Two-component developer

The two-component developer addresses issues of carrier resistance and toner spending by using polyester resin, ester wax, and silicone-coated iron powder carriers, enhancing low-temperature fixing and reducing development memory and fog for improved longevity and image quality.

JP7578481B2Active Publication Date: 2024-11-06SHARP KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020211414
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-11-06
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

Existing two-component developers using iron powder carriers face issues with increased carrier resistance, leading to development memory and fog, especially in high humidity environments, due to toner spending, which affects longevity and fixing performance.

Method used

A two-component developer is formulated with a specific combination of polyester resin, ester wax, and iron powder carrier, optimized by controlling carrier voltage, fluidity, and using silicone resin coating, along with external inorganic fine particles to stabilize resistance and reduce toner adhesion.

Benefits of technology

The developer achieves excellent low-temperature fixability, prevents fixing member contamination, and minimizes development memory and fog, ensuring extended longevity and improved image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578481000005
    Figure 0007578481000005
  • Figure 0007578481000006
    Figure 0007578481000006
  • Figure 0007578481000001
    Figure 0007578481000001
Patent Text Reader

Abstract

To provide a two-component developer which excels in low temperature fixability and suppresses the contamination of a fixing member during fixation, and furthermore does not cause the occurrence of toner-spent-derived development memory or fogging, and which also excels in life stability.SOLUTION: A two-component developer is provided which includes: a carrier; and a toner including at least a binding resin, a coloring agent and a mold-release agent. The binding resin is a polyester resin, the mold-release agent is an ester wax and has a dispersion diameter of 0.2 to 2.0 μm in the toner, the carrier is an iron powder carrier and has a carrier voltage value α(V) of 5≤α≤30 when applied to the carrier in an increment of 1 V by a bridge resistance measurement method and a current value flowing in the carrier is 10-5 A.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a two-component developer. More specifically, the present invention relates to a two-component developer that has excellent low-temperature fixing properties, suppresses contamination of a fixing member during fixing, does not cause development memory or fogging due to toner spent, and is excellent in life. [Background technology]

[0002] 2. Description of the Related Art In recent years, with the remarkable development of office automation equipment, image forming apparatuses using electrophotography, such as copying machines, printers, and facsimile machines, have come into widespread use. In an image forming apparatus using an electrophotographic system, an image is typically formed through a charging process in which the surface of a rotating electrophotographic photosensitive member (also called a "photosensitive member") is uniformly charged by a charging device; an exposure process in which an exposure device irradiates the charged photosensitive member surface with laser light to form an electrostatic latent image; a development process in which a developing device develops the electrostatic latent image on the photosensitive member surface using electrophotographic toner (also called "toner") to form a toner image; a transfer process in which a transfer device transfers the toner image on the photosensitive member surface onto recording paper (also called a "recording medium" or "transfer medium"); and a fixing process in which a fixing device heats the toner image to fix the toner image to the recording paper, thereby forming an image. Then, any residual transfer toner remaining on the photoreceptor surface after the image formation operation is removed by a cleaning device in a cleaning process and collected in a designated collection section, and any residual charge on the photoreceptor surface after cleaning is removed by a discharge device in a discharge process in preparation for the next image formation.

[0003] Developers for developing electrostatic latent images on the surface of a photoreceptor include one-component developers that contain only toner, and two-component developers that contain toner and a carrier for electrophotography (hereinafter also referred to as "carrier" or "carrier particles"). In a two-component developer, the carrier provides the functions of stirring, transporting and charging the toner, and the toner itself does not need to have the function of a carrier as in a one-component developer. Since the functions can be separated between the toner and the carrier, two-component developers have the advantage of being easier to control than one-component developers that contain only toner alone, and therefore easier to obtain high-quality images. The carrier has two basic functions: the function of stably charging the toner to a desired charge amount, and the function of transporting the toner to the photoconductor. The carrier is stirred in the developing tank, transported onto a magnet roller, forms magnetic chains, passes through a regulating blade, and returns to the developing tank again, and is used repeatedly. Therefore, the carrier is required to have stable basic functions, especially the function of stably charging the toner, during continuous use.

[0004] As carrier particles forming a two-component developer, iron powder carriers such as iron powder whose surface is covered with an oxide film or iron powder whose surface is coated with a resin have been conventionally used. For example, JP 2017-003990 A (Patent Document 1) describes a toner having toner particles containing an amorphous polyester resin, a crystalline polyester resin, and a wax, in which a cross section of the toner observed with a transmission electron microscope (TEM) shows that a wax domain and a crystal of the crystalline polyester resin are present, the area of ​​the cross section of the toner is occupied by the wax domains in an amount of 0.5% or more and 8.0% or less, and the area of ​​the crystalline polyester resin crystals in an amount of 0.5% or more and 8.0% or less, and Patent Document 1 discloses a toner characterized in that the number average diameter (Dw) of the wax domains is 60 nm or more and 240 nm or less, the crystals of the crystalline polyester resin have an aspect ratio of 5.0 or more and 25.0 or less, and the number average diameter (Dc) of the major axis length of the crystalline polyester resin crystals is 0.8 to 2.0 times the number average diameter (Dw) of the wax domains. Patent Document 1 describes surface-oxidized or unoxidized iron powder, and metal particles such as iron, as magnetic carriers that can be used. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-003990 A Summary of the Invention [Problem to be solved by the invention]

[0006] Here, the toner spent will be described. Figure 2 is a schematic diagram for explaining the basic structure of a toner and spent on an iron powder carrier. The upper left of Figure 2 shows toner 10, in which a release agent 6 such as ester wax and a colorant 7 are each dispersed and held in a binder resin 5 such as a polyester resin, and the upper right shows carrier 8. Since the particle diameters of toner and carrier are usually several nm and several tens of nm, respectively, the scale of Figure 2 is ignored. Toner spent 9 refers to the release agent 8 melted by heat adhering to the surface of carrier 8, especially to its recesses, as shown by the arrows at the top of Figure 2, and the release agent then acting as an adhesive on which toner and other substances adhere. As the toner spent progresses, the carrier resistance increases and the chargeability decreases, causing a deterioration in development memory and fogging in a high humidity environment.

[0007] Iron powder carriers have excellent properties such as low resistance, which makes initial development memory unlikely to occur, and their irregular shape makes it easy to scrape off toner from the sleeve, and the shape also makes development memory unlikely to occur.However, iron powder carriers have a heavy true specific gravity of about 7.8 and are highly magnetized, which means that they are subject to high stress when stirred and mixed with toner particles in the developing box, which makes them prone to coating peeling and toner spent, which can lead to problems such as increased development memory and fogging over their lifespan. Therefore, the present invention aims to provide a two-component developer that has excellent low-temperature fixing properties, suppresses contamination of a fixing member during fixing, is free from development memory and fogging due to toner spent, and is also excellent in life. [Means for solving the problem]

[0008] In order to solve the above problems, the inventors have conducted extensive research from the viewpoint that if an optimal spent state can be maintained and the resistance and charging performance of the carrier can be stabilized, the iron powder carrier can be used in combination with a low-temperature fixing toner while taking advantage of its advantageous characteristics with respect to development memory. As a result, the inventors have found that the above problems can be solved by using a specific binder resin, release agent and iron powder carrier in combination, thereby completing the present invention.

