Friction stir welding method, friction stir welding apparatus, and method for manufacturing welded members

By controlling the separation distance of rotating tools based on load in the friction stir welding method, the method addresses rotary tool wear and heat input issues, resulting in stable and high-quality joints with high melting point steel plates.

JP7578216B1Active Publication Date: 2024-11-06JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024545258
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-07-26
Filing Date
2024-05-27
Publication Date
2024-11-06
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

Conventional friction stir welding methods result in deteriorated joint properties when high melting point steel plates, such as those with a Si content of 2.0 to 5.0% by mass, are used, primarily due to rotary tool wear and insufficient heat input leading to poor plastic flow.

Method used

A friction stir welding method that controls the separation distance of rotating tools based on the load on the rotary tools, adhering to specific relationships to stabilize joint characteristics, using a friction stir welding apparatus with a measuring device, calculation device, and position adjustment mechanism to manage tool wear.

Benefits of technology

Stabilizes joint properties and enables the production of high-quality bonded members by preventing rotary tool wear and ensuring adequate heat input, even with high melting point steel plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578216000002
    Figure 0007578216000002
  • Figure 0007578216000001
    Figure 0007578216000001
Patent Text Reader

Abstract

The present invention provides a friction stir welding method that can stably obtain good joint characteristics at a joint even when a high melting point steel plate is used as the joined material. The present invention satisfies a predetermined relationship between the load of a rotary tool and the distance between the rotary tool and the rotary tool.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a friction stir welding method, a friction stir welding apparatus, and a method for manufacturing a welded member. [Background technology]

[0002] In friction stir welding, for example, double-sided friction stir welding, the workpieces are joined as follows. That is, a pair of rotating tools are placed on the front and back sides of the workpieces having at least two or more metal plates. Then, the rotating tools are pressed against the front and back sides of the workpieces, respectively, and moved in the joining direction while rotating the rotating tools. As a result, the metal plates are softened by frictional heat between the rotating tool and the workpieces, and the softened parts are stirred by the rotating tool. Then, plastic flow is generated in the area of ​​the workpieces that will become the joint, and the workpieces are joined. Hereinafter, the area where the workpieces are butted or overlapped and not yet joined is referred to as the "unjoined area", and the area that has been joined and integrated is referred to as the "joined area".

[0003] As a technique related to such friction stir welding, for example, Patent Document 1 describes: "The coefficient of dynamic friction between the material of the rotating tool or the material coated on the surface of the rotating tool and the steel plate is 0.6 or less, When a heating region is defined as a region in which a temperature TS (°C) of a surface of the steel plate heated by a heating means provided in front of the joining direction of the rotating tool satisfies the following formula (1), the minimum distance between the heating region and the rotating tool is equal to or less than a diameter of a shoulder portion of the rotating tool, an area of ​​the heating region is equal to or smaller than an area of ​​a maximum diameter portion of the pin portion of the rotary tool; A friction stir welding method, in which 65% or more of the area of ​​the heating region is located between a weld center line, which is a straight line on the surface of the steel plate that passes through the rotation axis of the rotating tool and is parallel to the welding direction, and a straight line that is parallel to the weld center line and is separated toward the retreating side by a distance equal to the maximum radius of the pin portion of the rotating tool. T ≥ 0.8 × T A1 (1) TA1 is the temperature represented by the following formula (2). T A1 (°C) = 723 - 10.7[%Mn] - 16.9[%Ni] + 29.1[%Si] + 16.9[%Cr] + 290[%As] + 6.38[%W] ··· (2) The above [%M] is the content (mass%) of element M in the steel sheet as the workpiece, and is set to 0 if not contained. is disclosed.

