Ferrite particles, carrier core material for electrophotographic developer, carrier for electrophotographic developer, and electrophotographic developer

Ferrite particles with a perovskite crystal phase component and controlled composition address the issue of carrier scattering and cracking in electrophotographic developers, ensuring high strength and resistance, thus extending developer lifespan.

JP7578260B2Active Publication Date: 2024-11-06POWDERTECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020140579
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-11-06
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Conventional carrier core materials for electrophotographic developers face challenges in suppressing carrier scattering, particularly under high temperature and high humidity environments, and struggle with controlling the internal sintered state and grain boundary strength, leading to cracking and chipping.

Method used

Ferrite particles with a specific composition (MnO)x(MgO)y(Fe2O3)z and containing a perovskite crystal phase component (RZrO3) are developed, characterized by controlled internal pores, high apparent density, and a resin coating layer, which enhance mechanical strength and resistance to environmental factors.

Benefits of technology

The ferrite particles effectively suppress carrier scattering, maintain high strength and resistance, and extend the lifespan of electrophotographic developers by reducing cracking and chipping, even under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578260000003
    Figure 0007578260000003
  • Figure 0007578260000001
    Figure 0007578260000001
  • Figure 0007578260000002
    Figure 0007578260000002
Patent Text Reader

Abstract

To provide a ferrite particle having high strength, including few cracks or chips, and in which carrier scattering can be curbed, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer.SOLUTION: A ferrite particle includes a crystal phase component consisting of a perovskite type crystal expressed by a composition formula of RZrO3 (here, R represents an alkali earth metal element), and in which, when a particle diameter of individual particles is expressed by a circle equivalent diameter in a cross-section in a reflected electronic image of a particle cross-section photographed by a scanning electron microscope, a content ratio of a particle including an inner hole having the maximum Feret's diameter larger than the particle diameter by more than 15% is 4% or less. The ferrite particle is used as a carrier core material for an electrophotographic developer. Using the ferrite particle, a carrier for an electrophotographic developer and an electrophotographic developer are obtained.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer. [Background technology]

[0002] The electrophotographic development method is a method of developing an electrostatic latent image formed on a photoreceptor by attaching the toner in the developer to the electrostatic latent image formed on the photoreceptor. The developer used in this method is divided into two-component developers consisting of toner and carrier, and one-component developers using only toner. As a development method using two-component developers, the cascade method was used in the past, but currently the magnetic brush method using a magnet roll is the mainstream.

[0003] In the magnetic brush method, the carrier and toner are stirred and mixed in a developing box filled with developer, giving the toner an electric charge. The carrier is then transported to the surface of the photoconductor by a developing roll that holds a magnet. At that time, the carrier transports the charged toner to the surface of the photoconductor. After a toner image is formed on the photoconductor by electrostatic action, the carrier remaining on the developing roll is collected back into the developing box, stirred and mixed with new toner, and reused for a certain period of time.

[0004] Unlike one-component developers, two-component developers have good controllability when designing developers because the magnetic and electrical properties of the carrier itself can be designed separately from the toner. Therefore, two-component developers are suitable for full-color developing devices that require high image quality and high-speed printing devices that require reliability and durability in maintaining images.

[0005] Compared to low-speed printing, high-speed printing imposes a larger agitation load, which makes the carrier more likely to crack or chip, resulting in so-called carrier scattering. Carrier scattering not only causes image defects, but also, if cracked or chipped carrier adheres to the photoconductor or fixing roller, the sharp edges may damage these.

[0006] To address these issues, for example, Patent Document 1 proposes using magnesium ferrite particles containing a predetermined amount of SiO2 as a carrier core material. It is said that by adding a predetermined amount of SiO2, the sintering state can be adjusted and the BET specific surface area can be set within a predetermined range, resulting in a high-strength carrier core material with fewer cracks and chips. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-28060 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, it is difficult to sufficiently suppress the occurrence of carrier scattering in a high-temperature and high-humidity environment with conventional carrier core materials, and the same is true for the carrier core material disclosed in the above Patent Document 1. In addition, in the carrier using the carrier core material disclosed in the above Patent Document 1, although the addition of SiO2 prevents abnormal grain growth and suppresses cracking and chipping during stirring, it is difficult to sufficiently control the internal sintering state. In addition, in the carrier core material disclosed in Patent Document 1, a predetermined degree of internal voids is generated to cause many grain boundaries to exist inside the particles, and the strength of the grain boundaries is increased to prevent a decrease in the mechanical strength of the carrier core material. In other words, in order to cause many grain boundaries to exist in the carrier core material disclosed in Patent Document 1, it is necessary to generate a predetermined degree of internal voids, but the size of the internal voids cannot be sufficiently controlled, and therefore it is considered that the strength of the grain boundaries varies.

[0009] Therefore, an object of the present invention is to provide ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer that have high strength, are less susceptible to cracking or chipping, and can suppress the occurrence of carrier scattering. [Means for solving the problem]

[0010] In order to solve the above problems, the ferrite particles according to the present invention , (MnO)x(MgO)y(Fe 2 O 3 )z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, x+y+z=100(mol%)) in an amount of 50 mass% or more, and SrZrO Composition of 3 In the formula The particle contains a crystalline phase component consisting of perovskite-type crystals represented by the formula: Ferrite particles, comprising a perovskite-type crystal component in an amount of 0.05% by mass or more and 4.00% by mass or less when a phase composition analysis of a crystal phase constituting the ferrite particles is performed by Rietveld analysis of an X-ray diffraction pattern. It is characterized by:

[0011] The apparent density of the ferrite particles according to the present invention is preferably within the range represented by the following formula. 2.15≦ Y ≦ 2.45 In the above formula, Y is the apparent density of the ferrite particles (g / cm 3 ).

[0012] The BET specific surface area of ​​the ferrite particles according to the present invention is preferably within the range represented by the following formula. 0.08≦X≦0.300 In the above formula, X is the BET specific surface area (m 2 / g).

[0015] The carrier core material for an electrophotographic developer according to the present invention is characterized by containing the above-mentioned ferrite particles.

[0016] The carrier for electrophotographic developer according to the present invention is characterized by comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles.

[0017] The electrophotographic developer according to the present invention is characterized by containing the above-mentioned carrier for electrophotographic developer and a toner.

[0018] The electrophotographic developer according to the present invention is also preferably used as a replenishing developer. Effect of the Invention

[0019] According to the present invention, it is possible to provide ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer which have high strength and can suppress the occurrence of carrier scattering even in a high-temperature and high-humidity environment. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a diagram showing a cross section of a ferrite particle, illustrating a method for determining the degree of dispersion of Zr in the ferrite particle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments of the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer according to the present invention will be described. In this specification, the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer mean an aggregate of individual particles, that is, powder, unless otherwise specified. First, the embodiments of the ferrite particles will be described. In addition, hereinafter, the ferrite particles according to the present invention will be described as being mainly used as a carrier core material for electrophotographic developer. However, the ferrite particles according to the present invention can be used for various applications such as magnetic ink, magnetic fluid, magnetic filler, various functional fillers such as fillers for bond magnets and fillers for electromagnetic wave shielding materials, electronic component materials, etc., and the application of the ferrite particles is not limited to the carrier core material for electrophotographic developer.

[0022] 1. Ferrite particles and carrier core material for electrophotographic developers First, an embodiment of the ferrite particles according to the present invention will be described. The ferrite particles according to the present invention are characterized in that they contain a crystalline phase component consisting of perovskite crystals represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element), and when the particle size of each particle is expressed as a circle equivalent diameter in a cross section in a backscattered electron image of the particle cross section photographed by a scanning electron microscope, the content of particles having internal voids whose maximum Feret diameter is greater than 15% of the particle size is 4% or less.

[0023] 1-1. Crystal phase components consisting of perovskite crystals First, a crystal phase component (perovskite-type crystal phase component) made of perovskite-type crystals represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element) will be described.

[0024] As a two-component electrophotographic developer carrier suitable for the magnetic brush method, a resin-coated carrier is used, in which magnetic particles are used as a core material and the surface is coated with resin. Ferrite particles, which are magnetic oxides mainly composed of ferric oxide (Fe2O3), are mainly used as the magnetic particles used as the core material. In order to suppress carrier scattering due to the reduction in carrier particle size, it is required to use ferrite particles with high magnetization and high resistance as the core material.

[0025] In recent years, multi-element ferrite particles containing metal elements such as Mg, Mn, Sr, and Ca in addition to Fe are widely used as core materials. When manufacturing ferrite, metal oxides, metal hydroxides, etc. containing metal elements of the desired composition are used as raw materials. In order to obtain highly magnetized ferrite particles, it is required to sufficiently advance the ferritization reaction of the raw materials so that unreacted raw materials that do not exhibit magnetism (hereinafter referred to as "unreacted raw materials") do not remain in the ferrite particles. However, in the case of multi-element ferrite, the ferrite formation temperature and formation speed differ depending on the combination of elements, and the ferrite reaction proceeds only at the contact surface between the raw materials, so that it is difficult to completely ferrite the raw materials under general firing conditions. Therefore, unreacted raw materials remain in the ferrite particles.

[0026] In addition, the raw materials for ferrite contain metals or metal compounds such as Na that are not involved in the ferrite reaction as unavoidable impurities. These unavoidable impurities do not exhibit magnetism. Therefore, in order to obtain highly magnetized ferrite particles, it is necessary to reduce the amount of unavoidable impurities. However, no matter how pure the raw materials used are, there are still traces of unavoidable impurities in the raw materials, and it is not realistic to completely remove the unavoidable impurities.

[0027] Furthermore, if there is a defect in the organizational structure of the ferrite particles, the magnetization of the ferrite particles will decrease. Structural defects that cause a decrease in magnetization include defects within the ferrite particles (e.g., lattice defects, etc.). In the case of multi-element ferrites, the ferrite reaction is more complex than in single-element ferrites, so structural defects are more likely to occur. Furthermore, if internal voids occur in the particles, especially if the internal voids have a large maximum Feret diameter compared to the particle size, the strength of the particles will decrease.

[0028] Therefore, in order to obtain ferrite particles with high magnetization, high resistance, and high strength, it is necessary to reduce the amount of unavoidable impurities in the ferrite particles. However, as described above, it is not realistic to completely remove the unavoidable impurities. Note that, since the unreacted raw materials (excluding the unavoidable impurities) are metal oxides, the presence of unreacted raw materials does not cause the ferrite particles to have low resistance.

[0029] Incidentally, ferrite particles are often polycrystalline bodies that are aggregates of single crystals. Even if the composition of ferrite particles is the same, the magnetic and electrical properties of the ferrite particles vary depending on the microstructure of the ferrite particles. Therefore, the present inventors have focused on the microstructure of ferrite particles and found that in order to obtain ferrite with high magnetization, high resistance, and high strength, it is important to contain a perovskite-type crystal phase component represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element), and have arrived at the present invention.

