Double-sided adhesive tape

The double-sided adhesive tape achieves both heat resistance and flexibility by optimizing the storage modulus ratio and compressive strength, addressing shrinkage issues and enhancing adhesion on complex surfaces.

JP7579081B2Active Publication Date: 2024-11-07SEKISUI CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020133976
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-09
Filing Date
2020-08-06
Publication Date
2024-11-07
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

Conventional double-sided adhesive tapes with foam base materials face challenges in balancing heat resistance and flexibility, leading to issues with shrinkage and adhesion on non-flat surfaces, especially in high-temperature environments, which affect the performance of electronic devices.

Method used

A double-sided adhesive tape with a foam base material and adhesive layers on both sides, characterized by a specific storage modulus ratio (G'(110°C)/G'(90°C) of 0.4 or more, a compressive strength of 400 kPa or less, and a thickness of 0.6 mm or less, utilizing a resin composition that includes polypropylene and elastomer resins to enhance heat resistance and flexibility.

Benefits of technology

The adhesive tape exhibits excellent heat resistance up to 100°C without shrinking and can be easily applied to non-flat surfaces, improving work efficiency and preventing display or light unevenness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579081000002
    Figure 0007579081000002
  • Figure 0007579081000001
    Figure 0007579081000001
Patent Text Reader

Abstract

To provide a double-sided adhesive tape having heat resistance and flexibility.SOLUTION: The double-sided adhesive tape includes a foam substrate and adhesive layers on both surfaces of the foam substrate. The double-sided adhesive tape has a ratio (G'(110°C) / G'(90°C)) of the storage modulus G'(110°C) at 110°C to the storage modulus G'(90°C) at 90°C of 0.4 or more and a 25% compressive strength at -30°C measured according to JIS K 6254 of 400 kPa or less. The thickness of the double-sided adhesive tape is 0.6 mm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a double-sided pressure-sensitive adhesive tape. [Background technology]

[0002] In the assembly of portable electronic devices such as mobile phones and personal digital assistants (PDAs), double-sided adhesive tapes are used (for example, Patent Documents 1 and 2). Double-sided adhesive tapes are also used to fix in-vehicle electronic device components, such as in-vehicle panels, to the vehicle body. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-242541 A [Patent Document 2] JP 2009-258274 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, portable electronic devices, in-vehicle electronic devices, etc., tend to have more complex shapes as their functionality increases, and so double-sided adhesive tapes are often used by attaching them to steps, corners, non-flat surfaces (curved surfaces), etc. In order to provide excellent conformability to such steps, corners, non-flat surfaces (curved surfaces), etc., double-sided adhesive tapes using a foam substrate are used. On the other hand, in recent in-vehicle electronic devices, for example, displays are sometimes installed at high positions exposed to direct sunlight in order to improve the driver's visibility. In such installation locations, the temperature can reach 100°C or higher, and double-sided adhesive tapes are required to have excellent heat resistance so that they do not shrink even in such high-temperature environments in order to prevent peeling. In addition, when double-sided adhesive tapes are used to fix display units or light source peripheries, the thermal shrinkage of the tape can lead to uneven display and uneven light. In order to prevent this, not only a low thermal shrinkage rate but also a low absolute value of shrinkage is required. From the viewpoint of suppressing the amount of shrinkage in the thickness direction, a thinner double-sided adhesive tape is required. However, in the case of double-sided adhesive tapes using conventional foam substrates, for example, if a foam substrate made of a polypropylene-based resin is used, the heat resistance is improved, but there is a problem that the flexibility is reduced. Double-sided adhesive tapes with poor flexibility are difficult to press, especially on non-flat surfaces (curved surfaces), and require long periods of pressing to adhere sufficiently.

[0005] In view of the above-mentioned circumstances, an object of the present invention is to provide a double-sided pressure-sensitive adhesive tape that has heat resistance and flexibility. [Means for solving the problem]

[0006] The present invention is a double-sided pressure-sensitive adhesive tape having a foam substrate and pressure-sensitive adhesive layers on both sides of the foam substrate, the double-sided pressure-sensitive adhesive tape having a ratio of storage modulus G'(110°C) at 110°C to storage modulus G'(90°C) at 90°C (G'(110°C) / G'(90°C)) of 0.4 or more, a 25% compressive strength at -30°C measured in accordance with JIS K 6254 of 400 kPa or less, and a thickness of 0.6 mm or less. The present invention will be described in detail below.

[0007] The double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention has a ratio (G'(110°C) / G'(90°C)) of the storage modulus G'(110°C) at 110°C to the storage modulus G'(90°C) at 90°C of 0.4 or more. By having the ratio (G'(110°C) / G'(90°C)) of 0.4 or more, the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention can exhibit excellent heat resistance, for example, not shrinking even when used in an environment where it is exposed to direct sunlight and the temperature becomes high at 100°C or more. From the viewpoint of improving heat resistance, the ratio (G'(110°C) / G'(90°C)) is preferably 0.45 or more, more preferably 0.50 or more. The upper limit of the ratio (G'(110°C) / G'(90°C)) is not particularly limited, but is substantially 1.5.