[0004] Patent Document 2 discloses "The shoulder portion and the pin portion of the rotary tool share the rotation axis and are made of a material harder than the steel sheet. When the region on the surface side of the steel sheet heated by a heating device provided in front of one joining direction of the rotary tool is defined as a heating region, during heating, A method for double-sided friction stir welding, characterized in that friction stir welding is performed by controlling so that the steel sheet surface temperature TP (°C) in the heating region satisfies formulas (1) to (3), and the gap G (mm) between the opposing shoulders and the thickness t (mm) of the steel sheet satisfy formula (5). In the range of -0.5×D ≤ W < -0.1×D, 40 ≤ TP ≤ 1200 ··· (1) In the range of -0.1×D ≤ W ≤ 0.1×D, 100 ≤ TP ≤ 1200 ··· (2) In the range of 0.1×D < W ≤ 0.5×D, 40 ≤ TP ≤ 1200 ··· (3) 0.4×t ≤ G ≤ t ··· (5) Here, W (mm) is the position separated in the width direction of the joint from the joint center line, D (mm) is the diameter of the shoulder of the rotary tool, G (mm) is the gap between the shoulders, t (mm) is the thickness of the steel sheet, respectively. is disclosed.

[0005] Patent Document 3 discloses "A rotating tool is pressed against an unjoined portion, which is an abutting portion or an overlapping portion between an end of a first electromagnetic steel strip and an end of a second electromagnetic steel strip, from both sides of the unjoined portion while rotating in opposite directions to each other, Next, the rotating tool is moved in a joining direction to join the first electromagnetic steel strip and the second electromagnetic steel strip, Furthermore, the diameter D (mm) of the shoulder portion of the rotary tool satisfies the relationship of the following formula (1), and RS×D is expressed by the rotation speed RS (rpm), the diameter D (mm) of the shoulder of the rotary tool, and the welding speed JS (mm / min). 3 / JS satisfies the relationship of the following formula (2). 4 × TJ ≤ D ≤ 10 × TJ (1) 200×TJ≦RS×D 3 / JS≦2000×TJ (2) Here, TJ is When the unjoined portion is a butt portion, the average value (mm) of the sheet thickness of the first electromagnetic steel strip and the sheet thickness of the second electromagnetic steel strip, If the unjoined portion is an overlapping portion, it is the thickness of the overlapping portion (mm). has been disclosed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2018 / 070316 [Patent Document 2] JP 2020-124739 A [Patent Document 3] JP 2023-041556 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the conventional friction stir welding method described in Patent Document 1 and the like, when a high melting point steel plate, for example a steel plate with a Si content of 2.0 to 5.0 mass %, is used as the material to be joined, the joint properties of the welded portion may deteriorate. Therefore, there is a demand for improvement in this respect.

[0008] The present invention has been developed in view of the above-mentioned current situation, and aims to provide a friction stir welding method (hereinafter also referred to as a friction stir welding method excellent in stability of joint characteristics of a joint) that makes it possible to obtain stable and good joint characteristics of a joint even when a high melting point steel plate is used as the welded material. Another aim of the present invention is to provide a friction stir welding device that can be suitably used for the above-mentioned friction stir welding method. Furthermore, another aim of the present invention is to provide a manufacturing method of a welded member. In this specification, any numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits, respectively. [Means for solving the problem]

[0009] The inventors have conducted extensive research to achieve the above object. First, the inventors investigated the cause of deterioration of joint characteristics of a joint when a high melting point steel plate is used as a workpiece in a conventional friction stir welding method. As a result, the inventors have obtained the following findings. That is, when a high melting point steel plate is used as a workpiece, the rotating tool is likely to wear or be damaged (hereinafter, also referred to as wear, etc.). This wear of the rotating tool, etc., causes insufficient heat input and poor plastic flow, which causes deterioration of the joint characteristics of the joint.

[0010] Therefore, the inventors have conducted further studies based on the above findings, and as a result, have obtained the following findings. There is a correlation between the wear progress of the rotating tool and the load on the rotating tool during joining. By controlling the separation distance of the rotating tool to satisfy a specified relationship according to the load on the rotating tool, it is possible to obtain stable and good joint characteristics of the joint, even when high-melting-point steel plates are used as the joined materials. The present invention was completed based on the above findings and through further investigation.