[0030] Although it is not clear why the inclusion of a perovskite-type crystal phase component represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element) can solve the above problems, the present inventors speculate as follows.

[0031] At the grain boundaries of ferrite particles, there are components that are not dissolved in ferrite, such as unreacted raw materials and unavoidable impurities. In addition, these components that are pushed out to the grain boundaries as the crystal grains grow are also present on the surface of the ferrite particles. When the crystal grains constituting the ferrite particles are large, the grain boundaries are continuously formed inside the ferrite particles like a flow path connecting one point to another point on the surface of the ferrite particles. The unavoidable impurities present on the surface and grain boundaries of the ferrite particles are easily ionized. Therefore, if unavoidable impurities such as Na are continuously distributed at the grain boundaries continuously formed inside the ferrite particles, when moisture adheres to the surface of the ferrite particles, the grain boundaries become like a conductive path, and the resistance of the ferrite particles decreases. However, as described above, it is difficult to completely remove the unreacted raw materials and unavoidable impurities in the ferrite particles.

[0032] On the other hand, since the perovskite-type crystal phase component represented by the composition formula of RZrO3 (where R is an alkaline earth metal element) is not dissolved in other crystal phases with different crystal structures such as spinel ferrite phase, the crystal phase component is dispersed in the grain boundaries of the ferrite particles. Therefore, the grain boundary volume of the ferrite particles containing the crystal phase component is relatively increased compared to the case where the crystal phase component is not contained. If the amount of inevitable impurities contained in the ferrite particles is the same, the distribution density of the inevitable impurities in the grain boundaries is relatively decreased when the grain boundary volume of the ferrite particles is relatively increased. In addition to the inevitable impurities, the crystal phase component, which is an insulating material, is present in the grain boundaries. In the ferrite particles according to the present invention, the grain boundaries are distributed in a complex manner within the particles, and the inevitable impurities and insulating materials such as the crystal phase component are distributed discontinuously within the grain boundaries, so that the grain boundaries can be prevented from functioning as conductive paths. Therefore, it is considered that the ferrite particles according to the present invention can also reduce the environmental dependency of resistance.

[0033] In addition, by uniformly dispersing the perovskite crystal phase component represented by the formula RZrO3 (where R is an alkaline earth metal element) in the ferrite particles and adopting the manufacturing method described below, it is easy to obtain ferrite particles with fewer internal voids, or even if internal voids are present, with a smaller maximum Feret diameter compared to the particle size and higher strength. In addition, according to the present invention, since the grain boundary volume can be relatively increased as described above, particles with high grain boundary strength can be obtained even without internal voids. Furthermore, since the perovskite crystal phase component is not dissolved in other crystal phase components with different crystal structures such as spinel ferrite phase, when these crystal phases segregate or grow abnormally, cracks and chips are likely to occur starting from the interface.

[0034] In addition, when the grain boundary volume of the ferrite particles is relatively small, the inevitable impurities are pushed out from the grain boundaries to the surface, resulting in a relatively large amount of inevitable impurities present on the ferrite particle surface. On the other hand, when the grain boundary volume of the ferrite particles is relatively large, the amount of inevitable impurities present on the surface of the ferrite particles can be relatively reduced. This makes it possible to increase the resistance of the ferrite particles. Furthermore, the environmental dependency of the resistance caused by the inevitable impurities on the surface of the ferrite particles can be reduced.

[0035] Furthermore, the perovskite-type crystal phase component represented by the composition formula RZrO3 (where R is an alkaline earth metal element) has high insulating properties, and the presence of the crystal phase component at the grain boundary or particle surface can increase the resistance of the ferrite particles. Furthermore, to obtain ferrite particles containing the crystal phase component, a compound containing Zr (e.g., ZrO2) is used as a raw material. For example, when a multi-element ferrite has a composition containing R, the raw material containing R and the compound containing Zr undergo a solid-phase reaction, so that the content of the unreacted raw material in the ferrite particles can be reduced. Therefore, the occurrence of structural defects can be suppressed, and ferrite particles with relatively high magnetization can be obtained, and ferrite particles with few internal voids and small maximum Feret diameters can be obtained even if internal voids exist.

[0036] For these reasons, it is presumed that by using ferrite particles containing a perovskite-type crystal phase component represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element), it is possible to achieve high magnetization, high resistance, and high strength for the reasons mentioned above.

[0037] In the ferrite particles, the perovskite-type crystal phase component represented by the composition formula RzO3 (wherein R is an alkaline earth metal element) means that the crystal phase component is contained at least inside the ferrite particles, and it is preferable that the crystal phase component is well dispersed inside the ferrite particles, and it is more preferable that the crystal phase component is uniformly dispersed on the surface and inside of the ferrite particles. The ferrite particles according to the present invention will be described in more detail below.

[0038] (1) R (alkaline earth metal elements) In the present invention, R is at least one element selected from the group consisting of Ca, Sr, Ba, and Ra, that is, an alkaline earth metal element. The alkaline earth metal element has an ionic radius sufficiently larger than that of zirconium, and forms a perovskite-type crystal structure with zirconium. In the present invention, R is more preferably at least one element selected from the group consisting of Sr, Ca, and Ba. These elements undergo a solid-phase reaction with zirconium under a predetermined temperature condition to form a perovskite-type crystal structure. Therefore, by controlling the firing temperature within a predetermined temperature range in the manufacturing process of the ferrite particles, ferrite particles containing a perovskite-type crystal phase component can be obtained.

[0039] (2) Crystalline phase component content When a phase composition analysis of the crystal phase constituting the ferrite particles is performed by Rietveld analysis of an X-ray diffraction pattern, the perovskite-type crystal phase component represented by the above-mentioned composition formula RZrO3 is preferably contained in an amount of 0.05 mass % or more and 4.00 mass % or less.

[0040] When the content ratio of the perovskite type crystal phase component represented by the composition formula RZrO3 is within the above range, it becomes easy to uniformly disperse the crystal phase component inside the ferrite particles, suppressing the occurrence of structural defects and making it easier to obtain ferrite particles with high magnetization and high resistance. In addition, by setting the content ratio within the above range, it is possible to suppress the segregation of the crystal phase component and the occurrence of internal voids, thereby obtaining ferrite particles with high strength that are less likely to crack or chip when subjected to mechanical stress. As a result, it is also possible to suppress carrier scattering caused by cracks and chips.

[0041] In order to obtain these effects, the ferrite particles preferably contain 0.10 mass % or more of the crystalline phase component, more preferably 0.15 mass % or more, and even more preferably 0.20 mass % or more of the crystalline phase component, and preferably 2.00 mass % or less of the ferrite particles.

[0042] (3) Zirconium content The ferrite particles preferably contain zirconium in an amount of 0.1 mol% or more and 3.0 mol% or less based on the main raw material. By containing zirconium within this range, the content ratio of the perovskite-type crystal phase component represented by the composition formula RZrO3 is approximately within the above range, and ferrite particles with high magnetization, high resistance, and high strength can be obtained. The content ratio of zirconium in the ferrite particles is more preferably 0.2 mol% or more. Furthermore, the content ratio of zirconium in the ferrite particles is more preferably 2.0 mol% or less, and even more preferably 1.5 mol% or less.

[0043] (4) Alkaline earth metal element content The content of the alkaline earth metal element (R) is more preferably 0.1 mol% or more and 3.0 mol% or less with respect to the main raw material. By including the alkaline earth metal element (R) within this range, the content of the perovskite crystal phase component represented by the composition formula RZrO3 is generally within the above range, and ferrite particles having high magnetization, high resistance, and high strength can be obtained. The content of the alkaline earth metal element (R) in the ferrite particles is more preferably 0.2 mol% or more. In addition, the content of the alkaline earth metal element (R) in the ferrite particles is more preferably 2.0 mol% or less, and even more preferably 1.5 mol% or less.

[0044] 1-2. Specified particle content As described above, the ferrite particles are characterized in that, when the particle diameter of each particle is expressed as a circle-equivalent diameter in a cross section in a backscattered electron image (cross-sectional SEM photograph) of a particle cross section taken by a scanning electron microscope, the content of particles (hereinafter referred to as "predetermined particles") having internal voids with a maximum Feret diameter greater than 15% of the particle diameter is 4% or less. Here, the circle-equivalent diameter refers to a value equivalent to the diameter of a perfect circle having the same cross-sectional area as the cross-sectional area of ​​the particle to be measured in the cross-sectional SEM photograph. The maximum Feret diameter refers to the projected width of the internal void of the particle to be measured, and refers to the maximum side length of the horizontal side length (horizontal Feret diameter) and the vertical side length (vertical Feret diameter) of a rectangle circumscribing the internal void to be measured. Such particles having internal voids with a maximum Feret diameter greater than 15% of the particle diameter have weak particle strength and are prone to cracking and chipping when mechanical stress is applied during stirring with toner, etc. In the ferrite particles, the content of the specific particles is 4% or less, so that when mechanical stress is applied, cracks or chips are prevented from occurring in the powder as a whole, and carrier scattering due to cracks or chips in the carrier can be suppressed. The content of the specific particles can be measured by the method described below.

[0045] The smaller the content of the specific particles, the higher the particle strength of the powder as a whole. Therefore, the content of the specific particles is more preferably 3.8% or less, and even more preferably 3.5% or less.

[0046] 1-3.Composition The composition of the ferrite particles is not particularly limited as long as it contains a perovskite-type crystal phase component represented by the composition formula RZrO3 (wherein R is an alkaline earth metal element). However, from the viewpoint of obtaining ferrite particles with high magnetization and high resistance, it is preferable that the ferrite particles mainly contain a crystal phase component (hereinafter, spinel-type crystal phase component) made of a spinel-type crystal represented by the composition formula (MO)a(Fe2O3)b (wherein M is at least one metal element selected from the group consisting of Fe, Mg, Mn, Cu, Zn, and Ni, a+b=100 (mol%)). Ferrite has a crystal structure such as a spinel-type crystal structure, a magnetoplumbite-type crystal structure, or a garnet-type crystal structure, and ferrite with a spinel-type crystal structure exhibits soft magnetism and is easy to adjust electrical properties such as resistance, making it suitable for use as a carrier core material for electrophotographic developers. The term "main component" means that, when the ferrite contains a plurality of crystal phase components (including the perovskite crystal phase component represented by the above-mentioned formula RZrO3 (wherein R is an alkaline earth metal element)), the spinel crystal phase occupies the largest proportion of these crystal phase components. In particular, the spinel crystal phase component is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, and even more preferably 90 mass% or more, and may be 95 mass% or more to 99 mass% or less, so that the majority of the spinel crystal phase component is the spinel crystal phase component. The content of the spinel crystal phase component can be determined by the ratio of metal elements when the raw materials are mixed. Generally, spinel ferrite is produced by a solid-phase reaction. In the ferritization reaction carried out in the firing process, a solid solution (spinel crystal phase) begins to be generated at about 850°C, and the ferritization reaction is completed at about 1250°C. By appropriately adjusting the firing temperature, firing time, firing atmosphere, and cooling time in the firing step, the spinel crystal phase can be selectively generated, and the content ratio of the spinel crystal phase in the ferrite particles can be determined.

