more.
[0024] <Average particle size> The average particle size of the fine particles (A) is preferably in the range of 100 to 500 nm. The average particle size in the present invention can be measured by a dynamic light scattering method, and the peak of the obtained volume particle size distribution data (histogram) is taken as the average particle size. The coefficient of variation (Cv value) of the average particle size of the fine particles (A) is preferably 30% or less, more preferably 20% or less. When the coefficient of variation is 30% or less, the regularity of the particle arrangement is improved, and the color development of the laminate is improved. The coefficient of variation is a value that indicates the uniformity of the particle size, and can be calculated by the following formula. Formula: Coefficient of variation Cv value (%) = standard deviation of particle size / average particle size x 100 [In the formula, the units of standard deviation and average particle size are the same]
[0025] <Reactive group> The fine particles (A) preferably have reactive groups that form crosslinks with the resin layer or primer layer described below. The reactive groups in the fine particles (A) enable crosslinking between the colloidal crystal layer and the resin layer, or between the colloidal crystal layer and the primer layer, thereby further improving the adhesion of the laminate. Examples of reactive groups that can be introduced into the fine particles (A) include epoxy groups, carboxy groups, hydroxyl groups, ketone groups, and hydrazide groups, and more preferably ketone groups. In particular, when the reactive group is a ketone group and the crosslinking agent is a hydrazide crosslinking agent, ketone-hydrazide crosslinking can be formed. Ketone-hydrazide crosslinking is preferably used because it does not adversely affect the physical properties of colloidal crystals and can form crosslinks at low temperatures and in a short time by volatilization of water, and is effective when using a film substrate that is easily damaged by heating. In addition, since ketone groups are highly hydrophilic, when an ethylenically unsaturated monomer having a ketone group is used in the copolymerization composition, it is considered that the ketone group is introduced to the outside of the resin fine particles, i.e., near the interface with the aqueous medium, and can efficiently form crosslinks with the hydrazide crosslinking agent.
[0026] When the fine particles (A) have a reactive group, the content of the reactive group is preferably in the range of 0.1 to 3.0 mmol / g, more preferably 0.5 to 3.0 mmol / g, based on the mass of the resin fine particles in the case of a single particle. In addition, in the case of a core-shell type particle, it is preferably in the range of 0.1 to 3.0 mmol / g, more preferably 0.5 to 3.0 mmol / g, based on the mass of the shell. By being 0.1 mmol / g or more, excellent adhesion is expressed by crosslinking even in a laminate having a small contact area between particles or between a particle and a substrate. In addition, by being 3.0 mmol / g or less, the affinity between the colloidal crystal layer and the resin layer is improved, and the adhesion of the laminate is excellent.
[0027] The colloidal crystal layer may contain a black coloring material. The black coloring material absorbs scattered light within the laminate to make the coloring clearer. As the black coloring material, black-colored particles, carbon black, graphite, etc. can be used. Carbon black is preferred from the viewpoints of having little effect on the reflection spectrum shape in the visible region and excellent durability such as weather resistance.
[0028] <Resin layer> The resin layer is provided on the colloidal crystal layer for the purpose of improving the adhesion of the colloidal crystal layer, and it is important that the resin layer is in contact with the colloidal crystal layer inside the cracks of the colloidal crystal layer. When the colloidal crystal layer and the resin layer are in contact inside the cracks, the resin layer partially forms a coating film in the direction perpendicular to the film surface of the laminate, and the laminate exhibits excellent adhesion. In addition, it is preferable that the primer layer described below and the resin layer are in contact inside the cracks of the colloidal crystal layer, since this further improves the adhesion of the laminate. The resin layer can be formed, for example, by applying a resin composition containing water and resin fine particles (B) onto the colloidal crystal layer and drying it as necessary to form a film. Alternatively, the resin layer can be formed by applying a dry laminating resin composition to a substrate, drying it, and then pressing and laminating it onto a laminate having a colloidal crystal layer.
[0029] <Resin fine particles (B)> The resin fine particles (B) are preferably present in the form of an aqueous dispersion in the resin composition for forming the resin layer. The resin fine particles (B) are preferably a polymer of an ethylenically unsaturated monomer, and more preferably an acrylic resin or a styrene-acrylic resin.
