Concrete floor structure and its manufacturing method

By applying a primer layer with specific resin and organosilicon compound amounts, the method enhances peeling resistance and smoothness in concrete floors, addressing unevenness issues and maintaining economic efficiency.

JP7579188B2Active Publication Date: 2024-11-07MU MATEX CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021050157
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-24
Publication Date
2024-11-07
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Existing concrete floor structures face issues with insufficient peeling resistance between the hardened self-leveling slurry layer and the floor coating layer due to small irregularities and slopes in the concrete surface, leading to undesirable finishes and decreased economic efficiency when attempting to smooth these irregularities.

Method used

A method involving the application of a primer layer containing a predetermined amount of resin component and organosilicon compound on the self-leveling material slurry cured product layer, adhering to specific coating amounts defined by formulas (1) and (2), to enhance the peeling resistance.

Benefits of technology

The method results in a concrete floor structure with improved peeling resistance and a smooth, aesthetically pleasing finish, maintaining economic efficiency by ensuring the primer penetrates and reinforces the self-leveling material slurry layer effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579188000002
    Figure 0007579188000002
  • Figure 0007579188000003
    Figure 0007579188000003
  • Figure 0007579188000001
    Figure 0007579188000001
Patent Text Reader

Abstract

To provide a manufacturing method of a concrete floor structure having excellent peeling resistance of a floor coating material layer to self-levelling material slurry hardened body layer.SOLUTION: The manufacturing method of a concrete floor structure 20 has a step to prepare a concrete floor substrate 10 having a concrete floor layer 2 and a self-levelling material slurry hardened body layer 6, a step to form a floor coating material primer layer 12 on a top face of the self-levelling material slurry hardened body layer 6 by coating the floor coating material primer containing resin component and organic silicon compound, and a step to form a floor coating material base coat layer 14 on a top face of the floor coating material primer layer 12. Coating amount (X(g / m2)) of the resin component in the floor coating material primer and the coating amount (Y(g / m2)) of the organic silicon compound satisfy following formulas (1) and (2): 75≤X≤110 (1); -0.5X+65≤Y≤-0.5X+75 (2).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a concrete floor structure and a method for manufacturing the same. [Background technology]

[0002] In buildings such as offices, factories, and warehouses, various resin-based floor coating materials are generally used to finish concrete floors. When these floor coating materials are used as finishing materials for concrete floors, the abrasion resistance, chemical resistance, etc. of the floor surface are improved.

[0003] Known methods for constructing the base layer when applying these floor coating materials include, for example, a concrete direct pressing method and a joint construction method using mortar or self-leveling material, etc. Patent Document 1 discloses an invention for a concrete floor structure characterized in that, as a joint construction method, a concrete floor base comprising a concrete floor layer and a self-leveling material slurry hardened body layer containing a self-leveling material is provided on the upper surface with a primer layer for floor coating material, and a base coat for floor coating material is applied and hardened on the upper surface. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-190315 A [Patent Document 2] JP 2009-257062 A Summary of the Invention [Problem to be solved by the invention]

[0005] Generally, when applying a floor coating to a concrete floor, a floor coating primer layer is applied to the surface of the concrete floor base, and then a floor coating base coat layer is formed. If special functions are required, a floor coating top coat layer may also be applied.

[0006] Usually, concrete floors in new buildings are made flat to a certain degree by pouring and compacting the fresh concrete, and then when the water on the concrete surface has receded, the surface is leveled with a plastering trowel or similar tool, and rough irregularities are smoothed out, and the concrete is cured and hardened. Therefore, the surface of the hardened concrete floor at the stage of applying the floor coating material is likely to have a wide variety of small irregularities or subtle inclinations, and in order to prevent this, high construction skills or a great deal of effort is required to smooth the surface. When the floor coating material base coat is applied and finished, the small irregularities or subtle inclinations are reflected as they are, resulting in a finish that is not desirable in terms of actual use and aesthetics. These can be improved by increasing the amount of the floor coating material base coat used, but there is a problem of reduced economic efficiency. On the other hand, if the amount of the floor coating material base coat used is set as the recommended average application amount, it is thought that the performance of the convex parts where the amount of application is small will be insufficient compared to when the appropriate amount of the floor coating material base coat layer is applied.

