Aging treatment method and manufacturing method of grain-oriented electrical steel sheet

By controlling carbon diffusion and adjusting aging amounts during the manufacturing process of grain-oriented electrical steel sheets, the magnetic properties are enhanced, addressing the need for improved magnetic performance.

JP7578188B2Active Publication Date: 2024-11-06JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023513543
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-15
Filing Date
2022-10-14
Publication Date
2024-11-06
Estimated Expiration
2042-10-14

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets require further improvement in magnetic properties to meet energy-saving demands for low iron loss and high magnetic flux density.

Method used

Control the carbon diffusion distance during the aging period from completion of cooling in annealing to final cold rolling by maintaining the steel plate at 60°C or less for 95% of the period and adjusting the aging amount through short-time heating before biting, predicting and adjusting aging amounts based on temperature history.

Benefits of technology

Improves the magnetic properties of grain-oriented electrical steel sheets by enhancing the texture, resulting in higher magnetic flux density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578188000001
    Figure 0007578188000001
  • Figure 0007578188000002
    Figure 0007578188000002
Patent Text Reader

Abstract

Provided is an oriented electromagnetic steel sheet that has superior magnetic characteristics. An aging treatment method by which a steel sheet is subjected to aging treatment prior to final cold rolling during an oriented electromagnetic steel sheet manufacturing process, wherein during the period from the end of cooling during pre-final cold rolling annealing until biting during the final cold rolling, the total carbon aging quantity is 0.02-0.5 μm in terms of carbon diffusion distance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aging treatment method for ageing a steel sheet before final cold rolling in the production process of grain-oriented electrical steel sheet, and a production method of grain-oriented electrical steel sheet. [Background technology]

[0002] Grain-oriented electrical steel sheets are widely used as materials for the iron cores of transformers, etc. In recent years, to save energy, grain-oriented electrical steel sheets are required to have low core loss at commercial frequencies and high magnetic flux density in low excitation magnetic fields. In order to meet these demands, various studies are being conducted to further improve the magnetic properties of grain-oriented electrical steel sheets.

[0003] Grain-oriented electrical steel is a material that has an easy magnetization axis of iron. <001> It has a crystal structure with a highly aligned orientation in the rolling direction of the steel sheet. This texture is formed during the final annealing process of the manufacturing process of grain-oriented electrical steel sheet through secondary recrystallization, which preferentially grows crystal grains with the (110)

[0001] orientation, known as the Goss orientation. Therefore, the crystal orientation of the secondary recrystallized grains has a significant effect on the magnetic properties of grain-oriented electrical steel sheet.

[0004] As one method for improving the magnetic properties of grain-oriented electrical steel sheets, a method has been proposed in which the morphology of C in the steel is controlled by controlling the cooling process after annealing before the final cold rolling.

[0005] For example, Patent Document 1 proposes a technique for increasing solute C by cooling an annealed steel sheet at a cooling rate of 150°C / min or more in a temperature range of 600 to 300°C.

[0006] Furthermore, Patent Document 2 proposes a technique for precipitating fine carbides having a grain size of 100 Å to 500 Å by subjecting an annealed steel sheet to rapid cooling and aging treatment under specific conditions.

[0007] The technologies proposed in Patent Documents 1 and 2 are believed to utilize the fact that solute C and the like adhere to defects such as dislocations introduced during cold rolling, forming a Cottrell atmosphere. This effect is also known in general steel as a method for increasing the {110} strength in the texture after recrystallization in annealing after cold rolling. The {110} texture acts as a good nucleus for secondary recrystallization, which ultimately improves the magnetic properties. In grain-oriented electrical steel sheets, improving the texture during recrystallization annealing is an extremely important factor.

[0008] Also, Patent Document 3 proposes a technique for improving the texture by forming lenticular carbides by performing aging treatment after annealing. Furthermore, Patent Document 3 shows that the form of carbon in steel can be controlled by the cooling pattern after annealing of the hot-rolled sheet. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 52-094825 [Patent Document 2] Japanese Patent Application Publication No. 58-157917 [Patent Document 3] Special Publication No. 38-014009 Summary of the Invention [Problem to be solved by the invention]

[0010] As mentioned above, conventionally, attempts have been made to improve the texture by utilizing solute C and carbides, but further improvements in the magnetic properties of grain-oriented electrical steel sheets are required.