[0030] <Ethylenically unsaturated monomer> As the ethylenically unsaturated monomer usable in the resin fine particles (B), the description of the ethylenically unsaturated monomer exemplified in the fine particles (A) can be cited.
[0031] <Reactive group> The resin fine particles (B) preferably have reactive groups that form crosslinks with the colloidal crystal layer or the primer layer described below. The reactive groups in the resin fine particles (B) enable crosslinks to be formed between the colloidal crystal layer and the resin layer, or between the resin layer and the primer layer, thereby further improving the adhesion of the laminate. Examples of reactive groups that can be introduced into the resin particles (B) include epoxy groups, carboxy groups, hydroxyl groups, ketone groups, and hydrazide groups, and more preferably ketone groups. In particular, when the reactive group is a ketone group and the crosslinking agent is a hydrazide crosslinking agent, ketone-hydrazide crosslinking can be formed. Ketone-hydrazide crosslinking is preferably used because it does not adversely affect the physical properties of colloidal crystals and can form crosslinks at low temperatures and in a short time by volatilization of water, and is effective when using a film substrate that is easily damaged by heating. In addition, since ketone groups are highly hydrophilic, when an ethylenically unsaturated monomer having a ketone group is used in the copolymerization composition, it is considered that the ketone group is introduced to the outside of the resin particles, i.e., near the interface with the aqueous medium, and can efficiently form crosslinks with the hydrazide crosslinking agent.
[0032] When the resin fine particles (B) have reactive groups, the content of the reactive groups is preferably in the range of 0.1 to 3.0 mmol / g, more preferably 0.5 to 3.0 mmol / g, based on the mass of the resin fine particles. By being 0.1 mmol / g or more, excellent adhesion is exhibited by crosslinking even in a laminate having a small contact area between particles or between a particle and a substrate. Also, by being 3.0 mmol / g or less, the affinity between the colloidal crystal layer and the resin layer is improved, improving the adhesion of the laminate.
[0033] <Average particle size> The average particle size of the resin fine particles (B) is preferably in the range of 80 to 1000 nm. If the average particle size is 80 nm or more, the components of the resin layer do not penetrate into the gaps between the particles of the colloidal crystal layer, but penetrate only into the cracks of the colloidal crystal layer, so that both the color development and the adhesion of the laminate are good. If the average particle size is 1000 nm or less, the resin layer penetrates into the cracks, so that the adhesion of the laminate is good.
[0034] <Glass transition temperature> The glass transition point (Tg) of the resin fine particles (B) is preferably in the range of -25 to 45°C, more preferably in the range of -10 to 30°C. If the Tg is -25°C or higher, the resin component of the resin layer can be prevented from flowing excessively and penetrating into the gaps between the particles of the colloidal crystal layer, resulting in excellent color development of the laminate. On the other hand, if the Tg is 45°C or lower, the film-forming properties of the resin fine particles (B) are sufficiently ensured, so that the color development of the laminate is good after drying of the resin layer composition, and the binding property of the resin layer to the colloidal crystal layer is improved, resulting in improved adhesion of the laminate. The above glass transition point can be determined by using a DSC (differential scanning calorimeter).
[0035] <Base material layer> The substrate is not particularly limited and can be appropriately selected depending on the application. Examples of the substrate include thermoplastic resin substrates such as polyvinyl chloride sheet, polyethylene terephthalate (PET) film, polypropylene film, polyethylene film, nylon film, polystyrene film, and polyvinyl alcohol film; metal substrates such as aluminum foil; glass substrates, paper substrates such as coated paper; and cloth substrates. The substrate may have a smooth or uneven coating surface. The substrate may be transparent, semi-transparent, or opaque, and a substrate that has been pre-colored, for example, black, may be used to make the color of the colloidal crystal layer more distinct. These substrates may be used alone or as a laminate consisting of two or more layers. The thickness of the substrate is not particularly limited and can usually be appropriately selected within the range of 5 to 500 μm.