[0009] Thus, according to the present invention, there is provided a two-component developer including a toner containing at least a binder resin, a colorant, and a release agent, and a carrier, The binder resin is a polyester resin, the release agent is an ester wax and has a dispersion diameter of 0.2 to 2.0 μm in the toner, The carrier is an iron powder carrier, and a bridge resistance measurement method is used to apply 1V to the carrier in steps of 1V, and the current flowing through the carrier is 10 -5 A, the carrier voltage value α(V) is 5≦α≦30. The present invention provides a two-component developer comprising: Effect of the Invention

[0010] According to the present invention, it is possible to provide a two-component developer that has excellent low-temperature fixing properties, suppresses contamination of a fixing member during fixing, is free from development memory and fogging due to toner spent, and is also excellent in life.

[0011] The two-component developer of the present invention exhibits the above-mentioned effects more effectively when it satisfies at least one of the following conditions (1) to (7). (1) The carrier has a flow rate of 9.0 to 20.0 sec / 50 g. (2) The carrier is an iron powder carrier coated with a silicone resin as a coating agent. (3) The carrier is an iron powder carrier coated with the above coating agent by a dipping method. (4) The toner contains 10 to 30 mass % of a tetrahydrofuran (THF) insoluble matter. (5) The toner is externally added with inorganic fine particles having an average primary particle size of 20 to 50 nm. (6) The inorganic fine particles are contained in an amount of 0.3 to 1.0 part by mass based on 100 parts by mass of the toner. (7) The toner further contains a styrene-acrylic copolymer resin as a release agent dispersant. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram of a measuring jig used for measuring a carrier voltage value. [Diagram 2] 1A and 1B are schematic diagrams for explaining a basic structure of a toner and spent on an iron powder carrier; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The two-component developer of the present invention is a two-component developer including a toner containing at least a binder resin, a colorant, and a release agent, and a carrier, The binder resin is a polyester resin, the release agent is an ester wax and has a dispersion diameter of 0.2 to 2.0 μm in the toner, The carrier is an iron powder carrier, and a bridge resistance measurement method is used to apply 1V to the carrier in steps of 1V, and the current flowing through the carrier is 10 -5 A, the carrier voltage value α(V) is 5≦α≦30. It is characterized by: Each of the components of the two-component developer of the present invention will be described below, and the binder resin, release agent and carrier, which are characteristic of the developer, will be described in detail.

[0014] (1) Toner The toner contains at least a binder resin, a colorant, and a release agent. As described later, the toner may contain an external additive, and the toner before the additive is particularly referred to as "toner base particles." (1-1) Binder resin The binder resin constituting the toner may be any resin known in the art, and polyester resins are preferably used. Polyester-based resins are classified into amorphous polyester-based resins and crystalline polyester-based resins. In general, it is known that crystalline polyester-based resins can lower the softening temperature and melt viscosity of a toner, and that when used in combination with an amorphous polyester-based resin, they can improve the low-temperature fixing properties of a toner. Amorphous resins and crystalline resins are distinguished by their crystallinity index, with resins having a crystallinity index in the range of 0.6 to 1.5 being crystalline resins, and resins having a crystallinity index less than 0.6 or more than 1.5 being amorphous resins. In other words, resins having a crystallinity index greater than 1.5 are amorphous, while resins having a crystallinity index less than 0.6 have low crystallinity and many amorphous portions. The crystallinity index is a physical property that is an index of the degree of crystallization of a resin, and is defined as the ratio of the softening temperature to the highest endothermic peak temperature (softening temperature / highest endothermic peak temperature). Here, the highest endothermic peak temperature refers to the temperature of the highest endothermic peak observed. In a crystalline polyester resin, the highest peak temperature is the melting point Tmp, and in an amorphous polyester resin, the highest endothermic peak is the glass transition temperature Tg. The degree of crystallization can be controlled by adjusting the types and ratio of raw material monomers, as well as production conditions (eg, reaction temperature, reaction time, cooling rate), and the like.

[0015] (1-1-1) Amorphous polyester resin The amorphous polyester resin is not particularly limited, but can be obtained, for example, by a polycondensation reaction between a carboxylic acid monomer containing terephthalic acid or isophthalic acid as a main component and a polyhydric alcohol containing ethylene glycol as a main component. The reaction conditions are the same as those for producing ordinary polyester resins, and for example, a dicarboxylic acid monomer and a polyhydric alcohol are reacted in a nitrogen gas atmosphere, optionally in the presence of an esterification catalyst, at a temperature of 190 to 240° C. to obtain an amorphous polyester resin. The reaction ratio of the polyhydric alcohol and the carboxylic acid monomer is preferably 1.3:1 to 1:1.2 in terms of the equivalent ratio of hydroxyl group to carboxyl group [OH]:[COOH].

[0016] The molar content of terephthalic acid or isophthalic acid in the dicarboxylic acid monomer is preferably 70 to 100%, and more preferably 80 to 100%. The dicarboxylic acid monomer may also include aromatic dicarboxylic acids such as fumaric acid, aliphatic dicarboxylic acids such as adipic acid, sebacic acid, and succinic acid, and may also include ester-forming derivatives of terephthalic acid or isophthalic acid, ester-forming derivatives of aromatic dicarboxylic acids, ester-forming derivatives of aliphatic dicarboxylic acids, and acid anhydrides and alkyl esters of these carboxylic acids. Furthermore, the dicarboxylic acid monomer may be used in combination with a trivalent or higher polycarboxylic acid such as trimellitic acid or pyromellitic acid, or an ester-forming derivative thereof. The above dicarboxylic acid monomers and polycarboxylic acid monomers can be used alone or in combination of two or more.

[0017] The molar content of ethylene glycol in the polyhydric alcohol is preferably 70 to 100%, and more preferably 80 to 100%. The polyhydric alcohol may include other polyhydric alcohols such as 1,3-propylene glycol, 1,4-butanediol, and the like. The above polyhydric alcohols can be used alone or in combination of two or more.

[0018] From the viewpoint of the fixing property, storage stability, durability, etc. of the toner, the amorphous polyester resin preferably has a glass transition temperature (Tg) of 50 to 70°C. If the glass transition temperature is outside this range, the balance between the fixing property, storage stability, and durability of the toner may be lost. In addition, from the viewpoint of achieving both low temperature fixability and hot offset resistance of the toner, the amorphous polyester resin preferably has a softening point (Tm) of 100 to 150°C. If the softening point is outside this range, the balance between the low temperature fixability and hot offset resistance of the toner may be lost.