[0011] The present invention has an object to solve the above-mentioned problems, and to provide a grain-oriented electrical steel sheet having excellent magnetic properties. [Means for solving the problem]

[0012] The present inventors have found that in the manufacturing process of grain-oriented electrical steel sheet, the magnetic properties of the grain-oriented electrical steel sheet can be improved by controlling the amount of carbon aging during the aging period from the completion of cooling in annealing before final cold rolling to the biting in final cold rolling, i.e., the diffusion distance of carbon, within a specific range. The present invention is based on the above findings and is summarized as follows.

[0013] 1. A method for ageing a steel sheet before final cold rolling in the manufacturing process of grain-oriented electrical steel sheet, comprising: The aging treatment method, wherein the total amount of carbon aging during the period from the completion of cooling in the annealing before final cold rolling to the biting in final cold rolling is 0.02 to 0.5 μm in terms of the diffusion distance of carbon.

[0014] 2. The temperature of the steel plate is maintained at 60°C or less for 95% or more of the period, The aging treatment method according to the above item 1, wherein the amount of aging is adjusted by heating the steel sheet immediately before the bite in the final cold rolling.

[0015] 3. Regarding the amount of aging A during the period from the completion of cooling in the annealing before final cold rolling to the final cold rolling mill charging, and the amount of aging B during the period from the final cold rolling mill charging to the bite, Predict the amount of aging B in advance, 2. The aging treatment method according to claim 1, wherein the aging amount A is adjusted based on the predicted aging amount B.

[0016] 4. A method for producing a grain-oriented electrical steel sheet, using the aging treatment method according to any one of 1 to 3 above. Effect of the Invention

[0017] According to the present invention, a grain-oriented electrical steel sheet having excellent magnetic properties can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described. Note that the following description shows a preferred embodiment of the present invention, and the present invention is not limited to the following description in any way.

[0019] In the present invention, the magnetic properties of the grain-oriented electrical steel sheet are improved by controlling the degree of aging of C during the period from the completion of cooling in the annealing before final cold rolling to the biting in final cold rolling. In the present invention, the degree of aging is expressed by the diffusion distance of C, and the diffusion distance of C is defined as the "amount of aging."

[0020] Specifically, in the present invention, the total aging amount of C during the above period is set to 0.5 μm or less in terms of the diffusion distance of C, thereby increasing the magnetic flux density of the grain-oriented electrical steel sheet that is finally obtained. The total aging amount is preferably set to 0.35 μm or less. According to this finding, the conditions for obtaining a grain-oriented electrical steel sheet with good properties can be expressed not by time or temperature but by the total aging amount of C. From this, it is considered that the diffusion of carbon to sites such as grain boundaries, distortions generated during cooling, and other precipitates, and the influence on the structure contributes to the improvement of properties. Therefore, if the aging amount of C is insufficient, a sufficient improvement effect on properties cannot be obtained. Therefore, the aging amount of C is set to 0.02 μm or more, preferably 0.10 μm or more.

[0021] From the viewpoint of controlling the amount of aging of such a small amount of C, the amount of solute carbon at the completion of cooling in the annealing before final cold rolling is preferably 50 ppm or more.

[0022] In the present invention, the method for adjusting the amount of carbon aging during the above-mentioned period is not particularly limited, and the adjustment may be performed by any method.

[0023] Here, the diffusion distance d (m) of C is the diffusion coefficient D (m 2Using the diffusion time t(s) and the diffusion distance t(s), it can be expressed as the following formula (1). Therefore, the total diffusion distance from the completion of cooling in the annealing before final cold rolling to the start of final cold rolling can be obtained by integrating the diffusion distances during the above-mentioned period. Note that the start of final cold rolling here refers to the time when the steel sheet is engaged with the rolls of the cold rolling mill that performs the final cold rolling. d = (2Dt) 1 / 2 …(1) Where: D: Diffusion coefficient of C (m 2 / s) t: diffusion time (s)