[0007] The effects on the finished surface of the coated floor caused by the unevenness or inclination of the concrete floor surface can be avoided by applying a self-leveling material slurry to the concrete floor surface and then applying a primer layer for the coated floor material. However, there are cases where the peel resistance between the hardened self-leveling material slurry layer, which has an excellent horizontal level and reduced small unevenness, and the coated floor material layer applied on the upper surface of the primer layer for the coated floor material is insufficient.

[0008] Therefore, a main object of the present invention is to provide a method for manufacturing a concrete floor structure having excellent peeling resistance of a floor coating material layer against a hardened self-leveling material slurry layer. [Means for solving the problem]

[0009] As a result of extensive trial and error by the inventors in an effort to solve the above problems, they discovered that the above problems could be solved by applying a primer for coated floor materials, which contains a resin component in a prescribed range and an organosilicon compound in a prescribed range, to the top surface of a self-leveling material slurry hardened body layer to form a primer layer for coated floor materials, and thus completed the present invention.

[0010] One aspect of the present invention relates to a manufacturing method (construction method) for a concrete floor structure. The manufacturing method (construction method) for a concrete floor structure includes a first step of preparing a concrete floor base comprising a concrete floor layer and a self-leveling material slurry hardened body layer made of a hardened body of a self-leveling material slurry containing a self-leveling material provided on the upper surface of the concrete floor layer, a second step of applying a floor coating primer containing a resin component and an organosilicon compound to the upper surface of the self-leveling material slurry hardened body layer of the concrete floor base to form a floor coating primer layer, and a third step of applying a floor coating base coat to the upper surface of the floor coating primer layer to form a floor coating base coat layer. In the second step, the amount of resin component contained in the floor coating primer is set to X (g / m 2 ), and the coating amount of the organosilicon compound contained in the floor coating primer is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and the following formula (2). 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2)

[0011] According to this manufacturing method, a concrete structure having excellent peeling resistance of the coating floor material layer against the self-leveling material slurry hardened body layer can be manufactured. The inventors believe that the reason for this effect is as follows. By applying a coating floor material primer containing a predetermined amount of resin component and a predetermined amount of organosilicon compound to the upper surface of the self-leveling material slurry hardened body layer, the coating floor material primer penetrates deeper into the self-leveling material slurry hardened body, and a layer reinforced by the coating floor material primer is generated deeper from the surface of the self-leveling material slurry hardened body. It is presumed that this action improves the peeling resistance of the coating floor material layer against the self-leveling material slurry hardened body layer.

[0012] The pot life of the primer for floor coating materials is preferably 30 minutes to 3 hours.

[0013] The resin components contained in the primer for coated floor materials are preferably an epoxy resin and a curing agent for the epoxy resin.

[0014] The organosilicon compound is preferably an alkoxysilane.

[0015] Another aspect of the present invention relates to a concrete floor structure. The concrete floor structure comprises, in this order, a concrete floor layer, a self-leveling material slurry hardened body layer, a primer layer for coated floor materials formed by applying a primer for coated floor materials containing a resin component and an organosilicon compound, and a base coat layer for coated floor materials. The amount of the resin component contained in the primer for coated floor materials is X (g / m 2 ), and the coating amount of the organosilicon compound contained in the floor coating primer is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and the following formula (2). 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2)

[0016] Such a concrete floor structure has excellent peeling resistance of the coating floor material layer against the hardened self-leveling material slurry layer. In addition, such a concrete floor structure is usually constructed by applying and hardening the self-leveling material slurry on the upper surface of the concrete floor layer having a wide variety of unevenness or inclination to form a hardened self-leveling material slurry layer having excellent horizontal level, and then applying the coating floor material base coat layer, so that the finished surface of the coating floor material also has excellent horizontal level, and tends to have good usability and aesthetics. Effect of the Invention

[0017] According to the present invention, a method for manufacturing a concrete floor structure having excellent peeling resistance of a coating floor material layer against a hardened layer of a self-leveling material slurry is provided. Also, according to the present invention, a concrete floor structure obtained by such a manufacturing method is provided. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a method for manufacturing a concrete floor structure, and FIGS. 1(a), (b), and (c) are process diagrams showing each step. [Diagram 2] FIG. 2 is a graph showing the relationship between the coating amount (g / m2) of the resin component and the coating amount (g / m2) of the organosilicon compound contained in the primer for floor coating materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings as appropriate. However, the present invention is not limited to the following embodiment.

