Block polymers and lithiation, their manufacturing methods and applications

The development of block polymers with specific molecular structures addresses the limitations of traditional lithium-ion battery binders by enhancing conductivity and compatibility, resulting in improved rapid charging and discharge performance with reduced impedance and gas generation.

JP7578836B2Active Publication Date: 2024-11-06AESC JAPAN LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023543272
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-28
Filing Date
2021-02-08
Publication Date
2024-11-06
Estimated Expiration
2041-02-08

AI Technical Summary

Technical Problem

Traditional lithium-ion battery binders, such as styrene-butadiene rubber and acrylic polymers, increase internal impedance, leading to poor rapid charging performance, and alternative conductive binders are complex and costly, with compatibility issues for silicon-based electrodes.

Method used

Development of block polymers with a structure represented by B-C-B-A, where A is polymerized from alkenylformic acid monomers, B from aromatic vinyl monomers, and C from acrylate monomers, specifically lithiated block polymers produced through a stepwise polymerization process using RAFT reagents and initiators.

Benefits of technology

The lithiated block polymers enhance ionic conductivity, reduce internal impedance, are cost-effective, compatible with various negative electrode systems, and improve rapid charging and low temperature discharge performance while minimizing gas generation at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578836000001
    Figure 0007578836000001
  • Figure 0007578836000002
    Figure 0007578836000002
  • Figure 0007578836000003
    Figure 0007578836000003
Patent Text Reader

Abstract

The present invention provides a block polymer and a lithiated block polymer, as well as a manufacturing method and application thereof. In the present invention, the block polymer has a structure represented by BCBA. Here, A represents polymer block A, B represents polymer block B, and C represents polymer block C. The polymer block A is polymerized from an alkenyl formate monomer. The polymer block B is polymerized from an aromatic vinyl monomer. The polymer block C is polymerized from an acrylate monomer. The block polymer described in the present application can be used as a lithium ion battery binder.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-references to related applications

[0002] This application claims priority to a Chinese application filed on January 28, 2021, bearing application number 2021101176824 and entitled "Block polymer and lithiation, its preparation method and application," which is incorporated herein by citation in its entirety.

[0003] FIELD OF THE DISCLOSURE

[0002] Embodiments of the present invention relate to the field of lithium ion batteries, and in particular to block polymers and lithiated block polymers, as well as methods of manufacture and applications thereof. [Background technology]

[0004] The negative electrode binder is one of the important auxiliary functional materials of lithium-ion batteries, and is the main source of the internal mechanical performance of the electrode, and its main function is to bind active materials with each other and with the current collector. Conventional binders are mainly styrene-butadiene rubber, acrylic polymer, acrylate, etc., and although these materials have relatively strong adhesive properties and relatively favorable electrochemical stability, they are non-conductive, which makes it easy for the internal impedance of the negative electrode to increase, resulting in poor fast charging performance of lithium-ion batteries.

[0005] In order to solve the above problems, the following two methods are mainly used in the prior art. First, the affinity between the active material and the binder is improved. For example, the patent document with registration number JP5373388B2 describes a mechanochemical treatment method for graphite particles, which makes the surface of graphite particles hydrophilic, uniforms the particle size, reduces the average particle size, improves the performance of improving the wettability of the surface, and improves the affinity with the water-based binder, thereby contributing to improving the charging efficiency of lithium-ion batteries. However, this method requires a special graphite particle treatment device, which is expensive, and the same effect cannot be achieved in a battery system using a negative electrode active material other than graphite (such as silicon).

[0006] Second, the conventional binder is replaced with a binder with better ion conductivity. For example, the patent document with registration number CN105489898B describes a conductive aqueous binder that can improve the conductivity of the entire battery, including graphene, carbon nanotubes, cross-linked polymers, and polyvalent metal ion water-soluble salt solutions, in which the graphene and carbon nanotubes are chemically bonded with cross-linked polymers to form a three-dimensional conductive network structure, and the cross-linked polymer is cross-linked with a polyvalent metal ion water-soluble salt solution to form a three-dimensional bonded network structure. However, the conductive aqueous binder is mainly a combination of various existing materials, so its composition is complicated, and the raw material cost for producing the conductive aqueous binder is relatively high, making it difficult to be widely used on a large scale, and there is also a compatibility problem when the conductive aqueous binder is used in a silicon-based negative electrode.