[0008] In the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention, the storage modulus G'(90°C) has a preferred lower limit of 70,000 Pa and a preferred upper limit of 350,000 Pa. When the storage modulus G'(90°C) is within this range, it is easy to adjust the value of G'(110°C) / G'(90°C) to a preferred range. From the same viewpoint, the more preferred lower limit of the storage modulus G'(90°C) is 100,000 Pa and the more preferred upper limit is 300,000 Pa. The storage modulus G' (90°C) can be adjusted by increasing the amount of polypropylene-based resin in the foamed base material, increasing the molecular weight of the propylene-based resin, increasing the propylene content of the elastomer-based resin, increasing the cyclic structure content of the elastomer-based resin, or the like.

[0009] In the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention, the storage modulus G'(110°C) has a preferred lower limit of 70,000 Pa and a preferred upper limit of 250,000 Pa. By setting the storage modulus G'(110°C) within this range, it is easy to adjust the value of G'(110°C) / G'(90°C) to a preferred range. The storage modulus G'(110°C) is more preferably set to a lower limit of 75,000 Pa and a more preferred upper limit of 200,000 Pa. The storage modulus G' (110°C) can be adjusted by increasing the amount of polypropylene resin in the foamed base material, increasing the molecular weight of the propylene resin, increasing the propylene content of the elastomer resin, increasing the cyclic structure content of the elastomer resin, or the like.

[0010] The storage modulus G'(90°C) and storage modulus G'(110°C) can be measured using a dynamic viscoelasticity measuring device (e.g., DVA-200 manufactured by IT Measurement & Control Co., Ltd.) at a frequency of 10 Hz and a heating rate of 3°C / min from -40°C to 140°C, and reading the storage modulus G' at 90°C and 110°C.

[0011] The double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention has a 25% compressive strength of 400 kPa or less at -30°C measured in accordance with JIS K 6254. The double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention can exhibit high flexibility by being affixed to, for example, a non-flat surface (curved surface) by short-time pressure bonding, improving workability. The 25% compressive strength at -30°C is preferably 300 kPa or less, more preferably 200 kPa or less. The lower limit of the 25% compressive strength at -30°C is not particularly limited, but is substantially 80 kPa. The above-mentioned 25% compressive strength at -30°C can be adjusted by increasing the ratio of the foam base material thickness to the tape thickness, increasing the foaming ratio, adjusting the blending balance of the polypropylene-based resin and the elastomer-based resin to an appropriate range, and so on.

[0012] In the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention, the 25% compressive strength at 23° C. measured in accordance with JIS K 6254 is preferably 75 kPa at the lower limit and 250 kPa at the upper limit. When the 25% compressive strength at 23° C. is within this range, the flexibility and stress relaxation properties of the foam substrate are increased, and peeling during use is less likely to occur. The more preferred lower limit of the 25% compressive strength at 23° C. is 80 kPa, and the more preferred upper limit is 220 kPa. The 25% compressive strength at 23° C. can be adjusted by reducing the amount of polypropylene resin in the foam base material, increasing the amount of elastomer resin, increasing the foaming ratio, or the like.

[0013] The double-sided adhesive tape according to one embodiment of the present invention has a tensile modulus in the MD direction of 10 N / mm 2 The tensile elongation at break is preferably 150% or more, which allows the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention to exhibit higher flexibility. The tensile modulus is 15N / mm 2 More preferably, it is 25N / mm 2 The upper limit of the tensile elastic modulus is not particularly limited, but is preferably 150 N / mm 2 is a substantial upper limit. The tensile elongation at break is more preferably 200% or more, and further preferably 300% or more. The upper limit of the tensile elongation at break is not particularly limited, but 560% is a preferred upper limit. The tensile modulus and tensile elongation at break can be measured by a method according to JIS K 7161. The tensile modulus and tensile elongation at break in the MD direction can be adjusted by adjusting the degree of crosslinking to an appropriate range, adjusting the blending balance of the polypropylene resin and the elastomer resin to an appropriate range, or the like. In this specification, "MD" means machine direction and refers to a direction that coincides with the extrusion direction of the polyolefin resin foam sheet, etc., and "TD" means transverse direction and refers to a direction perpendicular to MD and parallel to the foam sheet.

[0014] The thickness of the double-sided adhesive tape according to one embodiment of the present invention is 0.6 mm or less. By having the double-sided adhesive tape have a thickness of 0.6 mm or less, not only can the thermal shrinkage rate be low, but also the absolute value of shrinkage in the thickness direction can be low when fixing the periphery of a display or the periphery of a light source, and display unevenness can be suppressed and the double-sided adhesive tape can be suitably used. In the present invention, by adjusting the above ratio (G'(110°C) / G'(90°C)) and the above 25% compressive strength at -30°C to the desired range, it is possible to achieve both excellent heat resistance and flexibility in a double-sided adhesive tape having a thickness of 0.6 mm or less. From the viewpoint of using the double-sided adhesive tape without display unevenness or light unevenness, the thickness of the double-sided adhesive tape according to one embodiment of the present invention is preferably 0.5 mm or less, more preferably 0.4 mm or less. The lower limit of the thickness of the double-sided adhesive tape according to one embodiment of the present invention is not particularly limited, but is preferably 0.1 mm or more, more preferably 0.2 mm or more.

