Photocurable gel nail composition and gel nail method

The photocurable gel nail composition, combining urethane acrylate resin and cellulose resin, addresses adhesion and removability issues, offering improved curability and ease of peeling, enhancing safety and handling in nail applications.

JP7578966B2Active Publication Date: 2024-11-07JUJO CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020124914
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-22
Publication Date
2024-11-07
Estimated Expiration
2040-07-22

AI Technical Summary

Technical Problem

Existing photocurable gel nails face issues with adhesion, durability, and removability, with some compositions being difficult to handle and requiring complex peeling processes, while others lack sufficient durability or have high viscosity, making application challenging.

Method used

A photocurable gel nail composition comprising urethane acrylate resin and cellulose resin in specific ratios, along with additional components like (meth)acrylate monomers and photopolymerization initiators, to enhance adhesion, curability, and ease of peeling.

Benefits of technology

The composition provides excellent curability, adhesion to nails, and easy peeling, improving safety and handling, with the ability to form smooth, durable cured films that can be efficiently removed without complex processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578966000003
    Figure 0007578966000003
  • Figure 0007578966000004
    Figure 0007578966000004
  • Figure 0007578966000005
    Figure 0007578966000005
Patent Text Reader

Abstract

To provide photocurable gel nail compositions that are easy to apply, have excellent curability, and can be easily peeled off after use, and to provide gel nail methods.SOLUTION: Provided is a photocurable gel nail composition, containing (A) a urethane acrylate resin and (B) a cellulose resin, the photocurable gel nail composition containing (B) the cellulose resin in a value within the range of 1 to 50 pts.wt. with respect to 100 pts.wt. of (A) the urethane acrylate resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocurable composition for gel nails and a method for producing a gel nail. In particular, the present invention relates to a photocurable gel nail composition that is easy to apply to a substrate such as one's own nail, has excellent curing properties, and can be easily peeled off after use, and a gel nail method. [Background technology]

[0002] 2. Description of the Related Art Conventionally, as compositions used for decorating nails, there have been known nail polish compositions containing nitrocellulose or acrylic resin as a main component, with the resin dissolved in an organic solvent such as toluene, butyl acetate, or ethyl acetate. However, because nail polish contains a large amount of organic solvents, users may inhale the odor of the solvent, which can lead to poisoning and cause dizziness, headaches, and other problems. Furthermore, since it usually takes several tens of minutes for the volatile components of nail polish to dissipate, there is a problem that after applying the nail polish, the fingertips cannot be used freely until the nail polish dries.

[0003] As a result, photocurable gel nails have been actively developed and marketed because they do not contain organic solvents, have a fast curing reaction, are easier to handle than nail polish, and are safer. As such a photocurable gel nail, the present applicant has proposed a photocurable solventless gel nail that is composed of a urethane acrylate resin, a (meth)acrylate monomer, and a photopolymerization initiator (see, for example, Patent Document 1). More specifically, a photocurable gel nail containing a specified amount of a polyether-skeleton urethane acrylate oligomer, monofunctional and polyfunctional (meth)acrylate monomers, and a photopolymerization initiator has excellent adhesion to substrates such as natural nails and can be easily removed.

[0004] Also, a gel polish has been proposed that can be directly wiped off with a remover without the need for a complicated removal process (see, for example, Patent Document 2). More specifically, it is a gel polish containing an aliphatic urethane acrylate and an acrylate oligomer as resin components, a propoxylated neopentyl glycol diacrylate as an acrylate monomer component, and trimethylbenzoyldiphenylphosphine oxide as a photopolymerization initiator.

[0005] Furthermore, a gel polish composition that is excellent in oxygen permeability and has high gloss has been proposed (see, for example, Patent Document 3). More specifically, it is a gel polish composition that includes a multifunctional silicone urethane acrylate oligomer, a reactive acrylate oligomer, and an acrylate monomer, and a photoinitiator. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2013-043853 A (Claims, etc.) [Patent Document 2] JP 2017-061446 A (Claims, etc.) [Patent Document 3] Patent Publication No. 2017-535512 (Claims, etc.) Summary of the Invention [Problem to be solved by the invention]

[0007] However, although the light-curing gel nail described in Patent Document 1 is effective in terms of adhesion, it is not easy to remove after use, and requires a complicated process that includes at least three steps, such as polishing the nail surface, soaking in a remover, and scraping off with a metal pusher.

[0008] In addition, the gel polish described in Patent Document 2 does not require any complicated steps to peel off the gel polish layer, and can be directly wiped off using a cloth, cotton, or tissue paper coated with polish remover, but there was a problem in that the durability of the gel polish was not good. That is, when an attempt is made to improve the releasability of a gel polish layer made of gel polish, problems have been observed in that adhesion and durability are reduced.

[0009] Furthermore, the gel polish composition described in Patent Document 3 contains a multifunctional silicone urethane acrylate oligomer, which gives it excellent oxygen permeability, is less likely to damage natural nails, and is capable of forming a highly glossy gel polish layer; however, because the gel polish composition has a relatively high viscosity, it is difficult to handle when applied, and no consideration has been given to its releasability.

[0010] Therefore, after extensive research, the inventors discovered that a photocurable gel nail composition containing a specified urethane acrylate resin and a specified cellulose-based resin in a specified ratio is easy to apply, has excellent curing properties, and can be easily peeled off after use, thereby completing the present invention. That is, the present invention relates to a photocurable composition for gel nails, which has excellent curing properties and can be easily peeled off after use, and a method for applying gel nails. [Means for solving the problem]

[0011] According to the present invention, there is provided a photocurable composition for gel nails comprising (A) a urethane acrylate resin and (B) a cellulose-based resin, and the above-mentioned problems can be solved by including the cellulose-based resin (B) in an amount within the range of 1 to 50 parts by weight per 100 parts by weight of the urethane acrylate resin (A). In other words, by including such a predetermined amount of (A) urethane acrylate resin, not only is the curing property of the photocurable gel nail composition improved, but the adhesion is also increased, making it easier to apply to a substrate such as a nail. Furthermore, by including a predetermined amount of a cellulose-based resin as the component (B), when a cured film is formed, not only is the smoothness of the cured film improved, but the peelability is also improved, and the time required for peeling can be reduced.

