Anode for all-solid-state battery including coating layer and ion transfer layer and lithium secondary battery including the same

The negative electrode with a lithium-affinity coating and amorphous carbon ion transport layer addresses lithium dendrite issues in all-solid-state batteries, enhancing battery life and safety through uniform lithium distribution and inhibited dendrite growth.

JP7578815B2Active Publication Date: 2024-11-06LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023524198
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-16
Filing Date
2021-11-05
Publication Date
2024-11-06
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

Lithium secondary batteries, particularly all-solid-state batteries with high energy density, suffer from performance deterioration due to lithium dendrites, which can cause short circuits and reduce battery life.

Method used

A negative electrode for all-solid-state batteries comprising a conductive metal current collector with a coating layer containing a lithium-affinity material and an ion transport layer made of amorphous carbon, which disperses lithium ions uniformly and inhibits their growth into dendrites.

Benefits of technology

The solution prevents local attachment of lithium, lowers nucleation energy, and ensures uniform electrodeposition, thereby improving battery life and safety by preventing dendrite growth and short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578815000003
    Figure 0007578815000003
  • Figure 0007578815000004
    Figure 0007578815000004
  • Figure 0007578815000005
    Figure 0007578815000005
Patent Text Reader

Abstract

The present invention relates to an anode for an all-solid-state battery, the anode including: an anode current collector made of an electrically conductive metal material; a coating layer attached to one or both surfaces of the anode current collector and containing a lithium affinity material; and an ion transport layer positioned on the coating layer and containing amorphous carbon through which lithium ions can move; and a lithium secondary battery including the anode for an all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention claims the benefit of priority based on Korean Patent Application No. 2020-0146810 filed on November 5, 2020 and Korean Patent Application No. 2021-0034266 filed on March 16, 2021, and all contents disclosed in the documents of the relevant Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a negative electrode for an all-solid-state battery including a coating layer and an ion transport layer, and a lithium secondary battery including the same, and more particularly, to a technology capable of preventing localized lithium plating in the negative electrode and identifying a position of lithium electrodeposition to prevent a short circuit from occurring between a positive electrode and a negative electrode. [Background technology]

[0003] Lithium secondary batteries are reusable and have high energy density, and are attracting attention as a new energy source with environmentally friendly characteristics, since they can dramatically reduce the use of fossil fuels and do not produce by-products due to the use of energy.

[0004] The lithium secondary battery has been attracting attention not only as an energy source for wearable or portable devices, but also as an energy source for devices having high output and high energy density, such as electric vehicles, etc. As a result, research on lithium secondary batteries having high operating voltages and energy densities has become more active.

[0005] In a lithium secondary battery, charging and discharging are performed through a process in which lithium ions move between a positive electrode and a negative electrode. Some of the lithium ions that move to the negative electrode are attached to the surface of the negative electrode to form lithium nuclei, which may grow into lithium dendrites, which are branched crystals.

[0006] When lithium dendrites formed and grown on the surface of the negative electrode come into contact with the positive electrode, it can cause a short circuit in the lithium secondary battery, which can shorten the lifespan of the lithium secondary battery and pose a problem in ensuring stable performance.

[0007] Due to these problems, conventional lithium secondary batteries use graphite as the negative electrode material, which has the disadvantage of low energy density.

[0008] In order to increase the energy density, it has been proposed to use lithium as an anode active material in a highly stable all-solid-state battery. Methods for using lithium as an anode active material include using lithium or a lithium alloy as an anode active material, or using lithium precipitated at the interface between the anode current collector and the solid electrolyte by charging in a state where no anode active material layer is formed on the anode current collector as an active material.

[0009] When lithium is used as the negative electrode active material, lithium is deposited on the negative electrode during charging, and when the negative electrode active material layer is not formed, lithium is deposited on the negative electrode current collector. The lithium deposited on the negative electrode in this way can grow into lithium dendrites through the gaps in the solid electrolyte when the all-solid-state battery is repeatedly charged and discharged. The lithium dendrites can cause a short circuit or a decrease in capacity of the battery.

[0010] Patent Document 1 discloses an electrode including a composite layer composed of a first lithium affinity layer, a second lithium affinity layer, and a perovskite layer in order to prevent the formation of lithium dendrites.

[0011] Patent Document 1 discloses that by applying a structure in which lithium affinity layers are sequentially arranged on the surface of an electrode, lithium ions can be uniformly attached to the surface of the electrode, thereby preventing the generation of lithium dendrites.

[0012] Patent Document 1 proposes an improvement in the life characteristics of a lithium secondary battery containing a liquid electrolyte, and recognizes a method for preventing the formation of lithium dendrites by lowering the potential at which lithium nuclei are generated, but does not propose a technology that can specify the position at which lithium adheres.

[0013] In lithium secondary batteries, there is a strong need for a technology that can not only prevent lithium ions from being locally plated on a portion of the surface of the negative electrode, but also prevent lithium dendrites from growing on the positive electrode side even if lithium nuclei are formed. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Chinese Patent No. 110571413 Summary of the Invention [Problem to be solved by the invention]

[0015] The present invention has been made to solve the above problems, and an object of the present invention is to provide a negative electrode for an all-solid-state battery, which can prevent a decrease in performance of a lithium secondary battery, particularly an all-solid-state battery having a high energy density, caused by lithium dendrites and can improve the yield by extending the life of the lithium secondary battery, and a lithium secondary battery including the same. [Means for solving the problem]

[0016] To achieve the above object, the present invention provides an anode for an all-solid-state battery, the anode comprising: an anode current collector made of an electrically conductive metal material; a coating layer attached to one or both sides of the anode current collector and containing a lithium affinity material; and an ion transport layer located on the coating layer and containing amorphous carbon through which lithium ions can move.