[0019] From the viewpoint of achieving a balance between the heat resistance, thermal storage stability, and low-temperature fixability of the toner, the amorphous polyester resin preferably has a peak top molecular weight Mp of 3,000 to 10,500. If the peak top molecular weight is outside this range, the balance between the heat resistance, thermal storage stability, and low-temperature fixability of the toner may be lost. Here, the peak top molecular weight Mp means the molecular weight showing the maximum peak height of the tetrahydrofuran (THF) soluble matter in gel permeation chromatography (GPC) using tetrahydrofuran (THF) as the mobile phase and polystyrene as the standard substance.

[0020] In addition, the amorphous polyester resin preferably has an acid value of 0 to 60 mgKOH / g from the viewpoint of the charging characteristics of the toner, and a hydroxyl value of 0 to 50 mgKOH / g from the viewpoint of the hot offset resistance of the toner. If the acid value exceeds 60 mgKOH / g, the charging performance of the toner may decrease, and if the hydroxyl value exceeds 50 mgKOH / g, the hot offset resistance of the toner may become insufficient.

[0021] The amorphous polyester resin preferably has an SP value (solubility parameter) of 10.5 to 12.5. If the SP value is less than 10.5, the compatibility with the crystalline resin may progress too much, and the blocking resistance and hot offset resistance of the toner may be impaired. On the other hand, if the SP value exceeds 12.5, the compatibility with the crystalline resin may be too low, and the low-temperature fixing property may be insufficient.

[0022] (1-1-2) Crystalline polyester resin The crystalline polyester resin is not particularly limited, but is preferably composed of a linear saturated aliphatic polyester unit obtained by a polycondensation reaction between a carboxylic acid monomer containing, as a main component, an aliphatic dicarboxylic acid having 9 to 22 carbon atoms and a polyhydric alcohol containing, as a main component, an aliphatic diol having 2 to 10 carbon atoms. The reaction conditions are the same as those for producing a normal polyester resin, and for example, a crystalline polyester resin is obtained by reacting a dicarboxylic acid monomer with a polyhydric alcohol in a nitrogen gas atmosphere, optionally in the presence of an esterification catalyst, at a temperature of 190 to 240° C. From the viewpoint of the storage stability of the toner, the reaction ratio of the polyhydric alcohol to the carboxylic acid monomer is preferably 0.83:1 to 1.3:1 in terms of the equivalent ratio of hydroxyl group to carboxyl group [OH]:[COOH].

[0023] The molar content of dicarboxylic acid in the carboxylic acid monomer is preferably 90 to 100%. If the molar content of dicarboxylic acid is low, the rate and speed of crystallization may decrease, resulting in insufficient toner aggregation resistance. Examples of the aliphatic dicarboxylic acid having 9 to 22 carbon atoms include azelaic acid, zebaic acid, 1,10-decanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc. The carboxylic acid monomer and polycarboxylic acid monomer may contain an ester-forming derivative of these aliphatic dicarboxylic acids. Furthermore, the carboxylic acid monomer may be used in combination with a polycarboxylic acid having three or more valences, such as trimellitic acid or pyromellitic acid, or an ester-forming derivative thereof. The above carboxylic acid monomers can be used alone or in combination of two or more.

[0024] The molar content of the aliphatic diol having 2 to 10 carbon atoms in the polyhydric alcohol is preferably 80 to 100%. Examples of the aliphatic diol having 2 to 10 carbon atoms include ethylene glycol, 1,4-butanediol, and 1,6-hexanediol. Furthermore, examples of polyhydric alcohols that can be used in combination with the above aliphatic diols include trihydric or higher alcohols such as glycerin and trimethylolpropane. The above polyhydric alcohols can be used alone or in combination of two or more.

[0025] From the viewpoint of the fixing property, storage stability, durability, etc. of the toner, the crystalline polyester resin preferably has a melting point (Tmp) of 40 to 90°C. If the melting point is less than 40°C, the durability of the toner may be insufficient. On the other hand, if the melting point is more than 90°C, the fixing property of the toner may be insufficient. A more preferred melting point is 60 to 90°C. From the viewpoint of low-temperature fixing property and blocking resistance of the toner, the crystalline polyester resin preferably has a softening point (Tm) of 65 to 110°C. If the softening point is outside this range, the low-temperature fixing property and blocking resistance of the toner may become insufficient. Furthermore, from the viewpoint of crystallization speed and blocking resistance, the crystalline polyester resin preferably has a softening point (Tm) to melting point (Tmp) ratio (Tm / Tmp) of 1.0 to 1.4. On the other hand, if the softening point to melting point ratio is out of this range, the crystallization speed and blocking resistance may become insufficient.

[0026] From the viewpoint of the storage stability and low-temperature fixing property of the toner, the crystalline polyester resin preferably has a peak top molecular weight Mp of 10,000 to 90,000. If the peak top molecular weight is outside this range, the storage stability and low-temperature fixing property of the toner may become insufficient.

[0027] From the viewpoint of the charging characteristics of the toner, the crystalline polyester resin preferably has an acid value of 0 to 60 mgKOH / g, and from the viewpoint of the hot offset resistance of the toner, a hydroxyl value of 0 to 40 mgKOH / g. If the acid value exceeds 60 mgKOH / g, the charging performance of the toner may decrease, and if the hydroxyl value exceeds 40 mgKOH / g, the hot offset resistance of the toner may become insufficient.

[0028] The crystalline polyester resin preferably has an SP value of 9.3 to 10.0. If the SP value is less than 9.3, the compatibility with the amorphous polyester resin may be too low, and the durability of the toner may be insufficient. On the other hand, if the SP value is more than 10.0, the Tg of the binder resin may be lowered, and the blocking resistance of the toner may be reduced.

[0029] In the present invention, in order to impart the conflicting properties of low-temperature fixability and anti-spent property to the two-component developer in a well-balanced manner, it is preferable to use a combination of two or more kinds of amorphous polyester resins having different physical properties. For example, as described in the Examples, a combination of a resin having a softening point of 90 to 100°C and a resin having a softening point of 140 to 155°C can be used.

[0030] (1-1-3) Content The content of the binder resin in the toner is not particularly limited, but is preferably from 60 to 95% by mass, and particularly preferably from 70 to 90% by mass. When two types of amorphous polyester resins are used in combination as described above, the ratio is about 15:85 to 85:15, although it varies depending on the physical properties and resin types of the intended two-component developer.

[0031] (1-2) Coloring agent (1-2-1) Colorants As the colorant constituting the toner, various types and colors of organic and inorganic pigments and dyes commonly used in the art can be used, such as black, white, yellow, orange, red, purple, blue and green colorants.

[0032] Examples of black colorants include carbon black, copper oxide, manganese dioxide, aniline black, activated carbon, non-magnetic ferrite, magnetic ferrite, and magnetite. Examples of white colorants include zinc oxide, titanium oxide, antimony white, and zinc sulfide.

[0033] Examples of yellow colorants include yellow lead, zinc yellow, cadmium yellow, yellow iron oxide, mineral fast yellow, nickel titanium yellow, navel yellow, naphthol yellow S, Hansa Yellow G, Hansa Yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, tartrazine lake, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 15, CI Pigment Yellow 17, CI Pigment Yellow 93, CI Pigment Yellow 94, and CI Pigment Yellow 138.