[0024] The diffusion coefficient D(m 2 / s) is the diffusion constant D0 of C (m 2 / s), activation energy Q (kJ / mol), gas constant R (J K -1 mol -1 ) and temperature T (K) according to the following equation (2). D = D0exp(-Q / RT)…(2) Where: D0 = 1.24 × 10 -5 m 2 / s Q = 99.5 × {(1-30.9) / T} kJ / mol R=8.31446 J K -1 mol -1

[0025] As can be seen from the above formulas (1) and (2), the diffusion distance of carbon during the above period is determined by the temperature and time during the period. However, in an actual manufacturing environment, the temperature of the steel sheet changes from moment to moment between the completion of cooling in the annealing before final cold rolling and the engagement in final cold rolling. Therefore, it is desirable to grasp the temperature history of the steel sheet (coil) during the above period and adjust it so as to obtain the desired total aging amount.

[0026] Examples of the method for adjusting the diffusion distance of C during the above-mentioned period include a method of heating for a predetermined time before biting, and a method of controlling the temperature and time during the waiting time from annealing to rolling.

[0027] For example, in one embodiment of the present invention, the temperature of the steel sheet is kept at 60°C or less for 95% or more of the period, and the amount of aging can be adjusted by heating the steel sheet immediately before the bite in the final cold rolling.

[0028] As a method of heating before biting, it is preferable to use at least one selected from the group consisting of induction heating, direct current heating, and infrared heating. According to the heating method, the steel sheet can be heated to a desired temperature in a short time (hereinafter, heating by the method may be referred to as "short-time heating"). The heating conditions at this time may be adjusted so that the sum of the diffusion distance in the period before heating and the diffusion distance by the heating becomes the desired diffusion distance. The diffusion distance in the period before heating can be calculated based on the temperature history in that period. In addition, under typical manufacturing conditions, after the steel sheet is loaded into the rolling mill, it comes into contact with rolling oil and receives heat input or removal before biting. Therefore, when the short-time heating is performed, the heating conditions are determined taking into consideration the heat transfer between the steel sheet and the rolling oil.

[0029] In another embodiment of the present invention, an aging amount A during the period from the completion of cooling in the annealing before final cold rolling to the loading into the final cold rolling mill, and an aging amount B during the period from the loading into the final cold rolling mill to biting can be predicted in advance, and the aging amount A can be adjusted based on the predicted aging amount B.

[0030] That is, in a general manufacturing process of grain-oriented electrical steel sheet, the steel sheet after annealing before final cold rolling is temporarily placed in a yard or the like in a coiled state and then subjected to final cold rolling. At this time, if the temperature history from when the steel sheet is charged into the final cold rolling mill until it is bitten is known, the amount of aging B from when it is charged to when it is bitten can be predicted in advance.

[0031] Therefore, the aging amount B is predicted in advance, and the aging amount A during the period from the completion of cooling in the annealing before final cold rolling to the loading into the final cold rolling mill is adjusted based on the predicted value, thereby making it possible to obtain a desired total aging amount. Note that the method for adjusting the aging amount A is not particularly limited, and for example, the temperature and time when the steel sheet (coil) is stored in a yard or the like before being subjected to final cold rolling may be adjusted.

[0032] The temperature information used to calculate the diffusion distance may be obtained by actually measuring the temperature of the steel sheet (coil), or may be estimated from the environmental temperature, etc. It is also effective to use past results to improve the accuracy of the estimated value.

[0033] Other manufacturing processes are not particularly limited, and for example, a process similar to that used for manufacturing a general grain-oriented electrical steel sheet can be adopted.

[0034] For example, in one embodiment of the present invention, a steel slab is prepared, the steel slab is heated, and the heated steel slab is hot-rolled to form a hot-rolled steel sheet, and the hot-rolled steel sheet is subjected to at least one cold rolling. When cold rolling is performed only once, the cold rolling is the "final cold rolling". When cold rolling is performed two or more times, the cold rolling performed last among the two or more cold rollings is the "final cold rolling".

[0035] [Steel slab] The steel slab is not particularly limited and any steel slab can be used. The steel slab can be obtained by a known method, for example, a continuous casting method or an ingot casting-bloom rolling method.