[0015] A double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention comprises a foam substrate and pressure-sensitive adhesive layers on both sides of the foam substrate. By adjusting the resin composition constituting the foam base material and also adjusting the structure of the foam base material, it is possible to adjust the above ratio (G'(110°C) / G'(90°C)) and the above 25% compressive strength at -30°C to within the desired range, thereby achieving both excellent heat resistance and flexibility.

[0016] The resin constituting the foam base material is not particularly limited, and examples thereof include polyolefin resins, polyurethane resins, elastomer resins, acrylic resins, etc. Among them, a mixed resin containing a polypropylene resin and an elastomer resin is preferred because it is easy to adjust the ratio (G'(110°C) / G'(90°C)) and the 25% compressive strength at -30°C to the desired range.

[0017] The polypropylene resin is not particularly limited, and examples thereof include propylene homopolymers (homopolypropylenes) and copolymers of propylene and other olefins. These polypropylene resins may be used alone or in combination of two or more kinds.

[0018] The copolymer of propylene with another olefin may be any of a block copolymer, a random copolymer, and a random block copolymer, but a random copolymer (random polypropylene) is preferred. Examples of other olefins that can be copolymerized with propylene include α-olefins such as ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, and 1-decene. Of these, ethylene is preferred. When a copolymer of propylene and another olefin is used as the polypropylene-based resin, the lower limit of the propylene content in the copolymer is preferably 90% by weight, the upper limit is preferably 99.5% by weight, the more preferable lower limit is 95% by weight, and the more preferable upper limit is 99% by weight.

[0019] The elastomer resin is not particularly limited, and examples thereof include olefin rubber, acrylic rubber, urethane rubber, silicone rubber, ester rubber, etc. These elastomer resins may be used alone or in combination of two or more. Among them, olefin rubber is preferable because it has excellent compatibility with the polypropylene resin.

[0020] The olefin-based rubber is preferably an amorphous or low-crystalline rubber-like substance in which two or more olefin-based monomers are substantially randomly copolymerized. More specifically, from the viewpoint of improving moldability and flexibility in a balanced manner, ethylene-α-olefin-based copolymer rubber is preferred. The above-mentioned α-olefins include α-olefins having 3 to 15 carbon atoms, such as propylene, 1-butene, 2-methylpropylene, 3-methyl-1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene. These α-olefins may be used alone or in combination of two or more. Among them, α-olefins having 3 to 10 carbon atoms are preferred, propylene and 1-butene are more preferred, and propylene is even more preferred.

[0021] The ethylene-α-olefin copolymer rubber may contain other monomer units in addition to the ethylene units and the α-olefin units. Examples of the monomer that forms the other monomer unit include conjugated dienes having 4 to 8 carbon atoms, non-conjugated dienes having 5 to 15 carbon atoms, vinyl ester compounds, unsaturated carboxylic acid esters, and unsaturated carboxylic acids. Examples of the conjugated dienes having 4 to 8 carbon atoms include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. Examples of the non-conjugated dienes having 5 to 15 carbon atoms include dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-dicyclooctadiene, 7-methyl-1,6-octadiene, and 5-vinyl-2-norbornene. The vinyl ester compound includes vinyl acetate and the like. Examples of the unsaturated carboxylate include methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate. Examples of the unsaturated carboxylic acid include acrylic acid and methacrylic acid. These monomers may be used alone or in combination of two or more. Among them, non-conjugated dienes having 5 to 15 carbon atoms are preferred, and from the viewpoint of availability, 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene (DCPD) are more preferred, and DCPD is even more preferred.

[0022] The ethylene unit content in the ethylene-α-olefin copolymer rubber is preferably 30% by weight at its lower limit and 85% by weight at its upper limit. By setting the ethylene unit content in the ethylene-α-olefin copolymer rubber within the above range, the storage modulus G' can be adjusted, and excellent heat resistance and flexibility can be achieved at the same time. The ethylene unit content in the ethylene-α-olefin copolymer rubber is more preferably 40% by weight at its lower limit and 80% by weight at its upper limit, still more preferably 45% by weight at its lower limit and 75% by weight at its upper limit. The preferred lower limit of the content of the α-olefin unit in the ethylene-α-olefin copolymer rubber is 10% by weight, and the preferred upper limit is 60% by weight. By setting the content of the α-olefin unit in the ethylene-α-olefin copolymer rubber within the above range, the storage modulus G' can be adjusted, and excellent heat resistance and flexibility can be achieved at the same time. The more preferred lower limit of the content of the α-olefin unit in the ethylene-α-olefin copolymer rubber is 15% by weight, and the more preferred upper limit is 50% by weight. Furthermore, the preferred lower limit of the content of other monomer units such as non-conjugated dienes in the ethylene-α-olefin copolymer rubber is 0% by weight, and the preferred upper limit is 20% by weight. By setting the content of other monomer units such as non-conjugated dienes in the ethylene-α-olefin copolymer rubber within the above range, the storage modulus G' can be adjusted, and excellent heat resistance and flexibility can be achieved at the same time. The more preferred lower limit of the content of other monomer units such as non-conjugated dienes in the ethylene-α-olefin copolymer rubber is 1% by weight, and the more preferred upper limit is 10% by weight.