[0007] Furthermore, as a result of research, the present inventors have found that there are few descriptions in the prior art of improving the rapid charging performance of lithium ion batteries by improving the negative electrode binder from the viewpoint of molecular structure design. Summary of the Invention

[0008] An object of embodiments of the present invention is to provide block polymers and lithiated block polymers, as well as methods for preparing and applications thereof.

[0009] In order to solve the above technical problem, a first aspect of the present invention provides a block polymer having a structure represented by BCBA, where A represents polymer block A, B represents polymer block B, and C represents polymer block C.

[0010] The polymer block A is formed by polymerizing an alkenyl formic acid monomer.

[0011] The polymer block B is formed by polymerization of an aromatic vinyl monomer.

[0012] The polymer block C is formed by polymerization of an acrylate monomer.

[0013] In some preferred technical proposals, the polymerization degree of the polymer block A is 10-50, the polymerization degree of the polymer block B is 200-500, and the polymerization degree of the polymer block C is 400-1000.

[0014] In some preferred technical proposals, the structure of the alkenyl formate monomer is as follows: [ka] In the formula, R11 and R12 are independently hydrogen or C 1~4 is an alkyl group, 1~4 The alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl. Preferably, the alkenyl formate is acrylic acid.

[0015] In some preferred technical proposals, the structure of the aromatic vinyl monomer is as follows: [ka] In the formula, R21, R22, R23, R24, R25, and R26 are independently hydrogen or C 1~4 is an alkyl group, 1~4 The alkyl group is selected from a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, or a tert-butyl group. Preferably, R21, R22, R23, R24, R25, and R26 are hydrogen or a methyl group, and more preferably, the aromatic vinyl monomer is styrene.

[0016] In some preferred technical proposals, the structure of the acrylate monomer is as follows: [ka] In the formula, R31 is a straight or branched chain C 1~10 More preferably, R31 is a straight or branched C 4~8 More preferably, R31 is an alkyl group. [ka]

[0017] The block polymer of the present invention can be prepared by a conventional stepwise polymerization method in the art, which adds each polymer block A, polymer block B or polymer block C stepwise according to the specific block structure of the block polymer, thereby achieving stepwise polymerization of each polymer block.

[0018] A second aspect of the present invention is a method for producing the block polymer, comprising the steps of: Monomers that make up is subjected to a polymerization reaction to obtain the block polymer, where A represents polymer block A, B represents polymer block B, and C represents polymer block C.

[0019] In some preferred technical proposals, the polymer block CBA is prepared by the following method, which comprises the steps of: Monomers that make up In the polymer block CBA, A represents the polymer block A, B represents the polymer block B, and C represents the polymer block C.

[0020] In some preferred technical proposals, the polymer block BA is prepared by the following method, which comprises the steps of: Monomers that make upand the polymer block A are polymerized to obtain a block polymer BA. In the polymer block BA, A represents the polymer block A, and B represents the polymer block B.

[0021] In some preferred technical approaches, the polymerization reaction is carried out in the presence of a RAFT agent and an initiator.

[0022] Specifically, the method for producing the block polymer includes the steps of: (1) reacting the polymer block A and the polymer block B in the presence of a RAFT reagent and an initiator; Monomers that make up (2) In the presence of a RAFT reagent and an initiator, the polymer block C is polymerized to obtain a polymer block BA. Monomers that make up (3) In the presence of a RAFT reagent and an initiator, the polymer block B is polymerized to obtain a polymer block CBA. Monomers that make up and reacting said polymer block CBA with said block polymer.

[0023] A third aspect of the present invention provides a lithiated block polymer which is a lithiated product of the above block polymer.