[0017] The ion transport layer may further comprise a binder.

[0018] The negative electrode mixture layer may not be formed on the negative electrode current collector.

[0019] The lithium affinity material may be at least one of metals including Au, Ag, Pt, Zn, Si, and Mg, and metal oxides including CuO, ZnO, CoO, and MnO.

[0020] The lithium affinity material constituting the coating layer may be in the form of nanoparticles, and may be in the form of metal nanoparticles or metal oxide nanoparticles attached onto the negative electrode current collector.

[0021] The present invention also provides a method for manufacturing a negative electrode for an all-solid-state battery, which specifically includes the steps of: (a) preparing a negative electrode current collector; (b) forming a coating layer including a lithium affinity material on at least one outer surface of the negative electrode current collector; and (c) forming an ion transport layer on the coating layer, and each of the steps may be performed sequentially.

[0022] The present invention also provides a lithium secondary battery including the anode for an all-solid-state battery, a solid electrolyte layer, and a cathode.

[0023] In the lithium secondary battery according to the present invention, the negative electrode for the all-solid-state battery has the lithium affinity material dispersed in a coating layer, and lithium plating can occur on the lithium affinity material.

[0024] In the lithium secondary battery according to the present invention, the negative electrode for an all-solid-state battery may be subjected to lithium electrodeposition on one surface of the ion transport layer facing the negative electrode current collector.

[0025] In the lithium secondary battery according to the present invention, the negative electrode for the all-solid-state battery may include a monocell in which a coating layer and an ion transport layer are formed only on a first surface of a negative electrode current collector, and a positive electrode is disposed on the first surface.

[0026] In the monocell, a coating layer may be formed on the negative electrode current collector, and the ion transport layer may be formed on the coating layer.

[0027] In the lithium secondary battery according to the present invention, the negative electrode for an all-solid-state battery is a lithium secondary battery including a bi-cell in which a coating layer and an ion conduction layer are formed on a first surface and a second surface, respectively, of a negative electrode current collector, and a first positive electrode and a second positive electrode are disposed on the first surface and the second surface, respectively.

[0028] In the bicell, a coating layer may be formed on the negative electrode current collector, and the ion transport layer may be formed on the coating layer.

[0029] Furthermore, the present invention can also be provided in a form in which the means for solving the above problems are combined in various ways. Effect of the Invention

[0030] As described above, in the present invention, since the lithium affinity material is widely dispersed on the negative electrode current collector for an all-solid-state battery, lithium that has migrated to the negative electrode can be widely distributed, and therefore, it is possible to prevent an increase in lithium nucleation energy due to localized deposition of lithium on the surface of the negative electrode current collector.

[0031] In addition, since an ion transport layer including amorphous carbon is formed on the coating layer including the lithium affinity material, lithium ions can move toward the negative electrode current collector, and lithium is deposited on one side of the ion transport layer toward the negative electrode current collector. Therefore, even if lithium dendrites are formed, their growth toward the positive electrode through the ion transport layer can be delayed.

[0032] In this way, the structure consisting of a combination of a coating layer containing a lithium affinity material and an ion transfer layer can induce uniform electrodeposition of lithium on the surface of the negative electrode current collector.

[0033] Therefore, in an all-solid-state battery including such a negative electrode, the life span can be improved and safety can be ensured. [Brief description of the drawings]

[0034] [Figure 1] 1A to 1C are schematic diagrams illustrating a process for producing a negative electrode according to the present invention. [Diagram 2] 1 is a SEM photograph of the negative electrode produced in Example 2. [Diagram 3] 1 is a SEM photograph of a cross section of a negative electrode produced in Example 2. [Figure 4] 1 is a SEM photograph of the negative electrode produced in Comparative Example 1. [Diagram 5] 1 is a SEM photograph of the negative electrode produced in Comparative Example 2. [Figure 6] 1 is a SEM photograph of the negative electrode produced in Comparative Example 3. [Figure 7] 1 is an SEM photograph of a cross section of a negative electrode produced in Comparative Example 6. [Figure 8] 1 is a SEM photograph of the negative electrode produced in Comparative Example 7. [Figure 9] 1 is a SEM photograph of the negative electrode produced in Comparative Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, with reference to the accompanying drawings, a detailed description will be given of an embodiment of the present invention that can be easily implemented by a person having ordinary skill in the art to which the present invention pertains. However, in describing the operation principle of the preferred embodiment of the present invention in detail, if it is determined that a detailed description of related well-known functions or configurations may unnecessarily obscure the gist of the present invention, the detailed description thereof will be omitted.

[0036] In addition, the same reference numerals are used throughout the drawings for parts having similar functions and actions. Throughout the specification, when one part is said to be connected to another part, this includes not only a direct connection but also an indirect connection via another element between them. In addition, the inclusion of one component does not mean the exclusion of other components, but may further include other components, unless otherwise specified.

[0037] Furthermore, descriptions that limit or add components to specify the invention are applicable to all inventions unless otherwise specified, and are not limited to descriptions of a specific invention.

[0038] Furthermore, throughout the description of the present invention and the claims, the singular includes the plural unless otherwise stated.