[0020] [Method of manufacturing concrete floor structure] Fig. 1 is a schematic cross-sectional view showing one embodiment of a method for producing a concrete floor structure, and Fig. 1(a), (b), and (c) are process diagrams showing each process. The method for producing a concrete floor structure of this embodiment includes a first process (see Fig. 1(a)) of preparing a concrete floor base comprising a concrete floor layer and a self-leveling material slurry hardened body layer consisting of a hardened body of a self-leveling material slurry containing a self-leveling material provided on the upper surface of the concrete floor layer, a second process (see Fig. 1(b)) of applying a floor coating primer containing a resin component and an organosilicon compound to the upper surface of the self-leveling material slurry hardened body layer of the concrete floor base to form a floor coating primer layer, and a third process (see Fig. 1(c)) of applying a floor coating base coat to the upper surface of the floor coating primer layer to form a floor coating base coat layer. The concrete floor structure obtained by the manufacturing method of this embodiment is used for buildings, and is particularly suitable for use as a concrete floor structure for non-residential buildings where high durability is required, such as public facilities such as hospitals and stations (premises), factories, warehouses, etc.

[0021] <First step> In this process, a concrete floor base 10 is prepared, which comprises a concrete floor layer 2 and a self-leveling material slurry hardened body layer 6 consisting of a hardened body of a self-leveling material slurry containing a self-leveling material, which is provided on the upper surface of the concrete floor layer 2 (see Figure 1 (a)).

[0022] As shown in Fig. 1(a), the concrete floor base 10 can be obtained, for example, by pouring a self-leveling material slurry containing a self-leveling material into a concrete floor layer 2 having an unevenness or a slope, and forming a self-leveling material slurry hardened body layer 6 made of the hardened body of the self-leveling material slurry. Since the concrete floor layer 2 has a wide variety of small unevenness or subtle slopes intricately intertwined, forming the self-leveling material slurry hardened body layer 6 can improve workability or horizontality.

[0023] The concrete floor layer 2 forms the floor surface of a general concrete structure (building, architectural structure). The concrete floor layer 2 may be a concrete floor layer of a building or architectural structure. The concrete floor layer 2 may be a layer formed by mixing cement, fine aggregate, coarse aggregate, a fluidizing agent, water, etc. in a specific ratio to form a floor surface and hardening the mixture. The compressive strength (nominal strength) of the concrete floor layer is preferably 20 N / mm 2 More preferably, 30N / mm 2 More preferably, 35N / mm 2 More than 40N / mm 2 That's all.

[0024] The self-leveling material for forming the slurry hardened body layer 6 can be used without any particular limitation as long as it is a self-leveling material used as a base material for floor coating materials in the construction of the floor surface of a structure. In one embodiment, the self-leveling material may be a self-leveling material containing a hydraulic component and an admixture such as fine aggregate and a water reducing agent. The hydraulic component is preferably one that has fast hardening and fast drying properties.

[0025] The self-leveling material preferably satisfies all of the following conditions (A) to (D) in a self-leveling material slurry containing the self-leveling material and in its hardened body. By using such a self-leveling material, it becomes possible to construct a concrete floor base more efficiently and more stably.

[0026] Condition (A): The flow value measured in accordance with JASS 15M-103 is 190 mm or more, preferably 200 mm or more, and more preferably 210 mm or more.

[0027] By using a self-leveling material that satisfies condition (A), a floor surface that is easy to work with and has excellent smoothness can be formed.

[0028] Condition (B): The time period during which the surface of the cured body reaches a Shore hardness of 10 or more is within 6 hours, preferably within 4 hours, and more preferably within 2 hours.

[0029] By using a self-leveling material that satisfies condition (B), a floor surface with excellent quick hardening properties can be formed. In addition, since it takes a short time for light walking to occur, it is possible to move on to the second process early.

[0030] Condition (C): The time period during which the D-mode value of the moisture content on the surface of the hardened body reaches 870 or less as measured by a Kett moisture meter is within 72 hours, preferably within 48 hours, and more preferably within 24 hours.

[0031] By using a self-leveling material that satisfies condition (C), a floor surface with excellent quick-hardening properties can be formed. In addition, since the time required for the moisture content D mode value to reach 870 or less using a Kett moisture meter is short, it is possible to move on to the second process early.

[0032] Condition (D): Compressive strength at 28 days measured in accordance with JASS 15M-103 is 30N / mm 2 More than 35N / mm 2 More preferably, 40N / mm 2 That's all.

[0033] By using a self-leveling material that satisfies condition (D), it is possible to form a concrete floor structure with excellent durability as a base for a floor coating material used for running heavy machinery, etc.