[0012] In forming the photocurable composition for gel nails of the present invention, it is preferable that the urethane acrylate resin (A) contains at least a urethane acrylate resin (a1) having a weight average molecular weight in the range of 500 to 30,000. By configuring it in this manner, the photocurable gel polish composition can maintain suitable adhesion while improving curability and abrasion resistance, thereby providing a cured film with appropriate durability.

[0013] In forming the photocurable gel polish composition of the present invention, it is preferable that the (A) urethane acrylate resin further contains a urethane acrylate resin (a2) having a weight average molecular weight of less than 5,000, and consists of at least two types of urethane acrylate resins having different weight average molecular weights. By configuring in this way, it is possible to obtain not only the effect of adding the urethane acrylate resin (a1), but also the effect of improving the adhesiveness and flexibility of the cured film by adding the urethane acrylate resin (a2).

[0014] In forming the photocurable composition for gel nails of the present invention, the cellulose-based resin (B) is preferably a cellulose ester-based resin having a number average molecular weight in the range of 1,000 to 50,000. By configuring in this manner, it is possible to provide a photocurable composition for gel nails that has good adhesion while also being imparted with appropriate transparency.

[0015] In forming the photocurable composition for gel nails of the present invention, the cellulose-based resin (B) is preferably a cellulose acetate butyrate resin, a cellulose acetate propionate resin, or either one of them. By configuring in this way, various (meth)acrylate components can be uniformly dissolved, and the smoothness and releasability of the obtained cured film can be improved.

[0016] Furthermore, when preparing the photocurable gel nail composition of the present invention, it is preferable that the photocurable gel nail composition further contains a (meth)acrylate monomer component as component (C), and that the content thereof is within the range of 50 to 150 parts by weight per 100 parts by weight of the urethane acrylate resin (A). By configuring it in this manner, it is possible to improve the adhesion and peelability while also improving the handleability of the photocurable gel nail composition and safety when applying it to a substrate such as a nail.

[0017] Furthermore, when forming the photocurable gel nail composition of the present invention, it is preferable that the (C) (meth)acrylate monomer component is one or more selected from isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and dipentaerythritol hexaacrylate. By configuring in this manner, it is possible to further improve safety when applying the photocurable composition for gel nails to a substrate such as a nail.

[0018] Furthermore, when preparing the photocurable gel nail composition of the present invention, it is preferable that the photocurable gel polish composition further contains a photopolymerization initiator as component (D), and that the content thereof is within the range of 5 to 50 parts by weight per 100 parts by weight of the urethane acrylate resin (A). By configuring in this manner, the curing properties of the photocurable composition for gel nails can be improved, and the handling properties can be improved when applying it to a substrate such as a nail.

[0019] In addition, when forming the photocurable gel nail composition of the present invention, it is preferable that the (D) photopolymerization initiator is one or more selected from the group consisting of α-hydroxyketone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators. By configuring in this manner, the reactivity with the resin component is improved, and the curability of the photocurable composition for gel nails can be made more suitable.

[0020] Furthermore, when preparing the photocurable gel nail composition of the present invention, it is preferable that the photocurable gel nail composition further contains an organic solvent as component (E), and that the content of the organic solvent is within the range of 5 to 50 parts by weight per 100 parts by weight of the urethane acrylate resin (A). By configuring it in this manner, the viscosity of the photocurable gel nail composition can be adjusted to a suitable range while maintaining suitable peelability of the cured film, thereby improving handleability when applied to a substrate such as a nail.

[0021] In addition, when forming the photocurable gel nail composition of the present invention, it is preferable that the (E) organic solvent is one or more selected from ethyl acetate, propyl acetate, butyl acetate, and isobutyl acetate. By configuring in this manner, odors and irritation to nails, etc. resulting from the incorporation of the (E) organic solvent can be suppressed, thereby improving the safety of the photocurable gel nail composition when used.

[0022] Another aspect of the present invention is a gel nail method using any of the photocurable gel nail compositions described above, comprising the following steps (1) to (4): (1) A step of preparing a photocurable gel nail composition (2) A step of applying a photocurable gel nail composition to form a coating layer. (3) A process of photocuring the coating layer to form a cured film. (4) A process for peeling off the cured film after use By implementing it in this manner, it is possible to improve the safety of decorating nails, etc., and the ease of removal, compared to the use of conventional gel nails, etc. Effect of the Invention

[0023] According to the present invention, it is possible to provide a photocurable gel nail composition that can be easily applied to a substrate such as a natural nail, has excellent curing properties, and can be easily peeled off after use. In particular, a photocurable gel nail composition containing a specified component (B) in a specified ratio relative to a specified component (A) can achieve unpredictable effects on adhesion and releasability. [Brief description of the drawings]

[0024] [Figure 1] 1(a) to (c) are diagrams provided for explaining a method for forming a cured film having a single-layer structure. [Diagram 2] 2(a) to (d) are diagrams provided for explaining a method for forming a cured film having a multilayer structure. [Diagram 3] FIG. 3 is a diagram provided for explaining the relationship between the blending amount of the cellulose-based resin and the releasability of the cured film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] [First embodiment] The first embodiment of the present invention is a photocurable gel nail composition comprising (A) a urethane acrylate resin and (B) a cellulose-based resin, characterized in that the photocurable gel nail composition contains 1 to 50 parts by weight of the cellulose-based resin (B) per 100 parts by weight of the urethane acrylate resin (A). Each of the components of the first embodiment will be specifically described below.

[0026] 1. (A) Urethane acrylate resin (1) Type The photocurable composition for gel nails of the present invention is characterized by containing a urethane acrylate resin as component (A). The reason for this is that by using a urethane acrylate resin as component (A), the reactivity of the photocurable gel nail composition can be suppressed within a specified range, thereby improving the adhesion to substrates such as natural nails.

[0027] Moreover, such a urethane acrylate resin is preferably a urethane acrylate resin having a polyether skeleton. The reason for this is that if a polyether-skeleton urethane acrylate resin is used, by combining it with components (B) to (E) described below, it is possible to improve the releasability while maintaining excellent adhesion to substrates such as natural nails.