[0047] Furthermore, it is more preferable that the ferrite particles mainly contain a spinel crystal phase component represented by the formula (MnO)x(MgO)y(Fe2O3)z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, x+y+z=100 (mol%)). By combining the above composition with a conventional ferrite manufacturing method, it is possible to obtain ferrite with a spinel crystal phase component of 50 mass% or more.

[0048] By making the composition contain Mn, the magnetization on the low magnetic field side can be increased. In addition, by making the composition contain Mn, the reoxidation of ferrite during removal from the furnace after the main firing can be prevented. In particular, by making the Mn content 15 mol% or more, the relative increase in the Fe content can be suppressed, and the content ratio of the magnetite component in the ferrite particles can be suppressed from increasing. Therefore, the decrease in magnetization on the low magnetic field side can be suppressed, and the occurrence of carrier adhesion can be suppressed. In addition, since it becomes easy to adjust the resistance value to a good value for electrophotographic printing, the occurrence of image defects such as fog, deterioration of gradation, and whiteout can be suppressed. Furthermore, the toner consumption can be kept at an appropriate level. By making the Mn content 50 mol% or less, the resistance becomes too high, and the occurrence of image defects such as whiteout can be suppressed.

[0049] By making the composition contain Mg, it is possible to obtain ferrite particles with high resistance. In addition, by making the Mg content 2 mol% or more, the Mn content becomes appropriate relative to the Fe content, and it becomes easy to adjust the magnetization and resistance of the ferrite particles within a favorable range for electrophotographic printing. Therefore, it is possible to suppress the occurrence of image defects such as fog, deterioration of gradation, the occurrence of brush lines, and carrier scattering. Furthermore, when magnesium hydroxide is used as the Mg raw material, if the firing temperature during the production of the ferrite particles is low, hydroxyl groups may remain in the ferrite particles. By making the Mg content 35 mol% or less, it is possible to reduce the amount of residual hydroxyl groups present due to the raw material. Therefore, it is possible to suppress the electrical properties of the ferrite particles, such as the charge amount and resistance, from fluctuating due to the influence of the atmospheric humidity due to the residual hydroxyl groups, and to improve the environmental dependency of the electrical properties of the ferrite particles.

[0050] The ferrite particles are magnetic oxides whose main component is ferric oxide. By setting the Fe content to 45 mol% or more and 60 mol% or less, it becomes easy to adjust the magnetization and resistance of the ferrite particles to within a favorable range for electrophotographic printing.

[0051] 1-4.Magnetic properties When the ferrite particles are used as a core material of a carrier for electrophotographic developer, it is preferable that the saturation magnetization measured by VSM when a magnetic field of 1K·1000 / 4π·A / m is applied is 55 emu / g or more and 65 emu / g or less. When the saturation magnetization is 55 emu / g or more, the magnetic force of the core material is high, and carrier scattering caused by low magnetization can be suppressed well. In addition, although there is a trade-off between saturation magnetization and electrical resistance, when the saturation magnetization of the ferrite particles is within the above range, the balance between the two is good, and an electrophotographic developer capable of performing high-quality electrophotographic printing well can be obtained. In addition, even if the magnetization is high, if the resistance is low, carrier scattering due to low resistance may occur. By setting the saturation magnetization to 65 emu / g or less, carrier scattering due to low resistance can also be suppressed well.

[0052] 1-5.Electrical characteristics When measured with an electrode distance of 6.5 mm and an applied voltage of 1000 V, the resistance M in a normal temperature and humidity environment (23°C, 55% relative humidity) is 1.0×10 6 (Ω) or more 1.0×10 9.5 When the resistance value of the ferrite particles is within this range, when the ferrite particles are used as a core material and a resin coating layer is provided on the surface to form a carrier, the resin coating layer peels off during mixing with the toner, exposing the core material, and carrier scattering due to charge injection can be suppressed.

[0053] 1-6.Physical properties (1) Apparent density The apparent density of the ferrite particles is preferably within the range represented by the following formula. 2.15≦Y≦2.45 In the above formula, Y is the apparent density of the ferrite particles (g / cm 3 )

[0054] The apparent density here refers to a value measured by the funnel method in accordance with JIS Z 2504:2012. When the apparent density of the ferrite particles is within the range represented by the above formula, there are few internal voids, and even if there are internal voids, the maximum Feret diameter is small and the strength is high. Therefore, if a carrier having the ferrite particles as a core material is used, cracking and chipping can be prevented even if mechanical stress is applied during mixing and stirring with the toner.

[0055] When the apparent density of the ferrite particles is small, the number of internal voids tends to be large, or the maximum Feret diameter of the internal voids tends to be large. Therefore, when mechanical stress is applied to the carrier having the ferrite particles as a core material during mixing and stirring with the toner, cracks and chips are likely to occur. When the carrier cracks or chips, image defects due to carrier scattering may occur, or the carrier may adhere to the photoconductor drum or the fixing roller and damage them. On the other hand, when the apparent density of the ferrite particles exceeds 2.50, the internal voids are reduced, but the crystal grains become coarse due to oversintering. In this case, if the perovskite crystal phase component is segregated within the particles, as described above, when mechanical stress is applied, cracks and chips are likely to occur starting from the interface of the crystal phase, which is not preferable because it may cause image defects due to carrier scattering and damage to the photoconductor drum or the fixing roller.

[0056] In order to obtain these effects, the apparent density of the ferrite particles is preferably 2.18 or more, more preferably 2.20 or more, and more preferably 2.40 or less, and even more preferably 2.35 or less.

[0057] To obtain ferrite particles having an apparent density within the above range, the amount of the alkaline earth metal element-containing compound and zirconium oxide used as raw materials in producing the ferrite particles, the particle size and specific surface area of ​​zirconium oxide, the firing temperature, the firing time, the oxygen concentration of the atmosphere during firing, etc. can be appropriately adjusted. By adjusting these, segregation of the perovskite crystal phase component can be suppressed, and the crystal phase component can be uniformly dispersed on the particle surface and inside. In addition, for the reason described above, the occurrence of structural defects can be prevented, and the growth of other crystal phase components such as spinel ferrite phase can be suppressed. For these reasons, it is considered that ferrite particles having a desired apparent density can be obtained by appropriately adjusting the above conditions.

[0058] (2) BET specific surface area The BET specific surface area of ​​the ferrite particles is preferably within the range represented by the following formula. 0.08≦X≦0.300 In the above formula, X is the BET specific surface area (m 2 / g).

[0059] The BET specific surface area here can be a value measured using, for example, a specific surface area measuring device (model: Macsorb HM model-1208 (manufactured by Mountec Co., Ltd.)). When the BET specific surface area of ​​the ferrite particles is within the range expressed by the above formula, the surface irregularities of the ferrite particles are within an appropriate range for the particle size. Therefore, when the ferrite particles are used as a core material, the surface can be well coated with resin. In addition, since the difference in surface irregularities relative to the particle size is small, when mechanical stress is applied to the surface, the load is suppressed from convex portions, and cracks and chips can be prevented. Therefore, when the ferrite particles are used as a core material, peeling of the resin from the surface during mixing and stirring with the toner can be suppressed, and cracks and chips of the carrier can be prevented, and carrier scattering, etc. can be prevented.

[0060] On the other hand, when the BET specific surface area is less than 0.08, the unevenness of the ferrite particle surface relative to the particle size is small or too small, so that when the ferrite particle is used as a core material and the surface is coated with a resin, the resin is easily peeled off when mixed with a toner. When the resin peels off from the surface of the carrier, the core material is exposed at that part. That is, the surface of the ferrite particle is exposed, so that image defects due to carrier scattering and reduced charging ability are likely to occur. On the other hand, as the BET specific surface area increases, the unevenness of the ferrite particle surface relative to the particle size increases or increases, so that it becomes difficult to coat the convex parts of the ferrite particles with a resin, and the convex parts may be exposed. Therefore, it may not be possible to obtain a carrier having sufficient charging ability for the toner. In addition, when the surface unevenness increases, mechanical stress is applied to the convex parts of the carrier surface when mixed with a toner, etc., and the load is concentrated on the convex parts, which makes the carrier more likely to crack or chip. For these reasons, it is preferable to set the BET specific surface area to less than 0.300, since this makes it possible to maintain good carrier strength when the developer is used.

[0061] The ferrite particles having a BET specific surface area within the above range can be obtained by appropriately controlling the granulation conditions and sintering conditions when producing the ferrite particles. Examples of the granulation conditions include the slurry particle size during granulation, the atomizer disk rotation speed, the slurry discharge amount, and the drying temperature. Examples of the sintering conditions include the sintering temperature, the sintering time, and the atmospheric oxygen concentration during sintering. By adjusting these conditions, the raw material of the perovskite-type crystal phase component represented by the composition formula RZrO3 (where R is an alkaline earth metal element) can be well mixed and dispersed with other raw materials, and as a result, ferrite particles in which the crystal phase component is uniformly dispersed on the particle surface and inside can be obtained, and the apparent density of the ferrite particles can be adjusted to a desired range.

[0062] (3) Particle strength index When the particle strength index is determined by the method described in the examples below, the particle strength index of the ferrite particles is preferably 0.5 or less, more preferably 0.4 or less. The ferrite particles having a content of the above-mentioned specific particles of 4% or less have high strength, and even when mechanical stress is applied during stirring with toner, the occurrence of cracks and chips can be suppressed, and the occurrence of carrier scattering due to the generation of fine powder can be suppressed. Furthermore, when a carrier is used in which ferrite particles are used as a core material and the surface of the carrier has a resin coating layer, if cracks or chips occur, the ferrite particles as the core material are exposed, and the chargeability of the carrier changes, which may cause a decrease in image density or toner scattering. However, the ferrite particles have high particle strength, so these problems can be suppressed for a long period of time, and a carrier with a longer life and higher reliability can be realized.

[0063] (4) Volume average particle size (D 50 ) When the ferrite particles are used as a core material of a carrier for an electrophotographic developer, the volume average particle diameter (D 50 ) is preferably 24 μm or more and 40 μm or less. However, the volume average particle diameter referred to here is a value measured in accordance with JIS Z 8825:2013 by a laser diffraction / scattering method. When the volume average particle diameter is within this range, the charge imparting property to the toner is high, and the charge imparting property can be maintained for a long period of time. Therefore, the life of the electrophotographic developer can be extended.