[0034] The self-leveling material slurry for forming the self-leveling material slurry hardened body layer 6 can be obtained by mixing and kneading the self-leveling material and water. The mass ratio of water to the self-leveling material (mass of water / mass of self-leveling material) is preferably 18 to 26, more preferably 20 to 24. The self-leveling material and water are preferably mixed and kneaded using a hand mixer, and the mixing and kneading time is preferably within 3 minutes.

[0035] The self-leveling material slurry usually begins to harden 30 to 120 minutes after pouring (pouring and construction) is completed, depending on the temperature and humidity conditions at the construction site, and as the hardening progresses, the surface hardness increases and a hardened body of the self-leveling material slurry is formed, becoming self-leveling material slurry hardened body layer 6.

[0036] The self-leveling material slurry hardened body layer 6 can be formed, for example, by the following method. First, the self-leveling material slurry is cast (applied, poured) onto the upper surface of the concrete floor layer 2. Next, the surface of the cast self-leveling material slurry is made uniform using a trowel or a dragonfly. Thereafter, the self-leveling material slurry is cured to harden the self-leveling material slurry, thereby forming the self-leveling material slurry hardened body layer 6. When the self-leveling material slurry hardened body layer 6 is formed by such a method, the surface is hardened while being uniform, so that the self-leveling material slurry hardened body layer 6 having excellent smoothness can be obtained.

[0037] The thickness of the self-leveling material slurry hardened body layer 6 is preferably 1 to 100 mm, more preferably 5 to 50 mm, further preferably 7 to 40 mm, and particularly preferably 10 to 30 mm.

[0038] The concrete floor base 10 may further include a self-leveling material primer layer 4 between the concrete floor layer 2 and the self-leveling material slurry hardened body layer 6.

[0039] The primer layer 4 for the self-leveling material in the concrete floor layer 2 can be formed, for example, by applying a primer for the self-leveling material to the concrete floor layer 2 and drying the primer for the self-leveling material. When forming the primer layer 4 for the self-leveling material, it is preferable to clean in advance the surface of the concrete floor layer 2 on which the primer layer 4 for the self-leveling material is to be formed.

[0040] The main component of the primer for self-leveling materials may be, for example, a water-based resin emulsion. Examples of the resin constituting the resin emulsion include acrylic resin, styrene-acrylic copolymer resin, vinyl acetate resin, ethylene-vinyl acetate copolymer resin, vinyl acetate-Veova copolymer resin, and the like. Commercially available products can be used for these resins (resin emulsions). The resin of the resin emulsion is preferably an acrylic resin or a styrene-acrylic copolymer resin, more preferably a styrene-acrylic copolymer resin. The minimum film-forming temperature (MFT) of the resin constituting the resin emulsion is preferably 0°C or higher, and the glass transition temperature (Tg) is preferably 0°C or lower. The solid content concentration of the resin emulsion is preferably 7 to 25 mass% based on the total amount of the resin emulsion. When the resin emulsion is used as a primer for self-leveling materials, the coating amount of the resin emulsion is 30 to 100 g / m 2 It is preferable that:

[0041] The thickness of the self-leveling material primer layer 4 is preferably 5 to 200 μm, more preferably 10 to 150 μm, even more preferably 15 to 100 μm, and particularly preferably 20 to 75 μm, from the viewpoint of firmly adhering the concrete floor layer 2 and the self-leveling material slurry hardened layer 6.

[0042] When forming a self-leveling material slurry hardened layer 6 on the upper surface of the self-leveling material primer layer 4, it is preferable to pour the self-leveling material slurry at least one hour after applying the self-leveling material primer to the concrete floor layer 2.

[0043] <Second step> In this step, a floor coating primer containing a resin component and an organosilicon compound is applied to the upper surface 6A of the self-leveling material slurry hardened body layer 6, and the floor coating primer is dried as necessary to form a floor coating primer layer 12 (see FIG. 1(b)). This step is preferably carried out 24 hours or more after the self-leveling material slurry is poured to form the self-leveling material slurry hardened body layer 6 in the first step.

[0044] The coated floor material primer layer 12 is a layer used to improve adhesion of the coated floor material to the substrate, prevent absorption into the substrate, and prevent pinholes in the coated floor material. The coated floor material primer for forming the coated floor material primer layer 12 contains a resin component and an organosilicon compound. The coated floor material primer may be mainly composed of a resin component and an organosilicon compound.