[0039] Furthermore, throughout the description of the present invention and the claims, unless otherwise stated, "or" includes "and." Therefore, "including A or B" means all three cases including A, including B, or including A and B.

[0040] Additionally, all numerical ranges include the endpoints and all intermediate values ​​therebetween unless expressly stated to exclude.

[0041] The negative electrode for an all-solid-state battery according to the present invention may include a negative electrode current collector made of an electrically conductive metal material, a coating layer added to one or both sides of the negative electrode current collector and containing a lithium affinity material, and an ion transport layer located on the coating layer and containing amorphous carbon through which lithium ions can move.

[0042] The negative electrode for an all-solid-state battery according to the present invention does not include a separate negative electrode mixture layer on a negative electrode current collector. Therefore, in this specification, the expression that a coating layer is formed on the surface of the negative electrode is used in the same sense as the expression that a coating layer is formed on the surface of the negative electrode current collector.

[0043] The type of the negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the lithium secondary battery and has conductivity, and examples of the negative electrode current collector include copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, aluminum-cadmium alloy, etc. Also, the negative electrode current collector may be in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, or the like, with or without fine irregularities on the surface.

[0044] For example, when a sulfide-based solid electrolyte is used, copper sulfate may be formed when a copper-based negative electrode current collector is used. To prevent this, a nickel or stainless steel negative electrode current collector may be used.

[0045] The thickness of the negative electrode current collector is not particularly limited, and may be 5 μm to 30 μm, more specifically, 10 μm to 20 μm. If the thickness of the negative electrode current collector exceeds 30 μm, there is a problem that the capacity per volume of the electrode is reduced, and if the thickness of the negative electrode current collector is less than 5 μm, a folding phenomenon may occur during the manufacture of the electrode.

[0046] The lithium affinity material constituting the coating layer is a material that is highly reactive with lithium. A battery cell is manufactured by combining a positive electrode with a negative electrode on which the coating layer and the ion transport layer are formed. When the battery cell is charged and discharged, lithium plating and electrodeposition occur on the lithium affinity material constituting the coating layer for lithium ions that have moved to the negative electrode.

[0047] The lithium affinity material contained in the coating layer may be at least one of metals including Au, Ag, Pt, Zn, Si, and Mg, and metal oxides including CuO, ZnO, CoO, and MnO.

[0048] In the present invention, the lithium affinity material is dispersed over the entire surface of the negative electrode current collector, but the lithium affinity material may aggregate and exist in islands so that the negative electrode current collector is partially exposed.

[0049] In one specific example, the lithium affinity material may be distributed in a range of 5% to 100% based on the total area of ​​the negative electrode current collector, more specifically, in a range of 10% to 90%, and even more specifically, in a range of 30% to 80%. More specifically, the lithium affinity material may be distributed in a range of 50% to 70% based on the total area of ​​the negative electrode current collector.

[0050] If the area of ​​the lithium affinity material is less than 5% based on the total area of ​​the negative electrode current collector, it is difficult to obtain the effect due to the narrow distribution area of ​​the lithium affinity material, which is undesirable.

[0051] As described above, in the negative electrode for an all-solid-state battery according to the present invention, the lithium affinity material is not locally electrodeposited on only a part of the surface of the negative electrode current collector, but is dispersed over a wide area, thereby lowering the lithium nucleation potential. That is, the formation of lithium nuclei in a specific part of the surface of the negative electrode current collector can be minimized. Therefore, lithium can be uniformly electrodeposited and grown on the surface of the negative electrode current collector, thereby suppressing the formation of lithium dendrites.

[0052] In addition, in the present invention, an ion transport layer is formed on the coating layer, and the ion transport layer does not impede the movement of lithium ions from the positive electrode to the negative electrode or from the negative electrode back to the positive electrode, and the lithium ions moving to the negative electrode can be transported in the direction of the negative electrode current collector.

[0053] In this regard, FIG. 1 shows a schematic diagram of a process for producing a negative electrode according to the present invention.

[0054] 1, a coating layer containing a lithium affinity material (LPM) is formed on a negative electrode current collector, and an ion transport layer containing amorphous carbon is formed on the coating layer. Then, a battery is manufactured by stacking the thus manufactured negative electrode with a solid electrolyte layer and a positive electrode, and when charging and discharging are performed, lithium ions that have passed through the ion transport layer and moved to the negative electrode are attached and plated on the lithium affinity material, but even if lithium grows, it is unable to penetrate the ion transport layer.

[0055] That is, when lithium plated on the coating layer grows, the growth is inhibited by the ion conduction layer, so that the problem of lithium dendrites, which are formed by growing lithium nuclei, extending toward the positive electrode and coming into contact with the positive electrode, can be prevented.

[0056] In the negative electrode for an all-solid-state battery according to the present invention, the ion transport layer may be made of carbon black such as acetylene black, ketjen black, channel black, polytetrafluoroethylene black, lamp black, or thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as carbon fluoride, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives. More specifically, the ion transport layer may contain amorphous carbon such as carbon black.

[0057] The amorphous carbon has a disordered structure in which the hexagonal net planes of carbon atoms are small and the stacking growth is not well developed, and each fine crystallite composed of the hexagonal net planes is entangled with each other or mixed with an amorphous phase. As a result, lithium ions can be inserted into each gap and tip side generated by defects and incomplete stacking structure of the carbon layer in addition to being inserted between the planes of the graphite layer.