[0024] In some preferred technical proposals, the lithiated block polymer has a structure represented by general formula (I): [ka] In the formula, n is 10 to 50, x is 200 to 500, and y is 400 to 1000. z is 200 to 500. R41 is C 4~8 Preferably, R41 is: [ka] R42 and R43 are phenyl groups or C 1~4 A phenyl group substituted with an alkyl group, 1~4The phenyl group of the alkyl group is selected from phenyl groups substituted with methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl groups. Preferably, R42 and R43 are phenyl groups.

[0025] In some preferred technical proposals, the lithiated block polymer is as follows: [ka] In the formula, n is 10 to 50, x is 200 to 500, and y is 400 to 1000. z is 200 to 500.

[0026] A fourth aspect of the present invention provides a method for preparing a lithiated block polymer, the method comprising the steps of:

[0027] (1) Polyacrylic acid-styrene 2-Ethylhexyl acrylate (PAA-PSt-PEHA) is polymerized with styrene monomer to form polyacrylic acid-styrene- 2-Ethylhexyl acrylate -styrene (PAA-PSt-PEHA-PSt) is obtained.

[0028] (2) Polyacrylic acid-styrene- 2-Ethylhexyl acrylate -styrene (PAA-PSt-PEHA-PSt) to obtain the lithiated block polymer. [ka]

[0029] Here, in steps (1) and (2), n is 10-50, x is 200-500, y is 400-1000, and in step (2), z is 200-500.

[0030] In step (1), the polyacrylic acid-styrene- 2-Ethylhexyl acrylateThe mass ratio of the polystyrene (PAA-PSt-PEHA-PSt) to the styrene monomer is preferably (0.01 to 0.3):1, and more preferably (0.02 to 0.27):1.

[0031] In step (1), the polymerization reaction is preferably carried out in the presence of an initiator, and the initiator is preferably potassium persulfate, sodium persulfate or ammonium persulfate.

[0032] In the step (1), the temperature of the polymerization reaction is preferably 50 to 90°C, and more preferably 60 to 80°C.

[0033] In the step (1), the polymerization reaction time is preferably 2 to 8 hours.

[0034] In step (1), after the polymerization reaction, the product of the polymerization reaction, polyacrylic acid-styrene- 2-Ethylhexyl acrylate -styrene (PAA-PSt-PEHA-PSt) to a pH of 3–6.

[0035] In step (2), the lithium hydroxide is preferably an aqueous solution of lithium hydroxide, and the mass fraction of lithium hydroxide in the aqueous solution of lithium hydroxide is preferably 5% to 15%.

[0036] In step (1), the polyacrylic acid-styrene- 2-Ethylhexyl acrylate The preparation of (PAA-PSt-PEHA) includes the following steps: (A) Polyacrylic acid-styrene (PAA-PSt) and 2-Ethylhexyl acrylate The monomer is polymerized to form polyacrylic acid-styrene- 2-Ethylhexyl acrylate (PAA-PSt-PEHA) is obtained.

[0037] In the step (A), the mass ratio of the polyacrylic acid-styrene (PAA-PSt) to the 2-ethylhexyl acrylate is preferably (0.6-0.9):1, and more preferably (0.6-0.7):1.

[0038] In step (A), the polymerization reaction is preferably carried out in the presence of an initiator, and the initiator is preferably potassium persulfate, sodium persulfate or ammonium persulfate, for example potassium persulfate.

[0039] In the step (A), the temperature of the polymerization reaction is preferably 50 to 90°C, and more preferably 60 to 80°C.

[0040] In the step (A), the time for the polymerization reaction is preferably 2 to 8 hours, and more preferably 2 to 6 hours.

[0041] In step (A), the preparation of the polyacrylic acid-styrene (PAA-PSt) comprises the following steps:

[0042] (I) Polyacrylic acid and styrene monomer are polymerized to obtain polyacrylic acid-styrene (PAA-PSt). [ka] In the formula, n is 10 to 50, and x is 200 to 500.

[0043] In the step (I), the mass ratio of the polyacrylic acid to the styrene monomer is preferably 1:(3 to 90), and more preferably 1:(5 to 75).