[0036] <Primer layer> In order to further improve the fixation of the colloidal crystal layer on the substrate, it is preferable that the substrate has a primer layer. The primer layer can be formed by applying a primer layer resin composition onto the substrate before forming the colloidal crystal layer. The primer layer resin composition contains a resin component, and the resin forming the primer layer is not particularly limited, and examples thereof include acrylic resin, styrene acrylic resin, urethane resin, olefin resin, polyester resin, and composite resins obtained by compounding these resins. These resins may be used alone or in combination of two or more. From the viewpoints of adhesion to the substrate and colloidal crystal layer, resistance of the primer layer, etc., the primer layer preferably contains an acrylic resin, a styrene acrylic resin, or a urethane resin. The primer layer may also contain additives within a range that does not impair the effects of the present invention. Examples of such additives include ultraviolet absorbers, surfactants, and black coloring materials. The thickness of the primer layer is preferably 0.5 to 30 μm.
[0037] <Reactive group> The resin forming the primer layer preferably has a reactive group that forms a crosslink with the colloidal crystal layer or the resin layer. When the resin forming the primer layer has a reactive group, crosslinking can be formed between the primer layer and the colloidal crystal layer or between the primer layer and the resin layer, and the adhesion of the laminate is further improved. Examples of reactive groups that can be introduced into the resin forming the primer layer include epoxy groups, carboxy groups, hydroxyl groups, ketone groups, and hydrazide groups, and more preferably ketone groups. In particular, when the reactive group is a ketone group and the crosslinking agent is a hydrazide crosslinking agent, ketone-hydrazide crosslinking can be formed. Ketone-hydrazide crosslinking is preferably used because it does not adversely affect the physical properties of colloidal crystals and can form crosslinks at low temperatures and in a short time by volatilization of water, and is effective when using a film substrate that is easily damaged by heating. In addition, since ketone groups are highly hydrophilic, when an ethylenically unsaturated monomer having a ketone group is used in the copolymerization composition, it is considered that the ketone group is introduced to the outside of the resin fine particles, i.e., near the interface with the aqueous medium, and can efficiently form crosslinks with the hydrazide crosslinking agent.
[0038] When the primer layer has a reactive group, the content of the reactive group is preferably in the range of 0.1 to 3.0 mmol / g, more preferably 0.5 to 3.0 mmol / g, based on the mass of the primer layer. By being 0.1 mmol / g or more, excellent adhesion is exhibited by crosslinking even in a laminate having a small contact area between particles or between a particle and a substrate. Also, by being 3.0 mmol / g or less, the affinity between the primer layer and the colloidal crystal layer is improved, improving the adhesion of the laminate.
[0039] <Method of manufacturing laminate> The method for producing the laminate of the present invention preferably includes the following steps 1 and 2. Step 1) A step of applying a composition for colloidal crystals onto a substrate and drying it as necessary to form a colloidal crystal layer. Step 2) A step of applying a resin layer composition onto the colloidal crystal layer formed in step 1, and drying it as necessary, to form a resin layer.
[0040] When the particles that compose the colloidal crystal layer are core-shell type resin fine particles, it is preferable to carry out the following step 3 during or after step 1 and before step 2. Step 3) Heat treatment is carried out at 70° C. or higher, provided that the color development of the colloidal crystals is not impaired. By passing through step 3, the shells of the core-shell type resin particles flow, changing the surface state of the coating film, and the colloidal crystal layer and the resin layer are easily brought into contact with each other inside the cracks when the resin layer is formed, resulting in good adhesion of the laminate. The heating temperature in step 3 is preferably 80°C or higher, more preferably 200°C or lower, and even more preferably 150°C or lower.