[0011] That is, the gist and configuration of the present invention are as follows. 1. A friction stir welding method in which a pair of opposing rotary tools is pressed against the front and back surfaces of workpieces, respectively, and the workpieces are joined by moving the rotary tools in a joining direction while rotating the rotary tools, A friction stir welding method, wherein a load on the rotating tool and a separation distance of the rotating tool satisfy the following relationship: When 0.01≦dL<0.10 dL×0.1≦dD≦dL×1.0 When 0.10≦dL<0.30 dL×0.2-0.01≦dD≦dL×1.2-0.02 When 0.30≦dL<0.70 dL×0.4-0.07≦dD≦dL×1.4-0.08 Here, dL = ΔL / Lint, where Lint is the initial value of the load on the rotary tool, and ΔL is the change in the load on the rotary tool from Lint. Also, dD=ΔD / Dint, where Dint is the initial value of the separation distance of the rotating tool, and ΔD is the amount of change in the separation distance of the rotating tool from Dint.

[0012] 2. The friction stir welding method according to claim 1, wherein the load of the rotating tool is a load value in an axial direction of the rotating tool, a load value in a welding direction, or a torque value in a rotational direction.

[0013] 3. The friction stir welding method according to 1 or 2 above, which is butt welding or lap welding.

[0014] 4. A friction stir welding apparatus used in the friction stir welding method according to any one of 1 to 3, A pair of opposing rotary tools; a measuring device for measuring a load on the rotary tool; A calculation device that calculates a control range of the separation distance of the rotary tool based on the equation described in 1 from the load of the rotary tool measured by the measurement device; a position adjustment mechanism that changes a position of the rotation tool within a control range of the separation distance of the rotation tool calculated by the calculation device; and The friction stir welding apparatus has

[0015] 5. A method for producing a welded member, comprising joining workpieces by the friction stir welding method according to any one of 1 to 3 above to obtain a welded member. Effect of the Invention

[0016] According to the present invention, even when a high melting point steel plate is used as the joined material, it is possible to avoid deterioration of the joint characteristics of the joint and obtain stable and excellent joint characteristics of the joint. As a result, it is possible to stably manufacture high-quality joined members regardless of the type of joined material, and the industrial value of the present invention is extremely great. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram showing an example of friction stir welding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described based on the following embodiments. [1]Friction stir welding method First, a friction stir welding method according to an embodiment of the present invention will be described.

[0019] As described above, in the friction stir welding according to one embodiment of the present invention, as shown in FIG. 1, a pair of rotating tools are placed on the front side and the back side of the workpiece having at least two or more metal plates. Hereinafter, the rotating tool placed on the front side of the workpiece is referred to as the front side rotating tool. Also, the rotating tool placed on the back side of the workpiece is referred to as the back side rotating tool. In FIG. 1, reference numeral 1 denotes the rotating tool (front side rotating tool), 2 denotes the rotating tool (back side rotating tool), and 3 denotes the workpiece. Then, the pair of opposing rotating tools are pressed against the front and back sides of the workpiece, respectively, and the rotating tools are moved in the joining direction while rotating. That is, the front side rotating tool is pressed against the front side of the workpiece, and the back side rotating tool is pressed against the back side of the workpiece, respectively, and these rotating tools are moved in the joining direction while rotating. As a result, the metal plate is softened by the frictional heat between the rotating tool and the workpiece, and the softened part is stirred by the rotating tool. Then, plastic flow is generated in the region that will be the joining part of the workpiece, and the workpiece is joined.

[0020] In friction stir welding according to one embodiment of the present invention, it is extremely important to monitor the load on the rotating tool during welding and control the separation distance of the rotating tool so as to satisfy the relationship in the following equation (1) (consisting of three equations divided into cases) according to the (monitored) load on the rotating tool. When 0.01≦dL<0.10 dL×0.1≦dD≦dL×1.0 When 0.10≦dL<0.30 dL×0.2-0.01≦dD≦dL×1.2-0.02 (1) When 0.30≦dL<0.70 dL×0.4-0.07≦dD≦dL×1.4-0.08 Here, dL = ΔL / Lint, where Lint is the initial value of the load of the rotary tool, and ΔL is the change in the load of the rotary tool from Lint. Also, dD = ΔD / Dint, where Dint is the initial value of the separation distance of the rotary tool, and ΔD is the change in the separation distance of the rotary tool from Dint.