[0036] As described above, the present invention improves the magnetic properties by controlling the amount of aging, and the effect can be obtained regardless of the composition of the steel slab. Therefore, a steel slab with any composition can be used as the steel slab. However, from the viewpoint of further improving the magnetic properties, it is preferable to use a steel slab having the composition described below. In this specification, "%" and "ppm" refer to "% by mass" and "ppm by mass", respectively, unless otherwise specified.

[0037] In one embodiment of the present invention, it is preferable to use a steel slab containing C: 0.01 to 0.10% and Si: 2.0 to 4.5%.

[0038] C: 0.01 to 0.10% C is an element useful for improving the texture. From the viewpoint of further improving the texture, it is preferable that the C content is 0.01% or more. On the other hand, if the C content of the steel slab is too high, decarburization becomes difficult, and C may remain in the finally obtained grain-oriented electrical steel sheet. From the viewpoint of preventing magnetic aging due to the residual C and further improving the magnetic properties, it is preferable that the C content is 0.10% or less.

[0039] Silicon: 2.0% to 4.5% Si is an element that has the effect of improving iron loss by increasing electrical resistance. Therefore, from the viewpoint of enhancing the effect of adding Si, it is preferable that the Si content is 2.0% or more. On the other hand, if the Si content exceeds 4.5%, the steel sheet becomes brittle, and the cold rolling property is deteriorated. Therefore, from the viewpoint of manufacturability, it is preferable that the Si content is 4.5% or less.

[0040] Mn: 0.02-1.0% Mn is an element that has the effect of improving the hot workability of steel. Therefore, from the viewpoint of improving the hot workability, the Mn content is preferably 0.02% or more. On the other hand, if the Mn content is excessive, the magnetic flux density of the grain-oriented electrical steel sheet decreases. Therefore, the Mn content is preferably 1.0% or less, and more preferably 0.30% or less.

[0041] The present invention can be applied to both the case where the steel slab does not contain inhibitor-forming elements (inhibitor-less method) and the case where the steel slab contains inhibitor-forming elements.

[0042] When a steel slab that does not contain inhibitor-forming elements is used, the steel slab may have a composition containing, for example, C: 0.01-0.10%, Si: 2.0-4.5%, and Mn: 0.02-1.0%, with the balance being Fe and unavoidable impurities. The contents of the inhibitor-forming elements contained as impurities in the composition are preferably less than Al: 0.01%, less than N: 0.006%, less than S: 0.005%, less than Se: 0.005%, and less than O: 0.005%, respectively.

[0043] When a steel slab containing inhibitor-forming elements is used, the steel slab may contain, for example, C: 0.01-0.10%, Si: 2.0-4.5%, Mn: 0.02-1.0%, Al: 0.01% or more and 0.08% or less, N: 0.006% or more and 0.015% or less, S: 0.005% or more and 0.05% or less, Se: 0.005% or more and 0.05% or less, O: less than 0.005%, with the balance being Fe and unavoidable impurities.

[0044] The steel slab may optionally contain at least one selected from the following group in order to further improve the magnetic properties: B: 0.5ppm~1.0% Bi: 0.5 ppm to 1.0% Sb: 5ppm~1.0% Mo: 5ppm~1.0% Te: 5ppm~1.0% Sn: 5ppm~1.0% P: 5ppm~1.0% Ge: 5ppm~1.0% As: 5ppm to 1.0% Nb: 5ppm~1.0% Cr: 5ppm~1.0% Ti: 5ppm~1.0% Cu: 5ppm~1.0% Pb: 5ppm~1.0% Zn: 5ppm~1.0% In: 5ppm to 1.0%

[0045] [Slab heating] Next, the steel slab is heated prior to hot rolling. The heating temperature (slab heating temperature) in the heating step is not particularly limited. However, if the slab heating temperature is too low, hot rolling becomes difficult. Therefore, from the viewpoint of smoothly carrying out hot rolling, it is preferable to set the slab heating temperature to 1050°C or higher. On the other hand, if the temperature is too high, the steel slab will melt, so the slab heating temperature is set to the melting point of the steel slab or lower. Note that, in general, it is preferable to set the slab heating temperature to 1400°C or lower.