[0064] In contrast, the volume average particle size (D 50 If the volume average particle diameter (D 50) is less than 24 μm, the particle size is small, and the ferrite particles are likely to aggregate. When the ferrite particles are used as a core material and the surface is coated with a resin to form a carrier, if the ferrite particles are aggregated, the surface of each ferrite particle cannot be well coated with the resin. If the aggregate of the ferrite particles is subsequently loosened during the manufacture or use of the developer, the developer will have a high content of carrier with a large area not coated with resin. Therefore, when a developer is manufactured using a carrier having such ferrite particles as a core material, sufficient charge imparting properties to the toner may not be obtained, which is not preferable.

[0065] On the other hand, the volume average particle size (D 50 When the volume average particle size (D) exceeds 40 μm, the particle size of each particle constituting the powder becomes large. 50 ) is smaller than that of ferrite particles, the surface area of ​​the carrier that contributes to triboelectric charging with the toner is smaller when viewed as a whole powder. Therefore, sufficient charge imparting ability to the toner may not be obtained. In order to improve this, by increasing the surface area of ​​each ferrite particle by giving unevenness to the surface of each ferrite particle, the surface area of ​​the carrier that contributes to triboelectric charging with the toner can be increased. In this case, the charge imparting ability to the toner is improved, but it is not preferable because the carrier is likely to crack or chip due to mechanical stress applied to the protrusions on the carrier surface when mixed with the toner. In other words, it may not be possible to maintain the strength of the carrier when used as a developer, which is not preferable.

[0066] 2. Carrier for electrophotographic developer Next, the electrophotographic developer carrier according to the present invention will be described. The electrophotographic developer carrier according to the present invention is characterized by comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles. That is, the above-mentioned ferrite particles are characterized by being used as a core material of the electrophotographic developer carrier. The ferrite particles are as described above, so here, the resin coating layer will be mainly described.

[0067] (1) Type of coating resin The type of resin (coating resin) constituting the resin coating layer is not particularly limited. For example, fluororesin, acrylic resin, epoxy resin, polyamide resin, polyamideimide resin, polyester resin, unsaturated polyester resin, urea resin, melamine resin, alkyd resin, phenol resin, fluoroacrylic resin, acrylic-styrene resin, silicone resin, etc. can be used. In addition, modified silicone resins obtained by modifying silicone resins with acrylic resins, polyester resins, epoxy resins, polyamide resins, polyamideimide resins, alkyd resins, urethane resins, fluororesins, etc. may be used. For example, from the viewpoint of suppressing resin peeling due to mechanical stress received during stirring and mixing with toner, it is preferable that the coating resin is a thermosetting resin. Examples of thermosetting resins suitable for the coating resin include epoxy resins, phenol resins, silicone resins, unsaturated polyester resins, urea resins, melamine resins, alkyd resins, and resins containing them. However, as described above, the type of coating resin is not particularly limited, and an appropriate one can be selected depending on the type of toner to be combined and the usage environment.

[0068] The resin coating layer may be formed using one type of resin, or may be formed using two or more types of resin. When using two or more types of resin, one resin coating layer may be formed by mixing two or more types of resin, or multiple resin coating layers may be formed. For example, it is also preferable to provide a first resin coating layer having good adhesion to the ferrite particles on the surface of the ferrite particles, and provide a second resin coating layer on the surface of the first resin coating layer to impart the carrier with the desired charging performance.

[0069] (2) Resin coating amount The amount of resin (amount of resin coating) covering the surface of the ferrite particles is preferably 0.1% by mass or more and 10% by mass or less with respect to the ferrite particles used as the core material. If the amount of resin coating is less than 0.1% by mass, it becomes difficult to sufficiently coat the surface of the ferrite particles with resin, and it becomes difficult to obtain the desired charge-imparting ability. If the amount of resin coating exceeds 10% by mass, aggregation of carrier particles occurs during production, which not only reduces productivity such as a decrease in yield, but also fluctuates developer properties such as the fluidity of the developer in the actual machine or the charge-imparting ability to the toner, which is not preferable.

[0070] (3) Additives The resin coating layer may contain additives such as conductive agents and charge control agents for controlling the electrical resistance, charge amount, and charging speed of the carrier. Examples of conductive agents include conductive carbon, oxides such as titanium oxide and tin oxide, and various organic conductive agents. However, since the electrical resistance of the conductive agent is low, if the amount of the conductive agent added is too large, charge leakage is likely to occur. Therefore, the content of the conductive agent is preferably 0.25% by mass or more and 20.0% by mass or less, more preferably 0.5% by mass or more and 15.0% by mass or less, and even more preferably 1.0% by mass or more and 10.0% by mass or less, based on the solid content of the coating resin.

[0071] Examples of the charge control agent include various charge control agents and silane coupling agents that are generally used for toners. The types of these charge control agents and coupling agents are not particularly limited, but charge control agents such as nigrosine dyes, quaternary ammonium salts, organometallic complexes, and metal-containing monoazo dyes, aminosilane coupling agents, and fluorine-based silane coupling agents can be preferably used. The content of the charge control agent is preferably 0.25% by mass or more and 20.0% by mass or less, more preferably 0.5% by mass or more and 15.0% by mass or less, and even more preferably 1.0% by mass or more and 10.0% by mass or less, based on the solid content of the coating resin.

[0072] 3. Electrophotographic Developer Next, an embodiment of the electrophotographic developer according to the present invention will be described The electrophotographic developer contains the above-mentioned carrier for electrophotographic developer and a toner.

[0073] As the toner constituting the electrophotographic developer, for example, either a polymerized toner produced by a polymerization method or a pulverized toner produced by a pulverization method can be preferably used. These toners may contain various additives, and may be any toner as long as they can be used as an electrophotographic developer in combination with the above carrier.

[0074] Toner volume average particle size (D 50 The volume average particle diameter (D) of the toner is preferably 2 μm or more and 15 μm or less, and more preferably 3 μm or more and 10 μm or less. 50 ) within this range, an electrophotographic developer capable of performing high-quality electrophotographic printing can be obtained.

[0075] The mixture ratio of the carrier and the toner, that is, the toner concentration, is preferably 3% by mass or more and 15% by mass or less. An electrophotographic developer containing the toner at this concentration can easily obtain a desired image density and can more effectively suppress fogging and toner scattering.

[0076] On the other hand, when the electrophotographic developer is used as a replenishing developer, the toner content is preferably 2 parts by mass or more and 50 parts by mass or less per part by mass of the carrier.

[0077] The electrophotographic developer can be suitably used in various electrophotographic developing devices that apply a magnetic brush development method in which a carrier is attracted and attached to a magnetic drum or the like by magnetic force to form a brush-like toner, and a visible image is formed by attaching the toner to an electrostatic latent image formed on a photoconductor or the like while applying a bias electric field. The electrophotographic developer can be used not only in electrophotographic developing devices that use a DC bias electric field when applying a bias electric field, but also in electrophotographic developing devices that use an AC bias electric field in which an AC bias electric field is superimposed on a DC bias electric field.

[0078] 4. Manufacturing method The following describes the methods for producing the ferrite powder, the carrier core material for an electrophotographic developer, the carrier for an electrophotographic developer, and the electrophotographic developer according to the present invention.

[0079] 4-1. Ferrite powder and carrier core material for electrophotographic developers The ferrite powder and the carrier core material for an electrophotographic developer according to the present invention can be produced as follows.

[0080] First, raw materials are weighed in appropriate amounts so as to obtain a desired ferrite composition, and then pulverized and mixed in a ball mill or a vibration mill for 0.5 hours or more, preferably 1 hour to 20 hours, and then calcined.

[0081] For example, to produce ferrite particles mainly composed of a spinel-type crystal phase component represented by the composition formula (MnO)x(MgO)y(Fe2O3)z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, x+y+z=100 (mol%)), each raw material is weighed and pulverized and mixed so that x, y, and z are the desired values. As the raw materials, for example, it is preferable to use Fe2O3, Mg(OH)2 and / or MgCO3, and one or more manganese compounds selected from the group consisting of MnO2, Mn2O3, Mn3O4, and MnCO3.

[0082] The ferrite particles according to the present invention contain a perovskite-type crystalline phase component represented by the formula RZrO3 (wherein R is an alkaline earth metal element). Therefore, for the alkaline earth metal element (R), an oxide of the alkaline earth metal element (R) is used as a raw material, weighed out to obtain a desired amount, and pulverized and mixed with other raw materials. For Zr, ZrO2 can be used as a raw material.

[0083] Here, when manufacturing ferrite particles containing the perovskite crystal phase component in an amount of 0.05% by mass or more and 2.50% by mass or less (however, this is the mass fraction obtained when performing a phase composition analysis of the crystal phase constituting the ferrite particles by Rietveld analysis of the X-ray diffraction pattern), it is preferable to mix ZrO2: 0.1 to 3.0 in a molar ratio with respect to 100 of the main component raw material, and more preferably to mix ZrO2: 0.2 to 1.5 in a molar ratio with respect to 100 of the main component raw material. Also, it is preferable to mix an oxide of an alkaline earth metal element (R): 0.1 to 3.0 in a molar ratio with respect to 100 of the main component raw material, and more preferably to mix ZrO2: 0.2 to 1.5 in a molar ratio with respect to 100 of the main component raw material. The perovskite crystal phase component is generated by a solid-phase reaction between the oxide of an alkaline earth metal element (R) and ZrO2. Therefore, by appropriately changing the amounts and ratios of the oxide of the alkaline earth metal element (R) and ZrO2 added within the above-mentioned preferred ranges, it is possible to adjust the amount of the perovskite crystal phase component produced.

[0084] When producing the ferrite particles according to the present invention, ZrO2 is weighed out to a desired amount and pulverized and mixed with other raw materials. In order to uniformly disperse zirconium dioxide inside the particles, it is preferable to add zirconium dioxide when pulverizing and mixing the raw materials. It is also preferable to pulverize and mix raw materials other than ZrO2, calcinate them in the atmosphere, add ZrO2, and further pulverize and mix them. In this case, the pulverized mixture of raw materials other than ZrO2 is pelletized using a pressure molding machine or the like, calcined in the atmosphere at a temperature of 700°C to 1200°C, and then ZrO2 is added.