[0021] That is, when friction stir welding is performed using high melting point steel plates as the materials to be joined, the rotating tool is likely to wear out. This wear of the rotating tool causes insufficient heat input and poor plastic flow, which leads to deterioration of the joint characteristics of the joint. In this regard, the separation distance of the rotating tool is controlled so as to satisfy the relationship of the above formula (1) (consisting of three formulas divided into cases), preferably the following formula (2), depending on the load of the rotating tool during joining, which is correlated with the progress of wear of the rotating tool. This makes it possible to stably manufacture high-quality welded members regardless of the progress of wear of the rotating tool. When 0.01≦dL<0.10 dL×0.12≦dD≦dL×0.9 When 0.10≦dL<0.30 dL×0.24-0.012≦dD≦dL×1.1-0.02 (2) When 0.30≦dL<0.70 dL×0.48-0.084≦dD≦dL×1.3-0.08

[0022] When dL is less than 0.01, the separation distance of the rotating tools may be kept at Dint, i.e., dD=0, and joining may be performed. In addition, in the initial stage of joining, the workpieces that have plastically flowed may adhere to the rotating tools, increasing the tool load. In this case, too, the separation distance of the rotating tools may be kept at Dint, i.e., dD=0, and joining may be performed. When dL is 0.70 or more, it is recommended to replace the rotating tools. Here, the separation distance D of the rotating tools is the separation distance (shortest distance) between the front side rotating tool and the back side rotating tool in the thickness direction of the workpieces (hereinafter also referred to as the thickness direction) as shown in FIG. 1.

[0023] Moreover, Lint may be the load of the rotary tool when, for example, the rotary tool is not worn, the separation distance of the rotary tool is set to an initial value (Dint), and bonding is performed under the same bonding conditions as those in the actual bonding (planned for the actual bonding), for example. Lint can be obtained, for example, by performing a preliminary bonding test in advance.

[0024] ΔL can be expressed as ΔL=Lint-LT, where LT is the load of the rotary tool at time T. In other words, ΔL can be said to be the reduction in the load of the rotary tool from Lint.

[0025] Dint may be determined based on the materials to be joined and the joining conditions planned for the actual joining. For example, Dint is preferably 0.01×t to 0.5×t. Dint is more preferably 0.05×t or more. Dint is more preferably 0.3×t or less. Here, t is the thickness (mm) of the materials to be joined. In the case of butt joining, t is the average thickness of the materials to be joined, and in the case of lap joining, t is the thickness of the overlapping portion of the materials to be joined.

[0026] ΔD can be expressed as ΔD=Dint-DT, where DT is the separation distance of the rotary tool at time T. In other words, ΔD can be said to be the amount of decrease in the separation distance of the rotary tool from Dint.

[0027] The load of the rotating tool is preferably, for example, a load value in the axial direction of the rotating tool, a load value in the welding direction, or a torque value in the rotational direction. The load value in the axial direction of the rotating tool, the load value in the welding direction, or the torque value in the rotational direction each include values ​​derived from these values ​​(for example, values ​​in which the control range of dD according to the above formula (1) is the same as when the load value in the axial direction of the rotating tool, the load value in the welding direction, or the torque value in the rotational direction is used). The load value in the axial direction of the rotating tool, the load value in the welding direction, or the torque value in the rotational direction can be measured using a general load measuring device or torque measuring device.

[0028] In addition, when the loads of the front side rotary tool and the back side rotary tool are different, the relationship of the above formula (1) (preferably the above formula (2)) is satisfied in both the front side rotary tools.

[0029] Incidentally, monitoring the load of the rotary tool means measuring the load of the rotary tool at a predetermined interval. The measurement interval is not particularly limited, and is preferably set to, for example, 0.1 to 1.0 seconds. Incidentally, the measurement interval may be constant or may not be constant.