[0028] Here, the type of polyether skeleton polyol for obtaining the polyether skeleton urethane acrylate resin is not particularly limited, but it is preferable to use a polyether skeleton diol compound, since it is easily available industrially and is relatively inexpensive.

[0029] As the type of organic polyisocyanate compound for obtaining the polyether skeleton urethane acrylate resin, non-yellowing types such as isophorone diisocyanate, hexamethylene diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and trimethylhexamethylene diisocyanate are preferred. As the hydroxyacrylate for obtaining the polyether skeleton urethane acrylate resin, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, caprolactone-modified 2-hydroxyethyl acrylate, etc. are preferred. In the present invention, however, these polyether-skeleton urethane acrylate resins may be used alone, but it is also preferable to use other urethane acrylate resins, for example, polyester-skeleton urethane acrylate resins, polycaprolactone-skeleton urethane acrylate resins, polycarbonate-skeleton urethane acrylate resins, etc., in combination within a range in which the effects of the present invention can be better obtained.

[0030] (2) Weight average molecular weight (Mw) The weight average molecular weight of the urethane acrylate resin (A) is preferably set to a value within the range of 500 to 30,000. The reason for this is that by using a urethane acrylate resin having such a weight average molecular weight, it is possible to improve the curing properties while maintaining adhesion to substrates such as natural nails, and thereby obtain a predetermined hardness in the cured film. In other words, if the weight average molecular weight of the urethane acrylate resin is less than 500, the curability decreases, making the coating more likely to adhere poorly to substrates such as natural nails and to cause tack on the surface of the cured film. On the other hand, if the weight average molecular weight of the urethane acrylate resin exceeds 30,000, the curing time becomes long, and it may become difficult to obtain a desired hardness as a cured film. Therefore, the weight average molecular weight of the urethane acrylate resin is preferably within the range of 1,000 to 25,000, and more preferably within the range of 2,000 to 20,000.

[0031] (3) Compounding amount The amount of the urethane acrylate resin (A) blended is preferably within the range of 20 to 60% by weight relative to the total amount (100% by weight) of the photocurable composition for gel nails of the present invention. The reason for this is that, in combination with the second urethane acrylate resin (a2) described below, it is possible to obtain a predetermined hardness as a cured film while maintaining adhesion to the nail. That is, if the amount of urethane acrylate resin is less than 20% by weight, the curing time becomes excessively long, making it difficult to obtain the abrasion resistance and durability of the cured film. On the other hand, if the amount of urethane acrylate resin exceeds 60% by weight, the curability decreases excessively, making the composition more susceptible to poor adhesion to substrates such as natural nails. Therefore, the amount of urethane acrylate resin is preferably within the range of 25 to 55% by weight, and more preferably within the range of 30 to 50% by weight, relative to the total amount (100% by weight) of the photocurable gel nail composition.

[0032] (4) Acid value In addition, the acid value of the urethane acrylate resin (A) used in the present invention is preferably 10 mgKOH / g or less. The reason for this is that by setting the acid value of the urethane acrylate resin to such a value, it is possible to suppress outgassing that is generated by decomposition of the cured film formed by the resulting photocurable gel nail composition, and it is also possible to prevent corrosion of the adherend, such as the nail or plastic substrate. In the present invention, the acid value of the adhesive resin means a value measured in accordance with JIS K0070. Therefore, the acid value of the urethane acrylate resin is preferably 5 mgKOH / g or less, and more preferably 1 mgKOH / g or less.

[0033] (5)NCO content Furthermore, the (A) urethane acrylate resin may contain isocyanate groups (-N=C=O) that do not contribute to the reaction due to the manufacturing method thereof. Therefore, from the viewpoint of the health effects of inhaling or coming into contact with isocyanates, the content of isocyanate groups (NCO content) in the urethane acrylate resin is preferably 0.3% or less, more preferably 0.1% or less, and ideally 0. Therefore, by setting the NCO content within this range, it is possible to obtain a urethane acrylate resin (A) that is less irritating to nails and the surrounding skin and that is inhibited from yellowing due to heat or over time.

[0034] The urethane acrylate resin (A) can be selected from, for example, the EBECRYL series and KRM series of Daicel Allnex Corporation, and the Art Resin (registered trademark) series of Negami Chemical Industries, Ltd.

[0035] (6) Multiple urethane acrylate resins (6)-1 type Furthermore, when the urethane acrylate resin is composed of at least two kinds of urethane acrylate resins having different weight average molecular weights and the aforementioned urethane acrylate resin is the first urethane acrylate resin (a1), it is preferable that the urethane acrylate resin further contains a second urethane acrylate resin (a2). The reason for this is that by containing at least two types of urethane acrylate resins, the added effects of each urethane acrylate resin can be obtained, and the adhesion of the photocurable gel nail composition and the flexibility of the cured film can be improved. Examples of such urethane acrylate resin (a2) include di- to hepta-functional polyester-skeleton urethane acrylate resins having a weight average molecular weight described below, or polycaprolactone-based urethane acrylate resins, polycarbonate-based urethane acrylate resins, and polyether-based urethane acrylate resins.

[0036] (6)-2 Weight average molecular weight (Mw) The weight average molecular weight of the urethane acrylate resin (a2) is preferably less than 5,000. The reason for this is that when the weight average molecular weight of the urethane acrylate resin (a2) is 5,000 or more, the curing property decreases and the curing time becomes excessively long, making it difficult to obtain durability and flexibility as a cured film. Therefore, the weight average molecular weight of the urethane acrylate resin (a2) is more preferably within the range of 500 to 4,500, and further preferably within the range of 1,000 to 4,000. The weight average molecular weight of the urethane acrylate resin is a weight average molecular weight calculated as polystyrene, measured by gel permeation chromatography (GPC).