[0085] After all the raw materials including ZrO2 are ground and mixed, or after raw materials other than ZrO2 are ground and mixed and calcined, a predetermined amount of ZrO2 is added to the calcined product obtained, which is then ground in a ball mill or a vibration mill, and in either case, water is added to the ground mixture and finely ground using a bead mill or the like to obtain a slurry. The degree of grinding can be controlled by adjusting the diameter, composition, and grinding time of the beads used as media. In order to uniformly disperse the raw materials, it is preferable to use fine beads having a particle size of 1 mm or less as the media. In addition, in order to obtain ferrite particles whose content of the above-mentioned predetermined particles is within the range of the present invention, the volume average particle size (D 50 It is preferable to pulverize the powder so that the particle diameter (D) is 2.0 μm or less, and more preferably 1.5 μm or less. By adopting this method, it is possible to obtain ferrite particles having few internal voids, or even if internal voids are present, the particles have a small maximum Feret diameter. In addition, in order to suppress abnormal grain growth, it is possible to obtain ferrite particles having a particle diameter (D) on the coarse side of the grain size distribution. 90 ) is preferably pulverized to 3.5 μm or less. By adjusting these factors, the perovskite crystal phase components can be more uniformly dispersed from the surface to the interior of the particles.

[0086] Furthermore, in order to obtain ferrite particles having a BET specific surface area and an apparent density in the above-mentioned preferred ranges, the BET specific surface area is preferably 20 to 150 m 2 / g, and the volume average particle size (D 50 It is preferable to use ZrO2 having a particle size of 0.5 μm to 2.5 μm as the raw material. By using a raw material having such characteristics, it is possible to uniformly advance the growth of the perovskite type crystal phase component while dispersing ZrO2 well within the particles. It is possible to suppress the segregation of the crystal phase component within the particles and the abnormal grain growth of each crystal phase component. Therefore, even when mechanical stress is applied, it is possible to suppress the occurrence of cracks and chips at the interface between different crystal phases that are not solid-soluble with each other, and to improve the strength of the ferrite particles.

[0087] Next, it is preferable to add a dispersant, a binder, etc. to the slurry thus obtained as necessary to adjust the viscosity to 2 poise to 4 poise. At this time, polyvinyl alcohol or polyvinylpyrrolidone can be used as the binder.

[0088] The slurry prepared as above is sprayed and dried using a spray dryer to obtain a granulated product. In this case, the granulation conditions are preferably set to a discharge rate of 20 Hz to 50 Hz, an atomizer disk rotation speed of 11000 rpm to 20000 rpm, and a drying temperature of 100° C. to 500° C. For example, in order to obtain ferrite particles having an apparent density within the above range, it is preferable to set the atomizer disk rotation speed to 11000 rpm to 16000 rpm and a drying temperature to 150° C. to 300° C.

[0089] Next, it is preferable to classify the granulated material before firing it to remove fine particles contained in the granulated material in order to obtain a ferrite powder with a uniform particle size. The classification of the granulated material can be performed using a known air classification or a sieve.

[0090] Next, the classified granules are fired. It is preferable that the granules are fired as necessary after primary firing. When primary firing is performed, the firing temperature is preferably 600°C or higher and 900°C or lower.

[0091] The firing is preferably carried out in an inert atmosphere or a weakly oxidizing atmosphere at a temperature of 850° C. or higher for 4 hours to 24 hours, but the firing temperature is not particularly limited as long as the ferrite particles according to the present invention can be obtained. Here, an inert atmosphere or a weakly oxidizing atmosphere refers to an atmosphere of a mixed gas of nitrogen and oxygen in which the oxygen concentration is 0.1 volume % (1000 ppm) to 5 volume % (50,000 ppm), preferably 0.1 volume % (1000 ppm) to 3.5 volume % (35,000 ppm), more preferably 0.1 volume % (1000 ppm) to 2.5 volume % (25,000 ppm), even more preferably 0.1 volume % (1000 ppm) to 1.5 volume % (25,000 ppm), and even more preferably 0.1 volume % (1000 ppm) to 1.0 volume % (25,000 ppm).

[0092] Furthermore, in order to obtain ferrite particles having a content of the above-mentioned predetermined particles within the range of the present invention, the heating rate up to the main sintering temperature is 30° C. / hour or more and 100° C. / hour or less. time C. / hour or less, more preferably from 40 to 90.degree. C. / hour, and even more preferably from 50 to 85.degree. C. / hour.

[0093] For example, in order to produce ferrite particles mainly composed of a spinel-type crystal phase component represented by the composition formula (MnO)x(MgO)y(Fe2O3)z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, x+y+z=100 (mol%)), it is more preferable to hold the ferrite component made of spinel crystals at a temperature suitable for generating the ferrite component made of spinel crystals (850°C or higher and 1150°C or lower) for 3 hours or more in order to sufficiently generate the ferrite component made of spinel crystals while dispersing the zirconium component at the grain boundaries, and then hold the ferrite component at a temperature suitable for generating a perovskite-type crystal phase component represented by the composition formula RZrO3, such as strontium zirconate, for 1 hour or more to perform the main firing. In addition, at that time, by appropriately controlling the firing temperature, firing time, and atmospheric oxygen concentration during firing according to the type of alkaline earth metal element (R) and the amount of ZrO2 blended, the BET specific surface area can be within the range of the present invention.

[0094] For example, in the case of strontium zirconate (SrZrO3), in order to obtain an apparent density within the range of the present invention while sufficiently generating perovskite crystal phase components, it is preferable to maintain the firing temperature at a temperature of preferably 1170°C to 1400°C, more preferably 1180°C to 1350°C, and even more preferably 1200°C to 1330°C for one hour or more. In this case, the amount of zirconium oxide (ZrO2) blended is preferably 0.05 mol to 3.00 mol.

[0095] For example, in the case of calcium zirconate (CaZrO3) or barium zirconate (BaZrO3), it is preferable to pulverize the raw material, add a reaction accelerator, and then sinter at a predetermined temperature. In order to generate the perovskite crystal phase components of calcium zirconate (CaZrO3) or barium zirconate (BaZrO3), it is necessary to sinter at a high temperature of 2000°C or higher if no reaction accelerator is added. On the other hand, by pulverizing the raw material to a primary particle size of about several tens of nanometers and adding an aluminum compound (e.g., alumina (Al2O3), etc.) as a reaction accelerator, these perovskite crystal phase components can be generated even at a temperature of 1500°C or lower. In this way, the ferrite particles according to the present invention can be obtained by maintaining the temperature suitable for generating the perovskite crystal phase components according to the target composition and adjusting other conditions as necessary.

[0096] In addition, when the main firing is performed, it is preferable to use a firing furnace such as a tunnel kiln or elevator kiln in which the granulated material (material to be fired) is passed through the hot section while being moved, rather than a firing furnace such as a rotary kiln in which the granulated material is passed through the hot section while being moved. In a firing furnace such as a rotary kiln in which the granulated material is passed through the hot section while being moved, if the oxygen concentration in the firing atmosphere is low, the granulated material may adhere to the inner surface of the furnace when passing through the hot section, and the granulated material passing through the inside while flowing may not be able to be sufficiently heated. In that case, the granulated material passes through the hot section without being sufficiently sintered, so that the surface of the obtained fired material is sufficiently sintered, but the inside is often insufficiently sintered. Such fired material does not meet the strength required for a carrier core material for electrophotographic developer, and the ferrite reaction inside is insufficient, so that the magnetic properties and electrical properties required for a carrier core material for electrophotographic developer may not be met. Furthermore, if the sintering inside the fired product is insufficient, the perovskite crystal phase component represented by the composition formula RZrO3 cannot be sufficiently generated in the firing process, which makes it difficult to obtain the ferrite particles according to the present invention.

[0097] On the other hand, if the granulated material is placed in a sintering bowl or the like and passed through a hot section while remaining stationary, the inside of the sintered material can be sufficiently sintered, making it easy to obtain ferrite particles that are highly magnetized and highly resistive and in which the perovskite-type crystal phase component represented by the composition formula RZrO3 is sufficiently generated. For these reasons, it is preferable to use a tunnel kiln, elevator kiln, or the like when carrying out the main sintering step.

[0098] The fired product is then crushed and classified to obtain ferrite particles. As classification methods, the particle size is adjusted to the desired particle size using existing methods such as air classification, mesh filtration, and sedimentation. In the case of dry recovery, recovery can also be performed using a cyclone or the like. When adjusting the particle size, two or more of the above-mentioned classification methods may be selected and performed, or the conditions of one classification method may be changed to remove coarse particles and fine particles.

[0099] Thereafter, if necessary, the surface of the ferrite particles is heated at a low temperature to perform a surface oxidation treatment, thereby adjusting the surface resistance of the ferrite particles. The surface oxidation treatment can be performed by subjecting the ferrite particles to a heat treatment at 400°C to 730°C, preferably 450°C to 650°C, in an oxygen-containing atmosphere such as air, using a rotary electric furnace, a batch electric furnace, or the like. If the heating temperature during the surface oxidation treatment is lower than 400°C, the surface of the ferrite particles cannot be sufficiently oxidized, and the desired surface resistance characteristics may not be obtained. On the other hand, if the heating temperature is higher than 730°C, in the case of manganese-containing ferrite, the oxidation of manganese proceeds too much, and the magnetization of the ferrite particles decreases, which is not preferable. To form a uniform oxide film on the surface of the ferrite particles, it is preferable to use a rotary electric furnace. However, the surface oxidation treatment is an optional step.

[0100] 4-2. Carrier for electrophotographic developer The electrophotographic developer carrier according to the present invention is a carrier in which the above-mentioned ferrite particles are used as a core material and a resin coating layer is provided on the surface of the ferrite particles. The resin constituting the resin coating layer is as described above. When forming a resin coating layer on the surface of the ferrite particles, a known method such as a brush coating method, a spray drying method using a fluidized bed, a rotary drying method, a liquid immersion drying method using a universal stirrer, etc. can be adopted. In order to improve the ratio of the resin coating area to the surface of the ferrite particles (resin coating rate), it is preferable to adopt a spray drying method using a fluidized bed. In any case, the ferrite particles can be subjected to a resin coating treatment once or multiple times. The resin coating liquid used in forming the resin coating layer may contain the above-mentioned additives. In addition, since the amount of resin coating on the surface of the ferrite particles is as described above, a description thereof will be omitted here.

[0101] After applying the resin coating liquid to the surface of the ferrite particles, baking may be performed by an external heating method or an internal heating method as necessary. For the external heating method, a fixed or flow type electric furnace, a rotary type electric furnace, a burner furnace, etc. can be used. For the internal heating method, a microwave furnace can be used. When a UV-curable resin is used as the coating resin, a UV heater is used. Baking is required to be performed at a temperature equal to or higher than the melting point or glass transition point of the coating resin. When a thermosetting resin or a condensation crosslinking type resin is used as the coating resin, baking is required at a temperature at which the curing of these resins progresses sufficiently.

[0102] 4-3.Electrophotographic developer Next, a method for producing an electrophotographic developer according to the present invention will be described. The electrophotographic developer according to the present invention contains the above-mentioned carrier for electrophotographic developer and a toner. As the toner, either a polymerized toner or a pulverized toner can be preferably used as described above.