[0034] Examples of orange colorants include red yellow lead, molybdenum orange, permanent orange GTR, pyrazolone orange, Balkan orange, industren brilliant orange RK, benzidine orange G, industren brilliant orange GK, CI pigment orange 31, and CI pigment orange 43.

[0035] Examples of red colorants include red iron oxide, cadmium red, red lead, mercury sulfide, cadmium, permanent red 4R, lithol red, pyrazolone red, watching red, calcium salt, lake red C, lake red D, brilliant carmine 6B, eosin lake, rhodamine lake B, alizarin lake, brilliant carmine 3B, CI pigment red 2, CI pigment red 3, CI pigment red 5, CI pigment red 6, CI pigment red 7, CI pigment red 8, CI pigment red 9, CI pigment red 10, CI pigment red 11, CI pigment red 12, CI pigment red 13, CI pigment red 14, CI pigment red 15, CI pigment red 16, CI pigment red 17, CI pigment red 18, CI pigment red 19, CI pigment red 20, CI pigment red 21, CI pigment red 22, CI pigment red 23, CI pigment red 24, CI pigment red 25, CI pigment red 26, CI pigment red 27, CI pigment red 28, CI pigment red 29, CI pigment red 30, CI pigment red 31, CI pigment red 32, CI pigment red 33, CI pigment red 34, CI pigment red 35, CI pigment red 36, CI pigment red 37, CI pigment red 38, CI pigment red 39 ... Examples of pigment red include CI Pigment Red 7, CI Pigment Red 15, CI Pigment Red 16, CI Pigment Red 48:1, CI Pigment Red 53:1, CI Pigment Red 57:1, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 139, CI Pigment Red 144, CI Pigment Red 149, CI Pigment Red 166, CI Pigment Red 177, CI Pigment Red 178, and CI Pigment Red 222.

[0036] Purple colorants include, for example, manganese violet, fast violet B, and methyl violet lake. Examples of blue colorants include Prussian blue, cobalt blue, alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, partially chlorinated phthalocyanine blue, fast sky blue, indanthrene blue BC, CI pigment blue 15, CI pigment blue 15:2, CI pigment blue 15:3, CI pigment blue 16, and CI pigment blue 60. Examples of green colorants include chrome green, chromium oxide, pigment green B, mica light green lake, final yellow green G, and CI pigment green 7.

[0037] In the toner of the present invention, the above colorants may be used alone or in combination of two kinds, and the combination may be of different colors or the same color. Two or more kinds of colorants may be used in the form of composite particles. The composite particles can be produced, for example, by adding an appropriate amount of water, a lower alcohol, etc. to two or more kinds of colorants, granulating the mixture with a general granulator such as a high-speed mill, and drying the mixture. Furthermore, the colorants may be used in the form of master batches in order to disperse the colorants uniformly in the binder resin. The composite particles and the master batch are mixed into the toner composition during dry mixing.

[0038] (1-2-2) Content The content of the colorant in the toner is not particularly limited, but is preferably 0.1 to 20 parts by mass, and more preferably 0.2 to 10 parts by mass, relative to 100 parts by mass of the binder resin. If the content of the colorant is within the above range, it is possible to form an image having a high image density and excellent image quality without impairing various physical properties of the toner. In terms of the amount, the content of the colorant in the toner is preferably 0.1 to 15% by mass, and more preferably 0.2 to 8.0% by mass.

[0039] (1-3) Release agent (1-3-1) Ester wax The release agent constituting the toner has a function of imparting releasability to the toner when the toner is fixed onto a recording medium. The release agent constituting the toner of the present invention is an ester wax (also called "ester-based wax"). The ester wax has high polarity, is compatible with the binder resin, particularly the amorphous polyester resin, is structurally stable, and can impart favorable thermal properties to the toner. Examples of ester waxes include Nissan Electol Wax (manufactured by NOF Corporation, product names: WEP-5, WEP-14, WEP-15) as used in the examples, and these can be used alone or in combination of two or more.

[0040] (1-3-2) Melting point The release agent is preferably an ester wax having a melting point of 60 to 90°C. If the melting point of the release agent is less than 60° C., it may be difficult to ensure the heat resistance of the toner. On the other hand, if the melting point of the release agent is more than 90° C., low-temperature fixability may be impaired. The melting point of the release agent is more preferably 70 to 80° C. The melting point of a commercially available release agent may be determined based on data in a catalog or analysis table, but it can also be measured by a known method such as that described in the examples.

[0041] (1-3-3) Dispersion diameter The releasing agent has a dispersion diameter of 0.2 to 2.0 μm in the toner. Generally, if the wax dispersion diameter becomes large, the release agent (wax) is more likely to seep out during fixing, improving the peelability from the fixing roller and expanding the non-offset fixing region to the high temperature side, but the wax exposed area on the toner surface becomes larger, deteriorating the heat resistance. Therefore, although it is generally considered preferable that the wax dispersion diameter is 1.0 μm or less, by using the toner configuration of the present invention, a toner with excellent heat resistance and storage stability can be provided even if the wax dispersion diameter is 1.0 μm or more. If the wax dispersion diameter is less than 0.2 μm, the high temperature side of the fixing non-offset region cannot be sufficiently secured, and the high compatibility with the resin may cause the resin to become miscible, resulting in a deterioration in heat resistance. On the other hand, if the wax dispersion diameter exceeds 2.0 μm, the amount of spent increases, which may lead to a deterioration in development memory. In addition, the generation of free wax increases, which may make it difficult to secure heat resistance. The preferred wax dispersion diameter is 0.4 to 1.0 μm. The method for measuring the dispersed wax diameter will be described in detail in the Examples.

[0042] (1-3-4) Content The content of the release agent in the toner is not particularly limited, but is preferably 0.2 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and particularly preferably 1.0 to 8.0 parts by mass, relative to 100 parts by mass of the binder resin. If the content of the releasing agent is within the above range, it is possible to form an image having a high image density and excellent image quality without impairing various physical properties of the toner. In terms of the amount of the releasing agent, the content of the releasing agent in the toner is preferably 0.2 to 15% by mass, and more preferably 0.4 to 8.0% by mass.

[0043] (1-4) Other additives In addition to the above components, the toner may contain known additives such as a release agent, a dispersant, and a charge control agent, if necessary, within the range that does not impair the effects of the present invention. (1-4-1) Release agent dispersant The toner preferably further contains a styrene-acrylic copolymer resin as a release agent dispersant. By including the styrene-acrylic copolymer resin, the ester wax of the release agent can be easily dispersed in the binder resin at the above-mentioned dispersion diameter, and the occurrence of spent can be suppressed. The content of the release agent dispersant in the toner is not particularly limited, but is preferably 0.2 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and particularly preferably 1.0 to 5.0 parts by mass, relative to 100 parts by mass of the binder resin. In terms of the amount, the content of the release agent dispersant in the toner is preferably 0.2 to 15% by mass, and more preferably 0.4 to 8.0% by mass.