[0041] It is important that the colloidal crystal layer has cracks, and that the area ratio of the cracks is 0.1 to 30%. The cracks in the colloidal crystal layer can be controlled by the drying conditions in step 1, the type of solvent in the composition for colloidal crystals, the particle size of the fine particles (A), etc. For example, lowering the drying temperature reduces the crack area ratio in the colloidal crystal layer, while raising the drying temperature increases the crack area ratio. Also, the smaller the particle size of the fine particles (A), the lower the crack area ratio, while the larger the particle size, the higher the crack area ratio. EXAMPLES
[0042] The present invention will be described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0043] <Average particle size, Cv value> The average particle size was measured by diluting the microparticle dispersion 500 times with water, measuring about 5 ml of the diluted solution by dynamic light scattering measurement (measuring device manufactured by Nanotrack UPA Co., Ltd., Microtrack Bell Co., Ltd.), and the peak of the obtained volumetric particle size distribution data (histogram) was taken as the average particle size. The coefficient of variation Cv value, which indicates the uniformity of the particle size, was calculated by the following formula. Formula: Cv value (%) = standard deviation of particle size / average particle size x 100 [In the formula, the units of standard deviation and average particle size are the same]
[0044] <Glass transition temperature> The glass transition point was measured by DSC (differential scanning calorimeter manufactured by TA Instruments Co., Ltd.). Specifically, about 2 mg of a sample obtained by drying the resin fine particle dispersion was weighed on an aluminum pan, the aluminum pan was set in a DSC measurement holder, and the endothermic peak of the baseline shift (inflection point) chart to the endothermic side of the DSC curve obtained under the temperature increase condition of 5° C. / min was read to obtain the glass transition point.
[0045] <Production of fine particles (A)> [Production Example 1] Production of core-shell type resin particles 99.0 parts of styrene, 1.0 parts of acrylic acid, 4.0 parts of 25% aqueous solution of Aqualon AR-10 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., anionic reactive surfactant (polyoxyethylene styrenated phenyl ether sulfate salts) (solid content 1.0 part), and 39.0 parts of ion-exchanged water were mixed and stirred to prepare an emulsion of ethylenically unsaturated monomers in the first stage. 95.0 parts of ion-exchanged water and 1.5% of the emulsion in the first stage were added to a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently substituted with nitrogen, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.15 parts) was added as an initiator to start polymerization. The internal temperature was raised to 80°C and maintained at the same temperature, and the remainder of the emulsion and 4.2 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.11 parts) were added dropwise over 2 hours to react, synthesizing core particles. Next, 27.6 parts of styrene, 13.2 parts of n-butyl acrylate, 2.2 parts of methacrylic acid, 1.7 parts of 25% aqueous solution of Aqualon AR-10 (0.4 parts solids), and 16.7 parts of ion-exchanged water were mixed and stirred to prepare the emulsion of the second stage ethylenically unsaturated monomer. 20 minutes after the completion of the first stage dropwise addition, the dropwise addition of the second stage emulsion was started. While maintaining the internal temperature at 80°C, the reaction was allowed to proceed while dropping the second stage emulsion and 1.6 parts of a 2.5% aqueous solution of potassium persulfate (0.04 parts solids) over a period of 2 hours, to obtain an aqueous dispersion of core-shell type resin particles. After the reaction, water was added to adjust the solid content to 45.0%. 1.7 parts of 25% aqueous ammonia (NH3(aq)) was added to neutralize the core-shell type resin microparticles. The amount of aqueous ammonia blended was equivalent to the amount required to neutralize all carboxy groups contained in the shell (hereinafter, 1 equivalent). The average particle size of the obtained microparticles was 248 nm, the Cv value was 12.9%, the Tg of the core was 100.1°C, and the Tg of the shell was 51.8°C.
[0046] [Production Examples 2 to 7] Production of core-shell type resin microparticles A water dispersion of core-shell type resin microparticles was obtained in the same manner as in Production Example 1, except that the blending composition was changed to that shown in Table 1. The amount of water in the reaction vessel was 67% relative to the total amount of ethylenically unsaturated monomers. The emulsion of ethylenically unsaturated monomers was prepared by adding water so that the concentration of ethylenically unsaturated monomers in the emulsion was 69% and the concentration of surfactant was 0.69%. In the 2.5% aqueous solution of potassium persulfate, the ratios at the start of the reaction / when the first emulsion was added / when the second emulsion was added were the same as in Production Example 1. In addition, 1 equivalent of ammonia water was added to the carboxyl group contained in the shell to neutralize the core-shell type resin microparticles. In Production Examples 6 and 7, the amount of the first-stage emulsion charged into the reaction vessel was changed from 1.5% to 2.0% and 1.0%, respectively.
[0047] [Table 1]
[0048] [Production Example 8] Production of single-structure resin particles 99.0 parts of styrene, 1.0 part of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 1.0 part), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water and 3% of the emulsion were added, the internal temperature was raised to 80°C, and the atmosphere was fully replaced with nitrogen. Then, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl group contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 224 nm, the Cv value was 13.4%, and the Tg was 116.1°C.