[0058] The ion transport layer of the present invention includes amorphous carbon, which smoothly transports lithium ions to the negative electrode current collector. Lithium is electrodeposited on the outer surface of the ion transport layer facing the negative electrode current collector, but not on the outer surface of the ion transport layer facing the opposite direction. As a result, lithium dendrites are not generated on the outer surface of the ion transport layer facing the positive electrode, which can improve the life characteristics of the lithium secondary battery.

[0059] On the other hand, when the ion transport layer is formed of crystalline graphite such as natural graphite or artificial graphite, which is generally used as a negative electrode active material, lithium is inserted into the crystalline graphite and then electrodeposited on the outer surface of the ion transport layer facing the positive electrode. As the lithium is electrodeposited, it grows into lithium dendrites and passes through the solid electrolyte layer, causing a short circuit.

[0060] As a result, when an ion transport layer containing amorphous carbon is included as in the present invention, safety can be ensured compared to when crystalline graphite is used as the ion transport layer.

[0061] In one specific example, the ion transport layer may further include a binder to ensure binding strength between the carbon materials, which are the main components constituting the ion transport layer.

[0062] The ion transport layer may further include a binder for improving the binding strength of the ion transport layer to the coating layer and / or the negative electrode current collector.

[0063] That is, the binder may be used to ensure binding between the components of the ion transport layer, or may be used to ensure binding between the ion transport layer and a coating layer and / or a negative electrode current collector.

[0064] The binder may include, for example, one or more selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butylene rubber, fluororubber, and copolymers thereof.

[0065] The present invention also provides a method for manufacturing a negative electrode for an all-solid-state battery, which specifically includes the steps of: (a) preparing a negative electrode current collector; (b) forming a coating layer including a lithium affinity material on at least one outer surface of the negative electrode current collector; and (c) forming an ion transport layer on the coating layer, and each of the steps may be performed sequentially.

[0066] The lithium affinity material constituting the coating layer may be in the form of nanoparticles, and may be in the form of metal nanoparticles or metal oxide nanoparticles attached onto the negative electrode current collector.

[0067] The method of forming the coating layer on the negative electrode current collector and the method of forming the ion transport layer may be performed independently by any one or more of the following methods: immersion, spin coating, dip coating, spray coating, doctor blade, solution casting, drop coating, physical vapor deposition (PVD), and chemical vapor deposition (CVD).

[0068] The method of forming the coating layer and the method of forming the ion transport layer on the negative electrode current collector may be performed by a dry coating method.

[0069] The present invention provides a lithium secondary battery in which an electrode assembly including the anode for the all-solid-state battery, a solid electrolyte layer, and a cathode is housed in a battery case.

[0070] The positive electrode is prepared, for example, by applying a positive electrode mixture containing a positive electrode active material onto a positive electrode current collector and then drying the applied positive electrode mixture. If necessary, the positive electrode mixture may selectively further include a binder, a conductive material, a filler, and the like.

[0071] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, the positive electrode current collector may be made of stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may have fine irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0072] The positive electrode active material is a material capable of undergoing an electrochemical reaction and may include at least one of the positive electrode active materials represented by the following Chemical Formulas 1 to 3.

[0073] Li a Co 1-x M x O2(1) Li a Mn 2-y M y O4(2) Li a Fe 1-z M z PO4(3) In the above formula, 0.8≦a≦1.2; 0≦x≦0.8; 0≦y≦0.6, 0≦z≦0.5, M is one or more elements selected from the group consisting of Ti, Cd, Cu, Cr, Mo, Mg, Al, Ni, Nb, V and Zr.

[0074] That is, the positive electrode active material may include one or more materials selected from the group consisting of a lithium metal oxide having a layered structure represented by Chemical Formula 1, a lithium manganese-based oxide having a spinel structure represented by Chemical Formula 2, and a lithium-containing phosphate having an olivine structure represented by Chemical Formula 3.

[0075] The layered lithium metal oxide may be, but is not limited to, one or more selected from the group consisting of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium cobalt-nickel oxide, lithium cobalt-manganese oxide, lithium manganese-nickel oxide, lithium nickel-manganese-cobalt oxide, and materials substituted or doped with other elements.

[0076] The lithium nickel-manganese-cobalt oxide is Li 1+z Ni b Mn c Co 1-(b+c+d) M d O (2-e) A e (wherein, −0.5≦z≦0.5, 0.1≦b≦0.8, 0.1≦c≦0.8, 0≦d≦0.2, 0≦e≦0.2, and b+c+d<1. M=Al, Mg, Cr, Ti, Si, or Y, and A=F, P, or Cl.)

[0077] The lithium manganese-based oxide having a spinel structure is not limited in type, and may be, for example, one or more selected from the group consisting of lithium manganese oxide, lithium nickel manganese oxide, and materials substituted or doped with other elements.

[0078] The lithium-containing phosphate having an olivine structure is not limited in type, but may be, for example, lithium iron phosphate and those substituted or doped with other elements.

[0079] The other elements may be one or more elements selected from the group consisting of Al, Mg, Mn, Ni, Co, Cr, V, Fe and doped materials.

[0080] The binder is a component that promotes binding between the active material and the conductive material and between the active material and the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the mixture including the positive electrode active material. Examples of such binders include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), styrene-butylene rubber, fluororubber, and copolymers thereof.

[0081] The conductive material is usually added in an amount of 1 wt % to 30 wt % based on the total weight of the mixture including the positive electrode active material. The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as ethylene black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, graphene, and carbon nanotubes.