[0037] (6)-3 Blend amount The amount of the urethane acrylate resin (a2) is preferably within the range of 1 to 30% by weight based on the total amount (100% by weight) of the photocurable composition for gel nails of the present invention. The reason for this is that if the amount of urethane acrylate resin (a2) is less than 1% by weight, the effect of adding the urethane acrylate resin (a2) is not achieved, and poor adhesion to the nail is likely to occur, and tackiness is likely to occur in the cured film. On the other hand, if the amount of the urethane acrylate resin (a2) exceeds 30% by weight, the curability decreases excessively, making it difficult to obtain durability as a cured film. Therefore, the amount of the urethane acrylate resin (a2) is preferably within the range of 5 to 25% by weight, and more preferably within the range of 10 to 20% by weight, based on the total amount of the photocurable gel nail composition of the present invention.

[0038] (6)-4 Mixture ratio Furthermore, when the (A) urethane acrylate resin is composed of two types of urethane acrylate resin, namely, urethane acrylate resin (a1) and urethane acrylate resin (a2), it is preferable that, when the blending ratio of the two types of urethane acrylate resins is (a1)+(a2)=100, (a1) is a value within the range of 60 to 99, and (a2) is a value within the range of 1 to 40. The reason for this is that by containing the urethane acrylate resin (a2), which mainly contributes to the adhesiveness and flexibility of the cured film, in such a ratio relative to the urethane acrylate resin (a1), which mainly contributes to the curability and hardness and abrasion resistance of the cured film, a photocurable gel nail composition that has excellent curability and adhesion when applied to a human nail is obtained. Furthermore, by including the component (A) in such a ratio, a photocurable composition for gel nails having excellent releasability can be obtained. Therefore, when the blending ratio of the urethane acrylate resin (a1) and the urethane acrylate resin (a2) is (a1) + (a2) = 100, it is preferable that (a1) is within the range of 65 to 95 and (a2) is within the range of 5 to 35, and it is further preferable that (a1) is within the range of 70 to 90 and (a2) is within the range of 10 to 30.

[0039] 2. (B) Cellulose-based resin (1) Type The photocurable composition for gel nails is characterized by containing a cellulose-based resin as component (B). The reason for this is that by containing a cellulose-based resin, when the composition is laminated onto a substrate such as a natural nail to form a cured film, the cured film can be given smoothness and suitable releasability. Also, the cellulose-based resin has a relatively high polarity and exhibits good compatibility with the above-mentioned (A) urethane acrylate resin.

[0040] The type of cellulose-based resin is not particularly limited, but it is preferable to use, for example, cellulose ester resins such as nitrocellulose, cellulose acetate butyrate, cellulose acetate, and cellulose acetate propionate, either alone or in combination. The reason for this is that cellulose acetate resin and the like can be well miscible with the (A) urethane acrylate resin over a wide range, and can easily maintain adhesion to substrates such as natural nails, non-yellowing, and water resistance.

[0041] Among these cellulose-based resins, cellulose acetate butyrate resin or cellulose acetate propionate resin is more preferable. The reason for this is that these cellulose acetate butyrate resins and the like can be dissolved uniformly in various (meth)acrylate components. Therefore, it can be similarly applied to (meth)acrylate monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and isobornyl (meth)acrylate, which will be described later, to form a solution, and the resulting cured film can have smoothness and releasability.

[0042] (2) Number average molecular weight (Mn) The number average molecular weight of the cellulose resin is preferably within the range of 1,000 to 50,000. The reason for this is that if the number average molecular weight is less than 1000, poor adhesion to the substrate is likely to occur and the transparency of the cured film may decrease. On the other hand, if the number average molecular weight exceeds 50,000, the surface hardness of the cured film may become excessively high, resulting in reduced flexibility. Therefore, the number average molecular weight of the cellulose-based resin is more preferably within the range of 2,000 to 40,000, and even more preferably within the range of 3,000 to 30,000. The number average molecular weight of the cellulose-based resin is a polystyrene-equivalent number average molecular weight measured by gel permeation chromatography (GPC).

[0043] (3) Compounding amount Furthermore, the photocurable composition for gel nails of the present invention is characterized in that the blending amount of the cellulose-based resin (B) is within the range of 1 to 50 parts by weight per 100 parts by weight of the urethane acrylate resin (A). The reason for this is that, as shown in FIG. 3, if the amount of the (B) cellulose-based resin is less than 1 part by weight, the effect of adding the resin may not be achieved, and the resin may be prone to poor adhesion to the substrate, or it may be difficult to obtain improved peelability or smoothness of the cured film. On the other hand, if the amount of the cellulose-based resin (B) exceeds 50 parts by weight, the flexibility of the cured film decreases and transparency cannot be obtained. Therefore, the blending amount of the (B) cellulose-based resin is preferably within a range of 5 to 45 parts by weight, and more preferably within a range of 10 to 40 parts by weight, per 100 parts by weight of the (A) urethane acrylate resin.

[0044] Furthermore, in the photocurable gel nail composition of the present invention, when the cured film has a multi-layer structure consisting of a base layer, an intermediate layer, a protective layer, etc. as shown in Figure 2, it is preferable to vary the amount of (B) cellulose-based resin in the composition constituting the layers for each layer. The reason for this is that by varying the blending amount of the (B) cellulose-based resin for each layer of the cured film having a multi-layer structure, each layer can exhibit suitable physical properties, and the cured film as a whole can be made to have excellent adhesion, releasability, surface smoothness, etc. Therefore, for example, it is preferable that the amount of (B) cellulose-based resin in the undercoat layer is within the range of 10 to 40 parts by weight, the amount of (B) cellulose-based resin in the intermediate layer is within the range of 1 to 20 parts by weight, and the amount of (B) cellulose-based resin in the protective layer is within the range of 1 to 50 parts by weight.

[0045] The cellulose-based resin may be selected from, for example, the CAB series and CAP series manufactured by Eastman Chemical Company.

[0046] 3. (C) (Meth)acrylate Monomer (1) Type In addition, it is preferable that the photocurable composition for gel nails of the present invention contains a predetermined amount of a (meth)acrylate monomer component as component (C). The reason for this is that by containing a specific (meth)acrylate monomer component, the handleability of the photocurable gel polish composition can be adjusted and safety can be improved when applied to human nails.