[0049] [Production Example 9] Production of single-structure resin particles 85.6 parts of styrene, 12.1 parts of 2-acetoacetoxyethyl methacrylate, 2.3 parts of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 1.0 part), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water and 3% of the emulsion were added, the internal temperature was raised to 80°C, and the atmosphere was fully replaced with nitrogen. Then, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl group contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 230 nm, the Cv value was 12.1%, and the Tg was 102.1°C.
[0050] [Production Example 10] Preparation of silica particles As the silica particles, SeaHostar KE-W20 (average particle size 210 nm) manufactured by Nippon Shokubai Co., Ltd. was used.
[0051] [Production Example 11] Production of core-shell type resin particles In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 400 parts by weight of ion-exchanged water and 0.02 parts by weight of sodium dodecylbenzenesulfonate were charged and heated to 80° C. with stirring. Next, using 0.3 parts by weight of potassium persulfate as an initiator, a mixed liquid of 35 parts by weight of styrene, 10 parts by weight of methyl methacrylate, and 5 parts by weight of divinylbenzene as monomers was dropped over 100 minutes as a polymerizable monomer composition for forming the core portion, and after the completion of the dropping, the mixture was stirred for an additional 30 minutes to obtain core particles. After the stirring, a mixture of 20 parts by weight of methyl methacrylate, 15 parts by weight of n-butyl acrylate, 6 parts by weight of methacrylic acid, 6 parts by weight of hydroxyethyl acrylate, and 3 parts by weight of glycidyl methacrylate, which is a polymerizable monomer composition for forming the shell portion, and 0.2 parts by weight of octyl thioglycolate, a chain transfer agent, was added dropwise over 100 minutes. After the dropping, the mixture was stirred for another 2 hours and cooled to obtain an aqueous dispersion of core-shell type resin particles. After the reaction was completed, the solid content of the aqueous dispersion was adjusted to 20.0% with ion-exchanged water. The average particle size of the obtained microparticles was 220 nm, the Cv value was 12.6%, the Tg of the core was 100.1°C, and the Tg of the shell was 51.8°C.
[0052] <Production of fine particles (B)> [Production Example 12] Production of resin microparticles 40.2 parts of styrene, 57.8 parts of n-butyl acrylate, 2.0 parts of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content 1.0 part), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of an ethylenically unsaturated monomer. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water and 3% of the emulsion were added, the internal temperature was raised to 80°C, and the atmosphere was fully replaced with nitrogen. Then, 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl group contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 225 nm, the Cv value was 13.9%, and the Tg was 7.4°C.
[0053] [Production Examples 13 to 20] Production of resin microparticles An aqueous dispersion of resin fine particles was obtained in the same manner as in Production Example 12, except that the blending composition was changed to that shown in Table 2. The amount of water in the reaction vessel was 67% of the total amount of ethylenically unsaturated monomers. An emulsion of ethylenically unsaturated monomers was prepared by adding water so that the concentration of ethylenically unsaturated monomers in the emulsion was 69% and the concentration of surfactant was 0.69%. In addition, 1 equivalent of ammonia water was added to the carboxyl groups contained in the resin fine particles to neutralize the resin fine particles.
[0054] [Production Example 21] Production of resin microparticles An emulsion of an ethylenically unsaturated monomer was prepared by mixing and stirring 35.7 parts of styrene, 52.3 parts of n-butyl acrylate, 10.0 parts of 2-acetoacetoxyethyl methacrylate, 2.0 parts of methacrylic acid, 4.0 parts of a 25% aqueous solution of Aqualon AR-10 (solid content: 1.0 part), and 40.4 parts of ion-exchanged water. In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser, 68.9 parts of ion-exchanged water, 3% of the emulsion, and 2.0 parts of a 25% aqueous solution of Aqualon AR-10 were added, and the internal temperature was raised to 80°C and sufficiently replaced with nitrogen, after which 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remainder of the emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the reaction was continued for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 1 equivalent of ammonia water was added to the carboxyl groups contained in the resin fine particles to neutralize them, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water. The average particle size of the obtained fine particles was 105 nm, the Cv value was 14.9%, and the Tg was 8.2°C.