[0103] The polymerized toner can be produced by a known method such as a suspension polymerization method, an emulsion polymerization method, an emulsion aggregation method, an ester elongation polymerization method, or a phase inversion emulsification method. For example, a colored dispersion liquid in which a colorant is dispersed in water using a surfactant is mixed and stirred with a polymerizable monomer, a surfactant, and a polymerization initiator in an aqueous medium, and the polymerizable monomer is emulsified and dispersed in the aqueous medium, and polymerized while stirring and mixing, and then a salting agent is added to salt out the polymer particles. The particles obtained by salting out are filtered, washed, and dried to obtain a polymerized toner. Thereafter, an external additive may be added to the dried toner particles as necessary.

[0104] Furthermore, when producing the polymerized toner particles, a toner composition containing a polymerizable monomer, a surfactant, a polymerization initiator, a colorant, etc. The toner composition may contain a fixing improver and a charge control agent.

[0105] The pulverized toner is prepared by thoroughly mixing, for example, a binder resin, a colorant, a charge control agent, etc., in a mixer such as a Henschel mixer, then melt-kneading and uniformly dispersing in a twin-screw extruder, etc., cooling, finely pulverizing in a jet mill, etc., classifying, and then classifying, for example, with an air classifier, etc., to obtain a toner of a desired particle size. If necessary, wax, magnetic powder, viscosity modifier, and other additives may be added. Furthermore, external additives may be added after classification.

[0106] The present invention will now be described in detail with reference to examples and comparative examples, although the present invention is not limited to the following examples. EXAMPLES

[0107] (1) Ferrite particles In Example 1, ferrite particles containing a spinel-type crystal phase component represented by the composition formula (MnO)x(MgO)y(Fe2O3)z as the main component and a perovskite-type crystal phase component represented by the composition formula (R=Sr) of SrZrO3 were manufactured as follows. First, as the main component raw materials, MnO raw material, MgO raw material, and Fe2O3 raw material were weighed out so that the molar ratios were 38.3 in terms of MnO, 10.4 in terms of MgO, and 51.3 in terms of Fe2O3. In addition, the SrO raw material was weighed out so that the molar ratio was 100 in terms of the main component raw material and 0.8 in terms of SrO. Here, trimanganese tetroxide was used as the MnO raw material, magnesium oxide was used as the MgO raw material, ferric oxide was used as the Fe2O3 raw material, and strontium carbonate was used as the SrO raw material.

[0108] The weighed raw material was then pulverized for 5 hours in a dry media mill (vibration mill, 1 / 8 inch diameter stainless steel beads), and the resulting pulverized material was made into pellets of about 1 mm square using a roller compactor. The resulting pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder, and then heated at 800°C for 3 hours in a continuous electric furnace for preliminary firing. The raw material was then pulverized using a dry media mill (vibration mill, 1 / 8 inch diameter stainless steel beads) until the average particle size was about 5 μm. The pulverization time was 6 hours.

[0109] The resulting crushed material was mixed with water and a ZrO2 raw material with a BET specific surface area of ​​30 m 2 Zirconium dioxide with a mean particle size of 2 μm was added and ground for 6 hours using a wet media mill (horizontal bead mill, zirconia beads with a diameter of 1 mm). At this time, zirconium dioxide was added to the ground material so that the molar ratio of the main component raw material: 100 to ZrO2: 1.0 was achieved. The particle size of the resulting slurry (primary particle size of the ground material) was measured using a laser diffraction particle size distribution analyzer (LA-950, Horiba, Ltd.). 50 was 0.9 μm.

[0110] Further, an appropriate amount of dispersant was added to the slurry prepared as above, and 0.4 mass% of PVA (polyvinyl alcohol) was added as a binder relative to the solid content (the amount of the pre-calcined material in the slurry), followed by granulation and drying using a spray dryer. The particle size of the resulting granulated material was adjusted, and then the material was heated in a rotary electric furnace at 800°C for 2 hours in an air atmosphere to remove organic components such as the dispersant and binder.

[0111] The granulated material was then fired in a tunnel-type electric furnace at a firing temperature (holding temperature) of 1230°C for 3 hours in an atmosphere with an oxygen concentration of 0.3% by volume. The heating rate was 50°C / hour and the cooling rate was 110°C / hour. The fired material was crushed by a hammer crusher, and further classified by a gyro sifter (vibrating sieve) and a turbo classifier (air classifier) ​​to adjust the particle size. Low magnetic products were separated by magnetic separation to obtain ferrite particles.

[0112] The obtained ferrite particles were subjected to a surface oxidation treatment in a rotary electric furnace equipped with a hot section and a cooling section following the hot section, and then cooled to obtain ferrite particles subjected to the surface oxidation treatment. In the surface oxidation treatment, an oxide film was formed on the surface of the ferrite particles at 450°C in an air atmosphere in the hot section. The main production conditions of the ferrite particles in Example 1 are shown in Table 1.

[0113] (2) Carrier for electrophotographic developer The above ferrite particles were used as a core material, and the ferrite particles were coated with an acrylic resin as follows to obtain a carrier of Example 1.

[0114] First, an acrylic resin solution (resin solid content 10% by mass) was prepared by mixing an acrylic resin (Dianal LR-269, manufactured by Mitsubishi Rayon Co., Ltd.) with toluene. The resin solution was mixed with the ferrite particles of Example 1 using a universal stirrer to coat the surfaces of the ferrite particles with the resin solution. At that time, an amount of the resin solution was used such that the resin solid content was 1.5% by mass relative to the ferrite particles. Next, the ferrite particles to which the resin solution was attached were heated with stirring at 145°C for 3 hours using a heat exchange type stirring and heating device, and the volatile components contained in the resin solution were volatilized to dry the ferrite particles. As a result, a carrier for electrophotographic developer of Example 1 having a resin coating layer on the surface of the ferrite particles was obtained.

[0115] (3) Electrophotographic Developer The above-mentioned electrophotographic developer carrier and toner were mixed by stirring for 30 minutes using a Turbula mixer to obtain 1 kg of developer (toner concentration 7.5% by weight). The toner used was a commercially available negative toner (cyan toner, for DocuPrint C3530 manufactured by Fuji Xerox Co., Ltd.; average particle size approx. 5.8 μm) used in full-color printers. EXAMPLES

[0116] In this embodiment, the particle size of the slurry (the primary particle size of the pulverized material) D 50 The ferrite particles of Example 2 were produced in the same manner as in Example 1, except that the particle diameter was set to 1.4 μm. The main production conditions of Example 2 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for an electrophotographic developer. EXAMPLES

[0117] In this embodiment, the particle size of the slurry (the primary particle size of the pulverized material) D 50The ferrite particles of Example 3 were produced in the same manner as in Example 1, except that the particle diameter was set to 1.0 μm and the heating rate during main sintering was set to 80° C. / hour. The main production conditions of Example 3 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for an electrophotographic developer. EXAMPLES

[0118] In this embodiment, the particle size of the slurry (the primary particle size of the pulverized material) D 50 Ferrite particles of Example 4 were produced in the same manner as in Example 1, except that the particle diameter was set to 1.3 μm and the heating rate during main sintering was set to 75° C. / hour. The main production conditions of Example 4 are shown in Table 1. Furthermore, a carrier for electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for electrophotographic developer. Comparative Example

[0119] [Comparative Example 1] In this comparative example, the particle size of the slurry (the primary particle size of the pulverized particles) D 50 The ferrite particles of Comparative Example 1 were produced in the same manner as in Example 1, except that the average particle diameter was 2.3 μm, the heating rate during main firing was 150° C. / hour, and the firing temperature (retention temperature) during main firing was 1250° C. The main production conditions of Comparative Example 1 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for an electrophotographic developer.

[0120] [Comparative Example 2] In this comparative example, the particle size of the slurry (the primary particle size of the pulverized particles) D 50The ferrite particles of Comparative Example 2 were produced in the same manner as in Example 1, except that the average particle diameter was 2.2 μm, the temperature rise rate during main firing was 150° C. / hour, and the firing temperature (retention temperature) during main firing was 1300° C. The main production conditions of Comparative Example 2 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for an electrophotographic developer.

[0121] [Comparative Example 3] In this comparative example, the particle size of the slurry (the primary particle size of the pulverized particles) D 50 The ferrite particles of Comparative Example 3 were produced in the same manner as in Example 1, except that the average particle diameter was 2.3 μm, the heating rate during main firing was 150° C. / hour, and the firing temperature (retention temperature) during main firing was 1210° C. The main production conditions of Comparative Example 3 are shown in Table 1. In addition, a carrier for an electrophotographic developer was produced in the same manner as in Example 1, except that the ferrite particles were used as a core material, and an electrophotographic developer was produced using the carrier for an electrophotographic developer.

[0122] <evaluation> The ferrite particles of each Example and Comparative Example obtained as described above were evaluated for (1) the perovskite-type crystal phase component content, (2) the spinel-type crystal phase component content, (3) the degree of dispersion of Zr element, (4) the volume average particle size, (5) the content ratio of a specified particle, (6) the apparent density, (7) the BET specific surface area, (8) the particle strength index, (9) the saturation magnetization, and (10) the resistance. The evaluation methods / measurement methods and evaluation results are described below.

[0123] 1. Evaluation method / measurement method (1) Perovskite crystal phase content (mass%) The ferrite particles produced in each Example and Comparative Example were used as samples, and the perovskite crystal phase content in each ferrite particle was determined by Rietveld analysis of the powder X-ray diffraction pattern. Although it may be difficult to identify and quantify each crystal phase by waveform separation of the powder X-ray diffraction pattern, Rietveld analysis based on a crystal structure model makes it possible to identify and quantify each phase.

[0124] The X-ray diffraction device used was the "X'PertPRO MPD" manufactured by PANalytical. The X-ray source was a Co tube (CoKα rays). The optical system used was a focused optical system and a high-speed detector, the "X'Celarator". The measurement conditions were as follows. Scan speed: 0.08° / sec Divergence slit: 1.0° Scattering slit: 1.0° Receiving slit: 0.15mm Voltage and current of the sealed tube: 40kV / 40mA Measurement range: 2θ=15°~90° Number of times: 5

[0125] Based on the obtained measurement results, the crystal structure was identified as follows from the structure disclosed in "National Institute for Materials Science, "AtomWork" (URL: http: / / crystdb.nims.go.jp / )". Phase A: A crystalline phase consisting of manganese ferrite (spinel type crystals) Crystal structure: space group F d -3 m (No. 227) Phase B: A crystalline phase consisting of perovskite-type crystals represented by the composition formula RZrO3 Crystal structure: Space group P nma (No. 62) Phase C: Zirconium dioxide (zirconia) Crystal structure: Space group P -4 2 m (No. 111)

[0126] Next, the identified crystal structure was refined using the analytical software "RIETAN-FP v2.83 (http: / / fujioizumi.verse.jp / download / download.html)" to calculate the mass-converted abundance ratio as the phase composition ratio of each crystal phase. The profile function was the pseudo-Voigt function of Thompson, Cox and Hasting, and was asymmetrized by Howard's method. After confirming that the Rwp and S values, which indicate the accuracy of the fitting, were Rwp: 2% or less and S value: 1.5 or less, respectively, and that the main peaks of phases B and C were fitted at 2θ = 35 to 37°, each parameter was optimized.