[0047] As the type of (C) (meth)acrylate monomer, known monofunctional or polyfunctional monomers can be used. Therefore, for example, examples of monofunctional (meth)acrylate monomers include ethyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, phenyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and acryloylmorpholine. Examples of bifunctional (meth)acrylate monomers include diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and polypropylene glycol di(meth)acrylate. Examples of trifunctional (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, ethyl Examples of the (meth)acrylate monomer that can be used include ethylene oxide-modified trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, propoxylated glyceryl tri(meth)acrylate, and tetrafunctional (meth)acrylate monomers include ditrimethylolpropane tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate, and examples of the (meth)acrylate monomers include dipentaerythritol hydroxypenta(meth)acrylate, and examples of the (meth)acrylate monomers include dipentaerythritol hexa(meth)acrylate, and in the present invention, these (meth)acrylate monomer components can be used alone or in combination of two or more.

[0048] Among these, it is preferable to use a monofunctional (meth)acrylate monomer selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and isobornyl (meth)acrylate, since the monofunctional (meth)acrylate monomer has a PII value of 1.0 or less, has good compatibility with (A) the urethane acrylate resin and (B) the cellulose-based resin, and can suppress heat generation during curing. Here, skin irritation (PII value: Primary Irritation Index) is widely used as an indicator of the degree of skin damage such as skin irritation and rash caused by chemical substances, and is measured by the Draize method. The measured value is displayed in the range of 0 to 8, and a PII value of 1.0 or less indicates low irritation.

[0049] (2) Compounding amount The blending amount of the (C) (meth)acrylate monomer is preferably within the range of 40 to 150 parts by weight per 100 parts by weight of the (A) urethane acrylate resin. The reason for this is that by blending the (C) (meth)acrylate monomer in such a ratio, it is possible to improve adhesion to the nail and it is also easy to obtain a cured film that has excellent peelability after use of the gel nail.

[0050] That is, when the amount of the (C) (meth)acrylate monomer is less than 40 parts by weight, it becomes difficult to control the curing property, which may lead to poor adhesion to the nail and difficulty in handling. On the other hand, if the amount of the (C) (meth)acrylate monomer exceeds 150 parts by weight, the curability decreases, the curing time becomes excessively long, and tackiness may easily occur on the surface of the cured film. Therefore, the blending amount of the (C) (meth)acrylate monomer is preferably within a range of 50 to 140 parts by weight, and more preferably within a range of 60 to 130 parts by weight, per 100 parts by weight of the (A) urethane acrylate resin.

[0051] These (meth)acrylate monomers are commercially available from Kyoeisha Chemical Co., Ltd., Osaka Organic Chemical Industry Co., Ltd., Hitachi Chemical Co., Ltd., and the like.

[0052] 4. (D) Photopolymerization initiator (1) Type In addition, it is preferable to incorporate a predetermined amount of a photopolymerization initiator as component (D) in the photocurable gel nail composition of the present invention. The reason for this is that by containing a specific photopolymerization initiator, it becomes easier to obtain good curability in the photocurable gel nail composition.

[0053] The type of (D) photopolymerization initiator is not particularly limited as long as it generates radicals by ultraviolet light and the radicals polymerize a urethane acrylate resin or a (meth)acrylate monomer. For example, acylphosphine oxide photopolymerization initiators such as 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,2-dimethoxy-1,2-diphenylethane-1-one, and phenyl glyoxylic acid methyl ester, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propionyl, and the like can be used. Examples of the photopolymerization initiator include α-hydroxyketone-based photopolymerization initiators such as 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, and oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, and α-aminoalkylphenone-based photopolymerization initiators such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 and 2-dimethylamino-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, either singly or in combination of two or more.

[0054] Among such (D) photopolymerization initiators, an α-hydroxyketone-based photopolymerization initiator and an acylphosphine oxide-based photopolymerization initiator are preferred because they generate radicals when exposed to ultraviolet light, and the radicals react efficiently with a photopolymerizable oligomer and a photopolymerizable monomer, thereby accelerating the curing reaction.

[0055] (2) Compounding amount The blending amount of the (D) photopolymerization initiator is preferably within a range of 5 to 50 parts by weight per 100 parts by weight of the (A) urethane acrylate resin. The reason for this is that if the blending amount of the (D) photopolymerization initiator is less than 5 parts by weight, the curability is excessively reduced, and the durability of the cured film may decrease. On the other hand, if the amount of the photopolymerization initiator (D) exceeds 50 parts by weight, the curability increases excessively, which may lead to poor adhesion to nails and difficulty in handling. Therefore, the blending amount of the (D) photopolymerization initiator is preferably within the range of 10 to 45 parts by weight, and more preferably within the range of 15 to 40 parts by weight.

[0056] These (D) photopolymerization initiators are commercially available from IGM Resins bV, BASF, and the like.

[0057] 5. (E) Organic Solvents (1) Type In addition, the photocurable gel nail composition of the present invention preferably contains an organic solvent as component (E) in order to obtain ease of handling when applied to a substrate such as a nail and ease of removability after use of the gel nail.

[0058] The type of (E) organic solvent is not particularly limited as long as it is compatible with the components that constitute the photocurable gel nail composition of the present invention, and examples thereof include low molecular weight alcohol solvents such as methanol, ethanol, isopropanol, and butanol, alkylene glycol monoether solvents such as ethylene glycol monomethyl ether and propylene glycol monomethyl ether, aromatic solvents such as benzene, toluene, and xylene, acetate ester solvents such as propyl acetate, ethyl acetate, butyl acetate, and isobutyl acetate, ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, and ether solvents such as dibutyl ether, and the like. Among these, one or more organic solvents selected from ethyl acetate, propyl acetate, butyl acetate, and isobutyl acetate are preferred, since they have excellent compatibility, a relatively mild odor, and are less irritating to base materials such as nails.

[0059] (2) Compounding amount The blending amount of the (E) organic solvent is preferably within a range of 10 to 50 parts by weight per 100 parts by weight of the (A) urethane acrylate resin. The reason for this is that if the blend amount of (E) the organic solvent is less than 10 parts by weight, the viscosity of the photocurable gel polish composition of the present invention becomes too high, resulting in poor handleability. On the other hand, if the blending amount of the (E) organic solvent exceeds 50 parts by weight, the viscosity becomes too low, causing sagging during application and the cured film becoming too thin. Therefore, the blending amount of the (E) organic solvent is preferably within the range of 15 to 45 parts by weight, and more preferably within the range of 20 to 40 parts by weight.