[0055] [Table 2]
[0056] [Production Example 22] Production of resin microparticles In a reaction vessel equipped with a stirrer, a thermometer, two dropping funnels, and a reflux condenser, 185.0 parts of water, 42.9 parts of JONCRYL67 (styrene acrylic resin Mw12500, acid value 213mgKOH / g manufactured by BASF) as a polymer emulsifier, and 11.1 parts of 25% ammonia water were charged, and the temperature was raised while stirring to dissolve the polymer emulsifier. After further raising the temperature to 80°C under nitrogen reflux, a mixture of 21.0 parts of styrene, 69.0 parts of n-butyl methacrylate, and 10.0 parts of 2-acetoacetoxyethyl acrylate was dropped from one of the two dropping funnels over 2 hours. From the other, 3.6 parts of a 20% aqueous solution of ammonium persulfate was dropped over 2 hours. After completion of the dropping, the reaction was continued for another 5 hours to obtain an aqueous dispersion of resin fine particles. After completion of the reaction, the solid content of the aqueous dispersion was adjusted to 40.0% with ion-exchanged water. The average particle size of the obtained resin particles was 74 nm, the CV value was 23.1%, and the Tg was -1.3°C.
[0057] [Production Example 23] Production of resin microparticles In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 40.0 parts of water, 50.0 parts of methanol, 3.7 parts of methyl methacrylate, 5.3 parts of n-butyl acrylate, and 1.0 parts of 2-acetoacetoxyethyl methacrylate were charged. The temperature was further raised to 80°C under nitrogen reflux, and 4.2 parts of a 5% aqueous solution of ammonium persulfate were added. The reaction was continued for another 5 hours to obtain an aqueous dispersion of resin particles. After the reaction was completed, the solid content of the aqueous dispersion was adjusted to 10.0% with ion-exchanged water. The average particle size of the obtained resin particles was 766 nm, the CV value was 8.2%, and the Tg was -0.5°C.
[0058] [Production Example 24] Production of resin microparticles In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 20.0 parts of water, 60.0 parts of methanol, 3.7 parts of methyl methacrylate, 5.3 parts of n-butyl acrylate, and 1.0 parts of 2-acetoacetoxyethyl methacrylate were charged. The temperature was further raised to 80°C under nitrogen reflux, and 4.2 parts of a 5% aqueous solution of ammonium persulfate were added. The reaction was continued for another 5 hours to obtain an aqueous dispersion of resin particles. After the reaction was completed, the solid content of the aqueous dispersion was adjusted to 10.0% with ion-exchanged water. The average particle size of the obtained resin particles was 1132 nm, the CV value was 9.9%, and the Tg was -0.5°C.
[0059] <Preparation of Composition for Colloidal Crystals> [Production Example 25] To 100.0 parts of the aqueous dispersion of the core-shell type resin microparticles of Production Example 1, 1.0 part of Surfynol 420 (an acetylene-based nonionic surfactant manufactured by Nisshin Chemical Industry Co., Ltd.) as a surfactant and 2.3 parts of carbon black aqueous dispersion CW-1 (manufactured by Orient Chemical Industry Co., Ltd.) were added and stirred to prepare a composition for colloidal crystals.
[0060] [Examples 26-35] A composition for colloidal crystals was prepared in the same manner as in Production Example 25, except that the blending composition was changed to that shown in Table 3.
[0061] [Table 3]
[0062] <Preparation of Resin Layer Composition> [Manufacturing Example 36] To 100.0 parts of the aqueous dispersion of resin fine particles of Production Example 12, 0.5 parts of Emulgen 1108 (a nonionic surfactant manufactured by Kao Corporation) and 1.0 parts of Surfynol 420 were added as surfactants and stirred to prepare a composition for resin layer.
[0063] [Examples 37-48] A composition for resin layer was prepared in the same manner as in Production Example 36, except that the blending composition was changed to that shown in Table 4.
[0064] [Table 4]
[0065] <Preparation of primer layer composition> The compositions of Production Examples 36 to 40 in the above <Preparation of composition for resin layer> were also used as compositions for primer layer.