[0082] The filler is selectively used as a component that suppresses the expansion of the electrode, does not induce chemical changes in the battery, and is not particularly limited as long as it is a fibrous material. For example, the filler may be a polyolefin-based polymerizing agent such as polyethylene or polypropylene; or a fibrous material such as glass fiber or carbon fiber.

[0083] The solid electrolyte may be a sulfide-based solid electrolyte, an oxide-based solid electrolyte, or a polymer-based solid electrolyte.

[0084] The sulfide-based solid electrolyte contains sulfur atoms (S), has ion conductivity of a metal belonging to Group 1 or 2 of the periodic table, and can have electronic insulation. The sulfide-based solid electrolyte preferably contains at least Li, S, and P as elements and has lithium ion conductivity, but can contain elements other than Li, S, and P depending on the purpose or case.

[0085] Specific sulfide-based inorganic solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, L i2S-LiBr-P2S5, Li2SLi2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2 S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS 2, Li2S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, and Li 10 GeP2S 12 etc. may be used.

[0086] As a method for synthesizing the sulfide-based inorganic solid electrolyte material, an amorphization method can be used. Examples of the amorphization method include a mechanical milling method, a solution method, and a melt quenching method. This is because it allows processing at room temperature (25°C) and simplifies the manufacturing process.

[0087] The oxide-based solid electrolyte is preferably a compound that contains an oxygen atom (O), has the ionic conductivity of a metal belonging to Group 1 or 2 of the periodic table, and has electronic insulation properties.

[0088] As the oxide-based solid electrolyte, for example, Li xa La ya TiO3 [xa=0.3~0.7, ya=0.3~0.7] (LLT), Li xb La yb Zr zb M bb mb O nb (M bb is at least one element selected from Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn, xb satisfies 5≦xb≦10, yb satisfies 1≦yb≦4, zb satisfies 1≦zb≦4, mb satisfies 0≦mb≦2, and nb satisfies 5≦nb≦20.), Li xc B yc M cc zc O nc (M cc is at least one element selected from the group consisting of C, S, Al, Si, Ga, Ge, In, and Sn, xc satisfies 0≦xc≦5, yc satisfies 0≦yc≦1, zc satisfies 0≦zc≦1, and nc satisfies 0≦nc≦6.), Li xd (Al,Ga) yd (Ti,Ge) zd S ad P md O nd (where 1≦xd≦3, 0≦yd≦1, 0≦zd≦2, 0≦ad≦1, 1≦md≦7, 3≦nd≦13), Li (3-2xe) M ee xe D ee O(xe is a number between 0 and 0.1, and M ee represents a divalent metal atom. ee represents a halogen atom or a combination of two or more halogen atoms. xf S yf O zf (1≦xf≦5, 0 <yf≦3、1≦zf≦10)、Li xgS yg O zg (1≦xg≦3, 0 <yg≦2、1≦zg≦10)、Li3BO3-Li2SO4、Li2O-B2O3-P2O5、Li2O-SiO2、Li6BaLa2Ta2O 12 , LiPO (4-3 / 2w) N w (w is w<1), Li with LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zinc 0.25 GeO4, La with perovskite crystal structure 0.55 Li 0.35 TiO3, LiTi2P3O with NASICON (sodium super ionic conductor) type crystal structure 12 , Li 1+xh+yh (Al,Ga) xh (Ti,Ge) 2-xh S yh P 3-yh O 12 (where 0≦xh≦1, 0≦yh≦1), Li7La3Zr2O with a garnet-type crystal structure 12 Alternatively, a phosphorus compound containing Li, P and O can be used as the oxide-based solid electrolyte, such as lithium phosphate (Li3PO4), LiPON in which part of the oxygen in lithium phosphate is replaced with nitrogen, LiPOD, etc. 1 (D 1 The oxide-based solid electrolyte may be at least one selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, and Au. Alternatively, the oxide-based solid electrolyte may be LiA 1 ON(A 1 At least one selected from the group consisting of Si, B, Ge, Al, C, and Ga) can also be used.

[0089] The polymer-based solid electrolyte may be a solid polymer electrolyte formed by adding a polymer resin to a lithium salt that is independently solvated, or a polymer gel electrolyte formed by impregnating an organic electrolyte solution containing an organic solvent and a lithium salt in a polymer resin.

[0090] For example, the solid polymer electrolyte is not particularly limited as long as it is an ion-conductive material and is a polymer material generally used as a solid electrolyte material for all-solid-state batteries. The solid polymer electrolyte may include, for example, a polyether-based polymer, a polycarbonate-based polymer, an acrylate-based polymer, a polysiloxane-based polymer, a phosphazene-based polymer, polyethylene oxide, a polyethylene derivative, an alkylene oxide derivative, a phosphate ester polymer, polyethene lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, or a polymer containing an ionic dissociation group. Alternatively, the solid polymer electrolyte may be a polymer resin, and may include a branched copolymer in which an amorphous polymer such as polymethyl methacrylate (PMMA), polycarbonate, polysiloxane, and / or phosphazene is copolymerized with a comonomer on a PEO (polyethylene oxide) main chain, a comb-like polymer resin, and a crosslinked polymer resin.

[0091] The polymer gel electrolyte includes an organic electrolyte solution containing a lithium salt and a polymer resin, and the organic electrolyte solution is included in an amount of 60 to 400 parts by weight based on the weight of the polymer resin. The polymer applied to the gel electrolyte is not limited to a specific component, and may include, for example, polyvinylchloride (PVC), poly(methyl methacrylate) (PMMA), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), etc.