[0060] 6. (F) Colorants Furthermore, in order to improve the aesthetic and decorative properties of the photocurable gel nail composition of the present invention, a colorant can be blended as component (F). As the colorant (F), inorganic color pigments, organic color pigments, organic dyes, dyes, pearl pigments, glitter colorants, and the like that are generally used in cosmetics can be added. That is, preferred colorants include legal colorants (organic synthetic tar colorants) specified by the Ministry of Health, Labor and Welfare, as well as organic color pigments such as condensed azo pigments, diketopyrrolopyrrole pigments, perylene pigments, quinacridone pigments, isoindolinone pigments, dioxazine pigments, and phthalocyanine pigments, and inorganic color pigments such as titanium pigments and carbon black pigments. Examples of pearl pigments include natural pearls such as fish scale leaf, and synthetic pearl pigments such as metal oxide-coated mica, bismuth oxychloride, and basic lead carbonate. Examples of the glitter coloring agent include a metallic film obtained by depositing aluminum on a polyester film and providing a color layer thereon, and then cutting the film into a uniform shape. The amount of the colorant (F) to be added may be within a range that does not inhibit the photocuring speed, and may be, for example, within the range of 1 to 30 parts by weight per 100 parts by weight of the urethane acrylate resin (A).

[0061] 7. (G) Additives In addition, in the photocurable gel nail composition, at least one additive (G) selected from organic solvents, defoamers, leveling agents, ultraviolet absorbers, curing accelerators, fluorescent brighteners, pigment wetting agents, dispersants, flow adjusters, polymerization inhibitors, etc. may be blended for the purpose of adjusting the curability, viscosity, and applicability. The amount of these (G) additives to be added may be within a range that does not impair the curability or releasability of the present invention, and they can usually be used in a range of 0.1 to 10 parts by weight per 100 parts by weight of the (A) urethane acrylate resin.

[0062] 8.Viscosity It is also preferable that the viscosity of the photocurable gel nail composition of the present invention is within the range of 100 to 10,000 mPa s. When the viscosity of the photocurable gel nail composition is within this range, it is easy to handle and the coating thickness can be easily adjusted. Therefore, the viscosity of the photocurable gel nail composition is preferably set to a value within the range of 200 to 8000 mPa·s, and more preferably set to a value within the range of 300 to 5000 mPa·s. The viscosity of the photocurable gel nail was measured at 25°C using a B-type rotational viscometer (rotation speed: 60 rpm).

[0063] [Second embodiment] A second embodiment of the present invention is a gel nail method using a photocurable composition for gel nails, the gel nail method comprising the following steps (1) to (4): (1) A step of preparing a photocurable gel nail composition (2) A step of applying a photocurable gel nail composition to form a coating layer. (3) A process of photocuring the coating layer to form a cured film. (4) A process for peeling off the cured film after use The gel nail method according to the second embodiment of the present invention will be described in detail below with reference to Figs.

[0064] 1. Preparation process: Process (1) As shown in FIG. 1(a), a fingernail 10' is prepared as a substrate 10 on which a cured film is formed. At that time, if the surface of the nail of the finger 10' is dirty, it is preferable to clean it with a commercially available nail prep (Sofirah (registered trademark)) or the like. The substrate on which the cured film is formed is usually a natural nail, but may also be a synthetic plastic substrate such as an ABS or acrylic sheet. That is, by forming a cured film using the photocurable gel nail composition of the present invention on a synthetic plastic substrate such as an ABS sheet, it is possible to construct artificial nails or false nails.

[0065] Also, the photocurable composition for gel nails described in the first embodiment is prepared. That is, the photocurable gel nail composition can be prepared by known mixing methods. For example, a photocurable composition for gel nails can be prepared by uniformly mixing the ingredients using various mixing devices such as a propeller mixer, planetary mixer, bead mill, jet mill, three-roller mill, kneader, etc.

[0066] In addition, when carrying out the gel nail method of the second embodiment, it is also preferable to include a step of forming a cured film made of a colored photocurable gel nail composition containing a colorant (F) in order to form intermediate layer 16. The reason for this is that by carrying out the process in this manner, a three-dimensional effect can be imparted to the gel nail, and a color gel nail that is even more decorative and aesthetically pleasing can be obtained.

[0067] 2. Coating process: Process (2) Next, as shown in FIG. 1( b ), a photocurable composition for gel nails is applied onto the substrate (nail) 10 to form a coating layer 13 . Here, the method for applying the photocurable gel nail composition to the substrate (nail) 10 is not particularly limited, but for example, a brush, a spatula, a roller, a dropper, or the like can be used. The thickness of the coating layer 13 varies depending on the design, but is usually preferably in the range of 10 μm to 5 mm, more preferably in the range of 30 μm to 3 mm, and even more preferably in the range of 50 μm to 2 mm.

[0068] 3. Light curing process: Process (3) Next, as shown in FIG. 1( c ), the coating layer 13 is irradiated with ultraviolet light 14 a of a predetermined wavelength using an ultraviolet irradiator 14 to cure the photocurable composition for gel nails, thereby forming a cured film 20 . The cured film 20 may have a single-layer structure as shown in FIG. 1(c), or may have a multi-layer structure of two or more layers. For example, a three-layer structure in which a base layer 12 (base), an intermediate layer 16 (color), and a protective layer 18 (top) are laminated in this order from the substrate 10 side is preferable.