[0045] The resin component may be composed of, for example, a curable resin and a curing agent for the curable resin. Examples of the curable resin include epoxy resins such as solvent-based epoxy resins, solventless epoxy resins, and water-based epoxy resins. The curable resin is preferably an epoxy resin. When the curable resin is an epoxy resin, the curing agent for the curable resin may be a curing agent for the epoxy resin. Examples of the curing agent for the epoxy resin include amines such as aliphatic amines, aromatic amines, and modified amines (ketimines (ketoimines)); imidazoles; and acid anhydrides. The resin component is preferably an epoxy resin and a curing agent for the epoxy resin. The primer for the coated floor material is preferably one that has low viscosity and excellent impregnation. A commercially available product can be used as the primer for the coated floor material containing the resin component (for example, an epoxy resin and an epoxy resin curing agent).

[0046] By including an organic silicon compound in the primer for floor coating, the primer for floor coating penetrates deeper into the hardened self-leveling material slurry, and the layer reinforced by the primer for floor coating tends to form deeper from the surface of the hardened self-leveling material slurry.As the organic silicon compound, there are organic silicon compounds (alkoxysilanes) having an alkoxy group such as tetraethoxysilane and tetramethoxysilane.The organic silicon compound is preferably tetraethoxysilane.

[0047] The amount of resin components (curable resin and curing agent for the curable resin) contained in the primer for floor coating is X (g / m 2 ), and the coating amount of the organosilicon compound contained in the floor coating primer is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and formula (2). In other words, when the coordinates (X, Y) are plotted on a graph, it can be said that the coordinates (X, Y) are within the region that satisfies the conditions of the following formula (1) and formula (2). When the coating amount of the resin component and the coating amount of the organosilicon compound are within such ranges, the peeling resistance of the coated floor material layer against the self-leveling material slurry hardened body layer tends to be even better.

[0048] 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2)

[0049] X is 75 or more, preferably 80 or more, more preferably 85 or more, and even more preferably 90 or more. If X is less than 75, the action as a primer for coated floor materials tends to be insufficient. X is 110 or less, preferably 105 or less, and more preferably 100 or less. If X exceeds 110, the amount of resin component contained in the primer for coated floor materials becomes excessive, and the peeling resistance of the coated floor material layer against the self-leveling material slurry hardened body layer tends to decrease.

[0050] It is preferable that X and Y further satisfy the following formula (3) in addition to the conditions of formulas (1) and (2).

[0051] 10≦Y≦37.5 (3)

[0052] Y is 10 or more, preferably 15 or more, more preferably 20 or more. If Y is less than 10, the effect of improving the permeability of the primer for coated floor materials tends to be insufficient. Y is 37.5 or less, preferably 35 or less, more preferably 30 or less, and even more preferably 25 or less. If Y exceeds 37.5, the amount of resin component contained in the primer for coated floor materials is small, so that the function as a primer for coated floor materials tends to be insufficient.

[0053] The primer for coated floor materials may further contain a filler in addition to the resin component and the organosilicon compound. By further containing a filler, the primer for coated floor materials tends to fill fine irregularities in the surface layer of the hardened self-leveling material slurry and suppress the appearance of these fine irregularities on the surface of the coated floor material. In addition, the effect of preventing pinholes in the coated floor material tends to be more effective. The filler may be mainly composed of Portland cement, and may contain inorganic powder such as silica and talc as necessary. The mass ratio of the resin component to the filler is preferably in the range of, for example, resin component:filler=5:1 to 1:1.

[0054] The pot life (20°C) of the primer for floor coating materials is preferably long from the viewpoint of workability and penetration. More specifically, the pot life of the primer for floor coating materials is preferably 30 minutes to 3 hours, more preferably 60 minutes to 3 hours.

[0055] <Third process> In this step, a floor coating base coat is applied to the upper surface 12A of the floor coating primer layer 12, and if necessary, the floor coating base coat is dried to form a floor coating base coat layer 14 (see FIG. 1(c)). This step is preferably carried out at least two hours after the application of the floor coating primer in the second step.

[0056] The coated floor base coat layer 14 is a layer for imparting the main functions of the coated floor material, such as durability, mechanical strength, and elasticity. The main component of the coated floor base coat for forming the coated floor base coat layer 14 may be, for example, a resin-based base coat. Examples of the resin-based base coat include epoxy resin-based base coats such as solvent-based epoxy resin-based, solventless epoxy resin-based, and water-based epoxy resin-based. In addition to the resin-based base coat, the coated floor base coat may further contain organic pigments, inorganic pigments, talc, calcium carbonate, powdered silica, and other fillers, fine aggregates, and the like.