[0044] In step (I), the polymerization reaction is preferably carried out in the presence of an initiator, and the initiator is preferably potassium persulfate, sodium persulfate or ammonium persulfate.

[0045] In the step (I), the temperature of the polymerization reaction is preferably 50 to 90°C, and more preferably 60 to 80°C.

[0046] In the step (I), the time for the polymerization reaction is preferably 2 to 10 hours, and more preferably 2 to 8 hours.

[0047] In step (I), the method for producing the polyacrylic acid is not limited, but preferably, the method for producing the polyacrylic acid is a method for producing the polyacrylic acid by polymerizing an acrylic acid monomer in the presence of a RAFT reagent and an initiator. In the polymerization reaction, the mass ratio of the RAFT reagent, the initiator, and the acrylic acid monomer is preferably (0.5-1.0):(0.2-0.5):(10-20). The temperature of the polymerization reaction is preferably 50-90°C, more preferably 60-80°C. The time of the polymerization reaction is preferably 10-22 hours, more preferably 12-20 hours. The initiator is preferably potassium persulfate, sodium persulfate, or ammonium persulfate. The RAFT reagent is preferably as follows: [ka] In the formula, R is an isopropionic acid group, an acetate group, a 2-cyanoacetate group, or a 2-aminoacetate group. Z is C 4~12 Alkyl group, C 4~12 It is an alkylthio group, a phenyl group or a benzyl group, for example, 2-mercapto-S-thiobenzoylacetic acid.

[0048] A fourth aspect of the present invention provides the use of the above lithiated block polymer as a lithium ion battery binder.

[0049] Based on the general knowledge in the art, each of the above preferred conditions can be arbitrarily combined to obtain a preferred embodiment of the present invention.

[0050] All of the reagents and raw materials used in the present invention are commercially available.

[0051] The lithiated block polymers provided by the present invention have at least the following advantages over the prior art:

[0052] (1) From the viewpoint of molecular structure design, the present invention provides a lithiated block polymer that has superior ion conductivity and contributes to reducing the internal impedance of an electrode.

[0053] (2) The cost of the lithiated block polymer of the present invention is low, and at the same time, it is compatible with various negative electrode systems and can be easily spread.

[0054] (3) When the lithiated block polymer of the present invention is used as a binder, its adhesion is more favorable, and the negative electrode peel strength of the produced lithium ion battery is higher.

[0055] (4) When the lithiated block polymers of the present invention are used as binders, the lithium ion batteries produced have better fast charge capability, better low temperature discharge capability, and less gassing at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0056] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention clearer, various embodiments of the present invention will be described in detail below in conjunction with specific embodiments. However, it should be understood that those skilled in the art can understand that in various embodiments of the present invention, many technical details are provided to allow third parties to better understand the present application. However, the technical solutions claimed in this application can be realized without these technical details and various changes and modifications based on the following embodiments. For experimental methods without specific conditions in the following examples, generally follow conventional conditions or conditions recommended by manufacturers. Percentages and parts are by weight unless otherwise indicated.

[0057] Example 1 Lithiated polyacrylic acid-styrene- 2-Ethylhexyl acrylate - Preparation of styrene (PAA-PSt-PEHA-PSt)

[0058] Step 1: Preparation of polyacrylic acid (PAA) [ka]

[0059] 1.0 g of 2-mercapto-S-thiobenzoylacetic acid (molecular weight: 212.3 g / mol) and 3.0 to 17.0 g of purified acrylic acid monomer are weighed out, mixed, and poured into a 500 mL three-neck flask. Furthermore, 0.2 to 0.5 g of potassium persulfate is weighed out and dissolved in 5 to 10 g of deionized water, stored at a low temperature, placed in a hot water bath, a magnet is added, stirred and dissolved at room temperature, nitrogen gas is passed through for 30 minutes to remove oxygen, heated to 60 to 80°C, the potassium persulfate aqueous solution is added, and the mixture is reacted for 12 to 20 hours to obtain the polyacrylic acid (PAA).