[0092] In the negative electrode for the all-solid-state battery, lithium plating occurs on the lithium affinity material dispersed in the coating layer, and the ion transport layer can block the passage of lithium aggregated by the lithium plating, so that the growth of plated lithium can occur only between the ion transport layer and the coating layer.

[0093] In one specific example, the electrode assembly may be a mono-cell including one positive electrode and one negative electrode. In consideration of the purpose of preventing lithium dendrites from growing toward the positive electrode, the negative electrode for the all-solid-state battery may have a coating layer and an ion transport layer formed only on a first surface of a first surface and a second surface that are rectangular outer surfaces of a negative electrode current collector, and a positive electrode may be disposed on the first surface.

[0094] The negative electrode having a coating layer and an ion transport layer formed only on the first surface of the negative electrode as described above can also be applied to a C-type bi-cell in which a negative electrode is disposed on each side of a positive electrode, and the first surface of the negative electrode can be disposed so as to face the positive electrode.

[0095] In another specific example, the electrode assembly may be an A-type bicell in which a positive electrode is disposed on each of both sides of a negative electrode. In consideration of the purpose of preventing lithium dendrites from growing toward the positive electrode, the negative electrode for an all-solid-state battery may have a coating layer and an ion transport layer formed on each of first and second surfaces, which are rectangular outer surfaces of a negative electrode current collector, and a first positive electrode and a second positive electrode disposed on each of the first and second surfaces. EXAMPLES

[0096] Hereinafter, the present invention will be described with reference to examples, which are for easier understanding of the present invention and are not intended to limit the scope of the present invention.

[0097] <Example 1> To manufacture the positive electrode for the all-solid-state battery, LiNi was used as the positive electrode active material. 0.8 Co 0.1 Mn 0.1 O2, argyrodite (Li6PS5Cl) as a solid electrolyte, furnace black as a conductive material, and polytetrafluoroethylene as a binder were prepared in a weight ratio of 77.5:19.5:1.5:1.5, and dispersed and stirred in anisole to prepare a positive electrode slurry. The positive electrode slurry was applied to an aluminum current collector with a thickness of 14 μm using a doctor blade, and then vacuum dried at 100° C. for 12 hours to prepare a positive electrode.

[0098] To manufacture the solid electrolyte layer, argyrodite (Li6PS5Cl) as a solid electrolyte and polytetrafluoroethylene as a binder were dispersed in anisole at a weight ratio of 95:5 and stirred to prepare a solid electrolyte layer slurry. This was coated onto a polyethylene terephthalate release film and then vacuum dried at 100°C for 12 hours to prepare a solid electrolyte layer.

[0099] To manufacture an anode for an all-solid-state battery including a coating layer and an ion transport layer, Ag was sputtered to a size of 30 nm on a nickel current collector having a thickness of 10 μm to form a coating layer made of an Ag layer. Then, a slurry in which acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 97:3 was coated on the Ag layer to form an ion transport layer, which was then dried to manufacture an anode having a multi-layer structure.

[0100] The positive electrode, the solid electrolyte layer, and the negative electrode were sequentially stacked to prepare a lithium secondary battery.

[0101] <Example 2> A lithium secondary battery was manufactured in the same manner as in Example 1, except that furnace black was used instead of acetylene black to manufacture the ion transport layer.

[0102] <Comparative Example 1> A lithium secondary battery was manufactured in the same manner as in Example 1, except that the negative electrode did not include a coating layer or an ion transfer layer, and a nickel current collector was used alone.

[0103] <Comparative Example 2> A lithium secondary battery was manufactured in the same manner as in Example 1, except that only a coating layer of Ag was formed by sputtering on a nickel current collector to a size of 30 nm as the negative electrode.

[0104] <Comparative Example 3> A lithium secondary battery was manufactured in the same manner as in Example 1, except that a slurry in which furnace black and polyvinylidene fluoride were mixed in a weight ratio of 97:3 was coated on a nickel current collector as a negative electrode to form only an ion conduction layer.

[0105] <Comparative Example 4> A lithium secondary battery was manufactured in the same manner as in Example 1, except that a slurry in which artificial graphite and polyvinylidene fluoride were mixed in a weight ratio of 97:3 was coated on a nickel current collector as a negative electrode to form only an ion conduction layer.

[0106] <Comparative Example 5> A lithium secondary battery was manufactured in the same manner as in Example 1, except that natural graphite was used to manufacture the ion transport layer.

[0107] <Comparative Example 6> A lithium secondary battery was manufactured in the same manner as in Example 1, except that artificial graphite was used to manufacture the ion transport layer.

[0108] <Comparative Example 7> A battery was manufactured in the same manner as in Example 1, except that a mixture of furnace black and Ag in a weight ratio of 3:1 was prepared as a negative electrode, and a mixed layer composed of the mixture and polyvinylidene fluoride in a weight ratio of 97:3 was formed on a nickel current collector.

[0109] <Comparative Example 8> A battery was manufactured in the same manner as in Example 2, except that the ion transport layer prepared in Example 2 was formed on a nickel current collector as a negative electrode, and a coating layer was formed on the ion transport layer.

[0110] <Experimental Example 1> The batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 8 were charged at 0.05 C in a constant current-constant voltage mode up to 4.25 V at 60° C., and discharged at 0.05 C to 3.0 V to measure the initial charge-discharge capacity and efficiency. The thus measured charge capacity, discharge capacity, charge-discharge efficiency, and short occurrence rate are shown in Table 1 below.