[0023] Specific examples of the ethylene-α-olefin copolymer rubber include ethylene-propylene copolymer rubber (EPR), ethylene-propylene-diene copolymer rubber (EPDM) such as ethylene-propylene-5-ethylidene-2-norbornene copolymer rubber, and ethylene-propylene-dicyclopentadiene copolymer rubber.

[0024] As the olefin-based rubber, an olefin-based thermoplastic elastomer (TPO) can also be used. The olefin-based thermoplastic elastomer (TPO) has a polyolefin such as polyethylene or polypropylene as a hard segment and a rubber component such as EPM or EPDM as a soft segment. The olefin-based thermoplastic elastomer (TPO) can be any of a blend type, a dynamic crosslinking type, and a polymerization type.

[0025] When the foam base material is made of a mixed resin containing a polypropylene-based resin and an elastomer-based resin, the mixed resin may further contain other resins in addition to the polypropylene-based resin and the elastomer-based resin. The other resin is not particularly limited, but for example, a polyolefin resin other than a polypropylene resin, such as a polyethylene resin, such as an ethylene-propylene copolymer having ethylene as a main component, is preferable.

[0026] When the foam base material is made of a mixed resin containing a polypropylene resin and an elastomer resin, the preferred lower limit of the content of the polypropylene resin in the mixed resin is 30% by weight, and the preferred upper limit is 60% by weight, and the preferred lower limit of the content of the elastomer resin is 25% by weight, and the preferred upper limit is 50% by weight. By including the polypropylene resin and the elastomer resin within this range, the ratio (G'(90°C) / G'(110°C)) and the 25% compressive strength can be particularly easily adjusted to the desired range. The more preferred lower limit of the content of the polypropylene resin in the mixed resin is 35% by weight, and the more preferred upper limit is 50% by weight, and the more preferred lower limit of the content of the elastomer resin is 30% by weight, and the more preferred upper limit is 40% by weight.

[0027] The expansion ratio of the foam base material is not particularly limited, but the preferred lower limit is 2 cm 3 / g, with a preferred upper limit of 10 cm 3By setting the expansion ratio of the foam substrate within this range, the double-sided pressure-sensitive adhesive tape can exhibit excellent flexibility while maintaining its strength. From the viewpoint of the strength and flexibility of the double-sided pressure-sensitive adhesive tape, a more preferable lower limit of the expansion ratio is 3 cm. 3 / g, and a more preferable upper limit is 8 cm 3 / g, and a more preferable lower limit is 5 cm 3 / g, and a more preferable upper limit is 7 cm 3 / g. The expansion ratio can be calculated as the reciprocal of the density measured in accordance with JIS K 6767 using an electronic specific gravity meter (for example, "ED120T" manufactured by Mirage).

[0028] The thickness of the foam substrate is not particularly limited, but the preferred lower limit is 0.05 mm, and the preferred upper limit is 0.55 mm. By setting the thickness of the foam substrate within this range, the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention can be suitably used for fixing portable electronic device parts, in-vehicle electronic device parts, etc. From the viewpoint of being more suitably used for fixing the above-mentioned parts, the more preferred lower limit of the thickness of the foam substrate is 0.06 mm, the more preferred upper limit is 0.5 mm, the even more preferred lower limit is 0.08 mm, and the even more preferred upper limit is 0.45 mm.

[0029] The pressure-sensitive adhesive layers on both sides of the foam substrate (hereinafter, both layers may be simply referred to as "pressure-sensitive adhesive layers") may have the same composition or different compositions. The pressure-sensitive adhesive layer is not particularly limited, and examples thereof include an acrylic pressure-sensitive adhesive layer, a rubber pressure-sensitive adhesive layer, a urethane pressure-sensitive adhesive layer, a silicone pressure-sensitive adhesive layer, etc. Among these, an acrylic pressure-sensitive adhesive layer containing an acrylic copolymer is preferred because it is relatively stable against light, heat, moisture, etc. and can adhere to various adherends (low adherend selectivity).

[0030] The acrylic copolymer constituting the acrylic pressure-sensitive adhesive layer is preferably obtained by copolymerizing a monomer mixture containing butyl acrylate and / or 2-ethylhexyl acrylate, since the initial tack is improved and the layer can be applied to a non-flat surface (curved surface) by pressure bonding in a short time, and more preferably obtained by copolymerizing a monomer mixture containing butyl acrylate and 2-ethylhexyl acrylate. The preferred lower limit of the content of the butyl acrylate in the total monomer mixture is 40% by weight, and the preferred upper limit is 80% by weight. By keeping the content of the butyl acrylate within this range, it is possible to achieve both high adhesive strength and tackiness. The content of the 2-ethylhexyl acrylate in the total monomer mixture is preferably 10% by weight at the lower limit, 100% by weight at the upper limit, 30% by weight at the more preferred lower limit, 80% by weight at the more preferred upper limit, 50% by weight at the still more preferred upper limit, 60% by weight at the more preferred upper limit. By keeping the content of the 2-ethylhexyl acrylate within this range, high adhesive strength can be exhibited.