[0060] Step 2: Preparation of polyacrylic acid-styrene (PAA-PSt) [ka]

[0061] 98.0 to 245.0 g of styrene monomer is weighed out and slowly added to the flask after the reaction in step 1 using a syringe, and the reaction is continued at 60 to 80° C. for 2 to 8 hours to obtain the polyacrylic acid-styrene (PAA-PSt).

[0062] Step 3: Preparation of polyacrylic acid-styrene-2-ethylhexyl acrylate (PAA-PSt-PEHA) [ka]

[0063] 347.0 to 866.0 g of 2-ethylhexyl acrylate monomer is weighed out and slowly added to the flask after the reaction in step 2 using a syringe, and reacted continuously at 60 to 80° C. for 2 to 6 hours to obtain the polyacrylic acid-styrene-2-ethylhexyl acrylate (PAA-PSt-PEHA).

[0064] Step 4: Preparation of polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) [ka]

[0065] Measure 98.0 to 245.0 g of styrene monomer, slowly add it to the flask after the reaction in step 3 using a syringe, and react continuously at 60 to 80°C for 2 to 8 hours. Wash the reaction product with deionized water until the pH becomes 3 to 6, to obtain the polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt).

[0066] Step 5: Preparation of lithiated polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) [ka]

[0067] 500 g of the polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) obtained in step 4 is weighed out, and 15 to 25 g of a lithium hydroxide solution (containing 0.75 to 3.75 g of lithium hydroxide) having a mass fraction of 5% to 15% is added and reacted with stirring at a rotation speed of 300 rpm / h for 60 minutes to obtain the lithiated polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt).

[0068] Example 2: Manufacture of a lithium-ion battery

[0069] The lithiated polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) prepared in Example 1 is used as a battery binder to fabricate a 1 Ah soft pack battery.

[0070] Manufacture of positive electrode sheets

[0071] The positive electrode active material NCM811, conductive carbon black Super-P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry. The slurry is evenly applied to both sides of an aluminum foil, dried, rolled, and vacuum-dried at 80°, and an aluminum lead wire is welded using an ultrasonic welding machine to obtain a positive electrode plate with a thickness of 120 to 150 μm.

[0072] Manufacture of negative electrode sheets

[0073] A composite negative electrode active material (negative electrode consisting of 98% artificial graphite and 2% silicon oxide), conductive carbon black Super-P, lithium polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) prepared in Example 1, and a thickener, sodium carboxymethyl cellulose, are mixed in a mass ratio of 95:2:2:1, and then dispersed in deionized water to obtain a negative electrode slurry. This slurry is applied to both sides of copper foil, dried, rolled, and vacuum dried, and nickel lead wires are welded using an ultrasonic welding machine to obtain a negative electrode plate having a thickness of 80 to 100 μm.

[0074] Cell manufacturing

[0075] A 20 μm thick separator is placed between the positive and negative electrode plates, and then the sandwich structure consisting of the positive and negative electrode plates and the separator is rolled up. The rolled body is then flattened and placed in an aluminum foil packaging bag and vacuum baked at 85°C for 48 hours to obtain a cell ready for injection.

[0076] Cell injection chemical formation

[0077] Inject electrolyte into the cell in a glove box, vacuum seal and leave for 24 hours. Next, perform the initial charge routine formation according to the following steps: Charge to 3.05V at 0.02C constant current, charge to 3.75V at 0.05C constant current, charge to 4.05V at 0.2C constant current, vacuum seal. Then, charge to 4.2V at 0.33C constant current, leave at room temperature for 24 hours, and discharge to 3.0V at 0.2C constant current.

[0078] In Example 3, a lithium ion battery is manufactured in the same manner as in Example 2, except that artificial graphite is used as the negative electrode active material in the manufacture of the negative electrode sheet.

