Anode material, its manufacturing method and use, and lithium ion battery

A core-shell structured silicon-based negative electrode material with a porous carbon membrane and intercalated lithium ions addresses the limitations of silicon electrodes, enhancing both initial coulombic efficiency and cycle stability in lithium-ion batteries.

JP7579335B2Active Publication Date: 2024-11-07CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022521415
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-09
Filing Date
2020-09-29
Publication Date
2024-11-07
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing silicon-based negative electrode materials for lithium-ion batteries suffer from low reversible charge capacity, low initial coulombic efficiency, and poor cycle charge capacity retention due to irreversible solid electrolyte interface (SEI) formation and low lithium ion diffusion rates.

Method used

A core-shell structured negative electrode material is developed, comprising a silicon-containing core coated with an organic lithium salt and a porous carbon membrane, with lithium ions intercalated into the porous carbon, enhancing conductivity and stability.

Benefits of technology

The core-shell structure significantly improves initial coulombic efficiency and cycle charge capacity retention, thereby increasing the energy density of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579335000002
    Figure 0007579335000002
  • Figure 0007579335000003
    Figure 0007579335000003
  • Figure 0007579335000004
    Figure 0007579335000004
Patent Text Reader

Abstract

The present invention relates to the field of lithium-ion batteries. It discloses a negative electrode material, its manufacturing method, its use, and a lithium-ion battery. The negative electrode material has a core-shell structure, in which the core comprises a silicon-containing material, and the shell comprises an organic lithium salt and a porous carbon membrane, with at least some lithium ions intercalated in the porous carbon membrane. The manufacturing method of the negative electrode material includes the steps of: (1) mixing a silicon source and a carbon source, followed by calcining the mixture; (2) mixing the calcined product obtained in step (1) with an organic lithium salt; and (3) subjecting the material obtained by mixing in step (2) to vacuum freeze-drying. The negative electrode material of the present invention has an improved reversible charge capacity, and when used in a lithium-ion battery, can improve the energy density of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to the field of lithium ion batteries. More particularly, the present disclosure relates to a core-shell structured negative electrode material, its manufacturing method and its use, and a lithium ion battery. [Background technology]

[0002] Silicon has a theoretical capacity of 4200mAh / g, making it currently the battery anode material with the highest capacity per gram. Once successfully applied, it can significantly improve the energy density of lithium batteries, allowing them to achieve a range of 1000 kilometers on a single charge. However, silicon has a different charge / discharge mechanism than graphite. A solid electrolyte interface (SEI) film can continuously form at the interface between Si ions and Li ions in the electrolyte during charging and discharging. The formation of an irreversible SEI can consume many Li ions from the electrolyte and the cathode material. Therefore, the first cycle coulombic efficiency (also called initial coulombic efficiency, ICE) of silicon-based anode materials is usually only 65-85%, resulting in a large capacity loss. In addition, silicon has both a lower electrical conductivity and a lower lithium ion diffusion rate than graphite, which can limit silicon's performance at high current and high power conditions.

[0003] To solve the above problems, scientific researchers have proposed to improve the performance of silicon-based anode materials by doping, nanosizing, etc. Chinese patent CN101179126B discloses a doped silicon-based anode material for lithium-ion batteries. By doping with at least one element of boron, aluminum, gallium, antimony and phosphorus, the initial coulombic efficiency of the material is improved. CN101179126B requires high vacuum argon arc fusion welding in the fabrication process, which requires high reaction temperature (>1000°C), complex reaction (including fusion welding, low temperature blowing, rapid cooling, planetary ball mill grinding and other operations), and therefore high cost. CN108172775A discloses a phosphorus-doped silicon-based anode material. The examples show that the phosphorus-doped silicon-based anode has an initial coulombic efficiency of 91.7% with a specific capacity of 610.1mAh / g. The manufacturing method of CN108172775A requires spray drying, which results in low yield but high cost. CN103400971A discloses anode material doped with lithium silicate. When adding 50% amount of silicon and 35% amount of Li2SiO3, the resulting material has a specific capacity of 1156.2mAh / g and initial coulombic efficiency of 88.2%. There is room for further improvement of the cycle stability and initial coulombic efficiency of the raw material. CN111653738A discloses an anode material of amorphous carbon coated silicon-carbon with a core-shell structure. The material has a reversible charge capacity of 1765.54mAh / g, an ICE of 84.38%, and a charge capacity retention rate after 50 cycles of 82.24%, which leaves room for further improvement.