[0057] The application of the floor coating base coat can be carried out in accordance with the application instructions of each floor coating manufacturer, using an appropriate trowel, roller, or brush.

[0058] The manufacturing method of the concrete floor structure of this embodiment may further include a step of forming a floor coating top coat layer by applying a floor coating top coat to the upper surface of the floor coating base coat layer 14. This step is preferably carried out 24 hours or more after the floor coating base coat is applied in the fourth step.

[0059] The coated floor topcoat layer is a layer for protecting the coated floor basecoat layer 14, such as weather resistance, stain resistance, anti-slip properties, and matte finish, or for imparting various functions. The main component of the coated floor topcoat for forming the coated floor topcoat layer may be a resin-based topcoat. Examples of the resin-based topcoat include epoxy resin-based topcoats such as solvent-based epoxy resin-based, solventless epoxy resin-based, and water-based epoxy resin-based topcoats. One or more of these can be appropriately selected to form one or more coated floor topcoat layers.

[0060] The application of the floor coating top coat can be carried out in accordance with the application instructions of each floor coating manufacturer, using an appropriate selection of trowel, roller, or brush.

[0061] In this way, a concrete floor structure 20 can be obtained that has excellent peeling resistance of the floor coating layer against the hardened self-leveling material slurry layer.

[0062] [Concrete floor structure] A concrete floor structure of one embodiment is as shown in Fig. 1(c). The concrete floor structure 20 comprises, in this order, a concrete floor layer 2, a self-leveling material slurry hardened body layer 6, a coated floor material primer layer 12 formed by applying a coated floor material primer containing a resin component and an organosilicon compound, and a coated floor material base coat layer 14. The amount of resin component contained in the coated floor material primer applied is X (g / m 2 ), and the coating amount of the organosilicon compound contained in the floor coating primer is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and formula (2). Such a concrete floor structure has excellent peeling resistance of the floor coating material layer against the self-leveling material slurry hardened body layer.

[0063] 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2) EXAMPLES

[0064] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0065] [Materials used] (A) Self-leveling material Self-leveling material A-1: ​​Ultra-fast hardening cement-based self-leveling material (commercially available) (B) Primer for self-leveling materials Self-leveling primer B-1: A dispersion of styrene-acrylic copolymer resin emulsion (commercially available) with water added to adjust the solids concentration to 15% by mass. (C) Filler Filler C-1: Composition containing approximately 75% by mass of Portland cement (commercially available product) (D) Primer for floor coating A stock solution of epoxy resin, epoxy resin curing agent (ketimine), and organosilicon compound (tetraethoxysilane) (commercial product, one-liquid type, epoxy resin, epoxy resin curing agent, and organosilicon compound total amount is 100 mass%, epoxy resin and epoxy resin curing agent (ketimine) content: 92.5 mass%, organosilicon compound (tetraethoxysilane) content: 7.5 mass%), and an additive solution of organosilicon compound (tetraethoxysilane) (commercial product, organosilicon compound content: 100 mass%) were prepared. These were mixed as stock solutions or in a predetermined ratio, and filler C-1 was further added to prepare primers D-1 to D-5 for coating floor materials. Filler C-1 was added so that the amount was 50 mass% in terms of the outside ratio to the stock solution. Each of primers D-1 to D-5 for coating floor materials was 150 minutes (20 ° C.). Floor coating primer D-1: undiluted (100% by weight) - Floor coating primer D-2: A mixture of the original solution (92.0% by mass) and additive solution (8.0% by mass) - Floor coating primer D-3: A mixture of undiluted solution (85.0% by mass) and additive solution (15.0% by mass) - Floor coating primer D-4: A mixture of undiluted solution (77.5% by mass) and additive solution (22.5% by mass) -Floor coating primer D-5: A mixture of undiluted solution (73.5% by mass) and additive solution (26.5% by mass) (E) Floor coating base coat Floor coating base coat E-1: Epoxy resin base coat (commercially available, two-component type)

[0066] [Method of preparing self-leveling material slurry] The self-leveling material slurry was prepared by adding 390 g of water to 1.5 kg of the above self-leveling material A-1 and kneading for 3 minutes using a chemical stirrer. The preparation was carried out in a temperature- and humidity-controlled room set at a temperature of 20° C. and a humidity of 65% RH.