[0031] The monomer mixture may contain other copolymerizable polymerizable monomers other than butyl acrylate and 2-ethylhexyl acrylate as necessary. Examples of the other copolymerizable polymerizable monomers include (meth)acrylic acid alkyl esters having an alkyl group with 1 to 3 carbon atoms, (meth)acrylic acid alkyl esters having an alkyl group with 13 to 18 carbon atoms, and functional monomers. Examples of the (meth)acrylic acid alkyl ester in which the alkyl group has 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of the (meth)acrylic acid alkyl ester having an alkyl group of 13 to 18 carbon atoms include tridecyl methacrylate and stearyl (meth)acrylate. Examples of the functional monomer include hydroxyalkyl (meth)acrylate, glycerin dimethacrylate, glycidyl (meth)acrylate, 2-methacryloyloxyethyl isocyanate, (meth)acrylic acid, itaconic acid, maleic anhydride, crotonic acid, maleic acid, and fumaric acid.

[0032] To obtain the acrylic copolymer by copolymerizing the monomer mixture, the monomer mixture may be subjected to a radical reaction in the presence of a polymerization initiator. As a method for radically reacting the monomer mixture, i.e., a polymerization method, a conventionally known method may be used, such as solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc.

[0033] The weight average molecular weight (Mw) of the acrylic copolymer is preferably 400,000 at the lower limit and 1,500,000 at the upper limit. By setting the weight average molecular weight of the acrylic copolymer within this range, high adhesive strength can be exhibited. From the viewpoint of further improving adhesive strength, the weight average molecular weight is more preferably 500,000 at the lower limit and 1,400,000 at the upper limit. The weight average molecular weight (Mw) is the weight average molecular weight calculated using standard polystyrene standards by GPC (gel permeation chromatography).

[0034] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the acrylic copolymer is preferably 10.0 at the upper limit. If Mw / Mn is 10.0 or less, the proportion of low molecular weight components is suppressed, and the pressure-sensitive adhesive layer is prevented from softening at high temperatures, resulting in a decrease in bulk strength and a decrease in adhesive strength. From the same viewpoint, the upper limit of Mw / Mn is more preferably 5.0, even more preferably 3.0, and usually 1.0 or more.

[0035] The pressure-sensitive adhesive layer may contain a tackifier resin. Examples of the tackifier resin include rosin ester resins, hydrogenated rosin resins, terpene resins, terpene phenol resins, coumarone-indene resins, alicyclic saturated hydrocarbon resins, C5 petroleum resins, C9 petroleum resins, C5-C9 copolymer petroleum resins, etc. These tackifier resins may be used alone or in combination of two or more.

[0036] The content of the tackifier resin is not particularly limited, but a preferred lower limit is 10 parts by weight and a preferred upper limit is 60 parts by weight relative to 100 parts by weight of the resin (e.g., acrylic copolymer) that is the main component of the adhesive layer. When the content of the tackifier resin is 10 parts by weight or more, the adhesive strength of the adhesive layer can be suppressed from decreasing. When the content of the tackifier resin is 60 parts by weight or less, the adhesive layer can be prevented from hardening and thus reducing its adhesive strength or tackiness.

[0037] The pressure-sensitive adhesive layer preferably has a crosslinked structure formed between the main chains of the resins (e.g., the acrylic copolymer, the tackifier resin, etc.) constituting the pressure-sensitive adhesive layer by adding a crosslinking agent. The crosslinking agent is not particularly limited, and examples thereof include isocyanate-based crosslinking agents, aziridine-based crosslinking agents, epoxy-based crosslinking agents, metal chelate-based crosslinking agents, etc. Among them, isocyanate-based crosslinking agents are preferred. By adding an isocyanate-based crosslinking agent to the pressure-sensitive adhesive layer, the isocyanate group of the isocyanate-based crosslinking agent reacts with the alcoholic hydroxyl group in the resins (e.g., the acrylic copolymer, the tackifier resin, etc.) constituting the pressure-sensitive adhesive layer, and the crosslinking of the pressure-sensitive adhesive layer becomes loose. Therefore, the pressure-sensitive adhesive layer can disperse the peel stress applied intermittently, and the adhesive strength of the double-sided pressure-sensitive adhesive tape is further improved. The amount of the crosslinking agent added is preferably 0.01 to 10 parts by weight, and more preferably 0.1 to 7 parts by weight, per 100 parts by weight of the resin (for example, the acrylic copolymer) that is the main component of the pressure-sensitive adhesive layer.

[0038] The pressure-sensitive adhesive layer may contain a silane coupling agent for the purpose of improving adhesive strength. The silane coupling agent is not particularly limited, and examples thereof include epoxy silanes, acrylic silanes, methacrylic silanes, amino silanes, and isocyanate silanes.

[0039] The pressure-sensitive adhesive layer may contain a coloring material for the purpose of imparting light-shielding properties. The coloring material is not particularly limited, and examples thereof include carbon black, aniline black, titanium oxide, etc. Among these, carbon black is preferred because it is relatively inexpensive and chemically stable. The pressure-sensitive adhesive layer may contain conventionally known fine particles and additives, such as inorganic fine particles, conductive fine particles, antioxidants, foaming agents, organic fillers, and inorganic fillers, as required.