[0004] As mentioned above, some progress has been made in improving silicon-based negative electrode materials, but usually, it can only improve one performance of silicon-based negative electrode materials, rather than improving their comprehensive electrical properties. However, when used in high-energy density lithium-ion batteries, it is desired that the negative electrode material has excellent reversible charge capacity, initial coulombic efficiency and cycle charge capacity retention. In particular, it is desired that the negative electrode material has excellent initial coulombic efficiency and cycle charge capacity retention at the same time. Therefore, there is still a demand for developing a silicon-based negative electrode material that simultaneously improves initial coulombic efficiency, reversible charge capacity, cycle charge capacity retention and electrical conductivity. There is also a need for a simple method for producing such a silicon-based negative electrode material. Summary of the Invention

[0005] The present disclosure can solve the problems of low reversible charge capacity and low initial coulombic efficiency of silicon-based negative electrode materials in the prior art. The present disclosure provides a core-shell structured negative electrode material, a method for producing the negative electrode material, a negative electrode material obtained by the method, and a lithium ion battery. The negative electrode material of the present disclosure has improved reversible charge capacity (also called reversible charge specific capacity) and initial coulombic efficiency, and is particularly suitable for lithium ion batteries.

[0006] In order to achieve the above object, a first aspect of the present disclosure provides a negative electrode material, the negative electrode material having a core-shell structure, the core comprising a silicon-containing material, the shell comprising an organic lithium salt and a porous carbon membrane, and at least a portion of the lithium ions being inserted (intercalated) into the porous carbon membrane.

[0007] Preferably, the organic lithium salt is at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose and lithium alginate.

[0008] A second aspect of the present disclosure provides a method for producing a negative electrode material, comprising the steps of: (1) mixing a silicon source and a carbon source and then calcining the mixture; (2) mixing the fired product obtained in the step (1) with an organic lithium salt; and (3) A step of subjecting the material obtained by mixing in the step (2) to vacuum freeze-drying.

[0009] Preferably, the carbon source is a pitch, preferably at least one selected from the group consisting of petroleum pitch, coal tar pitch, natural pitch and modified pitch.

[0010] A third aspect of the present disclosure provides a negative electrode material produced by the above method.

[0011] A fourth aspect of the present disclosure provides the use of the above-described negative electrode material in a lithium-ion battery.

[0012] A fifth aspect of the present disclosure provides a lithium-ion battery including the above-described negative electrode material, a lithium-containing positive electrode material, a separator, and an electrolyte.

[0013] Specifically, the present disclosure may exemplify the following items:

[0014] 1. A silicon-carbon anode material, characterized in that the silicon-carbon anode material has a core-shell structure, the core comprises a silicon-containing material, and the shell comprises an organic lithium salt and a porous carbon membrane.

[0015] 2. The silicon-carbon anode material of item 1, wherein the porous carbon membrane covers the outer surface of the core, and the organic lithium salt is present in the porous carbon membrane.

[0016] 3. The organic lithium salt is present in an amount of 5 to 34 wt. %, the silicon-containing material is present in an amount of 65 to 90 wt. %, and the porous carbon membrane is present in an amount of 1 to 10 wt. %, based on the total amount of the silicon-carbon anode material; Preferably, relative to the total amount of the silicon-carbon negative electrode material, the organic lithium salt is present in an amount of 10 to 30% by weight, the silicon-containing material is present in an amount of 68 to 86% by weight, and the porous carbon film is present in an amount of 1 to 6% by weight. Preferably, the silicon-carbon negative electrode material further contains graphite. More preferably, the graphite is present in the core and / or the shell. Preferably, the mass ratio of the total amount of the silicon-containing material, the organic lithium salt, and the porous carbon film to the amount of the graphite is 1:1 to 10, and more preferably 1:1 to 5, for the silicon-carbon negative electrode material of item 1.

[0017] 4. The silicon-carbon negative electrode material of item 1, having a median particle size of 0.1 to 20 μm.

[0018] 5. The organic lithium salt is at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose, and lithium alginate. Preferably, the silicon-containing material is at least one selected from the group consisting of elemental silicon, SiO x (where 0.6 < x < 1.5) and silicon-containing alloys; preferably, the silicon-containing alloy is at least one selected from the group consisting of silicon-aluminum alloys, silicon-magnesium alloys, silicon-zirconium alloys, and silicon-boron alloys, for the silicon-carbon negative electrode material of any one of items 1 to 4.

[0019] 6. A method for manufacturing a silicon-carbon negative electrode material, comprising the following steps: (1) A step of mixing a silicon source and a carbon source and then firing the mixture; (2) A step of mixing the fired product obtained in the step (1) with an organic lithium salt; and, (3) A step of subjecting the material obtained by the mixing in the step (2) to vacuum freeze-drying.

[0020] 7. The silicon source is at least one selected from the group consisting of elemental silicon, SiO x (where 0.6 < x < 1.5) and a silicon-containing alloy; preferably, the silicon-containing alloy is at least one selected from the group consisting of a silicon-aluminum alloy, a silicon-magnesium alloy, a silicon-zirconium alloy, and a silicon-boron alloy; Preferably, the carbon source is at least one selected from the group consisting of petroleum pitch, coal tar pitch, natural pitch, and modified pitch, Preferably, the mass ratio of the silicon source to the carbon source is 1:(0.04 to 0.12) in the method of item 6.