[0067] [Self-leveling material property test] (1) Flow value The flow value was measured according to the method compliant with JASS 15M-103 "Quality Standard for Self-Leveling Materials" of the Architectural Institute of Japan. The measurement was carried out in a temperature-controlled room at a temperature of 20°C. The flow value of self-leveling material A-1 was 225 mm. (2) Shore hardness of the hardened surface The Shore hardness was measured using the self-leveling material slurry obtained above. The self-leveling material slurry was poured into a 130 x 190 mm resin mold to a thickness of 10 mm to obtain a test specimen. The time until the gloss of the slurry surface of the test specimen was completely lost (water-drawing time) was confirmed by visual inspection. Using the water-drawing time as the standard, the Shore hardness of the hardened surface was measured at various times using a spring type D hardness tester, and the time at which the Shore hardness reached 10 or more was determined. The time required for the Shore hardness of the self-leveling material A-1 to reach 10 or more was 1.5 hours. (3) Moisture content of the hardened body surface (D mode value of moisture content measured with a bucket moisture meter on the hardened body surface) The start of Shore hardness development was confirmed using the same test specimen as that used for the Shore hardness measurement. Based on the start of Shore hardness development, the moisture content of the hardened surface at each time was measured using a moisture meter (manufactured by Kett Electric Laboratory Co., Ltd., sometimes called a "Kett moisture meter") in accordance with the "Method of measuring various qualities of concrete base and grade" of the Concrete Floor Construction Technology Research Council. The measurement was performed in a constant temperature room at 20°C in D mode. The time at which the moisture content of the hardened surface reached 870 or less using the Kett moisture meter was determined as the moisture content of the hardened surface. The time at which the D mode value of the hardened surface of the self-leveling material A-1 reached 870 or less using the Kett moisture meter was 6 hours. (4) Compressive strength Compressive strength (N / mm2) was measured in accordance with the Architectural Institute of Japan JASS 15M-103 "Quality Standard for Self-Leveling Materials." Curing was performed in a constant temperature room at 20°C, and the material age was 28 days. The compressive strength of self-leveling material A-1 at 28 days was 42N / mm2. 2 It was.

[0068] [Creating concrete floor structure] Example 1 <Preparing the concrete floor base> A concrete floor base was prepared by providing a 10 mm thick self-leveling material slurry hardened body layer on the upper surface of a concrete pavement board (concrete floor layer) with a length of 300 mm, a width of 300 mm, and a thickness of 60 mm. The self-leveling material slurry hardened body layer was formed by uniformly applying 5.5 g of self-leveling material primer B-1 on the concrete pavement board (concrete floor layer) and drying it for one day to form a self-leveling material primer layer. Next, the above-mentioned self-leveling material slurry was poured onto the upper surface of the self-leveling material primer layer to a thickness of 10 mm, and cured for 6 days to form a self-leveling material slurry hardened body layer.

[0069] <Formation of primer layer for floor coating materials> The floor coating primer D-1 was applied to the upper surface of the self-leveling material slurry hardened body layer in the amount shown in Table 1, and dried for 3 hours to form a floor coating primer layer.

[0070] <Formation of base coat layer for floor coating material> One day after applying the floor coating primer, a predetermined amount of floor coating base coat E-1 was applied to the top surface of the floor coating primer layer to a thickness of 0.8 mm. The application was done in two steps, the first immediately after forming the floor coating primer layer, and the second 16 hours after applying the first. The second application was dried for 7 days to form a floor coating base coat layer, and the concrete floor structure of Example 1 was obtained.

[0071] [Peeling resistance test] In the obtained concrete floor structure, an incision was made with an electric cutter from the base coat layer of the plaster floor material to the surface of the hardened self-leveling material slurry layer. A reverse triangular ridge was inserted into the interface between the hardened self-leveling material slurry layer and the base coat layer of the plaster floor material from the incision by hitting it with a hammer, and the base coat layer of the plaster floor material was peeled off by applying force with hands, and the resistance at that time was evaluated by feeler. The evaluation was made on a five-point scale from 1 to 5 below, with 1 point being the easiest to peel off and higher points being more difficult to peel off. The results are shown in Table 1. (Evaluation points) 5 points: Very difficult to peel off 4 points: Not easy to peel off 3 points: Somewhat difficult to peel off 2 points: Easy to peel off 1 point: Very easy to peel off

[0072] (Examples 2 to 5 and Comparative Examples 1 to 8) The concrete floor structures of Examples 2 to 5 and Comparative Examples 1 to 8 were obtained in the same manner as in Example 1, except that the floor coating primer was changed to the type of floor coating primer shown in Table 1 and applied in the amount shown in Table 1. These concrete floor structures were evaluated in the same manner as the concrete floor structure of Example 1. The results are shown in Table 1.