[0069] When forming such a three-layered cured film 20'', as shown in FIG. 2(b), a clear photocurable composition for gel nails is applied to the substrate 10, and then photocured by exposure to ultraviolet light to form a clear base layer 12 having a thickness of 100 to 1000 μm. Next, as shown in FIG. 2(c), a color photocurable composition for gel nails containing a colorant is applied onto the base layer 12, and then a predetermined amount of ultraviolet light is applied to photocure the composition, thereby forming an intermediate layer 16 having a thickness of 100 to 1000 μm. Furthermore, as shown in FIG. 2(d), a clear photocurable composition for gel nails is applied onto the intermediate layer 16, and then a predetermined amount of ultraviolet light is applied to photocure the composition, thereby forming a clear protective layer 18 having a thickness of 100 to 1000 μm. Therefore, in the multilayered cured film 20, the undercoat layer 12 provides excellent adhesion to the base material 10, which is a nail, the intermediate layer 16 containing a colorant provides excellent decorativeness, and the protective layer 18 can further increase the durability of the intermediate layer 16 etc. The photocurable gel nail composition of the present invention can be applied to each of the undercoat layer 12 (base), the intermediate layer 16 (color), and the protective layer 18 (top). In particular, when used in the undercoat layer (base), it can be applied as a photocurable gel nail composition that has even better handling, adhesion, and peelability.

[0070] In the above-mentioned photocuring step, the amount of ultraviolet light 14a irradiated onto the coating layer 13 is set to 300 to 800 mJ / cm 2 . 2 In the case where the cured film has a multi-layer structure of two or more layers, it is preferable to irradiate each layer with about the same amount of ultraviolet light. In the photocuring process, for example, a photocurable gel nail composition 12' applied to a substrate (nail) 10 is irradiated with a predetermined amount of UV-LED from a gel nail curing device 14 (e.g., a UV-LED curing device, 32 W, wavelength 405 nm) to photocure the composition, thereby forming a cured film 20 on the substrate (nail) 10.

[0071] 4. Peeling process: step (4) The peeling process is a process in which the cured film is wiped with a cloth or cotton soaked in a remover containing a solvent such as acetone, and the cured film is peeled off. If necessary, you can use a file to scrape off the hardened film to make it easier for the remover to penetrate. In addition, if the cured film is difficult to peel off, a method can also be applied in which a cloth or cotton soaked in remover is placed on the nail, and then aluminum foil cut to a size that will cover the fingertip is wrapped around the cotton so that it does not slip off from above the cured film, and after leaving it for several minutes (preferably within 5 minutes), the aluminum foil and cotton are removed, and the cured film, which has become easier to remove as the remover has permeated it, can be poked off with a wooden stick or pusher. EXAMPLES

[0072] The present invention will be described in detail below based on examples. However, the present invention is not limited to these examples without any particular reason.

[0073] [Example 1] 1. Preparation of photocurable gel nail composition The following components (A) to (E) were mixed in a container in the proportions shown in Table 1, and then mixed using a stirrer until uniform, to obtain a transparent photocurable gel nail composition. The viscosity of the obtained photocurable gel nail composition was 2000 mPa·s (measurement temperature: 25°C).

[0074] (A) Urethane acrylate resin (a1-1) Urethane acrylate resin (7 functional groups, weight average molecular weight 5000) (a1-2) Urethane acrylate resin (weight average molecular weight 15,000) (a2) Urethane acrylate resin (weight average molecular weight 3000) (B) Cellulose-based resin (b1) Cellulose acetate butyrate resin (Number average molecular weight 6000, Tg 75℃, hydroxyl value 50mgKOH / g) (C) (Meth)acrylate Monomer (c1) 2-Hydroxypropyl methacrylate (c2) Isobornyl acrylate (c3) 2-Hydroxyethyl methacrylate (c4) dipentaerythritol hexaacrylate (D) Photopolymerization initiator (d1) 1-Hydroxy-cyclohexyl-phenyl-ketone (d2) Diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (E) Organic Solvents (e1) Butyl acetate (e2) Ethyl acetate

[0075] 2. Evaluation of photocurable gel nail compositions (1) Photocurable The photocurable composition for gel nails was applied to a nail as a substrate using a brush for gel nails to form a coating layer having a thickness of 0.1 mm. Next, the formed coating layer was irradiated with ultraviolet light at 400 mJ / cm using a gel nail UV device. 2 During the process of irradiating the coating layer and photocuring it to obtain a single-layer cured film, the photocurability of the photocurable composition for gel nails was evaluated according to the following criteria. The results are shown in Table 1. ◎: Tackle-free after 15 seconds of exposure. ○: Tackless after 30 seconds of exposure. △: A slight tackiness remained after 30 seconds of irradiation. ×: Uncured even after 30 seconds of irradiation.

[0076] (2) Adhesion 1 (resistance to external forces) The adhesion of the single-layer cured film formed on the nail as a substrate by photocuring the photocurable composition for gel nail was evaluated by carrying out a nail scratch test. That is, the nail on which the cured film was formed was scratched 10 times with another nail, and the change in appearance was evaluated according to the following criteria. The results are shown in Table 1. ⊚: There is no change in appearance between the cured film and the nail. A: Slight peeling was observed between the cured film and the nail. Δ: Partial peeling was observed between the cured film and the nail, and partial whitening was observed in appearance. ×: Significant peeling was observed between the cured film and the nail, and whitening was observed overall in appearance.

[0077] (3) Adhesion 2 (warm water resistance) The adhesion of a single-layer cured film formed on a nail as a substrate by photocuring the photocurable composition for gel nails was evaluated by hand washing with warm water at about 25°C. That is, hands with a cured film formed on the nails were washed with warm water (about 25°C) without using soap or the like, and then wiped with a towel-like material 20 times a day, and after continuing this for three days, the change in appearance was evaluated according to the following criteria. The results are shown in Table 1. ⊚: There is no change in the appearance of the cured film and the nail even after more than 3 days have passed. ○: Slight peeling was observed between the cured film and the nail within 3 days. Δ: Within one day, partial peeling was observed between the cured film and the nail, and partial whitening was observed in the appearance. ×: Within one day, significant peeling was observed between the cured film and the nail, and overall whitening was observed in appearance.

[0078] (4) Peelability The photocurable composition for gel nails was photocured to form a single-layer cured film on the nail as a substrate. The film was rubbed with an acetone-based remover (Sofirah (registered trademark)) to evaluate the peelability according to the following criteria. The results are shown in Table 1. ⊚: The cured film could be peeled off and removed with friction for less than 5 minutes. ◯: The cured film can be peeled off and removed with friction for less than 5 to 10 minutes. △: The cured film can be peeled off and removed with friction for less than 10 to 15 minutes. ×: The cured film could not be peeled off even after rubbing for 15 minutes or more.