[0021] 8. The mixing in the step (1) includes adding the silicon source and the carbon source into an organic solvent, and then performing ultrasonic stirring (preferably for 10 to 100 minutes), Preferably, the organic solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone, Preferably, the firing is performed at a temperature of 600 to 1000 °C (preferably 700 to 900 °C) for 10 to 240 minutes (preferably 20 to 60 minutes) in an inert atmosphere in the method of item 6.

[0022] 9. The organic lithium salt is at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose, and lithium alginate, Preferably, the organic lithium salt is used in an amount of 0.05 to 0.5 parts by weight (preferably 0.1 to 0.4 parts by weight) based on 1 part by weight of the silicon source, Preferably, the mixing in the step (2) includes adding the fired product obtained in the step (1) and the organic lithium salt into the solvent and stirring for 4 to 48 hours in any one of the methods of items 6 to 8.

[0023] 10. The method according to any one of items 6 to 9, wherein the vacuum freeze-drying step (3) is carried out at a temperature of -65°C or lower and at a vacuum degree of 120 Pa or lower for 4 to 48 hours.

[0024] 11. The method according to any one of items 6 to 10, further comprising the step of adding graphite in the step (1) and / or the step (2).

[0025] 12. The method further comprises a step (4) of mixing the product obtained in the vacuum freeze-drying step (3) with graphite, The method according to any one of items 6 to 10, preferably using the graphite in an amount of 1 to 15 parts by weight (preferably, 1 to 5 parts by weight) per part by weight of the product obtained in the vacuum freeze-drying in the step (3).

[0026] 13. A silicon-carbon negative electrode material produced by any one of the methods of items 6 to 12.

[0027] 14. Use of the silicon-carbon anode material of any one of items 1 to 5 and 13 in a lithium-ion battery.

[0028] 15. A lithium-ion battery comprising the silicon-carbon anode material of any one of items 1 to 5 and 13, a lithium-containing cathode material, a separator, and an electrolyte, Preferably, the lithium ion battery is a liquid lithium ion battery, a semi-solid lithium ion battery, or a solid lithium ion battery.

[0029] The core-shell structured anode material according to the present disclosure contains lithium elements, and at least a part of the lithium elements is inserted in the form of ions into the porous carbon film. It can not only solve the problems of low reversible charge capacity and low initial coulombic efficiency of conventional silicon-based anodes, but also suppress the crushing of electrode materials and uncontrollable growth of SEI film caused by the "volume effect" during charging and discharging of conventional silicon-based anodes. The anode material according to the present disclosure does not need to be pre-lithiated when used, and the reversible charge capacity of the anode material is greatly improved, and the energy density of lithium batteries can be greatly improved. [Brief description of the drawings]

[0030] [Figure 1] 1 shows a TEM image of the negative electrode material S-1 prepared in Example 1, where A is the nanosilicon core and B is the shell. [Diagram 2] 1 shows a full spectrum of X-ray photoelectron spectroscopy (XPS) of the negative electrode material S-1 produced in Example 1. [Diagram 3] 1 shows the Li-1s XPS spectrum of the negative electrode material S-1 produced in Example 1. [Figure 4] 1 shows the initial charge / discharge profile of the negative electrode material S-1 produced in Example 1. [Diagram 5] 1 shows the cycle stability profile of the negative electrode material S-1 prepared in Example 1. [Figure 6] 1 shows the initial charge / discharge profile of the negative electrode material D-1 produced in Comparative Example 1. [Figure 7] 1 shows the cycle stability profile of the negative electrode material D-1 prepared in Comparative Example 1. [Figure 8] 1 shows the Li-1s XPS spectrum of the negative electrode material D-2 prepared in Comparative Example 2. Detailed Description of the Invention

[0031] It should be understood that the endpoints and any values ​​within the ranges disclosed herein are not limited to the exact ranges or values, but include values ​​close to these ranges or values. For ranges of values, it is possible to combine between each endpoint of the range, between each endpoint and each point of the range, and between each point to give one or more new ranges of values, as if these ranges of values ​​were specifically disclosed herein. Except in the examples, all numerical values ​​of parameters in this specification should be understood as being modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value.

[0032] In this specification, the core-shell structure refers to an assembly structure formed by using one material (such as the carbon source and organic lithium salt in this disclosure) to uniformly coat another material (such as the silicon source in this disclosure) by chemical bonding or other forces.Preferably, the negative electrode material in the core-shell structure of this disclosure is nano-sized.

[0033] In this specification, the median particle size (or D 50 ) refers to the particle size when the cumulative particle size distribution rate reaches 50%. Median particle size is often used to represent the average particle size of a powder. In this disclosure, unless otherwise specified, the median particle size of a negative electrode material may be characterized by dynamic light scattering.

[0034] A first aspect of the present disclosure provides an anode material, the anode material having a core-shell structure, the core comprising a silicon-containing material, the shell comprising an organic lithium salt and a porous carbon membrane, and at least a portion of the lithium ions are intercalated in the porous carbon membrane.