[0127] Based on the results of the Rietveld analysis of the X-ray diffraction pattern obtained as described above, the content (mass%) of the perovskite-type crystal phase component (B phase) was determined when a phase composition analysis of the crystal phase constituting the ferrite particles was performed.

[0128] (2) Spinel-type crystal phase content (mass%) The results of the X-ray diffraction measurements of phases A, B, and C obtained above were analyzed with Fe2O3 (phase D), Mn2O3 (phase E), and strontium ferrite (phase F) added to determine the content (mass%) of the spinel-type crystal phase component in each ferrite particle.

[0129] (3) Dispersion degree of Zr element For the ferrite particles produced in each of the Examples and Comparative Examples, the degree of dispersion of Zr element defined by the following formula was measured. Dispersion degree of Zr = Zr(s) / Zr(c) however, Zr(s): Zr content (mass%) in the surface area of ​​the particle cross section measured by energy dispersive X-ray analysis Zr(c): Zr content (mass%) in the center of the particle cross section measured by energy dispersive X-ray analysis

[0130] Here, an explanation will be given with reference to Fig. 1. The central part of a cross section (particle cross section) of a ferrite particle is defined as follows. When the maximum diameter in the particle cross section (for example, an SEM image) is defined as a line segment Dx, the midpoint of the line segment Dx is defined as the center C of the particle cross section, and the end points of the line segment Dx are defined as points P. Then, the center C is defined as the central position of a square, and the length of one side is 35% of the length of the line segment Dx, which is defined as a square S. The area surrounded by this square S is defined as the central part.

[0131] The surface part of the cross section of the particle is defined as follows. Point P' is a point on the line segment Dx, and is located at a distance of 15% of the length of the line segment Dx from point P toward the center C. Rectangle R1 is a rectangle whose long side is a line segment having a length of 35% of the length of the line segment Dx, perpendicular to the line segment Dx, and having point P or point P' as its midpoint, and whose short side is a line segment having a length of 15% of the length of the line segment Dx. In the present invention, the area surrounded by this rectangle R1 in the cross section of the ferrite particle is defined as the surface part. Note that FIG. 1 shows the cross-sectional shape of the ferrite particle simplified to a circular shape for the purpose of explanation, and does not show the actual cross-sectional shape of the ferrite particle according to the present invention.

[0132] The central portion and the surface portion of the particle cross section thus defined are subjected to energy dispersive X-ray analysis (EDX analysis) to measure the content of Zr element in each region. The specific measurement method is as follows.

[0133] (a) Ferrite particles were embedded in resin and cross-sectional samples for measurement were prepared by ion milling. Ion milling was performed using an IM4000PLUS manufactured by Hitachi High-Technogies Corporation, with the ion beam acceleration voltage set to 6.0 kV in an argon atmosphere. The ferrite single particles to be analyzed here were determined by dividing the ferrite single particles into ferrite particles (powder) containing the ferrite single particles by the volume average particle size D. 50 Then, the maximum diameter Dx is D 50 ×0.8≦Dx≦D 50 The particles were in the range of ×1.2.

[0134] (b) The cross section of the ferrite particle to be analyzed is observed using a scanning electron microscope (SEM, Hitachi High-Technogies SU8020) with an acceleration voltage of 15 kV and a working distance of 15 mm. The magnification is set so that only one ferrite particle to be analyzed is present in the field of view and the entire particle fits within the field of view.

[0135] (c) Then, EDX analysis was performed on the center and surface (regions defined above) of the ferrite particle cross section. In the EDX analysis, mapping collection was performed for Fe, Mn, Mg, Sr, and Zr using an energy dispersive X-ray analyzer (Horiba, Ltd. EMax X-Max50), and the amount of each element (mass%) was calculated from the obtained X-ray spectrum peaks. The amount of Zr in the center of the obtained particle cross section was designated as "Zr(c)", and the amount of Zr in the surface of the particle cross section was designated as "Zr(s)".

[0136] The amount of Zr in the center of the particle cross section (Zr(c)) and the amount of Zr in the surface of the particle cross section (Zr(s)) obtained by EDX analysis can be substituted into the above-mentioned formula (1) to obtain the degree of dispersion of Zr in the ferrite particles being analyzed.

[0137] In this case, the amount of Zr in the surface region of the particle cross section was defined as four regions enclosed by rectangle R2 defined similarly to rectangle R1, and rectangles R3 and R4 defined based on points Q and Q' defined similarly to points P and P' above for a line Dy passing through center C of the particle cross section and perpendicular to line Dx, and the surface region was determined as the average amount of Zr in each region. Rectangles R1, R2, R3, and R4 were arranged at approximately equal intervals along the contour of the particle cross section.

[0138] (4) Volume average particle size (D 50 ) Volume average particle size (D 50) was measured using a Microtrack particle size analyzer (Model 9320-X100) manufactured by Nikkiso Co., Ltd., as follows. The ferrite particles manufactured in each Example and Comparative Example were used as samples, and 10 g of each sample and 80 ml of water were placed in a 100 ml beaker, 2 to 3 drops of a dispersant (sodium hexametaphosphate) were added, and an ultrasonic homogenizer (UH-150 type manufactured by SMT.Co.LTD.) was used with an output level set to 4 to disperse for 20 seconds, and bubbles formed on the surface of the beaker were removed to prepare a sample, and the volume average particle size of the sample was measured using the Microtrack particle size analyzer.

[0139] (5) Specified particle content The content of the above-mentioned predetermined particles was determined as follows. a) A cross-sectional sample for measurement was prepared by embedding the ferrite carrier core material in resin and subjecting it to cross-sectional processing by ion milling. Ion milling was performed using an IM4000PLUS manufactured by Hitachi High-Technogies Corporation, with the ion beam acceleration voltage set to 6.0 kV in an argon atmosphere.

[0140] b) The cross-section of the obtained cross-section sample was photographed with a scanning electron microscope (SEM, Hitachi High-Technogies SU8020) at an acceleration voltage of 1.0 kV, a working distance of 8 mm, and a field of view of 450 times magnification to observe the cross-section. If there are less than 100 particles in the field of view, the measurement location may be changed and multiple fields of view may be photographed.

[0141] c) The secondary electron image information was input via an interface into image analysis software (Image-Pro PLUS) manufactured by Media Cybernetics, Inc., and analyzed to determine the content of the above-mentioned specific particles.

[0142] The particles to be measured were 100 ferrite particles having a circle-equivalent diameter that satisfies the following condition (1). In the examples and comparative examples, ferrite particles were obtained by firing granulated powder having a roughly granular shape. Therefore, the obtained ferrite particles maintain roughly the same shape as the granulated powder. Particles that do not satisfy the following condition (1) are considered to have a volume average particle diameter D 50In contrast, these particles are thought to be particles with a particle size that is too small or too large, or the cross-sectional position is inappropriate, or the particles come into contact with each other during sample preparation, causing the particle shape to deviate significantly from a spherical shape, etc., and if such particles are included in the particles to be measured, they will not match the representative value for the powder.

[0143] Condition (1): 0.8X≦Y≦1.3X however, X: Volume average particle size D 50 (μm) Y: Equivalent circle diameter of the cross-sectional area of ​​the particle to be measured

[0144] d) For each particle to be measured, one particle was selected using the selection tool in the image analysis software, and the circle equivalent diameter Y was calculated from the particle area. After confirming that the above condition (1) was met, voids (internal voids) in the cross-sectional particle were selected to determine the maximum Feret diameter Z. Note that an internal void refers to a void that is not in contact with the outer periphery of the measured particle in the cross-sectional SEM photograph and is not continuous from the surface. Using the same method, evaluation was performed on 100 particles within the field of view that met the above condition (1).

[0145] e) The particles that satisfy the following formula for the circle equivalent diameter Y of the cross-sectional area of ​​the particle to be measured and the maximum Feret diameter Z of the internal void are defined as the above-mentioned specified particles, the number of the specified particles is counted, and the ratio of the specified particles to all measured particles (100 particles) is calculated. Note that one particle to be measured may have multiple internal voids. In such a case, when there is at least one internal void that satisfies the following condition, the particle to be measured is counted as the above-mentioned specified particle. 0.15Y≦Z however,

[0146] (6) Apparent density The apparent density was measured in accordance with JIS Z2504:2012 (Test method for apparent density of metal powder).

[0147] (7) BET specific surface area The ferrite particles produced in each Example and Comparative Example were used as samples, and the BET specific surface area was determined using a specific surface area measuring device (Macsorb HM model-1208, Mountec Co., Ltd.) according to the following procedure. First, about 20 g of the sample was placed in a glass petri dish, and then degassed to -0.1 MPa using a vacuum dryer. After degassing and confirming that the degree of vacuum in the glass petri dish had reached -0.1 MPa or less, the sample was heated at 200°C for 2 hours. About 5 to 7 g of the sample subjected to these pretreatments was placed in a standard sample cell dedicated to the specific surface area measuring device. The mass of the sample placed in the standard sample cell was accurately weighed using a precision balance. Then, the standard sample cell containing the sample was set in the measurement port, and the BET specific surface area was measured by the one-point method at a temperature of 10°C to 30°C and a relative humidity of 20% to 80%. The mass of the sample was input at the end of the measurement, and the calculated value was taken as the measured value of the BET specific surface area.

[0148] (8) Particle strength index The particle strength index of the ferrite particles produced in each of the Examples and Comparative Examples was determined as follows.

[0149] The particle strength index can be calculated from the difference in the amount of ferrite particles passing through a mesh before and after the crushing treatment.

[0150] (Amount passing through the mesh before crushing process X) The mesh passing amount X before the crushing treatment was determined as follows. When measuring the mesh passing amount X, a charge amount measuring device Blow-off (Kyocera Chemical TB-200) was used to measure ferrite particles weighed to have a volume of 30 mL as a sample.

[0151] First, the weight of a special cell (Faraday gauge) fitted with 635M (mesh) (opening 20 μm) is measured, 0.5000±0.0005 g of ferrite particles are weighed and put into the special cell (this is the put-in weight A), and the weight B of the special cell containing the ferrite particles is measured. Next, the special cell containing the ferrite particles is set in the blow-off of the charge amount measuring device, and the blow pressure is set to 0.5 kgf / cm. 2After blowing for 30 seconds, the special cell is removed and the weight C of the special cell containing the carrier core material after blowing is measured. Then, the amount of carrier core material passing through the mesh is calculated based on the following formula (1).