[0046] When using a steel slab containing an inhibitor-forming element, it is preferable to completely dissolve the inhibitor-forming element contained in the steel slab by heating, and therefore it is more preferable to set the slab heating temperature to 1300°C or higher.

[0047] On the other hand, when a steel slab not containing inhibitor-forming elements is used, it is not necessary to heat the slab to a high temperature because it is not necessary to dissolve the inhibitor-forming elements. Therefore, it is more preferable to set the slab heating temperature to 1050 to 1250°C.

[0048] [Hot rolling] Next, the heated steel slab is hot-rolled to obtain a hot-rolled steel sheet, and the hot-rolled steel sheet is subjected to at least one cold rolling. The hot rolling can be performed under any conditions without any particular limitation.

[0049] [Annealing] In addition, when cold rolling is performed only once, annealing is performed before the cold rolling. That is, a steel slab is hot rolled to obtain a hot-rolled steel sheet, and the hot-rolled steel sheet is annealed. In this technical field, the annealing performed on the hot-rolled steel sheet prior to cold rolling is called hot-rolled sheet annealing. Then, after the hot-rolled sheet annealing, aging treatment is performed before cold rolling.

[0050] On the other hand, when cold rolling is performed multiple times, it is preferable to perform annealing between each cold rolling. Annealing performed between cold rolling in this manner is called intermediate annealing in this technical field. Then, after annealing (final intermediate annealing) before the last cold rolling (final cold rolling) of the multiple cold rollings, aging treatment is performed before the final cold rolling. Note that, even when cold rolling is performed multiple times, it is preferable to perform annealing (hot-rolled sheet annealing) on ​​the hot-rolled steel sheet after hot rolling and before the first cold rolling.

[0051] [Cold rolling] Next, the aging treatment is performed as described above, and then cold rolling is performed. The conditions of the aging treatment are as described above. Cold rolling can be performed under any conditions without any particular limitation. However, if the total reduction in cold rolling is less than 80%, the (111) fiber structure (so-called γ fiber) required for secondary recrystallization is insufficient. In addition, if the total reduction exceeds 94%, the texture improvement effect of multiple annealing of the hot-rolled steel sheet cannot be obtained. This is because the {110}〈001〉 orientation, which is the nucleus of secondary recrystallization, decreases. Therefore, from the viewpoint of further improving the magnetic properties by controlling the texture, the total reduction in cold rolling is preferably 80 to 94%, and more preferably 82 to 91%.

[0052] Next, the process after the cold rolling will be described. In one embodiment of the present invention, for example, the cold-rolled steel sheet is subjected to primary recrystallization annealing, an annealing separator is applied to the surface of the steel sheet, and secondary recrystallization annealing is performed to obtain a grain-oriented electrical steel sheet.

[0053] The annealing separator is not particularly limited and any annealing separator can be used. For example, it is preferable to use an annealing separator containing at least one of magnesia, silica, and alumina, and it is more preferable to use an annealing separator containing at least one of magnesia, silica, and alumina as a main component.

[0054] When the annealing separator contains magnesia, in the subsequent secondary recrystallization annealing process, SiO2 present on the steel sheet surface reacts with magnesia (MgO) to form a forsterite (Mg2SiO4) coating. From the viewpoint of magnetic properties, it is preferable to use an annealing separator containing magnesia and form a forsterite coating in the secondary recrystallization annealing.

[0055] On the other hand, when an annealing separator that does not contain magnesia is used, a forsterite film is not formed. From the viewpoint of improving the punchability of the grain-oriented electrical steel sheet, it is preferable to use an annealing separator that does not contain magnesia.

[0056] After the application of the annealing separator, secondary recrystallization annealing is performed. The secondary recrystallization annealing is not particularly limited and may be performed according to a conventional method.

[0057] After the secondary recrystallization annealing, an insulating coating may be further formed. By providing an insulating coating, it is possible to reduce iron loss when the grain-oriented electrical steel sheets are stacked and used. The insulating coating may be formed according to a conventional method. For example, the insulating coating may be formed by applying a coating liquid containing a phosphate to the surface of the steel sheet and then baking it. The coating liquid preferably contains a phosphate and colloidal silica, and more preferably contains a phosphate, colloidal silica, and chromic acid.