[0066] [Example 49] A primer layer composition was prepared by adding 0.5 parts of Emulgen 1108 and 1.0 parts of Surfynol 420 as surfactants to 100.0 parts of Superflex 210 (polyurethane resin) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. and stirring the mixture.
[0067] [Example 50] A primer layer composition was prepared by adding 0.5 parts of Emulgen 1108 and 1.0 parts of Surfynol 420 as surfactants to 100.0 parts of Pluscoat Z-221 (polyester resin) manufactured by GOO Chemical Co., Ltd. and stirring the mixture.
[0068] <Manufacture of Laminate> [Example 1] A colloidal crystal layer composition shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater selected so that the thickness after drying would be 10.0 μm, and then dried at 50° C. for 1 minute to form a colloidal crystal layer. The resulting laminate was then heated at 80° C. for 3 minutes. Next, a resin layer composition shown in Table 5 was applied to the colloidal crystal layer using a bar coater selected so that the thickness after drying would be 10.0 μm, and then dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / colloidal crystal layer / resin layer.
[0069] [Example 2] The primer layer resin composition shown in Table 5 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater so that the thickness after drying was 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, the colloidal crystal layer composition shown in Table 5 was applied to the primer layer with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 50° C. for 1 minute to form a colloidal crystal layer. Furthermore, the obtained laminate was heated at 80° C. for 3 minutes. Next, the resin layer composition shown in Table 5 was applied to the colloidal crystal layer with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer / resin layer.
[0070] [Examples 3 to 31] A laminate was produced in the same manner as in Example 2, except that the combination was changed to that shown in Table 5.
[0071] [Comparative Example 1] The primer layer resin composition shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater so that the thickness after drying was 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, a colloidal crystal layer was formed on the primer layer using the colloidal crystal layer composition shown in Table 6 by the method described in paragraph
[0105] of JP-A 2015-27930. Furthermore, the obtained laminate was heated at 80° C. for 3 minutes. Next, the resin layer composition shown in Table 6 was applied to the colloidal crystal layer using a bar coater selected so that the thickness after drying was 10.0 μm, and then dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer / resin layer.
[0072] [Comparative Example 2] The primer layer resin composition shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater so that the thickness after drying was 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, the colloidal crystal layer composition shown in Table 6 was applied to the primer layer with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 100° C. for 30 seconds to form a colloidal crystal layer. Furthermore, the obtained laminate was heated at 80° C. for 3 minutes. Next, the resin layer composition shown in Table 6 was applied to the colloidal crystal layer with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer / resin layer.
[0073] [Comparative Example 3] The primer layer resin composition shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater so that the thickness after drying was 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, the colloidal crystal layer composition shown in Table 6 was applied with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 120° C. for 30 minutes to form a colloidal crystal layer. Furthermore, the obtained laminate was heated at 80° C. for 3 minutes. Next, the resin layer composition shown in Table 6 was applied on the colloidal crystal layer with a bar coater selected so that the thickness after drying was 10.0 μm, and dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer / resin layer.
[0074] [Comparative Example 4] The primer layer resin composition shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 with a bar coater so that the thickness after drying would be 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, the colloidal crystal layer composition shown in Table 6 was applied to the primer layer with a bar coater selected so that the thickness after drying would be 10.0 μm, and dried at 50° C. for 3 minutes to form a colloidal crystal layer. Next, the resin layer composition shown in Table 6 was applied to the colloidal crystal layer with a bar coater selected so that the thickness after drying would be 10.0 μm, and dried at 80° C. for 1 minute to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer / resin layer.
[0075] [Comparative Example 5] The primer layer resin composition shown in Table 6 was applied to the corona-treated surface of Toyobo Ester Film E5100 using a bar coater so that the thickness after drying would be 3.0 μm, and then dried in an oven at 50° C. for 3 minutes to form a primer layer. Next, the colloidal crystal layer composition shown in Table 6 was applied to the primer layer using a selected bar coater so that the thickness after drying would be 10.0 μm, and then dried at 50° C. for 1 minute to form a colloidal crystal layer. Furthermore, the obtained laminate was heated at 80° C. for 3 minutes to obtain a laminate having a configuration of PET / primer layer / colloidal crystal layer.