[0152] Amount passing through mesh (weight %) = (weight before blow B - weight after blow C) / input weight A × 100 (%) (1)

[0153] (Mesh passing amount after crushing process Y) The mesh passing amount Y after crushing was determined in the same manner as above after crushing the ferrite particles as follows: The crushing was performed by placing the particles in a sample case (inner diameter φ78 mm × inner height 37 mm, stainless steel) of a sample mill (SK-M2, Kyoritsu Riko Co., Ltd.) as a small grinder, and stirring for 30 seconds at a rotation speed of 15,000 rpm (unloaded) using an AC100V, 120W, 2.7A motor. The crushing blade in the sample mill was M2-04 (Kyoritsu Riko Co., Ltd.). A new crushing blade was used each time the crushing process for one sample was completed.

[0154] (particle strength index) Based on the amount of particles passing through the mesh before and after the crushing treatment obtained as described above, the particle strength index was calculated according to the following formula (2). Particle strength index (weight%)=mesh passing amount after crushing process Y (weight%)−mesh passing amount before crushing process X (weight%) (2)

[0155] (9) Saturation magnetization The saturation magnetization was measured using a vibrating sample magnetic measurement device (model: VSM-C7-10A (manufactured by Toei Kogyo Co., Ltd.)). The specific measurement procedure was as follows. First, the ferrite particles produced in each Example and Comparative Example were used as samples, and the samples were filled into a cell with an inner diameter of 5 mm and a height of 2 mm and set in the above-mentioned device. Then, a magnetic field was applied and swept up to 1 K·1000 / 4π·A / m (=1 kOe). Next, the applied magnetic field was reduced, and a hysteresis curve was created on a recording paper. From the data of this curve, the magnetization at an applied magnetic field of 1 K·1000 / 4π·A / m was read and taken as the saturation magnetization.

[0156] (10) Resistance The ferrite particles produced in each Example and Comparative Example were used as samples, and the resistance value M (Ω) was measured under a normal temperature and humidity environment (23°C, relative humidity 55%) by the following procedure. First, non-magnetic parallel plate electrodes (10mm x 40mm) were arranged facing each other with an inter-electrode distance of 6.5mm, and 200mg of sample was filled between them. The sample was held between the parallel plate electrodes by a magnet (surface magnetic flux density: 1500Gauss, area of ​​magnet in contact with electrode: 10mm x 30mm) attached to the parallel plate electrodes. Then, a voltage of 1000V was applied between the parallel plate electrodes facing each other, and the resistance was measured using an electrometer (KEITHLEY, insulation resistance meter model 16517A). The above-mentioned resistance value M is the resistance value measured by the above procedure under a normal temperature and humidity environment (23°C, relative humidity 55%) after exposing the sample to a constant temperature and humidity chamber in which the atmospheric temperature and humidity are adjusted by the method for 12 hours or more.

[0157] 2. Evaluation results Table 2 shows the measurement results for each of the above evaluation items. (1) Perovskite-type crystal phase component content, etc. As shown in Table 2, it was confirmed that the ferrite particles of Examples 1 to 4 contained 0.94% by mass to 0.97% by mass of perovskite-type crystal phase components, and the ferrite particles of Comparative Examples 1 to 3 contained 0.84% ​​by mass to 0.95% by mass of perovskite-type crystal phase components. It was also confirmed that the ferrite particles of Examples 1 to 4 contained 96.6% by mass to 97.4% by mass of a spinel-type crystal phase component, and the ferrite particles of Comparative Examples 1 to 3 contained 95.7% by mass to 96.7% by mass of a spinel-type crystal phase component. Furthermore, the Zr dispersion degree of the ferrite particles in each of the examples and comparative examples was 1.0, and it was confirmed that the ferrite particles were mainly composed of a spinel crystal phase component and had a perovskite crystal phase well dispersed within the particles.

[0158] (2) Volume average particle size (D 50 ) As shown in Table 2, the volume average particle size (D 50 ) were approximately 32 μm to 33 μm, and were confirmed to be of similar size.

[0159] (3) Specified particle content The content of the above-mentioned predetermined particles was 1% to 3% in the ferrite particles of Example 1 to Example 4, whereas the content of the above-mentioned predetermined particles was 5% to 8% in the ferrite particles of Comparative Example 1 to Comparative Example 3. The ferrite particles of each Example and the ferrite particles of each Comparative Example were manufactured using the same amount of the same raw material and manufactured to the same size, and both contained a perovskite crystal phase, but it was confirmed that by making the slurry particle size small and slowing the heating rate during firing, it is possible to prevent the generation of voids with a large maximum Feret diameter compared to the circle equivalent diameter, and to reduce the content of the above-mentioned predetermined particles. In addition, when a separate verification experiment was performed, it was also confirmed that the effect on the content of the predetermined particles was greater when the slurry particle size was kept constant and the heating rate was changed in the range of 50 ° C. / hour to 150 ° C. / hour than when the slurry particle size was changed in the range of 0.9 μm to 2.3 μm and the heating rate was constant.

[0160] (4) Apparent density and BET specific surface area The apparent densities of the ferrite particles in Examples 1 to 4 and Comparative Examples 1 and 2 are approximately the same (2.28 g / cm 3 ~2.32g / cm 3), whereas the apparent density of the ferrite particles of Comparative Example 3 was 2.14 g / cm 3 The ferrite particles of Comparative Example 3 had a content of the above-mentioned specific particles of 8%, which was higher than that of other ferrite particles, and this is believed to have resulted in a lower apparent density. The ferrite particles of Examples 1 to 4 had a larger BET specific surface area than the ferrite particles of Comparative Examples 1 and 2, but had a smaller BET specific surface area than the ferrite particles of Comparative Example 3. This result is considered to be due to the difference in firing temperature.

[0161] (5) Particle strength index The particle strength index of the ferrite particles of Example 1 to Example 4 is 0.3 or less, whereas the ferrite particles of Comparative Example 1 to Comparative Example 3 are 0.6 to 1.0, and it was confirmed that the higher the content of the predetermined particles, the lower the particle strength index, and the stronger the ferrite particles obtained. In particular, it was confirmed that the ferrite particles of Comparative Example 3, which has a higher content of the predetermined particles than the others, have a particle strength index of 1.0, and have a lower strength than the others. The content of the predetermined particles of the ferrite particles of Comparative Example 1 and Comparative Example 2 is 5%, and the content of the predetermined particles of the ferrite particles of Example 3 is 3%. On the other hand, the BET specific surface area of ​​the ferrite particles of Comparative Example 1 and Comparative Example 2 is smaller than the BET specific surface area of ​​the ferrite particles of Example 3, and the surface unevenness is small. However, the particle strength index of the ferrite particles of Comparative Example 1 and Comparative Example 2 is lower than that of the ferrite particles of Example 3, and it was confirmed that ferrite particles with extremely high particle strength can be obtained by obtaining ferrite particles with a low content of the predetermined particles.

[0162] (6) Saturation magnetization and resistance It was confirmed that the saturation magnetization and resistivity of each ferrite particle were comparable, and that the magnetic and electrical properties were comparable.

[0163] As described above, the ferrite particles of Examples 1 to 4 and the ferrite particles of Comparative Examples 1 to 3 have high saturation magnetization and resistance, and can effectively suppress carrier scattering due to low magnetization, etc. On the other hand, the ferrite particles of Examples 1 to 4 have a lower content of the above-mentioned specific particles and higher particle strength than the ferrite particles of Comparative Examples 1 to 3. Therefore, the ferrite particles of Examples 1 to 4 can better prevent cracking and chipping when subjected to mechanical stress, and can effectively suppress carrier scattering associated with the generation of fine powder, compared to the ferrite particles of Comparative Examples 1 to 3.

[0164] [Table 1]

[0165] [Table 2] [Industrial Applicability]

[0166] The ferrite particles according to the present invention have high magnetization and high resistance, and further have high particle strength. Therefore, by using the ferrite particles as a carrier core material, cracks and chips are reduced, and the occurrence of carrier scattering caused by cracks and chips can be effectively suppressed. Therefore, a developer with a longer life than conventional ones can be obtained, and the adhesion of the carrier to the photoconductor and the fixing roller, which causes damage to these, can be suppressed, so that the life of the electrophotographic developing device can be extended.

Claims

1. A material comprising 50 mass % or more of a spinel-type crystal phase component represented by the composition formula (MnO)x(MgO)y(Fe2O3)z (where 15≦x≦50, 2≦y≦35, 45≦z≦60, and x+y+z=100 (mol %)), Contains a crystalline phase component consisting of a perovskite type crystal represented by the composition formula SrZrO3, Ferrite particles, in which when the particle size of each particle is expressed as a circle equivalent diameter in a cross section in a backscattered electron image of the particle cross section photographed by a scanning electron microscope, the content of particles having internal voids whose maximum Feret diameter is larger than 15% of the particle size is 4% or less, When a phase composition analysis of a crystal phase constituting the ferrite particles is performed by Rietveld analysis of an X-ray diffraction pattern, the ferrite particles contain 0.05 mass % or more and 4.00 mass % or less of a crystal phase component consisting of a perovskite type crystal. The ferrite particles are characterized by:

2. 2. The ferrite particles according to claim 1, characterized in that the apparent density of the ferrite particles is within the range represented by the following formula: 2.15≦Y≦2.45 In the above formula, Y is the apparent density of the ferrite particles (g / cm 3 ).

3. 3. The ferrite particles according to claim 1, wherein the BET specific surface area of ​​the ferrite particles is within the range represented by the following formula: 0.08≦X≦0.300 In the above formula, X is the BET specific surface area (m 2 / g).

4. A carrier core material for an electrophotographic developer, comprising the ferrite particles according to any one of claims 1 to 3.

5. 5. A carrier for electrophotographic developer comprising the ferrite particles according to claim 1 and a resin coating layer provided on the surface of the ferrite particles.

6. 6. An electrophotographic developer comprising the carrier for electrophotographic developer according to claim 5 and a toner.

7. The electrophotographic developer according to claim 6, which is used as a replenishment developer.

Citation Information

Patent Citations

  • Ferrite carrier for development in electrophotography

    JP1984228664A

  • Spherical ferrite particle and its manufacturing method, and magnetic carrier for electrophotographic development consisting of spherical ferrite particles

    JP2005314176A

  • Carrier core material for electrophotographic developer and method for producing the same, carrier for the electrophotographic developer, and electrophotographic developer carrier

    JP2011028060A

  • Ferrite carrier core material for electrophotographic developer and ferrite carrier, method for producing the same and electrophotographic developer containing the same

    JP2011227452A

  • Ferrite particle, and carrier for electrophotographic development and electrophotographic developer using the same,

    JP2013103869A