[0079] Comparative Example 1: Manufacturing of lithium-ion batteries using conventional SBR binder

[0080] Manufacture of positive electrode sheets

[0081] The positive electrode active material NCM811, conductive carbon black Super-P, and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 96:2:2, then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry. The slurry is evenly applied to both sides of an aluminum foil, dried, rolled, and vacuum-dried at 80°, and an aluminum lead wire is welded using an ultrasonic welding machine to obtain a positive electrode plate with a thickness of 120 to 150 μm.

[0082] Manufacture of negative electrode sheets

[0083] A composite negative electrode active material (negative electrode made of 98% artificial graphite + 2% silicon oxide), conductive carbon black Super-P, SBR, and a thickener, sodium carboxymethylcellulose, are mixed in a mass ratio of 95:2:2:1, and then dispersed in deionized water to obtain a negative electrode slurry. This slurry is applied to both sides of copper foil, dried, rolled, and vacuum dried, and nickel lead wires are welded using an ultrasonic welding machine to obtain a negative electrode plate with a thickness of 80 to 100 μm.

[0084] Cell manufacturing

[0085] A 20 μm thick separator is placed between the positive and negative electrode plates, and the sandwich structure consisting of the positive and negative electrode plates and separator is rolled up. The rolled body is then flattened, placed in an aluminum foil packaging bag, and vacuum baked for 48 hours to obtain a cell ready for injection.

[0086] Cell injection chemical formation

[0087] Inject electrolyte into the cell in a glove box, vacuum seal and leave for 24 hours. Next, perform the initial charge routine formation according to the following steps: Charge to 3.05V at 0.02C constant current, charge to 3.75V at 0.05C constant current, charge to 4.05V at 0.2C constant current, vacuum seal. Then, charge to 4.2V at 0.33C constant current, leave at room temperature for 24 hours, and discharge to 3.0V at 0.2C constant current.

[0088] In Comparative Example 2, a lithium ion battery was manufactured in the same manner as in Comparative Example 1, except that artificial graphite was used as the negative electrode active material in the manufacture of the negative electrode sheet.

[0089] Test Example 1 Polyacrylic acid-styrene- 2-Ethylhexyl acrylate -styrene (PAA-PSt-PEHA-PSt)

[0090] Polyacrylic acid-styrene- 2-Ethylhexyl acrylate 0.01 g of styrene was dissolved in 5 ml of tetrahydrofuran solvent, and the molecular weight and molecular weight distribution curve were measured by gel permeation chromatography. The results are shown in Table 1.

[0091] [Table 1]

[0092] Test Example 2 Lithium-ion battery performance test

[0093] (1) Quick charging capability test At 25°C, a constant current charging test was performed on the batteries manufactured in the examples and comparative examples at a rate of 2C, and the rate of charge capacity retention was calculated. The rate of charge retention of battery at 2C=capacity released after charging at a rate of 2C / capacity released after charging at a rate of 1 / 3C, and the results are shown in Table 2.

[0094] [Table 2]

[0095] (2) Peel strength test The negative electrode sheets produced in the examples and comparative examples were cut into strips measuring 2 cm wide x 10 cm wide, and 3M VHB double-sided adhesive tape of the same size was attached to a rectangular stainless steel plate of the same size (the plate was wiped clean with alcohol before application). The tape was then rolled back and forth three times with a roller of a certain weight to ensure close contact between the tape and the steel plate. The sheet (active material side) was then precisely attached to the other side of the tape, and the roller was rolled three times in the same way. Finally, the sheet was placed in a universal material testing machine to test the peel strength.

[0096] Place a part of the steel plate in the clamp below the machine, clamp the steel plate vertically to the ground, gently tear it from the bottom to the center position of the sheet, bend it 180° to the top of the machine and clamp it, control the machine to adjust the position of the upper clamp, open the test software, set the test conditions to a tensile speed of 50 mm / min, reset all initial parameters to zero, and start the test. The results obtained are shown in Table 3.

[0097] [Table 3]

[0098] (3) High-temperature gas generation performance test The initial weight and initial volume (measured by the water draining method) of the batteries manufactured in the examples and comparative examples were measured, and they were placed in a 60°C environment, and were taken out every 7 days until the 28th day, when they were removed and cooled to room temperature, and their volumes were measured, and the volume increase rate was calculated. Each time a measurement was completed, the batteries were returned to 60°C and charged at a current of 0.03 C. The results obtained are shown in Table 4.