[0076] <Evaluation of the laminate> The obtained laminate was evaluated as follows, and the results are shown in Tables 5 and 6.
[0077] <Crack area ratio> The surface of the laminate was observed with an optical microscope, and the ratio of the total area of cracks contained in an area of 200 μm×300 μm was expressed as a percentage using image analysis software WinROOF (Mitani Shoji Co., Ltd.).
[0078] <Contact between colloidal crystal layer and resin layer inside the crack> The cross section of the laminate was observed by SEM to confirm whether or not the colloidal crystal layer and the resin layer were in contact inside the crack.
[0079] <Presence or absence of voids> The presence or absence of voids in the colloidal crystal layer was judged as follows. First, a cross section of the obtained laminate was cut out and analyzed based on the Barrett-Joyner-Halenda method (BJH method), and the peak top of the nitrogen adsorption isotherm on the adsorption side was determined as the most frequent pore size. In the BJH method, the standard t curve was calculated using the Harkins-Jura type equation, and analysis was performed based on the volume frequency distribution. For the measurement, a device named BELSORP-maxII manufactured by Microtrack Bell Co., Ltd. was used. When voids with a mode pore size of 10 to 200 nm were detected by the nitrogen adsorption method, the gaps between the particles forming the colloidal crystal were determined to be air, and the presence of voids was evaluated.
[0080] [Color development] The reflectance spectrum of the laminate was measured in the wavelength range of 350 to 850 nm using an ultraviolet-visible near-infrared spectrophotometer (V-770D manufactured by JASCO Corporation, integrating sphere unit ISN-923). The reflectance at each wavelength is the relative reflectance measured using a standard white board with a known reflectance (SRS-99-010 manufactured by Labsphere) as a reference. The reflectance spectrum was measured from the colloidal crystal layer side for all laminates. For the obtained reflectance spectrum, the difference (ΔR) between the maximum reflectance due to the structural color and the baseline reflectance not due to the structural color was calculated. The larger the ΔR, the better the color development. The obtained ΔR was evaluated according to the following criteria. S: ΔR is 20% or more (very good) A: ΔR is 10% or more and less than 20% (good) B: ΔR is 5% or more and less than 10% (usable) C: ΔR is less than 5%, or the reflectance peak due to structural color cannot be identified (unusable)
[0081] [Adhesion] The laminate was subjected to a tape adhesion test based on JIS K5600 and observed for peeling of the coating film. The evaluation criteria were as follows: S: Scratches or peeling area is less than 5% (very good) A: Scratches or peeling area is 5% or more, but less than 15% (good) B: Scratches or peeling area is 15% or more but less than 35% (usable) C: Scratches or peeling area is 35% or more (unusable)
[0082] [Table 5]
[0083] [Table 6]
Claims
1. A laminate comprising a substrate, a colloidal crystal layer that develops color through the interference of light, and a resin layer, arranged in that order, and which satisfies the following conditions (1) to (4): (1) Cracks having a width of 500 nm or more are formed in the colloidal crystal layer. (2) The area ratio of cracks having a width of 500 nm or more in the colloidal crystal layer is 0.1 to 30%. (3) The colloidal crystal layer has gaps between the particles. (4) The colloidal crystal layer and the resin layer are in contact with each other inside a crack having a width of 500 nm or more.
2. The laminate according to claim 1 , further comprising a primer layer between the substrate and the colloidal crystal layer.
3. 3. The laminate according to claim 1, wherein the particles constituting the colloidal crystal layer are core-shell type resin fine particles.
4. The method for producing a laminate according to claim 3, comprising the following steps 1 to 3, and including step 3 during step 1 or between steps 1 and 2: (Step 1) Forming a colloidal crystal layer on a substrate (Step 2) A step of forming a resin layer on the colloidal crystal layer formed in step 1. (Step 3) Heating at 70° C. or higher
Citation Information
Patent Citations
Thin film of particulate-arrayed body, its manufacturing method and manufacturing apparatus for the thin film of particulate arrayed body
JP2006208453A
Structural color coating film-forming coating composition and method for forming multilayer coating film
JP2009249527A
Composition for structural color expression and structural color expression membrane
JP2014047231A
Optical laminate
JP2015093419A
Adhesive sheet
JP2022058134A