[0040] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but the preferred lower limit of the thickness of the pressure-sensitive adhesive layer on one side is 0.01 mm, and the preferred upper limit is 0.1 mm. By setting the thickness of the pressure-sensitive adhesive layer within this range, the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention can be suitably used for fixing portable electronic device parts, in-vehicle electronic device parts, etc. From the viewpoint of being more suitably used for fixing the above parts, etc., the more preferred lower limit of the thickness of the pressure-sensitive adhesive layer is 0.015 mm, and the more preferred upper limit is 0.09 mm.

[0041] The double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention may, if necessary, have layers other than the foam substrate and the pressure-sensitive adhesive layer.

[0042] An example of a method for producing the double-sided pressure-sensitive adhesive tape according to an embodiment of the present invention is as follows. First, a solution of adhesive A that constitutes the adhesive layer is prepared, and this solution of adhesive A is applied to the surface of the foam substrate, and the solvent in the solution is completely dried and removed to form the adhesive layer A. Next, a release film is superimposed on the formed adhesive layer A with its release-treated surface facing the adhesive layer A. Next, a release film different from the above release film is prepared, a solution of adhesive B is applied to the release-treated surface of this release film, and the solvent in the solution is completely dried and removed to produce a laminated film in which adhesive layer B is formed on the surface of the release film. The obtained laminated film is superimposed on the back surface of the foam substrate on which adhesive layer A is formed, with adhesive layer B facing the back surface of the substrate to produce a laminate. Then, by pressing the above laminate with a rubber roller or the like, a double-sided adhesive tape can be obtained that has adhesive layers on both sides of the foam substrate and in which the surface of the adhesive layer is covered with a release film.

[0043] Alternatively, two sets of laminate films can be prepared in a similar manner, and these laminate films are laminated on either side of a substrate with the adhesive layer of the laminate film facing the foam substrate to produce a laminate, and the laminate is then pressed with a rubber roller or the like to produce a double-sided adhesive tape.

[0044] The double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention exhibits high heat resistance and does not shrink even when placed in a position exposed to direct sunlight and exposed to high temperatures of 100° C. or more. In addition, since the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention has excellent flexibility, it can be applied to, for example, non-flat surfaces (curved surfaces) by pressure bonding in a short time, improving workability.

[0045] The use of the double-sided pressure-sensitive adhesive tape according to one embodiment of the present invention is not particularly limited, and it is used, for example, for fixing portable electronic device parts, in-vehicle electronic device parts, etc. Among them, it is particularly suitable for fixing in-vehicle electronic device parts. The shape of the double-sided pressure-sensitive adhesive tape according to an embodiment of the present invention for these applications is not particularly limited, but examples include a rectangular shape, a picture frame shape, a circular shape, an oval shape, a doughnut shape, and the like.

[0046] Examples of articles in which the double-sided pressure-sensitive adhesive tape according to an embodiment of the present invention can be used include flat panel displays used in TVs, monitors, portable electronic devices, etc., camera modules for portable electronic devices, internal components for portable electronic devices, interiors for vehicles, interiors and exteriors of home appliances (e.g., TVs, air conditioners, refrigerators, etc.), etc. Examples of adherends to which the double-sided pressure-sensitive adhesive tape according to an embodiment of the present invention can be used include side panels, back panels, various nameplates, decorative films, ornamental films, etc. of portable electronic devices. Effect of the Invention

[0047] According to the present invention, it is possible to provide a double-sided pressure-sensitive adhesive tape that has heat resistance and flexibility. [Brief description of the drawings]

[0048] [Figure 1] 1A and 1B are schematic diagrams ((a) top view, (b) side view) illustrating an evaluation sample when evaluating film wrinkles in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0050] (Preparation of acrylic adhesive solution A) 52 parts by weight of ethyl acetate was placed in a reactor equipped with a thermometer, a stirrer, and a cooling tube, and the reactor was heated to start refluxing. 30 minutes after the ethyl acetate boiled, 0.08 parts by weight of azobisisobutyronitrile was added as a polymerization initiator. A monomer mixture consisting of 70 parts by weight of butyl acrylate, 27 parts by weight of 2-ethylhexyl acrylate, 3 parts by weight of acrylic acid, and 0.2 parts by weight of 2-hydroxyethyl acrylate was added dropwise evenly and gradually over 1 hour and 30 minutes to react. 30 minutes after the dropwise addition, 0.1 parts by weight of azobisisobutyronitrile was added, and the polymerization reaction was continued for another 5 hours. Ethyl acetate was added to the reactor to dilute it and cool it, thereby obtaining a solution of an acrylic copolymer with a solid content of 40% by weight. The weight average molecular weight of the obtained acrylic copolymer was measured by GPC using a Water's "2690 Separations Model" column, and it was found to be 710,000. To 100 parts by weight of the solid content of the obtained acrylic copolymer, 15 parts by weight of polymerized rosin ester having a softening point of 150° C., 10 parts by weight of terpene phenol having a softening point of 145° C., and 10 parts by weight of rosin ester having a softening point of 70° C. were added. Furthermore, 30 parts by weight of ethyl acetate (manufactured by Fuji Chemicals Co., Ltd.) and 3.0 parts by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., product name "Coronate L45") were added and stirred, thereby obtaining an acrylic adhesive solution A.