[0079] [Examples 2 to 5, Comparative Examples 1 to 2] In Examples 2 to 5 and Comparative Examples 1 and 2, photocurable compositions for gel nails were obtained in the same manner as in Example 1, except that the compounding ratios of components (A) to (E) were changed as shown in Table 1, and the compositions were photocured to evaluate the photocurability, etc.

[0080] [Table 1]

[0081] [Examples 6 to 8, Comparative Examples 3 to 4] In Examples 6 to 8 and Comparative Examples 3 and 4, the cured film had a multilayer structure consisting of an underlayer and an intermediate protective layer as shown in Table 2, and the photocurability and other properties were evaluated in the same manner as in Example 1. The obtained evaluation results are shown in Table 2. That is, in the first step, a photocurable composition for gel nails having the same composition as in Examples 1, 2, and 5 and Comparative Examples 1 and 2 was applied to a nail as a substrate, and then photocured to form a base layer. Next, in the second step, a color photocurable gel nail composition was applied onto the base layer, the color photocurable gel nail composition being the same as that in Example 1 and Comparative Example 2, and containing 20 parts by weight of a perylene-based red pigment (Pigment Red 149) as a colorant (F), and then photocured to form an intermediate layer. Next, in the third step, a photocurable composition for gel nails similar to those in Examples 1, 3, and 4 and Comparative Examples 1 and 2 was applied onto the intermediate layer, and then photocured to form a protective layer. In Table 2, if the composition of the photocurable gel nail composition forming each layer is the same as in Examples 1 to 5, it is indicated as Compositions 1 to 5. If the composition is the same as in Comparative Examples 1 and 2, it is indicated as Compositions 6 and 7. If a colorant is included, this is also indicated.

[0082] [Table 2] [Industrial Applicability]

[0083] According to the photocurable gel nail composition of the present invention, by blending a specified urethane acrylate resin and a specified cellulose-based resin in a specified ratio, the gel nail is easy to apply, has excellent curing properties, and can be easily peeled off after use. In particular, when peeling off after use, not only a single-layered cured film but also a multi-layered cured film can be easily peeled off, so that the peeling process can be completed in a short time. Therefore, the photocurable gel nail composition of the present invention and the gel nail method using the same can be suitably used not only for natural nails, but also for artificial nails and false nails. [Explanation of symbols]

[0084] 10: Base material (claw) 10´:Finger 12: Base layer 13: Coating layer 14: Gel nail hardener (ultraviolet light device) 14a: Radiation (ultraviolet rays) 16: Middle class 18 :Protective layer 20: Single layer cured film 20´: Multi-layered (2-layer) hardened film 20´´: Multi-layered (3-layer) hardened film

Claims

1. A photocurable composition for gel nails (excluding di[hydroxyethyltrimethacrylic]trimethylhexyldicarbamate in an amount of 40% by mass to 60% by mass of the total amount), comprising (A) a urethane acrylate resin, (B) a cellulose-based resin, (C) a (meth)acrylate monomer component, and (D) a photopolymerization initiator, Relative to 100 parts by weight of the urethane acrylate resin (A), The content of the (B) cellulose-based resin is set to a value within a range of 25 to 75 parts by weight, The content of the (C) component is set to a value within a range of 90 to 150 parts by weight, The content of the (D) component is set to a value within a range of 10 to 50 parts by weight, the (A) urethane acrylate resin contains a first urethane acrylate resin (a1) and a second urethane acrylate resin (a2) as two types of urethane acrylate resins having different weight average molecular weights, and when the total amount of the first urethane acrylate resin (a1) and the second urethane acrylate resin (a2) is taken as 100% by weight, the first urethane acrylate resin (a1) has a value within a range of 60 to 99% by weight and the second urethane acrylate resin (a2) has a value within a range of 1 to 40% by weight, and (B) a number average molecular weight of the cellulose-based resin is within a range of 1,000 to 50,000.

2. The photocurable gel nail composition as described in claim 1, characterized in that the at least two types of urethane acrylate resins having different weight average molecular weights are a urethane acrylate resin (a1) having a weight average molecular weight in the range of 500 to 30,000, and a urethane acrylate resin (a2) having a weight average molecular weight of less than 5,000.

3. 3. The photocurable composition for gel nails according to claim 1, wherein the cellulose-based resin (B) is a cellulose acetate butyrate resin, a cellulose acetate propionate resin, or either one of them.

4. The photocurable gel nail composition according to any one of claims 1 to 3, characterized in that the (C) (meth)acrylate monomer component is one or more selected from the group consisting of isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and dipentaerythritol hexaacrylate.

5. The photocurable gel nail composition according to any one of claims 1 to 4, characterized in that the (D) photopolymerization initiator is one or more selected from the group consisting of α-hydroxyketone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators.

6. The photocurable gel nail composition described in any one of claims 1 to 5, characterized in that the photocurable gel nail composition further contains an organic solvent as component (E), and the content of the organic solvent is within the range of 10 to 50 parts by weight per 100 parts by weight of the urethane acrylate resin (A).

7. The photocurable composition for gel nails according to claim 6, characterized in that the (E) organic solvent is one or more selected from the group consisting of ethyl acetate, propyl acetate, butyl acetate, and isobutyl acetate.

8. A gel nail method using a photocurable gel nail composition described in any one of claims 1 to 7, comprising the following steps (1) to (4). (1) A step of preparing the photocurable gel nail composition (2) A step of applying the photocurable gel nail composition to form a coating layer. (3) A step of photocuring the coating layer to form a cured film. (4) A step of rubbing and peeling off the cured film after use with a remover.

Citation Information

Patent Citations

  • Replaceable volatile solvent based phototherapy nail polish and preparation method thereof

    CN108434019A

  • Composition for removable gel application for nails, and method for using the same

    JP2011032259A

  • Photocuring type primer for manicure (gel nail) and manicuring (gel nail) method

    JP2013043853A

  • Gel nail polishes as well as methods of their production and use

    JP2017061446A

  • Gel Polish Composition

    JP2017535512A