[0030] The joining conditions other than the above are not particularly limited and may be in accordance with the usual method. For example, the rotation speed of the rotary tool is preferably 300 to 2000 rpm. In addition, the rotation direction of the rotary tool is preferably opposite between the front side rotary tool and the back side rotary tool. From the viewpoint of improving the working efficiency, the joining speed is preferably 0.5 m / min or more, more preferably 0.8 m / min or more. The positions of the tips of the front side rotary tool and the back side rotary tool may be appropriately set in accordance with the usual method so as to satisfy the relationship of the above formula (1). For example, it is preferable that the positions of the tips of the front side rotary tool and the back side rotary tool are symmetrical in the thickness direction with respect to the thickness center position of the joined material.

[0031] Examples of joining methods include butt joining and lap joining. In butt joining, the end faces of the materials to be joined are placed opposite each other, and a rotating tool is pressed against the butt portion including the end faces (butt surfaces) of the materials to be joined while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined. In lap joining, at least a portion of the ends of the materials to be joined are overlapped, and the rotating tool is pressed against the overlap portion while rotating. Then, in this state, the rotating tool is moved in the joining direction to join the materials to be joined.

[0032] The rotating tool to be used is not particularly limited, and a general rotating tool used in double-sided friction stir welding can be used. Note that it is preferable to use a material harder than the workpiece for the tip of the rotating tool.

[0033] The metal plate used for the material to be joined is not particularly limited. The metal plate used for the material to be joined is preferably a high melting point steel plate with a melting point of 1350°C or more (particularly, 1400°C or more) at which the wear of the rotary tool is particularly likely to occur, for example, a steel plate with a Si content of 2.0 to 5.0 mass%. The composition of such a steel plate can be exemplified by a composition of C: 0.1% or less, Si: 2.0 to 5.0%, Al: 2.0% or less, and Mn: 1.0% or less, with the balance being Fe and unavoidable impurities, for example. The unavoidable impurities are P: 0.2% or less, S: 0.01% or less, and N: 0.01% or less. The above-mentioned composition may contain at least one selected from the group consisting of Cr: 1% or less, Ni: 1% or less, Cu: 1% or less, Sn: 0.2% or less, Sb: 0.2% or less, Ca: 0.01% or less, REM: 0.05% or less, and Mg: 0.01% or less, in terms of mass %. All elements other than Si and Fe may be 0 mass %. The C content is more preferably 0.001 mass % or more. The Mn content and the Al content are more preferably 0.01 mass % or more. The metal plates used for the joined materials may be of the same steel type or different steel types. Furthermore, the thickness of each metal plate used for the joined materials is preferably 0.2 to 3.2 mm.

[0034] [2]Friction stir welding equipment Next, a friction stir welding apparatus according to an embodiment of the present invention will be described. A friction stir welding apparatus according to one embodiment of the present invention is a friction stir welding apparatus that can be suitably used in the friction stir welding method described above in [1], A pair of opposing rotary tools; a measuring device for measuring a load on the rotary tool; A calculation device that calculates a control range of the separation distance of the rotary tool based on the load of the rotary tool measured by the measurement device based on the above formula (1), preferably the above formula (2); a position adjustment mechanism that changes a position of the rotation tool within a control range of the separation distance of the rotation tool calculated by the calculation device; and has.

[0035] The aspects of the rotary tool are as described above.

[0036] The mode of the measuring device is not particularly limited. For example, the measuring device may be a general load measuring device or torque measuring device capable of measuring the load value in the axial direction of the rotating tool, the load value in the welding direction, or the torque value in the rotation direction. In particular, the measuring device may be a load measuring device or torque measuring device capable of monitoring (measuring at a predetermined interval) the load value in the axial direction of the rotating tool, the load value in the welding direction, or the torque value in the rotation direction.

[0037] Examples of the calculation device include one that has an input unit that inputs data such as various settings and the load of the rotary tool measured at predetermined intervals by a measuring device, a calculation unit that processes the input data, a storage device that stores the data, etc., and an output unit that outputs an operation signal to the position adjustment mechanism based on the results of the calculation by the calculation unit.

[0038] The embodiment of the position adjustment mechanism is not particularly limited, and may be, for example, an electric drive device that moves the rotary tool in the axial direction.