[0051] (Preparation of acrylic adhesive solution B) An acrylic adhesive solution B was obtained in the same manner as in "(Preparation of acrylic adhesive solution A)" above, except that 60 parts by weight of butyl acrylate, 37 parts by weight of 2-ethylhexyl acrylate, and 2.2 parts by weight of an isocyanate crosslinking agent were used.

[0052] (Preparation of Rubber-Based Adhesive Solution C) To 100 parts by weight of an SIS block copolymer (manufactured by Zeon Corporation, product name "Quintac3450"), 45 parts by weight of a C5 petroleum resin with a softening point of 100°C and 15 parts by weight of a coumarone resin with a softening point of 120°C were added and stirred to obtain a rubber-based adhesive solution C.

[0053] (Preparation of urethane adhesive solution D) 2.6 parts by weight of an isocyanate crosslinking agent was added to 100 parts by weight of a urethane resin (manufactured by AGC Corporation, product name "Eufine C") and stirred to obtain a urethane adhesive solution D.

[0054] Example 1 (1) Preparation of foam substrate A mixed resin was obtained by mixing 40 parts by weight of homopolypropylene resin (Prime Polymer Co., Ltd., E-253G) as a polypropylene resin, 35 parts by weight of ethylene-propylene random copolymer (Sumitomo Chemical Co., Ltd., AD571) as an elastomer resin, and 25 parts by weight of linear low-density polyethylene (Tosoh Corporation, ZF231) as other resins. 3.5 parts by weight of azodicarbonamide as a thermal decomposition type foaming agent, 1 part by weight of zinc oxide as a decomposition temperature regulator, and 0.5 parts by weight of 2,6-di-t-butyl-p-cresol as an antioxidant were fed to an extruder to 100 parts by weight of the mixed resin. The mixture was melt-kneaded at 190°C and extruded into a long sheet-like foam raw material with a thickness of 0.1 mm. Next, both sides of the long sheet-like foam raw material were crosslinked by irradiating 4.0 Mrad of electron beams at an accelerating voltage of 500 kV. The crosslinked foam raw material was continuously sent into a foaming furnace maintained at 250°C by hot air and an infrared heater to heat and foam the foam, thereby obtaining a foam base material with a thickness of 0.15 mm. The expansion ratio of the obtained foam base material was calculated using an electronic specific gravity meter (Mirage's "ED120T") in accordance with JIS K-6767, and found to be 3 cm 3 / g.

[0055] (2) Manufacturing of double-sided adhesive tapes A release paper having a thickness of 150 μm was prepared, and the acrylic adhesive solution A was applied to the release-treated surface of the release paper, and dried at 100° C. for 5 minutes to form an acrylic adhesive layer having a thickness of 0.025 mm. This acrylic adhesive layer was bonded to the surface of the obtained foam substrate. Next, in the same manner, the same acrylic adhesive layer was bonded to the opposite surface of the foam substrate after peeling off the PET separator. Then, the substrate was cured by heating at 40° C. for 48 hours. As a result, a double-sided adhesive tape having an overall thickness of 0.2 mm was obtained.

[0056] (3) Measurement of each physical property The obtained double-sided adhesive tape was subjected to measurements using a dynamic viscoelasticity measuring device (DVA-200 manufactured by IT Measurement and Control Co., Ltd.) at a frequency of 10 Hz and a heating rate of 3°C / min from -40°C to 140°C, and the storage modulus G' (90°C) and storage modulus G' (110°C) were measured. In addition, the 25% compressive strength of the obtained double-sided pressure-sensitive adhesive tape was measured by a method in accordance with JIS K 6254. Furthermore, the tensile modulus of elasticity and the tensile elongation at break of the obtained double-sided pressure-sensitive adhesive tape were measured by a method in accordance with JIS K 7161.

[0057] (Examples 2 to 13, Comparative Examples 1 to 9) A double-sided adhesive tape was produced in the same manner as in Example 1, except that in preparing the foam substrate, the resin composition and density were as shown in Table 1, and the thickness of the acrylic adhesive layer per side was 0.05 mm.

[0058] Example 14 In producing the double-sided adhesive tape, the same procedure as in Example 3 was repeated except that acrylic adhesive solution B was used instead of acrylic adhesive solution A, to produce a double-sided adhesive tape having an acrylic adhesive layer thickness of 0.05 mm per side.

[0059] Example 15 In producing the double-sided adhesive tape, the same procedure as in Example 3 was repeated except that the rubber-based adhesive solution C was used instead of the acrylic adhesive solution A, to produce a double-sided adhesive tape with a rubber-based adhesive layer thickness of 0.05 mm per side.

[0060] Example 16 In producing the double-sided adhesive tape, the same procedure as in Example 1 was repeated except that urethane-based adhesive solution D was used instead of acrylic adhesive solution A, to produce a double-sided adhesive tape having a urethane-based adhesive layer thickness of 0.025 mm per side.

[0061] (evaluation) The double-sided pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Table 1.