[0111] [Table 1]

[0112] Referring to Table 1, all the lithium secondary batteries prepared in the examples and comparative examples, except for Comparative Example 1, were measured to have similar charge / discharge efficiencies.

[0113] In the case of Comparative Example 1, in which only the negative electrode current collector was used as the negative electrode, the nucleation potential was high and it was difficult to suppress the growth of lithium dendrites, resulting in low charge / discharge efficiency and the highest rate of short circuit occurrence.

[0114] In Comparative Example 2, in which only a coating layer was formed on the negative electrode current collector, and Comparative Example 3, in which only an ion conduction layer was formed on the negative electrode current collector, it was confirmed that the short circuit occurrence rate was significantly reduced compared to Comparative Example 1.

[0115] Comparative Examples 4, 5, and 6, in which crystalline carbon was used, showed a very high incidence of short circuits.

[0116] When a coating layer and an ion transport layer are sequentially formed on a current collector as in Examples 1 and 2, the nucleation potential can be lowered and lithium dendrites cannot grow through the ion transport layer, so that no short circuit occurs.

[0117] In the case of Comparative Example 7 in which the ion conduction layer and the coating layer were mixed, the short circuit occurrence rate was low, but referring to the following Experimental Example 2, it is confirmed that there is a problem in the number of charge / discharge cycles.

[0118] In the case of Comparative Example 8, in which an ion transport layer was formed on a current collector and a coating layer was formed on the ion transport layer, the short circuit occurrence rate was still measured to be high. This is believed to be due to the deposition of lithium on the surface of the ion transport layer and / or the coating layer.

[0119] In this way, when the negative electrode includes an ion transport layer using amorphous carbon, a lithium secondary battery with improved safety can be manufactured.

[0120] <Experimental Example 2> In order to evaluate the life characteristics of each of the batteries prepared in Examples 1 and 2 and Comparative Examples 1 to 8, charging and discharging were performed in a voltage range of 4.2V to 3.7V under the condition of 0.1C charge / 0.1C discharge.

[0121] The charging and discharging was continued until a short circuit occurred, and the number of cycles and the capacity retention rate immediately before the short circuit occurred are shown in Table 2 below.

[0122] [Table 2]

[0123] Referring to Table 2, in the case of Example 1 and Example 2, no short circuit occurred until the batteries were charged and discharged 400 times.

[0124] In comparison with Comparative Example 1, Comparative Example 2 in which a coating layer is formed and Comparative Example 3 in which an ion conduction layer is formed show the effect of increasing the number of charge / discharge cycles and improving the life characteristics, but still shows a low capacity retention rate compared with Examples 1 and 2.

[0125] Comparative Examples 4, 5, and 6, which used crystalline carbon, exhibited very low charge / discharge cycles.

[0126] In the case of Comparative Example 7, in which a mixed layer in which an ion conduction layer and a coating layer were mixed was applied, the capacity retention rate was improved compared to Comparative Examples 2 and 3, and in the case of Comparative Example 8, in which a current collector, an ion conduction layer, and a coating layer were formed in that order, the time when a short circuit occurred was delayed compared to Comparative Example 3. However, it can be seen that the life characteristics of the batteries of Examples 1 and 2 are improved by more than twice as much as the battery of Comparative Example 7 and by about eight times as much as the battery of Comparative Example 8.

[0127] Comparative Examples 5 and 6, which differ only in that crystalline graphite is used in the ion transport layer, not only show a significantly low number of charge / discharge cycles, but also have a capacity retention rate of 70% to 80%, while Examples 1 and 2, which use amorphous carbon in the ion transport layer, show a capacity retention rate of 80% or more even after 400 charge / discharge cycles.

[0128] Therefore, it can be confirmed that the cycle characteristics are improved when the ion transport layer contains amorphous carbon.

[0129] SEM photographs of the negative electrodes prepared in Example 2, Comparative Examples 1 to 3, and Comparative Examples 6 to 8 are shown in Figures 2 to 9. Figure 2 is an SEM photograph of the negative electrode prepared in Example 2, and Figure 3 is an SEM photograph of a cross section of the negative electrode prepared in Example 2. Figures 4, 5, and 6 are SEM photographs of the negative electrodes prepared in Comparative Examples 1, 2, and 3, respectively, and Figure 7 is an SEM photograph of a cross section of the negative electrode prepared in Comparative Example 6. Figures 8 and 9 are SEM photographs of the negative electrodes prepared in Comparative Examples 7 and 8, respectively.

[0130] 2 to 9, the negative electrodes of FIG. 2 (Example 2) and FIG. 6 (Comparative Example 3) have an ion transport layer formed on the surface. It can be seen that many pores are formed inside the ion transport layer, allowing lithium ions to move toward the negative electrode. In the case of Example 2, the distribution range of lithium ions in the coating layer is wide, which reduces the nucleation potential, making it difficult for lithium nuclei to be formed by lithium ions that have passed through the ion transport layer, and even if lithium nuclei are formed, they cannot grow to the extent that they penetrate the ion transport layer. This can be interpreted as indicating that the short circuit occurrence rate was 0%.

[0131] However, in the case of Comparative Example 3 (FIG. 6) which does not include a coating layer, the nucleation potential is high and localized growth of lithium nuclei occurs, resulting in lower life characteristics than Comparative Example 2 (FIG. 5).