[0039] The configuration of the device other than the above is not particularly limited, and may be the same as that of a conventionally known friction stir welding device.

[0040] [3] Manufacturing method for joining components Next, a method for manufacturing a joint member according to one embodiment of the present invention will be described. A manufacturing method of a welded member according to one embodiment of the present invention is to obtain a welded member by welding workpieces by a friction stir welding method. Here, the welded member has two or more base materials (workpieces) and a welded portion between the base materials (a welded portion that welds the base materials together). Each base material is composed of a metal plate that is a welded material. The welded portion is a region that has become a recrystallized structure by hot working due to frictional heat between a rotary tool and the workpieces and plastic flow. Other conditions than those mentioned above are not particularly limited, and may be in accordance with a conventional method. The number of base materials to be welded at one welded portion may be two or more. The number of base materials to be welded at one welded portion may be, for example, two, or may be between three and five. EXAMPLES

[0041] Two steel plates with a melting point of 1450°C (Si content: 4.0% by mass) and a thickness of 2 mm were butted together and friction stir welded on both sides under the conditions shown in Table 1. The welding was performed under each condition until the dL of the rotating tool reached 0.70. For the rotating tool (front side rotating tool and back side rotating tool), a WC flat-tip tool was used under all conditions. Conditions not specified were as described above or in accordance with the usual method. In both cases, the welding conditions were almost the same on both sides, so only one side is listed in Table 1. In addition, the appearance observation described later was performed on both sides of the joint of the joining members.

[0042] Here, in the invention example No.1, the friction stir welding device described in [2] above was used. Then, while monitoring the load on the rotating tool, the distance between the rotating tool was controlled to satisfy the above formula (1) according to the load on the rotating tool, and welding was performed. In addition, Lint was the load on the rotating tool measured in a preliminary welding test. That is, in the preliminary welding test, in a state where the rotating tool was not worn out, the distance between the rotating tool was set to 0.400 mm, and welding was performed according to the welding conditions planned for the actual welding, and the load on the rotating tool at that time was measured. On the other hand, in the comparative example No.2, welding was performed with the distance between the rotating tool kept at Dint. In the comparative example No.3, the distance between the rotating tool was appropriately changed outside the range of the above formula (1), and welding was performed. The other conditions were in accordance with the usual method. For the load on the rotating tool, the load value in the axial direction of the rotating tool was used.

[0043] The joints of the thus obtained joint members were visually observed and evaluated for joint efficiency at each position where dL was 0.05, 0.09, 0.10, 0.20, 0.30, 0.50, and 0.69. The evaluation results are shown in Table 1. When the visual observation and the joint efficiency were evaluated as "good" at all positions, it was determined that excellent joint property stability was obtained.

[0044] In the appearance observation, those parts where no burrs or defects were visually observed at each position of the joint of the joining parts were rated as "good", and those parts where either burrs or defects were observed were rated as "poor".

[0045] In evaluating joint efficiency, joint efficiency (= breaking strength of joint / breaking strength of base material x 100) of over 90% was rated as "excellent," 70% to 90% was rated as "good," and less than 70% was rated as "poor."

[0046] Here, the breaking strength of the joint was measured as follows. That is, test pieces of the same shape as the No. 1 test piece specified in JIS Z 3121 (2013) were taken from each position of the joint of the obtained joint member so that the joining direction and thickness direction were perpendicular to the longitudinal direction of the test piece and the joint part was located at the center of the parallel part. Next, a tensile test in accordance with JIS Z 3121 (2013) was performed using the taken test pieces to determine the maximum test force (N). The maximum test force (N) thus determined was then multiplied by the cross-sectional area (mm 2 ) was used as the breaking strength of the joint at each position.

[0047] The breaking strength of the base material can also be referred to as the tensile strength (TS) of the base material (the material to be joined). In other words, the breaking strength of the base material can be measured by conducting a tensile test in accordance with JIS Z 2241 (2022). For example, a JIS No. 5 test piece is taken from the base material or the same material as the base material. Then, a tensile test is conducted using the taken test piece at a crosshead speed of 10 mm / min to measure the tensile strength (TS). When the breaking strength differs depending on the base material, the maximum breaking strength of each base material is used in the evaluation of joint efficiency.