[0099] [Table 4]

[0100] (4) Low-temperature discharge capacity test The batteries manufactured in the examples and comparative examples are used to measure the discharge capacity retention rate at -20°C. At 25°C, the fully charged battery is discharged to 3.0V at 1C, and the initial discharge capacity is recorded as DC(25°C). Then, at 25°C, the battery is charged to 4.2V at a constant current and voltage of 1C, with a cutoff current of 0.05C. Next, the battery is cooled to -20°C and left for 4 hours, and then discharged to 3.0V at 1C, and the discharge capacity DC(-20°C) is recorded. The discharge capacity retention rate at -20°C=100%*DC(-20°C) / DC(25°C). The results are shown in Table 5.

[0101] [Table 5]

[0102] Those skilled in the art will understand that the above-described embodiments are specific examples for realizing the present invention, and that in actual implementation, various changes in shape and details are possible without departing from the spirit of the present invention.

Claims

1. It has a structure represented by B-C-B-A, A represents polymer block A, B represents polymer block B, and C represents polymer block C, The polymer block A is formed by polymerizing an alkenyl formate monomer, The polymer block B is formed by polymerizing an aromatic vinyl monomer, The polymer block C is a lithiated block polymer, which is a lithiated product of a block polymer, characterized in that the polymer block C is polymerized from an acrylate monomer.

2. The structure of the alkenyl formate monomer is as follows: 【Chemistry 1】 In the formula, R11 and R12 are independently hydrogen or C 1~4 is an alkyl group, and / or the aromatic vinyl monomer has the structure: 【Chemistry 2】 In the formula, R21, R22, R23, R24, R25, and R26 are independently hydrogen or C 1~4 is an alkyl group, and / or the structure of the acrylate monomer is: 【Chemistry 3】 In the formula, R31 is a straight or branched chain C 1~10 2. The lithiated block polymer of claim 1, wherein the lithiated block polymer is an alkyl group.

3. the alkenyl formate monomer is acrylic acid; and / or the aromatic vinyl monomer is styrene; And / or the lithiated block polymer according to claim 2, characterized in that the structure of the acrylate monomer is as follows: 【Chemistry 4】 In the formula, R31 is a straight or branched chain C 4~8 It is an alkyl group.

4. In the block polymer, The degree of polymerization of the polymer block A is 10 to 50, The degree of polymerization of the polymer block B is 200 to 500, The lithiated block polymer according to any one of claims 1 to 3, characterized in that the degree of polymerization of the polymer block C is 400 to 1000.

5. A method for producing the lithiated block polymer according to any one of claims 1 to 4, comprising the steps of: (1) a step of polymerizing the polymer block A and the monomers constituting the polymer block B in the presence of a RAFT reagent and an initiator to obtain a polymer block B-A; (2) a step of polymerizing the monomer constituting the polymer block C with the polymer block B-A in the presence of a RAFT reagent and an initiator to obtain a polymer block C-B-A; (3) reacting the monomer constituting the polymer block B with the polymer block C-B-A in the presence of a RAFT reagent and an initiator to obtain the block polymer; A method for producing a lithiated block polymer, comprising:

6. The lithiated block polymer according to any one of claims 1 to 4, characterized in that the lithiated block polymer has a structure represented by general formula (I): 【Chemistry 5】 In the formula, n is 10 to 50, x is 200 to 500, and y is 400 to 1000. z is 200 to 500. R41 is C 4~8 R42 and R43 are phenyl groups or C 1~4 It is a phenyl group substituted with an alkyl group.

7. 7. The lithiated block polymer of claim 6, wherein the lithiated block polymer is: 【Chemistry 6】 In the formula, n is 10 to 50, x is 200 to 500, and y is 400 to 1000. z is 200 to 500.