[0044] (1-4-2) Charge control agents As the charge control agent, charge control agents for controlling positive charge and negative charge that are commonly used in the art can be used. Examples of charge control agents for controlling positive charges include nigrosine dyes, basic dyes, quaternary ammonium salts, quaternary phosphonium salts, aminopyrine, pyrimidine compounds, polynuclear polyamino compounds, aminosilanes, nigrosine dyes and derivatives thereof, triphenylmethane derivatives, guanidine salts, and amidine salts. Examples of charge control agents for controlling negative charges include oil-soluble dyes such as oil black and spiron black, metal-containing azo compounds, azo complex dyes, metal naphthenates, metal complexes and metal salts of salicylic acid and its derivatives (metals include chromium, zinc, zirconium, etc.), boron compounds, fatty acid soaps, long-chain alkyl carboxylates, and resin acid soaps. In the toner of the present invention, the above charge control agents can be used alone or in combination of two or more.

[0045] The content of the charge control agent in the toner is not particularly limited, but is preferably 0.5 to 3 parts by mass, and more preferably 1 to 2 parts by mass, relative to 100 parts by mass of the binder resin. If the content of the charge control agent is within the above range, it is possible to form an image having a high image density and excellent image quality without impairing various physical properties of the toner. In terms of the amount, the content of the charge control agent in the toner is preferably 0.4 to 2.5% by mass, and more preferably 0.8 to 1.5% by mass.

[0046] (1-5) External additives The toner may contain an external additive in order to improve its transportability, chargeability, and stirring property with the carrier in a two-component developer. As the external additive, an external additive commonly used in the technical field can be used, and examples thereof include inorganic fine particles such as silica and titanium oxide. Those that have been surface-treated (hydrophobized) with a silicone resin, a silane coupling agent, or the like are preferred, and silica particles are particularly preferred in terms of imparting electrostatic charge to the toner. The external additive is preferably inorganic fine particles having an average primary particle size of 6 to 200 nm. The amount of the external additive added is not particularly limited, but is preferably 0.2 to 5.0 parts by mass, and more preferably 0.5 to 2.5 parts by mass, relative to 100 parts by mass of the toner.

[0047] In the present invention, the toner is preferably externally added with large-diameter inorganic fine particles (also referred to as "second inorganic fine particles") having an average primary particle diameter of 20 to 50 nm, instead of or together with the above-mentioned inorganic fine particles (also referred to as "first inorganic fine particles" for distinction). By adding inorganic fine particles having a large particle diameter to the outside, the adhesive force between the toner and the carrier can be reduced, and the occurrence of spent can be suppressed. The second inorganic fine particles are preferably added in an amount of 0.3 to 1.0 part by mass with respect to 100 parts by mass of the toner. If the amount of the second inorganic fine particles added is less than 0.3 parts by mass, the adhesive force is not sufficiently reduced, and a significant effect on the development memory may not be obtained. On the other hand, if the amount of the second inorganic fine particles added is more than 1.0 parts by mass, the toner fluidity decreases, and the toner may not fall from the toner cartridge. A more preferable amount of the second inorganic fine particles added is 0.5 to 1.0 parts by mass. When the first inorganic fine particles and the second inorganic fine particles are used in combination, the total amount of them added is preferably 0.5 to 2.5 parts by mass with respect to 100 parts by mass of the toner.

[0048] (1-6) Toner properties In the present invention, the toner preferably contains 10 to 30% by mass of tetrahydrofuran (THF) insoluble matter. By setting the content of the THF insoluble matter in the toner within the above range, the occurrence of spent can be suppressed. If the content of the THF insoluble matter is less than 10% by mass, the adhesion of the toner to the carrier is not sufficiently reduced, and a significant effect on the development memory may not be obtained. On the other hand, if the content of the THF insoluble matter is more than 30% by mass, the low-temperature fixability may be impaired. The content of the THF insoluble matter is more preferably 15 to 20% by mass. The method for measuring the THF insoluble matter will be described in detail in the Examples.

[0049] (2) Career (2-1) Carrier voltage value The carrier constituting the two-component developer together with the toner is an iron powder carrier, and the bridge resistance measurement method is used to apply 1V stepwise to the carrier, and the current flowing through the carrier is 10 -5 When A, the carrier voltage value α (V) is 5≦α≦30. By setting the carrier voltage value within the above range, the occurrence of spent toner can be suppressed. If the carrier voltage value is less than 5 V, the carrier resistance is too low, which may cause deterioration of fog, whereas if the carrier voltage value is more than 30 V, the carrier resistance is too high, which may cause development memory. The carrier voltage value is more preferably 8 to 20V. The method for measuring the carrier voltage value will be described in detail in the Examples.

[0050] (2-2) Carrier fluidity The carrier preferably has a flowability of 9.0 to 20.0 sec / 50 g. Iron powder carriers inherently have uneven surfaces, and the release agent that has detached from the toner tends to adhere to the concave portions. By setting the fluidity, which is an index of the amount of unevenness, within the above range, it is possible to suppress the adhesion of the release agent and thereby suppress the occurrence of spent toner. If the carrier fluidity is less than 9.0 sec / 50 g, the unevenness is small, so the amount of spent is less than expected, and the effect of the resistance drop due to the peeling of the coating becomes large, which may lead to worsening of fogging. On the other hand, if the carrier fluidity exceeds 20.0 sec / 50 g, the unevenness is large, so the amount of spent cannot be sufficiently suppressed, and no improvement effect against development memory may be observed. The fluidity of the carrier is more preferably 10.0 to 15.0 seconds / 50 g. The fluidity of the carrier can be measured in accordance with JIS Z2502:2012 "Metal powder - Flowability measurement method", and the measurement method will be described in detail in the examples.

[0051] (2-3) Carrier surface coating The carrier is preferably an iron powder carrier that has been coated (surface treated) with a coating agent commonly used in the art. By covering the carrier with a coating agent, the occurrence of spent toner can be suppressed. Examples of the coating agent include silicone resin, acrylic resin, and fluorine resin. In the present invention, iron powder coated with silicone resin is preferred as the coating agent in terms of spent resistance and antistatic properties. The coating method may be any method known in the art, but in the present invention, it is preferable that the carrier is an iron powder carrier coated with the coating agent by a dipping method. In the spray drying method, the surface of the carrier is uniformly covered with a coating agent, which increases the carrier resistance and may easily cause development memory.

[0052] (2-4) Average primary particle size of carrier The average primary particle size of the carrier is preferably from 60 to 100 μm, and more preferably from 60 to 80 μm. If the average primary particle size of the carrier is less than 60 μm, it becomes subject to regulations under the Fire Service Act and becomes difficult to handle, whereas if the average primary particle size of the carrier is more than 100 μm, the charge imparting ability may be significantly impaired when spent occurs.

[0053] (2-5) Carrier and toner blend ratio The blending ratio of the carrier and the toner is not particularly limited, but the concentration of the toner is preferably 3.0 to 10.0% by mass, more preferably 4.0 to 7.5% by mass, based on the total mass of the carrier and the toner. If the toner concentration is less than 3.0% by mass, the amount of toner available for development may be insufficient to ensure sufficient image density, whereas if the toner concentration is more than 10.0% by mass, the toner may not be charged sufficiently, resulting in increased fogging.