[0073] [Table 1]

[0074] Figure 2 shows the amount of resin component (g / m2) applied to the primer for floor coating. 2 ) and the amount of organic silicon compound applied (g / m 2 ) and the applied amount of the resin component X (g / m 2 ) on the horizontal axis, and the coating amount Y (g / m 2) on the vertical axis. In FIG. 1, the four straight lines are X=75, X=110, Y=-0.5X+65, and Y=-0.5X+75. The black dots in FIG. 1 correspond to Examples 1 to 5, and the peeling resistance test was 4 points or more. On the other hand, the white dots in FIG. 1 correspond to Comparative Examples 1 to 8, and the peeling resistance test was 3 points or less. From these results, it was found that X and Y satisfy the conditions of formula (1) and formula (2) (the coordinates (X, Y) are within the region that satisfies the conditions of formula (1) and formula (2)), thereby providing excellent peeling resistance. From the above, it was confirmed that the concrete floor structure obtained by the manufacturing method of the present invention has excellent peeling resistance of the coating floor material layer against the self-leveling material slurry hardened body layer. [Explanation of symbols]

[0075] 2...Concrete floor layer, 4...Primer layer for self-leveling material, 6...Hardened slurry layer of self-leveling material, 10...Concrete floor base, 12...Primer layer for coated floor material, 14...Base coat layer of coated floor material, 20...Concrete floor structure.

Claims

1. A first step of preparing a concrete floor base including a concrete floor layer and a self-leveling material slurry hardened body layer formed on an upper surface of the concrete floor layer and made of a hardened body of a self-leveling material slurry containing a self-leveling material; A second step of applying a primer for floor coating material containing a resin component and an organosilicon compound to the upper surface of the self-leveling material slurry hardened body layer of the concrete floor base to form a primer layer for floor coating material; A third step of applying a floor coating base coat to the upper surface of the floor coating primer layer to form a floor coating base coat layer; Equipped with The self-leveling material slurry hardened body layer has a D mode value of moisture content measured by a Kett moisture meter on the hardened body surface of the self-leveling material slurry hardened body layer of 870 or less; In the second step, the coating amount of the resin component contained in the primer for floor coating material is X (g / m 2 ), and the coating amount of the organosilicon compound contained in the primer for floor coating material is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and the following formula (2). 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2)

2. The method for manufacturing a concrete floor structure according to claim 1, wherein the pot life of the primer for floor coating is 30 minutes to 3 hours.

3. 3. The method for manufacturing a concrete floor structure according to claim 1, wherein the resin components contained in the primer for floor coating material are an epoxy resin and a hardener for the epoxy resin.

4. The method for manufacturing a concrete floor structure according to any one of claims 1 to 3, wherein the organosilicon compound is an alkoxysilane.

5. A method for manufacturing a concrete floor structure described in any one of claims 1 to 3, wherein the primer for floor coating further contains a filler including Portland cement.

6. A concrete floor layer; A hardened layer of a self-leveling material slurry; A primer layer for a coated floor material formed by applying a primer for a coated floor material containing a resin component and an organosilicon compound; A floor coating base coat layer; In this order, The self-leveling material slurry hardened body layer has a D mode value of moisture content measured by a Kett moisture meter on the hardened body surface of the self-leveling material slurry hardened body layer of 870 or less; The coating amount of the resin component contained in the primer for floor coating material is X (g / m 2 ), and the coating amount of the organosilicon compound contained in the primer for floor coating material is Y (g / m 2 ), X and Y satisfy the conditions of the following formula (1) and the following formula (2). 75≦X≦110 (1) -0.5X+65≦Y≦-0.5X+75 (2)

Citation Information

Patent Citations

  • Primer composition

    JP1990227482A

  • Formation of moisture-permeable waterproof laminated coating film

    JP1999290771A

  • Technique for laminating floor moisture-permeable coating film

    JP2001340806A

  • Surface-treating material for concrete and unevenness- modifying material for concrete

    JP2003213199A

  • Primer for resin coating film

    JP2005187683A