[0035] Such an arrangement can not only improve the lithium ion permeability but also significantly improve the initial coulombic efficiency of the material. Preferably, the negative electrode material according to the present disclosure may further include a phosphorus-containing coating layer. The phosphorus-containing coating layer may be between the core and the shell. The phosphorus-containing coating layer may include a polymer having a polycyclic aromatic hydrocarbon structural segment. In one variation, the polymer having a polycyclic aromatic hydrocarbon structural segment may include a polymer having a polycyclic aromatic hydrocarbon structural segment. 13 The C-NMR spectrum contains signal peaks at 110 ppm to 140 ppm, indicating the presence of polycyclic aromatic hydrocarbon structural segments. 13 Message on chemical shifts of polycyclic aromatic hydrocarbons in C-NMR spectra is Harris, KJ, Reeve ZEM, et al. Electrochemical Changes in Lithium-Battery Electrodes Studied Using 7 Li NMR and Enhanced 13 C NMR of Graphene and Graphitic Carbons [J]. Chem. Mater. 2015, 27, 9, pp 3299-3305, which is fully incorporated herein by reference. The phosphorus in the phosphorus-containing coating layer and the silicon in the silicon-containing material are bonded via a chemical bond, preferably P(O)-O-Si. The bond between the phosphorus and silicon via P(O)-O-Si can be determined by X-ray photoelectron spectroscopy or 29 It may be characterized by Si-NMR spectroscopy.

[0036] Preferably, the negative electrode material according to the present disclosure may further contain graphite. Although the theoretical capacity of carbon is much lower than that of silicon, by introducing graphite into the negative electrode material, the low conductivity of silicon can be compensated, and at the same time, the maintenance of the cycle charge capacity can be significantly improved. Furthermore, the use of graphite is not subject to the problem of volume expansion that the silicon negative electrode material undergoes during charge and discharge. The position of graphite in the present invention is not particularly limited. Due to differences in processing conditions in the product, graphite may be present in the core, in the shell, or in both.

[0037] According to a preferred embodiment of the present disclosure, graphite is present in the core and / or the shell.

[0038] Preferably, the silicon-containing material is at least one selected from the group consisting of elemental silicon, SiO x (where 0.6 < x < 1.5) and silicon-containing alloys. The silicon-containing material may be commercially available or may be prepared by known methods.

[0039] Preferably, the silicon-containing alloy is at least one selected from the group consisting of silicon-aluminum alloy, silicon-magnesium alloy, silicon-zirconium alloy, and silicon-boron alloy. The content of silicon in the silicon-containing alloy may be selected within a wide range. For example, silicon may be present in an amount of 10 to 50% by weight based on the total amount of the silicon-containing alloy. The manufacturing method of the silicon-containing alloy is not particularly limited. In this specification, a specific method for manufacturing the silicon-containing alloy is provided. However, the present disclosure is not limited thereto. For example, the manufacturing method of the silicon-aluminum alloy may include the following steps: 1) a step of ball-milling aluminum powder and silicon powder for 30 minutes under the protection of an inert atmosphere; and 2) a step of treating the mixture obtained in the above step at 900°C for 10 hours.

[0040] Preferably, the organic lithium salt may be a salt formed from a compound containing an organic acid functional group (preferably a carboxyl group) and an alkaline compound containing lithium. Preferably, the organic lithium salt may be at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose, and lithium alginate. The molecular weight of the organic lithium salt may be selected within a wide range. Preferably, the weight average molecular weight of the organic lithium salt may be 2000 to 5000000, more preferably 80000 to 300000.

[0041] The content of the components in the negative electrode material according to the present disclosure may be selected within a wide range. Preferably, the organic lithium salt may be present in an amount of 5 to 34 wt%, the silicon-containing material may be present in an amount of 65 to 90 wt%, and the porous carbon membrane may be present in an amount of 1 to 10 wt%, based on the total amount of the negative electrode material. More preferably, the organic lithium salt may be present in an amount of 10 to 30 wt%, the silicon-containing material may be present in an amount of 68 to 86 wt%, and the porous carbon membrane may be present in an amount of 1 to 6 wt%, based on the total amount of the negative electrode material.

[0042] According to a preferred embodiment of the present disclosure, the negative electrode material may further comprise graphite, more preferably, the graphite may be present in the core and / or the shell, more preferably, the graphite is present in the shell.

[0043] The content of graphite may be selected within a wide range, and preferably, the mass ratio of the amount of graphite to the total amount of the silicon-containing material, the organic lithium salt, and the porous carbon membrane is 1:1-10, more preferably 1:1-5.

[0044] Preferably, the median diameter of the negative electrode material is 0.1 to 20 μm (for example, 0.1 μm, 0.5 μm, 1 μm, 10 μm, 15 μm, 20 μm, and any value in the range formed by any two of these values).