[0054] (3) Manufacturing method of two-component developer The two-component developer of the present invention can be produced by a method known in the art. For example, at least a binder resin, a colorant, and a release agent are mixed, melted, and kneaded, the resulting molten and kneaded mixture is cooled and solidified, pulverized, and finely pulverized, and the finely pulverized mixture is classified. An external additive is optionally added to the resulting toner, and the toner is further mixed with a carrier to obtain a two-component developer. The toner of the present invention can be produced by a wet method or a dry method. The dry method is preferred in terms of the fewer number of steps and the lower equipment costs, and among these, the pulverization method is particularly preferred. The conditions for each of the following steps may be appropriately set depending on the target material and the desired physical properties.

[0055] For mixing, a known device commonly used in the technical field can be used, for example, a Henschel-type mixer such as Henschel Mixer (product name, manufactured by Mitsui Mining Co., Ltd. (now Nippon Coke and Engineering Co., Ltd.)), Super Mixer (product name, manufactured by Kawata Corporation), or Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.), an Ang Mill (product name, manufactured by Hosokawa Micron Corporation), Hybridization System (product name, manufactured by Nara Machinery Works, Ltd.), or Cosmo System (product name, manufactured by Kawasaki Heavy Industries, Ltd.), etc. The melt kneader may be a known device commonly used in the technical field, for example, a general kneader such as a twin-screw extruder, a triple roll, a lab blast mill, etc. Specifically, for example, a single-screw or twin-screw extruder such as TEM-100B (trade name, manufactured by Toshiba Machine Co., Ltd.), PCM-65 / 87, PCM-30 (all of which are trade names, manufactured by Ikegai Corporation), or an open-roll type kneader such as Kneadex (trade name, manufactured by Mitsui Mining Co., Ltd.) may be used. For the fine pulverization, a known device commonly used in the art, such as a jet pulverizer that uses a supersonic jet stream to pulverize the material, or an impact pulverizer that introduces a solidified material into the space formed between a rotor and a stator (liner) rotating at high speed, can be used. For classification, a known device commonly used in the art, for example, a classifier capable of removing over-pulverized toner particles by centrifugal force and wind force, such as a swirling wind classifier (rotary wind classifier), can be used. EXAMPLES

[0056] The present invention will be specifically described below with reference to examples and comparative examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. In the examples and comparative examples, the physical properties were measured by the methods described below.

[0057] [Carrier voltage value (V)] The carrier voltage value is measured using a measuring jig 1 as shown in FIG. The measurement jig 1 is composed of a magnet 2, an aluminum electrode 3, and a substrate (acrylic resin plate) 4. The electrodes 3 are spaced 1 mm apart, forming parallel plate electrodes measuring 10 mm x 40 mm. 200 mg of carrier (carrier core material) is inserted between these electrodes, and then a magnet 2 (surface magnetic flux density 1500 gauss, magnet area of ​​opposing parts 10 mm x 30 mm) is placed so that the north and south poles face each other, holding the carrier between the electrodes. A DC voltage is applied to this electrode 3 in 1 V steps, and the current value is measured, reaching a current value of 1.0 x 10 -5 Measure the voltage at time A and use this as the carrier voltage value (V).

[0058] [Carrier fluidity (sec / 50g)] Measure the carrier flow rate in accordance with JIS Z2502:2012 "Metal powder - Flow rate measurement method."

[0059] [Tetrahydrofuran (THF) insolubles (%)] Approximately 3.0 g of toner, which has been weighed in advance, is dissolved in 1000 mL of THF at 45°C for 15 minutes, and the insoluble matter is filtered off using an Omnipore membrane filter (Merck, product name: JAWP04700). The insoluble matter remaining on the membrane filter is dried at 85°C for 10 hours, and the mass of the resulting dried matter is measured to calculate the THF insoluble matter (%).

[0060] [Melting point Tm (℃) of release agent (wax)] Using a differential scanning calorimeter (manufactured by Seiko Electronics Industries Co., Ltd. (currently Hitachi High-Tech Science Corporation), model: DSC220), 1 g of a sample of the release agent is heated from a temperature of 20°C to 200°C at a heating rate of 10°C / min, and then rapidly cooled from 200°C to 20°C. This operation is repeated twice to measure the DSC curve. The temperature of the endothermic peak corresponding to the melting of the DSC curve measured in the second operation is taken as the melting point Tm (°C) of the release agent.

[0061] [Dispersion diameter of release agent (wax) (μm)] The toner is embedded in epoxy resin, and the surface is polished using an ultramicrotome (manufactured by Reichert, product name: Ultracut N) to obtain a sample. The wax dispersion state of the obtained sample is observed using a scanning transmission electron microscope (manufactured by Hitachi High-Technologies Corporation, model: S-4800). 200 to 300 wax parts are randomly extracted from the obtained electron microscope photograph data, and the image is analyzed using image analysis software (product name: A-zo-kun, manufactured by Asahi Kasei Engineering Co., Ltd.) to determine the circle equivalent diameter (μm) of the wax, which is defined as the wax dispersion diameter (μm).

[0062] [Average primary particle size of inorganic fine particles (nm)] The inorganic microparticles are photographed using a scanning electron microscope (SEM) (Hitachi High-Technologies Corporation, model: S-4800), and the particle diameters (long diameters) of 100 inorganic microparticles are randomly selected from the obtained image and the average particle diameter of the 100 particles is calculated, which is regarded as the average primary particle diameter (nm) of the inorganic microparticles.

[0063] [Melting point of release agent (wax): ℃] Using a differential scanning calorimeter (manufactured by PerkinElmer Japan Co., Ltd., model: Diamond DSC), 0.01 g of wax is heated from a temperature of 20°C to 200°C at a heating rate of 10°C / min, and then rapidly cooled from 200°C to 20°C. This operation is repeated twice to measure the DSC curve, and the temperature of the endothermic peak corresponding to melting on the DSC curve measured in the second operation is regarded as the melting point of the wax (°C).

[0064] [Example 1] (Toner preparation process: mixing, kneading, pulverization / classification) Binder resin: amorphous polyester resin A (softening point: 152.0°C) 42% by mass : Amorphous polyester resin B (softening point: 99.0°C) 42% by mass Colorant: Carbon black (Cabot Corporation, product name: Regal 330) 6% by mass Release agent: 3% by mass of ester wax A (melting point: 76°C, product name: WE-15, manufactured by NOF Corporation) Release agent dispersant: styrene acrylic copolymer resin (manufactured by Mitsui Chemicals, Inc., product name: SA800) 5% by mass Charge control agent: Salicylic acid compound (Orient Chemical Industry Co., Ltd., product name: BONTRON E-84) 2% by mass

[0065] The above materials were premixed for 5 minutes using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd. (now Nippon Coke and Engineering Co., Ltd.), model: FM20C), and then melt-kneaded using a twin-screw extruder (manufactured by Ikegai Corporation, model: PCM-65) under conditions of a cylinder setting temperature of 110°C, a barrel rotation speed of 300 rpm, and a raw material supply rate of 80 kg / hour to obtain a molten kneaded product. The resulting molten mixture was cooled using a belt drum flaker (manufactured by Nippon Coke & Engineering Co., Ltd., model: MBD55-70) and then coarsely pulverized, then finely pulverized using a jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd., model: IDS-2), and further classified using an air classifier (manufactured by Nippon Pneumatic Mfg. Co., Ltd., model: DXF-20) to obtain a toner having an average particle size of 6.5 μm.

[0066] (External addition process) To 100 parts by mass of the obtained toner base particles, 1.2 parts by mass of commercially available inorganic fine particles A (silica fine particles, average primary particle diameter 7 nm, manufactured by Aerosil Corporation, product name: R976) were added, and the mixture was stirred for 2 minutes using an air flow mixer (Henschel mixer, manufactured by Mitsui Mining Co., Ltd. (now Nippon Coke and Engineering Co., Ltd.), model: FM20C) with the tip speed of the stirring blade set to 40 m / sec, to obtain an externally added toner.

[0067] (Iron powder carrier preparation process) (Preparation of Coating Resin Liquid) Coating resin A (silicone-based, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR240) 0.470 parts by mass Coating resin B (silicone-based, manufactured by Shin-Etsu Chemical Co., Ltd., product name: KR251) 0.470 parts by mass Conductive particles (Cabot Corporation, product name: VULCAN XC-72) 0.0375 parts by mass Coupling agent (manufactured by Dow Corning Toray Co., Ltd., product name: AY43-059) 0.0225 parts by mass Solvent (toluene) 12 parts by weight The above materials were mixed to prepare 13.0 parts by mass of a coating resin liquid, and the coating resin liquid obtained by a dipping method was used to coat the surface of 100 parts by mass of an iron powder carrier core material (volume average particle size: 60 μm, manufactured by Kanto Denka Kogyo Co., Ltd.). Thereafter, the mixture was subjected to a curing process at a curing temperature of 200° C. for a curing time of 1 hour, and then sieved through a sieve with an opening of 150 μm to obtain a resin-coated carrier.

[0068] (Preparation process of two-component developer) Next, the obtained toner with external additives and the resin-coated carrier were mixed so that the concentration of the toner with external additives relative to the total amount of the two-component developer was adjusted to 5%, thereby obtaining a two-component developer with a toner concentration of 5%.

[0069] (Example 2 23 and Comparative Examples 1 to 4) A two-component developer was obtained in the same manner as in Example 1, except that the resin ratios (%) of amorphous polyester resins A and B, the type and blending ratio (%) of the release agent in the toner preparation process, and the presence or absence of a release agent dispersant; the use of second inorganic fine particles (large particle size) in the external addition process, and the type and blending ratio; and the amount (parts) of the coating resin liquid used in the iron powder carrier preparation process were as shown in Tables 1 and 2.

[0070] The English symbols of the release agents and external additives in Tables 1 and 2 have the following meanings: Ester wax B (melting point: 79°C, NOF Corporation, product name: WE-14) Inorganic fine particles B (silica fine particles, average primary particle diameter 16 nm, manufactured by Aerosil Co., Ltd., product name: R972) Inorganic fine particles C (silica fine particles, average primary particle diameter 20 nm, manufactured by Aerosil Co., Ltd., product name: NX90S) Inorganic microparticles D (silica microparticles, average primary particle diameter 30 nm, manufactured by Shin-Etsu Chemical Co., Ltd., product name: sol-gel silica spherical microparticles X-24-9404-30) Inorganic fine particles E (silica fine particles, average primary particle diameter 50 nm, manufactured by Titan Kogyo Co., Ltd., product name: ES-650E) Inorganic fine particles F (silica fine particles, average primary particle diameter 115 nm, manufactured by Cabot Corporation, product name: TG-C191)

[0071] [evaluation] Regarding the following items, Examples 1 to 23 The two-component developers prepared in Comparative Examples 1 to 4 were evaluated, and a comprehensive evaluation was made based on the results. The obtained results are shown in Tables 3 and 4.

[0072] [Rating 1: Development memory] A commercially available copying machine (manufactured by Sharp Corporation, model: MX-M316FV) modified for the evaluation was filled with two-component developer, and 10,000 sheets of a document with a print rate of 1% were printed. Next, a development memory confirmation chart (having eight solid circular images arranged perpendicular to the paper feed direction at the leading edge in the paper feed direction, with a halftone image behind them) was printed, and the number of circular images that were repeated as ghost images on the halftone image along the paper feed direction was confirmed, and the "development memory" was judged from the number according to the following criteria. ◎: Excellent (no repeated ghost images) 〇: Good (one ghost image) △: Possible (ghost image twice) ×: Not possible (ghost image appears 3 or more times)

[0073] [Rating 2: Overlap] After evaluating the development memory, the surface potential of the drum was set to 600 V, and the development bias was adjusted to change the potential difference between the development bias and the drum surface potential from 200 to 350. The whiteness of the non-image area in the image obtained at each potential difference was measured using a spectrophotometer (manufactured by Nippon Denshoku Industries Co., Ltd., model: ZE6000), and the "fogging" was judged from the averaged value according to the following criteria. ◎: Excellent (whiteness less than 0.5) ○: Good (whiteness is 0.5 or more and less than 1.0) △: Acceptable (whiteness is 1.0 or more and less than 2.0) ×: Unacceptable (whiteness is 2.0 or more)

[0074] [Evaluation 3: Low temperature fixability] A fixed image was formed using a two-component developer using a commercially available copying machine (model: MX-5100FN, manufactured by Sharp Corporation) modified for the evaluation. First, a sample image including a solid image (a rectangle measuring 20 mm in length and 50 mm in width) was formed as an unfixed image on a recording paper (manufactured by Sharp Corporation, PPC paper, model: SF-4AM3). At this time, the amount of toner adhering to the recording paper in the solid image was 0.5 mg / cm 2 It was adjusted to be. Next, a fixed image was produced using a hard roller fixing device. The fixing process speed was set to 120 mm / sec, and the temperature of the fixing roller was increased in increments of 5° C. from 110° C. to determine the minimum temperature at which low-temperature offset did not occur. "Low temperature offset" is defined as a phenomenon in which toner is not fixed to the recording paper during fixing, but remains attached to the fixing belt and adheres to the recording paper after the fixing belt has made one revolution. From the obtained results, the "low temperature fixability" was judged according to the following criteria. ◎: Excellent (minimum temperature is 105℃ or less) ○: Good (minimum temperature is 110℃ or higher and less than 120℃) △: Possible (minimum temperature is 120℃ or higher and less than 130℃) ×: Not possible (minimum temperature is 130℃ or higher)