[0048] [Table 1]

[0049] As shown in Table 1, in the examples of the invention, the joints of the joint members obtained after joining were evaluated as good in appearance observation and joint efficiency at all positions where dL=0.05, 0.09, 0.10, 0.20, 0.30, 0.50, and 0.69, and excellent stability of joint characteristics of the joints was obtained. On the other hand, in the comparative examples, at least one of the appearance observation and joint efficiency was evaluated as poor at the positions where dL=0.05, 0.09, 0.10, 0.20, 0.30, 0.50, and 0.69, and the desired stability of joint characteristics of the joints was not obtained.

[0050] In addition, when butt joining or lap joining was performed using various high melting point steel plates (various steel plates having the above-mentioned preferred chemical composition, melting points of 1400 to 1530°C, and thicknesses of 0.2 to 3.2 mm) as the joining materials, when the load on the rotating tool and the separation distance of the rotating tool were controlled to satisfy the above formula (1) using the axial load value of the rotating tool, the load value in the joining direction, or the torque value in the rotational direction as the load on the rotating tool, excellent stability of the joint characteristics of the joint was obtained. [Explanation of symbols]

[0051] 1 Rotation tool (front side rotation tool) 2 Rotation tool (reverse side rotation tool) 3 Material to be joined

Claims

1. A friction stir welding method comprising pressing a pair of opposing rotary tools against a front surface and a rear surface of workpieces, respectively, and moving the rotary tools in a joining direction while rotating the workpieces, thereby joining the workpieces, A friction stir welding method, wherein a load on the rotating tool and a distance between the rotating tools satisfy the following relationship: When 0.01≦dL<0.10 dL x 0.1 ≤ dD ≤ dL x 1.0 When 0.10≦dL<0.30 dL x 0.2 - 0.01 ≤ dD ≤ dL x 1.2 - 0.02 When 0.30≦dL<0.70 dL x 0.4 - 0.07 ≤ dD ≤ dL x 1.4 - 0.08 Here, dL=ΔL / Lint. Lint is the initial value of the load of the rotary tool. ΔL is the change in the load of the rotary tool from Lint. In addition, dD=ΔD / Dint, where Dint is the initial value of the separation distance of the rotary tool, and ΔD is the amount of change in the separation distance of the rotary tool from Dint.

2. The friction stir welding method according to claim 1 , wherein the load of the rotating tool is a load value in an axial direction of the rotating tool, a load value in a welding direction, or a torque value in a rotational direction of the rotating tool.

3. The friction stir welding method according to claim 1 , wherein the friction stir welding method is butt welding or lap welding.

4. The friction stir welding method according to claim 2, which is a butt joint or a lap joint.

5. A friction stir welding apparatus used in the friction stir welding method according to any one of claims 1 to 4, A pair of opposing rotary tools; a measuring device for measuring a load on the rotary tool; a calculation device that calculates a control range of the separation distance of the rotary tool based on the load of the rotary tool measured by the measurement device and based on the formula defined in claim 1; a position adjustment mechanism that changes a position of the rotation tool within a control range of the separation distance of the rotation tool calculated by the calculation device; and The friction stir welding apparatus has

6. A method for producing a welded member, comprising the steps of: welding workpieces by the friction stir welding method according to any one of claims 1 to 4 to obtain a welded member.

Citation Information

Patent Citations

  • Device and method for friction stir welding

    JP2022071403A

  • Both- side friction stir bonding method, bonding device, bonding method of metal plate in cold rolling facility and cold rolling facility

    WO2011024320A1

  • Double-sided friction stir welding method for metal plate and double-sided friction stir welding device

    WO2019054400A1

  • Both surface friction agitation joint method and both surface friction agitation joint device

    JP2020124739A

  • Friction stir welding method for electromagnetic steel strip, and method for manufacturing electromagnetic steel strip

    JP2023041556A