[0045] A second aspect of the present disclosure provides a method for producing a negative electrode material, comprising the steps of: (1) mixing a silicon source and a carbon source and then calcining the mixture; (2) mixing the fired product obtained in the step (1) with an organic lithium salt; and (3) A step of subjecting the material obtained by mixing in the step (2) to vacuum freeze-drying.

[0046] Preferably, the silicon source may be the silicon-containing material described above, or a silicon-containing precursor that can be converted to a silicon-containing material by calcination. More preferably, the silicon source may be the silicon-containing material described above. Suitable materials may be selected as described above, and will not be repeated here.

[0047] Preferably, the carbon source is pitch, preferably at least one selected from the group consisting of petroleum pitch, coal tar pitch, natural pitch and modified pitch. The preferred configuration is favorable for the formation of porous carbon, thereby improving the electrochemical performance of the prepared negative electrode material.

[0048] Petroleum pitch, coal tar pitch, natural pitch and modified pitch have the meanings commonly understood by those skilled in the art and may be commercially available.

[0049] The amount of the carbon source depends on the amount of the silicon source.Preferably, the mass ratio of the silicon source to the carbon source is 1:(0.04-0.12), for example, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.10, 1:0.11, 1:0.12, and any value in the range formed by any two of these values.

[0050] Preferably, the mixing in step (1) includes adding the silicon source and the carbon source to an organic solvent and stirring the organic solvent with ultrasonic waves. This preferred configuration is advantageous for uniformly coating the carbon source on the silicon surface.

[0051] The ultrasonic agitation time may be selected within a wide range. The ultrasonic agitation time is determined based on whether the silicon source and the carbon source can be dispersed in the organic solvent. Preferably, the ultrasonic agitation time is 10 to 100 minutes, more preferably 20 to 60 minutes.

[0052] The organic solvent may be an organic solvent commonly used in the art, and may be preferably at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone.

[0053] The amount of organic solvent may be selected within a wide range, for example the solids content of the slurry obtained by mixing may be 10-35% by weight.

[0054] According to one embodiment of the present disclosure, the method may further include a step of separating the mixed material after the mixing in step (1) and a step of calcining the solid obtained by the separation. The separation may be operated by any conventional separation method in the art (e.g., centrifugation). Preferably, the method may further include a step of drying the solid obtained by the separation and then calcining it. The drying conditions may be selected within a wide range. Preferably, the drying is performed at a temperature of 80-150° C. for 1-10 hours.

[0055] Preferably, the firing may be performed at a temperature of 600 to 1000°C (preferably 700 to 900°C) under an inert atmosphere for 10 to 240 minutes (preferably 20 to 60 minutes). The inert atmosphere may be provided by at least one selected from the group consisting of nitrogen, helium, argon, and krypton. The examples of the present disclosure use nitrogen for illustration purposes. However, the present disclosure is not limited thereto.

[0056] The heating rate during firing is not particularly limited. For example, it may be 1 to 10° C. / min. In the embodiment of the present disclosure, 5° C. / min is adopted for the purpose of explanation. However, the present disclosure is not limited thereto.

[0057] According to one embodiment of the present disclosure, the method may include a step of cooling the fired product obtained in step (1) (preferably to 50° C. or less (e.g., room temperature of 25° C.)) and then carrying out step (2). The cooling may be natural cooling.

[0058] Suitable materials for the organic lithium salt may be selected as described above and will not be repeated here.

[0059] Preferably, the organic lithium salt is used in an amount of 0.05 to 0.5 parts by weight (preferably, 0.1 to 0.4 parts by weight) per part by weight of the silicon source.

[0060] The operation of step (2) of mixing the calcined product obtained in step (1) with an organic lithium salt is not particularly limited. Preferably, the mixing in step (2) may include a step of adding the calcined product obtained in step (1) and the organic lithium salt to a solvent and stirring for 4 to 48 hours. The amount of the solvent may be selected within a wide range. For example, the solid content of the slurry obtained by mixing may be 10 to 35% by weight. Preferably, the solvent is water.

[0061] The vacuum freeze drying in step (3) can maintain the structure of the porous carbon obtained by the baking in step (1) and can insert at least a portion of the lithium ions into the porous carbon film.

[0062] Theoretically, the lower the temperature and vacuum degree of vacuum drying, the better. However, as the temperature and vacuum degree decrease, the energy consumption increases. In fact, there are operational constraints on the vacuum freeze-drying apparatus. Considering the energy consumption and effect, it is preferable to carry out the vacuum freeze-drying in step (3) at a temperature of -65°C or lower (preferably -80°C to -65°C) and a vacuum degree of 120 Pa or lower (preferably 90 to 120 Pa).

[0063] The time for the freeze-drying may be chosen within a wide range. Preferably, the freeze-drying is carried out for a period of 4 to 48 hours, preferably 8 to 32 hours.

[0064] Preferably, the present invention may further include a step of forming a phosphorus-containing coating layer before step (1). For example, the formation may be accomplished by a method including the steps of: (a) contacting a silicon-containing material, a phosphorus source, and a solvent at 30 to 80° C. to graft the phosphorus source onto the surface of the silicon-containing material; and (b) subjecting the silicon-containing material to baking at an elevated temperature to convert the phosphorus source around the silicon-containing material into a phosphorus-containing coating layer comprising a polymer having a polycyclic aromatic hydrocarbon structural segment; The temperature-raising firing is Heating at a first temperature of 400-500°C at a first heating rate; Heating at a second temperature of 600 to 800 ° C. at a second heating rate, the second heating rate being lower than the first heating rate; and maintaining at a second temperature.

[0065] The phosphorus source may be any phosphorus-containing precursor that can be converted, for example by polycondensation, into a polymer having polycyclic aromatic hydrocarbon structural segments. A preferred phosphorus source is selected from the group consisting of organic polybasic phosphoric acids and their esters or salts. Preferably, the organic polybasic phosphoric acid is phytic acid. A preferred solvent in step (a) may be at least one selected from the group consisting of toluene, N,N-dimethylformamide, N,N-dimethylacetamide and N-methylpyrrolidone. Preferably, the solvent may be present in an amount such that the solids content of the material obtained in step (a) is 5-40% by weight. Preferably, the temperature-raising calcination may include heating to a first temperature of 450-500°C (e.g., 480°C) at a first heating rate of 1-10°C / min, preferably 5-10°C / min; then heating to a second temperature of 600-650°C (e.g., 620°C) at a second heating rate of 1-5°C / min, preferably 1-3°C / min; and maintaining at the second temperature for 1-8 hours, preferably 2-4 hours.

[0066] Preferably, the method further comprises the step of adding graphite, which may be added in step (1) and / or step (2), or after step (3).

[0067] According to a preferred embodiment of the present disclosure, the method may further include adding graphite in step (1) and / or step (2). In particular, the adding of graphite in step (1) may include, but is not limited to, mixing a silicon source, a carbon source, and graphite, and then calcining the mixture. In particular, the adding of graphite in step (2) may include, but is not limited to, mixing the calcined product obtained in step (1), an organic lithium salt, and graphite.

[0068] According to another preferred embodiment of the present disclosure, the method may further comprise a step (4) of mixing the product obtained by vacuum freeze drying in step (3) with graphite.

[0069] In step (4), it is preferable to add graphite, which is advantageous for easily adjusting the reversible charge capacity of the produced negative electrode material.

[0070] According to another preferred embodiment of the present disclosure, graphite is used in an amount of 1 to 15 parts by weight (preferably 1 to 5 parts by weight) per part by weight of the product obtained in the vacuum freeze-drying in step (3).

[0071] A third aspect of the present disclosure provides a negative electrode material produced by the above method. The negative electrode material may have the structure and chemical composition described above, which will not be repeated here.

[0072] The fourth aspect of the present disclosure provides the use of the above-mentioned negative electrode material in a lithium ion battery.Compared with conventional pure graphite negative electrode materials, the above-mentioned negative electrode material contains silicon, which has a higher theoretical capacity, and significantly improves the reversible charge capacity.Therefore, when the above-mentioned negative electrode material is used in a lithium ion battery, the energy density of the lithium ion battery can be improved.

[0073] A fifth aspect of the present disclosure provides a lithium-ion battery including the negative electrode material of the present disclosure, a lithium-containing positive electrode material, a separator, and an electrolyte.

[0074] The lithium ion battery of the present disclosure has a structure well known to those skilled in the art. In general, a separator is disposed between a positive electrode and a negative electrode. The positive electrode comprises a positive electrode material, and the negative electrode comprises a negative electrode material. The chemical composition of the positive electrode material is not particularly limited. The positive electrode material may be any lithium-based positive electrode material commonly used in the art.

[0075] In the lithium ion batteries of the present disclosure, the separator may be selected from a variety of separators commonly used in lithium ion batteries, such as a polypropylene microporous film, a polyethylene mat, a glass fiber mat, or an ultra-fine glass fiber paper.

[0076] In the lithium ion battery of the present disclosure, the electrolyte may be various conventional electrolytes, such as non-aqueous electrolytes. The non-aqueous electrolyte is a solution formed by an electrolyte lithium salt in a non-aqueous solvent. Any conventional non-aqueous electrolyte known to those skilled in the art may be used. For example, the electrolyte may be at least one selected from the group consisting of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorosilicate (LiSiF6). The non-aqueous solvent may be selected from the group consisting of linear esters and cyclic esters, and mixtures thereof. The linear ester may be at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC), methyl propyl carbonate (MPC), and dipropyl carbonate (DPC). The cyclic ester may be at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0077] The present invention will be described in detail from the following examples, which are intended to illustrate the invention and are not intended to limit the invention in any way.

[0078] [Test Method] (1. Material Identification) (1.1 Transmission electron microscope (TEM) image) The morphology of the negative electrode material samples was characterized by transmission electron microscopy. Specifically, the transmission electron microscope used was a JEM-2100 transmission electron microscope manufactured by JEOL Ltd., and the test conditions included an acceleration voltage of 160 KV. The samples were placed on a copper support net and then inserted into the electron microscope for observation. A magnification of 800,000 was used for the observation.

[0079] (1.2 Total X-ray photoelectron spectroscopy spectrum) The negative electrode material samples were characterized with an ESCALAB 250Xi X-ray photoelectron spectroscopy tester from ThermoFisher Scientific Company, USA. The test conditions were room temperature 25 °C, vacuum degree 5 × 10 -10 It included less than mba, an operating voltage of 15 kV, Al Kα as the radiation source, a full spectrum pass energy of 100 eV, and a step length of 1.0 ev.

[0080] (1.3 Li-1s XPS spectrum) The negative electrode material samples were characterized with an ESCALAB 250Xi X-ray photoelectron spectroscopy tester from ThermoFisher Scientific Company, USA. The test conditions were room temperature 25 °C, vacuum degree 5 × 10 -10 The devices included less than mba, an operating voltage of 15 kV, Al Kα as the radiation source, a narrow spectral pass energy of 30 eV, a step length of 0.05 ev, and a beam spot of 500 μm.

[0081] (1.4 Median particle size (D 50 )) The median particle size is characterized by dynamic light scattering according to GB / T 19077-2016.

[0082] (2. Electronic properties of materials) The negative electrode materials prepared in the following examples and comparative examples were assembled into lithium ion battery samples. The electrochemical properties of the obtained lithium ion battery samples were tested using a Wuhan blue battery test system (CT2001B). The test conditions included a voltage range of 0.005V to 3V. Each negative electrode material was assembled into 10 samples in the form of coin cells. The battery performance of the samples was tested under the same voltage and current. The average value was used as the measured value.

[0083] (2.1) Initial charge / discharge profile The assembled lithium-ion battery sample was subjected to a first charge / discharge under a voltage range of 0.05V-3V and a current ratio (current rate) of 0.1C, and the first charge / discharge profile was obtained. The battery test system (CT2001B) gave the first discharge capacity and the first charge capacity of the tested battery. The first discharge capacity was the specific capacity of the negative electrode material, and the first charge capacity was the reversible charge capacity of the negative electrode material. The initial coulombic efficiency (also called "ICE") could be calculated from:

[0084] ICE = reversible charge capacity of negative electrode material / specific capacity of negative electrode material (2.2) Cycling stability test The assembled lithium-ion battery samples were subjected to charging and discharging for selected cycles (e.g., 20, 50, or 100 cycles) at a current rate of 0.2 C. The reversible charge capacity of the samples at each cycle was measured. The cycle charge capacity retention rate of each cycle was calculated according to the following:

[0085] Cycle charge capacity retention rate = Reversible charge capacity at selected cycle / Reversible charge capacity at first charge × 100% The cycling stability profile was plotted by taking the cycle number as the X-axis and the cycling charge capacity retention as the Y-axis.

[0086] (3. Reagents) In the following examples and comparative examples, the petroleum pitch used was purchased from TIPCO Company under the brand PMA. The coal tar pitch was purchased from Longxin material Trade Co., Ltd. under the brand Low Temperature Pitch (100-115).

[0087] A lithium polyacrylate was prepared. Specifically, 10 g of polyacrylic acid having a weight average molecular weight of 240,000 was added to 40 g of deionized water to prepare a polyacrylic acid solution having a concentration of 20% by mass. 3.4 g of lithium hydroxide was added to the polyacrylic acid solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium polyacrylate.

[0088] Lithium polymethacrylate was prepared. Specifically, 10 g of polymethacrylic acid having a weight average molecular weight of 240,000 was added to 40 g of deionized water to prepare a polymethacrylic acid solution having a concentration of 20% by mass. 3.4 g of lithium hydroxide was added to the polymethacrylic acid solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium polymethacrylate.

[0089] A lithium polymaleate was prepared. Specifically, 10 g of polymaleic acid having a weight average molecular weight of 240,000 was added to 40 g of deionized water to prepare a polymaleic acid solution having a concentration of 20% by mass. 3.4 g of lithium hydroxide was added to the polymaleic acid solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium polymaleate.

[0090] A lithium polyfumarate was prepared. Specifically, 10 g of polyfumaric acid having a weight average molecular weight of 240,000 was added to 40 g of deionized water to prepare a polyfumaric acid solution having a concentration of 20% by mass. 3.4 g of lithium hydroxide was added to the polyfumaric acid solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium polyfumarate.