[0058] Furthermore, after the secondary recrystallization annealing, flattening annealing can be performed to adjust the shape of the steel sheet. In addition, when an insulating coating is formed, the flattening annealing can also serve as baking of the insulating coating. EXAMPLES

[0059] Example 1 A steel slab was prepared containing 0.035% C, 3.4% Si, 0.07% Mn, 0.006% Al, 0.005% N, 0.003% S, 0.001% Se, 0.03% Sb, and 0.001% O, with the balance being Fe and unavoidable impurities. The steel slab was heated and then hot-rolled to obtain a hot-rolled sheet having a thickness of 2.2 mm.

[0060] Next, the hot-rolled sheet was subjected to hot-rolled sheet annealing to obtain a hot-rolled annealed sheet. In the hot-rolled sheet annealing, the hot-rolled sheet was first soaked at 1030°C for 30 seconds, and then mist-cooled from 900°C to 100°C at 30°C / s. In this example, the hot-rolled sheet annealing is the annealing before the final cold rolling.

[0061] The hot-rolled annealed sheet after the mist cooling was subjected to pickling under the conditions shown in Table 1. The solute carbon content after the mist cooling was 80 ppm.

[0062] The pickled steel sheet was subjected to final cold rolling to obtain a cold-rolled steel sheet having a final thickness of 0.20 mm. The temperature history from pickling to biting in the final cold rolling was as shown in Table 1.

[0063] In some examples, before the final cold rolling, short-time heating was performed under the conditions shown in Table 1. The short-time heating was performed by induction heating. In each example, the heat input due to contact with the rolling oil was as shown in Table 1.

[0064] The total aging amount (converted into the diffusion distance of carbon) calculated from the temperature history using the above-mentioned formulas (1) and (2) is also shown in Table 1.

[0065] In Example No. 5, the amount of aging B from the time of charging into the final cold rolling mill to the time of biting was calculated in advance from the heat input condition to the steel sheet due to contact with the rolling oil, and the amount of aging A from the time of completion of cooling in the annealing before final cold rolling to the time of charging into the final cold rolling mill was adjusted based on the amount of aging B so that the total amount of aging became the value shown in Table 1.

[0066] The cold-rolled steel sheet was then subjected to primary recrystallization annealing at a soaking temperature of 800°C for a soaking time of 30 s. Next, an annealing separator containing 95% MgO and 5% TiO2 was applied as a water slurry to the steel sheet surface, dried, and subjected to secondary recrystallization annealing (finish annealing). A coating solution containing phosphate-chromate-colloidal silica in a weight ratio of 3:1:3 was applied to the surface of the finish annealed sheet thus obtained, and baked at 800°C.

[0067] The magnetic properties of the grain-oriented electrical steel sheet thus obtained were examined at the widthwise center. Specifically, after stress relief annealing at 800°C for 3 hours, the magnetic flux density B8 was measured when excited at 800 A / m.

[0068] [Table 1]

[0069] Example 2 Steel slabs containing the components shown in Table 2 and having a composition consisting of the balance Fe and unavoidable impurities were prepared. After heating these steel slabs, they were hot-rolled to obtain hot-rolled sheets having a thickness of 2.5 mm, and then hot-rolled sheet annealing was performed. The hot-rolled sheet annealing was performed by soaking at 1000°C for 30 seconds, cooling from 900°C to 100°C at 10°C / s, and pickling at 80°C for 3 minutes. Thereafter, the sheet was cold-rolled to a thickness of 1.5 mm, followed by intermediate annealing by soaking at 1050°C for 1 minute, and then cooling from 900°C to 100°C at 50°C / s. In this embodiment, the intermediate annealing is the annealing before the final cold rolling. The solute carbon after intermediate annealing and cooling was 150 ppm.

[0070] Then, the amount of aging by heating just before biting was adjusted according to the amount of aging in the rolling entry looper (actually, heating at 105°C for 2 seconds and rolling oil contact heat input at 55°C for 5 seconds) so that the total amount of aging was 0.25 μm, and the cold rolled steel sheet was bitten into the cold roll. This resulted in a cold rolled steel sheet with a final thickness of 0.18 mm.