8. 1. A method for producing a lithiated block polymer, comprising the steps of: (1) a step of polymerizing polyacrylic acid-styrene-2-ethylhexyl acrylate (PAA-PSt-PEHA) with a styrene monomer to obtain polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt); (2) treating polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) with lithium hydroxide to obtain the lithiated block polymer; A method for producing a lithiated block polymer, comprising: 【Chemistry 7】 In the steps (1) and (2), n is 10 to 50, x is 200 to 500, and y is 400 to 1000. In the step (2), z is 200 to 500.

9. the mass ratio of the polyacrylic acid-styrene-2-ethylhexyl acrylate-styrene (PAA-PSt-PEHA-PSt) to the styrene monomer is (0.01 to 0.3):1; And / or, in step (1), the polymerization reaction is carried out in the presence of an initiator, And / or, in step (1), the temperature of the polymerization reaction is 50 to 90° C., And / or, in step (1), the polymerization reaction time is 2 to 8 hours; and / or, in step (1), after the polymerization reaction, further comprising washing the polymerization product with deionized water to a pH of 3 to 6; And / or, in step (2), the lithium hydroxide is an aqueous solution of lithium hydroxide, and the mass fraction of lithium hydroxide in the aqueous solution of lithium hydroxide is 5% to 15%.

10. The method according to claim 8, comprising the step of: (A) polymerizing polyacrylic acid-styrene (PAA-PSt) and 2-ethylhexyl acrylate monomer to obtain polyacrylic acid-styrene-2-ethylhexyl acrylate (PAA-PSt-PEHA). 【Chemistry 8】 In step (A), n is 10 to 50, and x is 200 to 500.

11. In step (A), the mass ratio of the polyacrylic acid-styrene (PAA-PSt) to the 2-ethylhexyl acrylate is (0.6 to 0.9):1; And / or, in step (A), the polymerization reaction is carried out in the presence of an initiator, And / or, in step (A), the temperature of the polymerization reaction is 50 to 90° C., And / or the method according to claim 10, characterized in that in step (A), the polymerization reaction time is 2 to 8 hours.

12. The preparation of polyacrylic acid-styrene (PAA-PSt) includes the steps of: The method according to claim 10, comprising the step of: (I) polymerizing polyacrylic acid and a styrene monomer to obtain polyacrylic acid-styrene (PAA-PSt). 【Chemistry 9】 In the formula, n is 10 to 50 and x is 200 to 500.

13. In step (I), the mass ratio of the polyacrylic acid to the styrene monomer is 1:(3 to 90); And / or, in step (I), the polymerization reaction is carried out in the presence of an initiator, And / or, in step (I), the temperature of the polymerization reaction is 50 to 90° C., And / or the method according to claim 12, characterized in that in step (I), the polymerization reaction time is 2 to 10 hours.

14. The method for producing polyacrylic acid according to claim 12, characterized in that the method comprises polymerizing an acrylic acid monomer in the presence of a RAFT reagent and an initiator to obtain polyacrylic acid.

15. In the polymerization reaction, the mass ratio of the RAFT reagent, the initiator, and the acrylic acid monomer is (0.5-1.0):(0.2-0.5):(10-20), And / or the temperature of the polymerization reaction is 50 to 90° C., and / or the polymerization reaction time is 10 to 22 hours; and / or the initiator is potassium persulfate, sodium persulfate or ammonium persulfate; And / or the process according to claim 14, characterized in that the RAFT reagent is: 【Chemistry 10】 In the formula, R is an isopropionic acid group, an acetate group, a 2-cyanoacetate group, or a 2-aminoacetate group; Z is C 4~12 Alkyl group, C 4~12 It is an alkylthio group, a phenyl group or a benzyl group.

16. Use of the lithiated block polymer according to any one of claims 1 to 4, 6 and 7 as a binder for a lithium ion battery.

Citation Information

Patent Citations

  • Water-based electrode bonding agent for sulfur positive pole and preparing method

    CN106433530A

  • Silicon-based lithium ion battery negative electrode

    CN108306021A

  • Lithium-ion battery electrode prepared by water-based binder

    CN108470884A

  • Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery