Anode active material, anode active material layer, lithium ion battery, and method for producing anode active material

Doping clathrate-type Si particles with specific metals in lithium ion batteries addresses the volume change issue, improving stability and performance by enhancing internal conductivity.

JP7578649B2Active Publication Date: 2024-11-06TOYOTA JIDOSHA KK +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022114226
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-15
Publication Date
2024-11-06
Estimated Expiration
2042-07-15

AI Technical Summary

Technical Problem

Si particles as an active material in batteries undergo significant volume changes during charging and discharging, which can lead to structural instability.

Method used

A negative electrode active material is developed using clathrate-type Si particles doped with metals such as Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V, with a content of 0.01 to 1.60% by mass, to improve internal conductivity and reduce volume changes during charging and discharging.

Benefits of technology

The doped clathrate-type Si particles effectively reduce volume changes during charging and discharging, enhancing the stability and performance of lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578649000003
    Figure 0007578649000003
  • Figure 0007578649000001
    Figure 0007578649000001
  • Figure 0007578649000002
    Figure 0007578649000002
Patent Text Reader

Abstract

To provide a negative electrode active material which is reduced in volume changes during charging and discharging.SOLUTION: A negative electrode active material of the present disclosure is clathrate type Si particles containing at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb and V. A negative electrode active material layer of the present disclosure includes the negative electrode active material of the present disclosure. A lithium ion battery of the present disclosure includes the negative electrode active material layer of the present disclosure. A production method of the present disclosure includes: providing a mixture of NaSi alloy powder, a Na trap agent, and at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb and V; and heating the mixture at a heating temperature of 250-500°C for a heating time of 30-200 hours.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a negative electrode active material, a negative electrode active material layer, a lithium ion battery, and a method for manufacturing a negative electrode active material.

Background Art

[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Also, Si is known as an active material used in batteries.

[0003] Patent Document 1 discloses an active material having a crystal phase of silicon class rate type II and having a composition of Na x Si 136 (1.98 < x < 2.54).

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] Si particles as an active material are effective in increasing the energy density of the battery, but have a large volume change during charge and discharge.

[0006] Si particles having a class rate type structure described in Patent Document 1 are advantageous for reducing the volume change during charge and discharge.

[0007] However, there is still a need to reduce the volume change of Si particles during charge and discharge.

[0008] The main object of the present disclosure is to provide a negative electrode active material with reduced volume change during charge and discharge. [Means for solving the problem]

[0009] The present inventors have found that the above object can be achieved by the following means: Aspect 1 A negative electrode active material which is a clathrate-type Si particle containing at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V. Aspect 2 2. The negative electrode active material according to aspect 1, wherein a content of the metal relative to the total amount of the clathrate-type Si particles is 0.01 to 1.60% by mass. Aspect 3 3. The negative electrode active material according to claim 1 or 2, wherein the metal is interstitially doped into the clathrate-type Si particles. Aspect 4 The negative electrode active material according to any one of aspects 1 to 3, wherein the clathrate type Si particles at least partially have a clathrate II type structure. Aspect 5 The negative electrode active material according to any one of Aspects 1 to 4, which is for use in a lithium ion battery. Aspect 6 A negative electrode active material layer containing the negative electrode active material according to any one of the first to fifth aspects. Aspect 7 A lithium ion battery comprising, in this order, a negative electrode current collector layer, the negative electrode active material layer according to embodiment 6, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer. Aspect 8 Providing a mixture of NaSi alloy powder, a Na trapping agent, and at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V; and heating the mixture at a heating temperature of 250 to 500° C. for a heating time of 30 to 200 hours; It has A method for producing a negative electrode active material. Aspect 9: 9. The method of claim 8, comprising mechanically milling a Si source, a NaH source, and the metals, and heating to obtain the mixture of the NaSi alloy powder and the metals. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a negative electrode active material that mainly reduces volume change during charging and discharging. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram of a lithium ion battery according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0013] 《Negative electrode active material》 The negative electrode active material of the present disclosure is a clathrate-type Si particle containing at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V.

[0014] The negative electrode active material of the present disclosure is preferably for use in a lithium ion battery, and the following description will be given on the assumption that it is for use in a lithium ion battery. However, this does not preclude application of the negative electrode active material to other types of batteries in which the carrier ions are different from lithium ions.

[0015] Without being limited by theory, the principle by which the negative electrode active material particles of the present disclosure reduce volume change during charging and discharging of a battery is believed to be as follows.

[0016] It is known that Si-based negative electrode active materials, such as those used in lithium ion batteries, have large expansion and contraction during charging and discharging. Clathrate-type Si particles are an example of an active material that reduces the expansion and contraction of such Si-based negative electrode active materials during charging and discharging.

[0017] The negative electrode active material of the present disclosure contains at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V in the clathrate type Si particle, thereby improving the electrical conductivity in the clathrate type Si particle. Therefore, the negative electrode active material of the present disclosure reduces the reaction with lithium in the particle, i.e., the bias in the absorption and release of lithium, during charging and discharging of the battery. As a result, the negative electrode active material of the present disclosure reduces the volume change during charging and discharging of the battery.

[0018] The content of at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V in the entire clathrate type Si particles is preferably 0.01 to 1.60 mass %.

[0019] When the metal content is 0.01% by mass or more, the electrical conductivity inside the clathrate-type Si particles can be improved. On the other hand, when the metal content is 1.60% by mass or less, the crystal structure of the clathrate-type Si particles, particularly the clathrate structure, is easily maintained, so that the amount of lithium that can be absorbed by the clathrate-type Si particles due to the introduction of the metal into the clathrate-type Si particles is less affected.

[0020] The metal content in the clathrate type Si particles may be 0.01 mass% or more, 0.10 mass% or more, 0.15 mass% or more, or 0.17 mass% or more, and may be 1.60 mass% or less, 1.00 mass% or less, 0.50 mass% or less, or 0.20 mass% or less.

[0021] It is preferable that the metal is interstitially doped into the clathrate-type Si particles, that is, the metal is doped in such a manner that the metal does not replace the crystal lattice of the clathrate-type Si particles but penetrates into the crystal lattice. When the metal is doped in such a manner, the crystal structure of the clathrate-type Si particles is easily maintained.

[0022] In addition, the clathrate-type Si particles preferably have at least a partial clathrate II structure, which can store a large amount of lithium in its internal cage structure and therefore tends to expand and contract less during charging and discharging.

[0023] The clathrate type Si particles may have, for example, both a portion having a clathrate I type structure and a portion having a clathrate II type structure.

[0024] The shape of the clathrate type Si particles may be, for example, particulate. The average particle size (D50) of the clathrate type Si particles is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the clathrate type Si particles may be, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0025] 《Negative electrode active material layer》 The negative electrode active material layer of the present disclosure contains the negative electrode active material of the present disclosure. The negative electrode active material layer of the present disclosure may further contain, optionally, a solid electrolyte, a conductive assistant, and a binder.

[0026] <Solid electrolyte> The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in a lithium ion battery can be used. For example, the solid electrolyte may be, but is not limited to, a sulfide solid electrolyte, an oxide solid electrolyte, or a polymer electrolyte.

[0027] Examples of sulfide solid electrolytes include, but are not limited to, sulfide-based amorphous solid electrolytes, sulfide-based crystalline solid electrolytes, and argyrodite-type solid electrolytes.

[0028] A specific example of a sulfide solid electrolyte is the Li2S-P2S5 system (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0029] An example of an oxide solid electrolyte is Li7La3Zr2O 12、 Li 7-x La3Zr 1-x Nb x O 12、 Li 7-3x La3Zr2Al x O 12 , Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4, or Li 3+x PO 4-x N x (LiPON), but is not limited to these.

[0030] The sulfide solid electrolyte and the oxide solid electrolyte may be glass or crystallized glass (glass ceramic).

[0031] Examples of the polymer electrolyte include, but are not limited to, polyethylene oxide (PEO), polypropylene oxide (PPO), and copolymers thereof.

[0032] <Conductive assistant> The conductive additive is not particularly limited. For example, the conductive additive may be a carbon material such as VGCF (Vapor Grown Carbon Fiber), Ketjen Black (KB), Acetylene Black (AB), and carbon nanofiber, or a metal material, but is not limited thereto.

[0033] <Binder> The binder is not particularly limited. For example, the binder may be, but is not limited to, a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), or styrene butadiene rubber (SBR), or a combination thereof.

[0034] Lithium-ion battery The lithium ion battery of the present disclosure includes, in this order, a negative electrode current collector layer, a negative electrode active material layer of the present disclosure, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer. The lithium ion battery of the present disclosure may be a secondary battery.

[0035] FIG. 1 is a lithium-ion battery 1 according to one embodiment of the present disclosure.

[0036] The lithium ion battery 1 of the present disclosure has, in this order, a negative electrode current collector layer 11, a negative electrode active material layer 12 of the present disclosure, a solid electrolyte layer 13, a positive electrode active material layer 14, and a positive electrode current collector layer 15.

[0037] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, the material may be stainless steel (SUS), aluminum, copper, nickel, iron, titanium, carbon, or a resin current collector, but is not limited to these.

[0038] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0039] <Solid electrolyte layer> The solid electrolyte layer is a layer containing a solid electrolyte and, optionally, a binder and the like.

[0040] For the solid electrolyte and the binder, reference can be made to the descriptions of "<Solid electrolyte>" and "<Binder>" in the "<Negative electrode active material layer>" section above, respectively.

[0041] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally a solid electrolyte, a conductive assistant, a binder, and the like.

[0042] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0043] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y M y The material may be, but is not limited to, a Li-Mn spinel substituted with a different element having a composition represented by O4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn).

[0044] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.

[0045] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0046] For the solid electrolyte, conductive additive, and binder, see the descriptions in the above "<Solid electrolyte>", "<Conductive additive>", and "<Binder>" in "<Negative electrode active material layer>", respectively.

[0047] <Positive electrode current collector layer> The material and shape of the positive electrode current collector layer are not particularly limited, and the materials and shapes described in the above "Negative electrode current collector layer" may be used. In particular, the material of the positive electrode current collector layer is preferably aluminum. The shape is preferably a foil.

[0048] <<Method for producing negative electrode active material>> The manufacturing method of the present disclosure is a method for manufacturing a negative electrode active material, comprising: providing a mixture of a NaSi alloy powder, a Na-trapping agent, and at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V; and heating the mixture at a heating temperature of 250 to 500° C. for a heating time of 30 to 200 hours.

[0049] By mixing a NaSi alloy powder with a Na-trapping agent and heating the mixture at a predetermined temperature for a predetermined time, Na is desorbed from the NaSi alloy, and clathrate-type Si particles having a clathrate-type structure, particularly a clathrate II type structure, are generated.

[0050] The manufacturing method of the present disclosure can improve the electrical conductivity inside the clathrate-type Si particles produced by adding at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V to the raw material during the production process of the clathrate-type Si particles.

[0051] The Na-trapping agent is not limited to one that reacts with a NaSi alloy to receive Na from the NaSi alloy, but may also react with Na desorbed from the NaSi alloy, specifically, Na vapor.

[0052] Specific examples of the Na-trapping agent include particles of CaCl2, CaBr2, CaI2, Fe3O4, FeO, MgCl2, ZnO, ZnCl2, MnCl2, AlF3, etc. As the Na-trapping agent, AlF3 particles are particularly preferred.

[0053] The heating temperature may be 250° C. or more, 300° C. or more, or 350° C. or more, and may be 500° C. or less, 450° C. or less, 400° C. or less, or 350° C. or less.

[0054] The heating time may be 30 hours or more, 40 hours or more, 50 hours or more, or 100 hours or more, and may be 200 hours or less, 180 hours or less, 160 hours or less, or 100 hours or less.

[0055] In the manufacturing method of the present disclosure, at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V may be added in advance during the production of the NaSi alloy powder.

[0056] That is, a Si source, a NaH source, and a metal may be mechanically milled and heated to obtain a mixture of NaSi alloy powder and a metal.

[0057] At least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V may be prepared as metal particles and mixed with the raw material, or may be derived from the cutter of the cutter mill used in the mechanical milling performed in the clathrate type Si particle production process. When the metal is derived from the cutter of the cutter mill, it is preferable to use a cutter mill when mixing, for example, the Na source and the Si source during the production of the NaSi alloy powder. When a cutter mill is used during the production of the NaSi alloy powder, the newly formed surface is exposed in the produced NaSi alloy powder, and the specific surface area of ​​the NaSi alloy powder is likely to increase. Therefore, even when a cutter mill is used in the clathrate type Si particle production process performed after the NaSi alloy powder production process, the metal derived from the cutter mill is likely to be further mixed into the NaSi alloy powder. EXAMPLES

[0058] Examples 1 to 4 and Comparative Example 1 Preparation of Active Material Comparative Example 1 Si particles were used as the Si source and Na particles were used as the Na source, and the Si particles and Na particles were mixed in a molar ratio of 1:1, placed in a crucible, sealed in an Ar atmosphere, and heated at 700°C to obtain a NaSi alloy. The obtained NaSi alloy was heated under vacuum (approximately 1 Pa) at 340°C to remove Na, and an intermediate having a silicon clathrate type II crystal phase was obtained.

[0059] The intermediate and Li metal were weighed out in a molar ratio of Li / Si=1.7 and mixed in a mortar in an Ar atmosphere to obtain an alloy compound. The alloy compound was reacted with ethanol in an Ar atmosphere to form voids inside the primary particles, thereby obtaining an active material.

[0060] Example 1 As the Si source, Si powder (Si powder having no voids inside the primary particles) was prepared. This Si source and Li metal were weighed out in a molar ratio of Li / Si=4.75 and mixed in a mortar in an Ar atmosphere to obtain an alloy compound. The obtained alloy compound was reacted with ethanol in an Ar atmosphere to obtain Si having voids inside the primary particles. Using this Si source and NaH as the Na source, a NaSi alloy was produced.

[0061] The NaH used was washed with hexane in advance. The Na source and the Si source were weighed out to a molar ratio of 1.05:1, and mixed using a cutter mill made of stainless steel (SUS304). The mixture was heated in a heating furnace under an Ar atmosphere at 400°C for 40 hours to obtain a powdered NaSi alloy.

[0062] Using the obtained NaSi alloy and further using AlF3 as a Na trapping agent, a silicon clathrate production process was carried out by the solid phase method.

[0063] Specifically, NaSi alloy and AlF3 were weighed out to a molar ratio of 1:0.20 and mixed using a cutter mill made of stainless steel (SUS304) to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a reaction vessel and heated in a heating furnace under Ar atmosphere at a heating temperature of 270°C for a heating time of 120 hours to cause a reaction.

[0064] The resulting reaction product is believed to contain the desired active material, as well as NaF and Al as by-products.

[0065] The reaction product was washed with a mixed solvent of HNO3 and H2O in a volume ratio of 10:90. This removed by-products from the reaction product. After washing, the mixture was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a powdered active material.

[0066] Example 2 An active material of Example 2 was obtained in the same manner as in Example 1, except that the heating conditions in the silicon clathrate production step by the solid phase method were an Ar atmosphere, a heating temperature of 290° C., and a heating time of 100 hours.

[0067] Example 3 A reaction product containing an active material was obtained in the same manner as in Example 1, except that the heating conditions in the silicon clathrate production step by the solid phase method were an Ar atmosphere, a heating temperature of 310° C., and a heating time of 60 hours.

[0068] The obtained reaction product was mixed with ZnCl2 and further heated in an Ar atmosphere at 310°C for 60 hours. The mass ratio of Si to ZnCl2 was 4:3.

[0069] Then, the mixture was washed with a mixed solvent of HNO3 and H2O in a volume ratio of 90:10. This removed by-products from the reaction product. After washing, the mixture was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain the active material of Example 3.

[0070] Example 4 The active material of Example 4 was obtained in the same manner as in Example 3, except that the heating conditions in the silicon clathrate production process by the solid-phase method were an Ar atmosphere, a heating temperature of 290°C, a heating time of 160 hours, and the mixing ratio of Si and ZnCl2 was 4:4.

[0071] Energy dispersive X-ray spectroscopy The crystallites of each active material were measured by energy dispersive X-ray spectroscopy (TEM-EDX). Each active material had a clathrate II type crystal structure.

[0072] The metal content (mass %) in the active material of each example was also measured. The measurement results are shown in Table 1.

[0073] <Creating a lithium-ion battery> Using the active material of each example, a lithium ion battery of each example was fabricated as follows.

[0074] (Formation of negative electrode body) Butyl butyrate, 5wt% butyl butyrate solution of polyvinylidene fluoride (PVDF) binder, vapor grown carbon fiber (VGCF) as a conductive additive, the synthesized active material, and Li2S-P2S5 glass ceramic as a sulfide solid electrolyte were added to a polypropylene container, and the mixture was stirred for 30 seconds with an ultrasonic dispersing device (UH-50 manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.) to obtain a negative electrode composite slurry.

[0075] The negative electrode mixture was applied onto a Cu foil by a blade method using an applicator, and then dried for 30 minutes on a hot plate heated to 100° C. to obtain a negative electrode body.

[0076] (Formation of solid electrolyte layer) Heptane, a 5 wt% heptane solution of butylene rubber (BR)-based binder, and Li2SP2S5-based glass ceramic as a sulfide solid electrolyte were added to a polypropylene container and stirred for 30 seconds with an ultrasonic disperser (UH-50, manufactured by SMT Co., Ltd.). Next, the container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.) to obtain a solid electrolyte slurry.

[0077] The solid electrolyte slurry was applied onto an Al foil serving as a release sheet by a blade method using an applicator, and dried on a hot plate heated to 100° C. for 30 minutes to form a solid electrolyte layer.

[0078] Three solid electrolyte layers were fabricated.

[0079] (Formation of positive electrode body) A polypropylene container is filled with butyl butyrate, a 5 wt% butyl butyrate solution of a PVDF-based binder, and LiNi with an average particle size of 6 μm as the positive electrode active material. 1 / 3 Co 1 / 3 Mn 1 / 3O2, Li2S-P2S5-based glass ceramic as a sulfide solid electrolyte, and VGCF as a conductive additive were added to a container and stirred for 30 seconds with an ultrasonic disperser (UH-50 manufactured by SMT).

[0080] Next, the container was shaken for 3 minutes with a shaker (TTM-1, manufactured by Shibata Scientific Co., Ltd.), further stirred with an ultrasonic dispersing device for 30 seconds, and then shaken with the shaker for 3 minutes to obtain a positive electrode composite slurry.

[0081] The positive electrode mixture slurry was applied onto an Al foil by a blade method using an applicator, and dried for 30 minutes on a hot plate heated to 100° C. to form a positive electrode body.

[0082] (Battery Assembly) The positive electrode body and the first solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 100 kN / cm and a temperature of 165° C. to obtain a positive electrode laminate.

[0083] The negative electrode body and the second solid electrolyte layer were laminated in this order, and the laminate was set in a roll press and pressed at a pressure of 60 kN / cm and a temperature of 25° C. to obtain a negative electrode laminate.

[0084] Furthermore, the Al foil as a release sheet was peeled off from the surfaces of the solid electrolyte layers of the positive electrode laminate and the negative electrode laminate, and then the Al foil as a release sheet was peeled off from the third solid electrolyte layer.

[0085] The positive electrode laminate and the negative electrode laminate were laminated on each other so that the solid electrolyte layer sides of each were facing the third solid electrolyte layer, and the laminate was set in a flat uniaxial press and pre-pressed at 100 MPa and 25° C. for 10 seconds, and finally the laminate was set in a flat uniaxial press and pressed for 1 minute at a pressure of 200 MPa and a press temperature of 120° C. This produced an all-solid-state battery.

[0086] <Charging and discharging lithium-ion batteries> The all-solid-state battery of each example was restrained at a predetermined restraining pressure using a restraining jig, and the amount of restraining pressure fluctuation was measured when the battery was charged at a constant current and constant voltage at a 10-hour rate (1 / 10C) up to 4.55 V. The amount of restraining pressure fluctuation is the difference between the maximum and minimum values ​​of the restraining pressure.

[0087] The volume expansion coefficient was calculated based on the amount of change in the confining pressure of the all-solid-state battery of each example. Specifically, the amount of change in the confining pressure was considered to be proportional to the amount of expansion of the active material, and the expansion coefficient of the active material of Examples 1 to 4 was calculated as a relative value with the expansion coefficient of the active material in Comparative Example 1 set to 100.00.

[0088] The expansion rate of each example is shown in Table 1.

[0089] <result> Table 1 shows the amount (mass %) of metal in the active material and the expansion coefficient of the particles for each example.

[0090] [Table 1]

[0091] The active materials of Examples 1 to 4, in which the metal content was 0.19 to 1.58% by mass, had significantly lower expansion rates during charging and discharging of a lithium ion battery than the active material of Comparative Example 1, in which the metal content was 0.01% by mass. Specifically, the active materials of Examples 1 to 4 had expansion rates of 27.5%, 25.0%, 18.75%, and 30.0%, respectively. The metals significantly mixed in Examples 1 to 4 are considered to be derived from the cutter mill made of stainless steel (SUS304) used in the clathrate Si manufacturing process. In particular, the use of a cutter mill in the manufacture of NaSi alloys is considered to be the factor that allowed the metals to be mixed in to the extent shown in Examples 1 to 4.

[0092] Examples 5 to 14 Using VASP ver.5.4.1, a model of a clathrate-type Si particle having a type II clathrate structure was created, and a structure was created in which randomly selected Si atoms in the model were replaced with different elements.

[0093] After that, the software was used to perform structural optimization using the pseudopotential PBEsol, and the expansion / contraction rate was calculated using the most stabilized structure.

[0094] The types of elements substituting the Si atoms in Examples 5 to 14 and the expansion / shrinkage rates are as shown in Table 2.

[0095] [Table 2]

[0096] As shown in Table 2, it is predicted that the expansion and contraction rate will also be reduced in clathrate-type Si particles in which some of the Si atoms are replaced with Zr, Ag, B, C, Co, Cr, Nb, Pd, Ti, and V. [Explanation of symbols]

[0097] 1 Lithium-ion battery 11 Negative electrode current collector layer 12 Negative electrode active material layer 13 Solid electrolyte layer 14 Cathode active material layer 15 Positive electrode current collector layer

Claims

1. A negative electrode active material comprising clathrate-type Si particles containing at least one metal selected from the group consisting of Mo, Pd, Zr, Ag, Co, Cr, Nb, and V.

2. The clathrate type Si particles contain at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V, The content of the metal relative to the total amount of the clathrate type Si particles is 0.02 to 1.60 mass %. Negative electrode active material.

3. 3. The negative electrode active material according to claim 1, wherein the metal is interstitially doped into the clathrate type Si particles.

4. 3. The negative electrode active material according to claim 1, wherein the clathrate type Si particles at least partially have a clathrate II type structure.

5. The negative electrode active material according to claim 1 or 2, which is for a lithium ion battery.

6. A negative electrode active material layer comprising the negative electrode active material according to claim 1 or 2.

7. A lithium ion battery comprising, in this order, a negative electrode current collector layer, the negative electrode active material layer according to claim 6, a solid electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

8. Providing a mixture of NaSi alloy powder, a Na trapping agent, and at least one metal selected from the group consisting of Mo, Fe, Zn, Mg, Pd, Zr, Ag, Co, Cr, Nb, and V; and heating the mixture at a heating temperature of 250 to 500° C. for a heating time of 30 to 200 hours; It has A method for producing a negative electrode active material.

9. 9. The method of claim 8, comprising mechanically milling a Si source, a NaH source, and the metal, and heating to obtain the mixture of the NaSi alloy powder and the metal.

Citation Information

Patent Citations

  • Electrode active material, electrode, battery, manufacturing method of electrode active material

    JP2016066418A

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158003A

  • Method for producing negative electrode active material

    JP2022034998A

  • Alloys Of Clathrate Allotropes For Rechargeable Batteries

    US20130280609A1

  • Type ii clathrates for rechargeable battery anodes

    US20150380724A1