[0071] The cold-rolled steel sheet was then subjected to primary recrystallization annealing at a soaking temperature of 800°C for a soaking time of 30 s. Next, an annealing separator containing 95% MgO and 5% TiO2 was applied as a water slurry to the steel sheet surface, dried, and subjected to secondary recrystallization annealing (finish annealing). A coating solution containing phosphate-chromate-colloidal silica in a weight ratio of 3:1:3 was applied to the surface of the finish annealed sheet thus obtained, and baked at 800°C.

[0072] The magnetic properties of the grain-oriented electrical steel sheet thus obtained were examined at the widthwise center. Specifically, after stress relief annealing at 800°C for 3 hours, the magnetic flux density B8 was measured when excited at 800 A / m.

[0073] As can be seen from the results of Examples 1 and 2 above, in the examples where aging treatment satisfying the conditions of the present invention was performed, grain-oriented electrical steel sheets having high magnetic flux density could be obtained.

[0074] [Table 2]

Claims

1. A method for ageing a steel sheet before final cold rolling in a process for producing grain-oriented electrical steel sheet from a steel slab, comprising: The steel slab comprises, in mass %, C: 0.01 to 0.10%, Si: 2.0 to 4.5%, Mn: 0.02 to 1.0%, Al: 0.01-0.08%, N: 0.006 to 0.015%, S: 0.005-0.05%, Se: 0.005 to 0.05%, and O: less than 0.005%, with the balance being Fe and unavoidable impurities; The aging treatment method includes a process for aging in which a total amount of carbon aging during a period from completion of cooling in annealing before final cold rolling to biting in final cold rolling is 0.02 to 0.5 μm in terms of the diffusion distance of carbon.

2. The composition of the components is, in ppm by mass and % by mass, B: 0.5ppm to 1.0%, Bi: 0.5ppm to 1.0%, Sb: 5ppm to 1.0%, Mo: 5ppm to 1.0%, Te: 5ppm to 1.0%, Sn: 5ppm to 1.0%, P: 5ppm to 1.0%, Ge: 5ppm to 1.0%, As: 5ppm to 1.0%, Nb: 5ppm to 1.0%, Cr: 5ppm to 1.0%, Ti: 5ppm to 1.0%, Cu: 5ppm to 1.0%, Pb: 5ppm to 1.0%, Zn: 5 ppm to 1.0%, and In: 5ppm to 1.0% The aging treatment method according to claim 1 , further comprising at least one selected from the group consisting of:

3. The temperature of the steel plate is maintained at 60° C. or less for 95% or more of the period, The aging treatment method according to claim 1 , wherein the amount of aging is adjusted by heating the steel sheet immediately before the bite in the final cold rolling.

4. The temperature of the steel plate is maintained at 60°C or less for 95% or more of the period, The aging treatment method according to claim 2 , wherein the amount of aging is adjusted by heating the steel sheet immediately before the bite in the final cold rolling.

5. A method for age-hardening a steel sheet before final cold rolling in a manufacturing process of grain-oriented electrical steel sheet, comprising: The total aging amount of carbon during the period from the completion of cooling in the annealing before final cold rolling to the biting in the final cold rolling is 0.02 to 0.5 μm in terms of the diffusion distance of carbon, Regarding the amount of aging A during the period from the completion of cooling in the annealing before the final cold rolling to the charging into the final cold rolling mill, and the amount of aging B during the period from the charging into the final cold rolling mill to the biting, The amount of aging B is predicted in advance, and adjusting the aging amount A based on the predicted aging amount B.

6. A method for producing a grain-oriented electrical steel sheet, using the aging treatment method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for producing general-oriented siliconsteel

    CN1978673A

  • JP1963-014009B

  • Preparation of unidirectional silicon steel sheet

    JP1977094825A

  • Manufacture of unidirectional silicon steel plate with superior magnetic characteristic

    JP1983157917A

  • Method for cold rolling grain-oriented magnetic steel sheet

    JP1989215925A