[0132] The negative electrode in Fig. 4 (Comparative Example 1) is the surface of a nickel current collector, while Fig. 5 (Comparative Example 2) and Fig. 9 (Comparative Example 8) are in a state where a coating layer is formed on the surface of the negative electrode. As can be seen from the experimental results, the case of Comparative Example 8 shows a higher short circuit occurrence rate and poorer life characteristics than Comparative Example 2.

[0133] The negative electrode in Fig. 8 (Comparative Example 7) had a mixed layer formed on the surface, and therefore the short circuit occurrence rate was 0%. However, the negative electrode in Fig. 8 (Comparative Example 7) showed poor life characteristics compared to Examples 1 and 2 in which an ion conduction layer was formed on the coating layer.

[0134] FIG. 3 is a SEM photograph of a cross section of the negative electrode prepared in Example 2, and FIG. 7 is a SEM photograph of a cross section of the negative electrode prepared in Comparative Example 6.

[0135] Referring to FIG. 3, it can be seen that in the negative electrode of Example 2, lithium was electrodeposited on one side of the ion transport layer containing furnace black facing the negative electrode current collector (Ni foil).

[0136] Referring to FIG. 7, it can be seen that in the negative electrode of Comparative Example 6, lithium was electrodeposited on one side of the ion conduction layer containing artificial graphite opposite to the side facing the negative electrode current collector (Ni foil).

[0137] That is, when the ion transfer layer contains crystalline graphite such as artificial graphite, lithium electrodeposition occurs on the outer surface of the ion transfer layer facing the positive electrode, and lithium dendrites grow and penetrate the solid electrolyte layer to come into contact with the positive electrode, resulting in a short circuit after a short number of charge / discharge cycles.

[0138] On the other hand, when the battery includes an ion transport layer containing amorphous carbon such as furnace black, lithium electrodeposition is performed only on the outer surface of the ion transport layer toward the negative electrode current collector, so that high cycle characteristics and capacity retention rate can be ensured, and as a result, a lithium secondary battery with improved performance can be provided.

[0139] Those skilled in the art will appreciate that various applications and modifications within the scope of the present invention are possible based on the above content. [Industrial Applicability]

[0140] The present invention relates to a negative electrode for an all-solid-state battery including a coating layer and an ion transport layer, and a lithium secondary battery including the same. Specifically, the present invention relates to a technology that can prevent localized lithium plating in the negative electrode and identify the position of lithium electrodeposition to prevent a short circuit from occurring between a positive electrode and a negative electrode, and thus can be used industrially.

Claims

1. A negative electrode for an all-solid-state battery, A negative electrode current collector made of an electrically conductive metal material; a coating layer that is applied to one or both sides of the negative electrode current collector and that contains a lithium affinity material; an ion transport layer located on the coating layer and including amorphous carbon through which lithium ions can travel; Including, The lithium affinity material is at least one of metals including Au, Ag, Pt, Zn, Si, and Mg, and metal oxides including CuO, ZnO, CoO, and MnO; The coating layer containing the lithium affinity material is an island-shaped coating layer that partially exposes the negative electrode current collector.

2. The negative electrode for an all-solid-state battery according to claim 1 , wherein the ion transport layer further comprises a binder.

3. The negative electrode for an all-solid-state battery according to claim 1 , wherein a negative electrode mixture layer is not formed on the negative electrode current collector.

4. The negative electrode for an all-solid-state battery according to claim 1 , wherein the lithium affinity material is Ag.

5. The negative electrode for an all-solid-state battery described in any one of claims 1 to 4, wherein the coating layer is distributed in a range of 30% or more and 80% or less based on the total area of ​​the negative electrode current collector.

6. A lithium secondary battery comprising the negative electrode for an all-solid-state battery according to any one of claims 1 to 5, a solid electrolyte layer, and a positive electrode.

7. The negative electrode for the all-solid-state battery includes the lithium affinity material dispersed in the coating layer, 7. The lithium secondary battery according to claim 6, wherein lithium plating occurs on the lithium affinity material.

8. 8. The lithium secondary battery according to claim 6, wherein the negative electrode for the all-solid-state battery is subjected to lithium electrodeposition on one surface of the ion conduction layer facing the negative electrode current collector.

9. The negative electrode for an all-solid-state battery has a first surface and a second surface of the negative electrode current collector, and the coating layer and the ion conduction layer are formed only on the first surface of the negative electrode current collector, The lithium secondary battery according to claim 6 , comprising a monocell having a positive electrode disposed on the first surface.

10. The lithium secondary battery according to claim 9 , wherein the coating layer is formed on the negative electrode current collector, and the ion transfer layer is formed on the coating layer.

11. The negative electrode for an all-solid-state battery includes a first surface and a second surface of the negative electrode current collector, the coating layer and the ion conduction layer being formed on the first surface and the second surface of the negative electrode current collector, respectively; The lithium secondary battery according to claim 6 , comprising a bicell in which a first positive electrode and a second positive electrode are disposed on the first surface and the second surface, respectively.

12. The lithium secondary battery according to claim 11 , wherein the coating layer is formed on the negative electrode current collector, and the ion transfer layer is formed on the coating layer.

Citation Information

Patent Citations

  • Electrode with composite layer structure and lithium battery

    CN110571413A

  • Battery system and vehicle on which battery system is mounted

    JP2019021515A

  • All-solid type secondary battery and charging method thereof

    JP2019096610A