[0062] (1) Heat resistance evaluation The obtained double-sided adhesive tape was cut into a 10 mm×10 mm square sample in the MD and TD directions. This sample was heated at 110° C. for 500 hours and then naturally cooled to 23° C. Similarly, a sample was heated at 120° C. for 500 hours and then naturally cooled to 23° C. After natural cooling, the shrinkage rates in the MD and TD directions were calculated and evaluated according to the following criteria. ◎: Shrinkage rate in both MD and TD directions after heating at 120℃ is 5% or less Good: The shrinkage rate in the MD and / or TD directions after heating at 120°C exceeds 5%, but the shrinkage rates in both the MD and TD directions after heating at 110°C are 5% or less ×: Shrinkage rate in MD and / or TD after heating at 110°C exceeds 5%

[0063] (2) Evaluation of compressive adhesion The obtained double-sided adhesive tape was cut into a square of 20 mm x 20 mm in the MD and TD directions, the release paper on one side was peeled off, and the tape was attached to a SUS plate (125 mm x 50 mm x 2 mm). The release paper on the other side was then peeled off, and a SUS plate (25 mm x 25 mm x 2 mm) with a gripping area for pulling in the vertical direction was attached. After pressing with a 5 kg weight for 1 second, the tape was left at room temperature for 24 hours, and a tensile test was performed in the surface direction at a speed of 10 mm / min to measure the adhesive strength. The measured adhesive strength was converted to a force per 100 μm of tape thickness (N / 100 μm) and evaluated according to the following criteria. ◎:60N / 100μm or more ○: 35N / 100μm or more, less than 60N / 100μm ×: Less than 35N / 100μm

[0064] (3) Film wrinkle evaluation As an alternative evaluation of display unevenness and light unevenness, a wrinkle evaluation was performed using a film. The wrinkle evaluation was performed by preparing the evaluation sample shown in Figure 1. That is, the obtained double-sided adhesive tape was cut into a rectangular shape of 2 mm (MD direction) x 80 mm (TD direction) to obtain two double-sided adhesive tapes 1. The release paper on one side of the double-sided adhesive tape 1 was peeled off and the tape was attached to a glass plate 2 (120 mm x 50 mm x 2 mm) at the position shown in Figure 1. Next, the release paper on the other side of the double-sided adhesive tape 1 was peeled off, and a polyimide film 3 (manufactured by Toray DuPont Co., Ltd., Kapton 200V, thickness 50 μm) cut into a rectangle of 90 mm x 50 mm was attached while stretching it so as not to wrinkle. A glass plate of the same size was placed on the polyimide film 3, and a 5 kg weight was pressed from above for 10 seconds, and then the glass plate was left to stand at room temperature for 24 hours to obtain an evaluation sample. Thereafter, the evaluation sample was left to stand in an environment at 110°C for 2 hours, and after 2 hours had passed, it was taken out to room temperature and naturally cooled to 23°C. After natural cooling, the presence or absence of wrinkles in the polyimide film 3 was checked and evaluated according to the following criteria. ○: No film wrinkles were observed around the double-sided adhesive tape 1 ×: Film wrinkles were observed around the periphery of the double-sided adhesive tape 1.

[0065] [Table 1] [Industrial Applicability]

[0066] According to the present invention, it is possible to provide a double-sided pressure-sensitive adhesive tape that has heat resistance and flexibility. [Explanation of symbols]

[0067] 1 Double-sided adhesive tape 2 Glass plate 3 Polyimide film

Claims

1. A double-sided pressure-sensitive adhesive tape having a foam substrate and pressure-sensitive adhesive layers on both sides of the foam substrate, the double-sided pressure-sensitive adhesive tape has a ratio (G'(110°C) / G'(90°C)) of a storage modulus G'(110°C) at 110°C to a storage modulus G'(90°C) at 90°C of 0.4 or more, a 25% compressive strength at -30°C measured in accordance with JIS K 6254 of 400 kPa or less, and a thickness of the double-sided pressure-sensitive adhesive tape of 0.6 mm or less; The double-sided adhesive tape has a tensile modulus of 10 N / mm in the MD direction. 2 or more, and the tensile elongation at break is 150% or more; The foam base material is made of a mixed resin containing a polypropylene-based resin and an elastomer-based resin. Double-sided adhesive tape.

2. 2. The double-sided pressure-sensitive adhesive tape according to claim 1, wherein the foam substrate is made of a mixed resin containing 30 to 60% by weight of a polypropylene resin and 25 to 50% by weight of an elastomer resin.

3. The foam base material has an expansion ratio of 2 to 10 cm 3 The double-sided pressure-sensitive adhesive tape according to claim 1 or 2, wherein the viscosity is 1 / g.

4. The double-sided pressure-sensitive adhesive tape according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive layer is an acrylic pressure-sensitive adhesive layer containing an acrylic copolymer.

5. The double-sided pressure-sensitive adhesive tape according to any one of claims 1 to 4, which is used for fixing an on-vehicle electronic device part.

Citation Information

Patent Citations

  • Driving mechanism control device

    JP2008176750A

  • Impact-absorbing tape

    JP2009242541A

  • Pressure-sensitive adhesive sheet for front plate of display device

    JP2009258274A

  • Double-sided adhesive tape, double-sided adhesive tape for fixing onboard component, and double-sided adhesive tape for fixing onboard head up display cover

    JP2018154849A

  • Adhesive tape

    JP2019044181A