[0075] [Rating 4: Filming] Filming is likely to occur in two-component developers in which inorganic fine particles having an average primary particle diameter of 20 to 50 nm are externally added to the toner. Since it was confirmed that filming did not occur in the two-component developer of Example 1, the two-component developers of Examples 12 to 20 were evaluated. After evaluating the development memory, the drum surface is observed with a scanning transmission electron microscope (manufactured by Hitachi High-Technologies Corporation, model: S-4800) to see whether or not inorganic fine particles have adhered thereto. From the results obtained, "filming" was judged according to the following criteria. ○: Good (no adhesion observed) △: Fair (some adhesion was observed, but no image defects occurred) ×: Not possible (there is adhesion and poor image quality)

[0076] [Evaluation 5: Amount of toner falling] A decrease in the amount of toner falling, like filming, is likely to occur in two-component developers in which inorganic microparticles having an average primary particle diameter of 20 to 50 nm are externally added to the toner. Since it was confirmed that no decrease in the amount of toner falling was observed in the two-component developer of Example 1, the two-component developers of Examples 12 to 20 were evaluated. After evaluating the development memory, 500 sheets of a document with a print rate of 25% were printed continuously to check whether image density reduction occurred (if the amount of toner falling is small, toner replenishment cannot keep up and image density reduction occurs). Image density (ID) was measured using a spectrodensitometer (X-Rite, model: X-Rite504). From the results obtained, the "amount of toner falling" was judged according to the following criteria. ○: Good (no image density decrease, good, ID=1.30 or more) △: Passable (image density is slightly reduced but within the acceptable range, ID=1.25 or more and less than 1.30) ×: Not possible (amount of toner falling is small, causing a decrease in image density, ID=less than 1.25)

[0077] [comprehensive evaluation] Based on the above evaluation results, an overall evaluation was made according to the following criteria. ◎: Excellent (Good in all evaluation items, with at least one excellent item. Usable) ○: Good (Good on average. Even if there are some items that are fair, it is fine if there are other excellent items. Usable) △: Fair (Below good on average. However, there are no items that are bad. Usable.) ×: Not available (There is even one item that is not available. : Not available)

[0078] [Table 1]

[0079] [Table 2]

[0080] [Table 3]

[0081] [Table 4]

[0082] The following can be seen from Tables 1 to 4: (1) The two-component developer satisfying the requirements of the present invention (Examples 1 to 23) has excellent low-temperature fixing properties, suppresses contamination of the fixing member during fixing, does not cause development memory or fogging due to toner spent, and has excellent life. (2) The iron powder carrier has the advantage that it is unlikely to cause initial development memory, and by controlling the amount of spent toner, the life span of the iron powder carrier, which was a problem in the past, can be overcome.

[0083] (3) When the effects of each of the two-component developer and toner compositions are considered, the following can be seen. (a) Wax dispersion diameter If the thickness is less than 0.2 μm, the wax effect will not be achieved and the fixation will deteriorate, and if the thickness exceeds 2.0 μm, the amount of spent will increase and the development memory will deteriorate. (b) Carrier voltage If the voltage is less than 5V, the carrier resistance is too low, which causes the fogging to worsen, and if the voltage is more than 30V, the carrier resistance is too high, which causes development memory. (c) Carrier mobility At less than 9.0 sec / 50 g, the unevenness is small, so the amount of spent is less than expected, and the effect of the resistance drop due to the peeling of the coating becomes large, which may lead to worsening of fogging. At more than 20.0 sec / 50 g, the unevenness is large, so the amount of spent cannot be sufficiently suppressed, and no improvement effect on development memory may be seen.

[0084] (d) Silicone resin coating From the viewpoints of spent resistance and electrostatic chargeability, silicone-based resins are preferred as coating agents; acrylic-based resins have high surface energy and are prone to causing spent, while fluorine-based resins have low surface energy and are advantageous in terms of spent resistance, but are negatively charged and therefore difficult to use from the viewpoint of electrostatic chargeability. (e) Immersion method The coating method is preferably a dipping method. In the spray-drying method, the carrier surface is uniformly coated with the coating agent, which increases the carrier resistance and may easily cause development memory. (f) Tetrahydrofuran (THF) insolubles If the content of THF insoluble matter is less than 10% by mass, the elasticity of the toner is low, and the reduction in adhesion to the carrier is insufficient, so that a significant effect on development memory may not be obtained. If the content of THF insoluble matter exceeds 30% by mass, low-temperature fixability may be impaired.

[0085] (g) Second inorganic fine particles Regarding the particle size, if it is less than 20 nm, the spacer effect for reducing the adhesive force between the toner and carrier is small, and sufficient ability to suppress spent may not be expected. If it exceeds 50 nm, another problem of filming occurs, which is undesirable. Regarding the amount added, if it is less than 0.3 parts by mass, the adhesive force reduction is insufficient and a large effect on suppressing spent may not be obtained. If the amount added of the second inorganic fine particles exceeds 1.0 part by mass, the fluidity of the toner decreases, and the toner may not fall out of the toner cartridge. (h) Styrene-acrylic copolymer resin By including a styrene-acrylic copolymer resin, the ester wax of the release agent can be easily dispersed in the binder resin at the above-mentioned dispersion diameter, and the occurrence of spent can be suppressed. (i) Release agent dispersant in toner The content is not particularly limited, but is preferably 1.0 to 5.0 parts by weight per 100 parts by weight of the binder resin. If it is less than 1.0 part by weight, the effect as a dispersant may not be fully exhibited, and if it exceeds 5.0 parts by weight, low-temperature fixability may be impaired. [Explanation of symbols]

[0086] 1 Measuring tool 2. Magnets 3 electrodes 4. Board 5. Binder resin (polyester resin) 6 Release agent (ester wax) 7. Colorants 8. Career 9 Toner Spent 10 Toner

Claims

1. A two-component developer including a toner containing at least a binder resin, a colorant, and a release agent, and a carrier, The binder resin is a polyester resin, the release agent is an ester wax and has a dispersion diameter of 0.2 to 2.0 μm in the toner; the toner contains 10 to 30% by mass of a tetrahydrofuran (THF) insoluble matter, The carrier is an iron powder carrier, and a bridge resistance measurement method is used to apply 1 V stepwise to the carrier, and the current flowing through the carrier is 10 -5 A carrier voltage value α (V) of 8 to 20 V and a flow rate of 9.0 to 20.0 sec / 50 g. A two-component developer comprising:

2. 2. The two-component developer according to claim 1, wherein the carrier is an iron powder carrier coated with a silicone resin as a coating agent.

3. 3. The two-component developer according to claim 1, wherein the toner comprises inorganic fine particles having an average primary particle size of 20 to 50 nm added externally.

4. 4. The two-component developer according to claim 3, wherein the inorganic fine particles are contained in an amount of 0.3 to 1.0 part by mass with respect to 100 parts by mass of the toner.

5. 5. The two-component developer according to claim 1, wherein the toner further contains a styrene-acrylic copolymer resin as a release agent dispersant.

Citation Information

Patent Citations

  • Toner

    JP2016042135A

  • Toner and production method of toner

    JP2017003990A