[0091] Lithium carboxymethylcellulose was prepared. Specifically, 10 g of sodium carboxymethylcellulose having a weight average molecular weight of 120,000 was added to 40 g of deionized water to prepare a sodium carboxymethylcellulose solution having a concentration of 20% by mass. 3.1 g of lithium hydroxide was added to the sodium carboxymethylcellulose solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium carboxymethylcellulose.

[0092] Lithium alginate was prepared. Specifically, 10 g of sodium alginate having a weight average molecular weight of 80,000 was added to 40 g of deionized water to prepare a sodium alginate solution having a concentration of 20% by mass. 1.2 g of lithium hydroxide was added to the sodium alginate solution. The mixture was heated at 40° C. under stirring until all solids were dissolved, and then dried at 100° C. for 4 hours to obtain lithium alginate.

[0093] The polyacrylic acid, polymethacrylic acid, polymaleic acid, polyfumaric acid, sodium carboxymethylcellulose and sodium alginate used were purchased from Aladdin reagent company.

[0094] In the following Examples and Comparative Examples, room temperature was set to 25°C.

[0095] Example 1 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a particle size of 120 nm and 0.12 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0096] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0097] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0098] (4) 0.125 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum of 100 Pa, and dried for 12 hours. The result was lithium-containing negative electrode material S-1. The median particle size and the content of each component of lithium-containing negative electrode material S-1 are shown in Table 1.

[0099] The lithium-containing negative electrode material S-1 was sampled and the above-mentioned material identification test was carried out. Figure 1 is a TEM image of the lithium-containing negative electrode material S-1. As can be seen from the figure, the silicon nanoparticles were uniformly coated to form a core-shell structure, and the outer surface of the core was covered with a porous carbon film. Figure 2 was the full XPS spectrum of the lithium-containing negative electrode material S-1. As can be seen from the spectrum, the negative electrode material contained the elements of lithium, carbon, and silicon. Figure 3 was the Li-1s XPS spectrum of the lithium-containing negative electrode material S-1. As shown in Figure 3, a significant signal peak appeared at a binding energy of 64.1 eV. This signal peak corresponded to the complex of LiC6. The formation of the complex LiC6 indicated that the lithium ions had moved into the porous carbon film and were between the layers of the carbon atoms. That is, the lithium ions had been inserted into the porous carbon film.

[0100] A CR2016 coin battery was assembled using the lithium-containing negative electrode material S-1 obtained in Example 1 and the metallic lithium sheet as the positive electrode and the negative electrode, respectively, a 1 mol / L LiPF6 solution as the electrolyte (a mixture of vinyl carbonate and diethyl carbonate in a volume ratio of 3:7 was used as the solvent), and a polypropylene microporous membrane as the separator. The battery was subjected to a test for detecting electrical properties as described above to characterize the electrical properties of the lithium-containing negative electrode material S-1 of Example 1.

[0101] 4 is a profile of the initial charge and discharge of a coin battery based on the lithium-containing negative electrode material S-1 of Example 1. As shown in the figure, the lithium-containing negative electrode material S-1 of Example 1 had a reversible charge capacity of 3000 mAh / g and an ICE of 86.9%.

[0102] 5 is a cycle stability profile of a coin battery based on the lithium-containing negative electrode material S-1 of Example 1. As shown in the figure, the lithium-containing negative electrode material S-1 of Example 1 had a charge capacity retention rate of about 92% after 20 charge-discharge cycles at a current rate of 0.2C.

[0103] Comparative Example 1 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a particle size of 120 nm and 0.12 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0104] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0105] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained, which was designated as anode material D-1.

[0106] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the anode material D-1 obtained in Comparative Example 1.

[0107] Figure 6 shows the initial charge-discharge profile of a coin battery based on the negative electrode material D-1 of Comparative Example 1. As shown in the figure, the negative electrode material D-1 of Comparative Example 1 had a reversible charge capacity of 908 mAh / g and an ICE of 38.9%.

[0108] Figure 7 shows the cycle stability profile of the coin cell based on the negative electrode material of Comparative Example 1. As shown in the figure, the negative electrode material of Comparative Example 1 had a charge capacity retention rate of 6% after 12 charge-discharge cycles at a current rate of 0.2C.

[0109] Comparative Example 2 Example 1 was repeated, except that the resulting slurry was subjected to ultrasonic stirring and then air-dried for 12 hours (at a temperature of 100° C.) to obtain lithium-containing negative electrode material D-2.

[0110] The lithium-containing negative electrode material D-2 was sampled and the above-mentioned material identification test was performed. Figure 8 is the Li-1s XPS spectrum of the lithium-containing negative electrode material D-2. As shown in Figure 8, a signal peak appeared at a binding energy of 56.3 eV. This was due to the signal peak of the organic lithium salt (i.e., lithium polyacrylate). There was no significant signal peak at a binding energy of 64.1 eV corresponding to the LiC6 complex. This indicates that no intercalation of lithium ions occurred in the porous carbon film.

[0111] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Comparative Example 2. The test results showed that the material of Comparative Example 2 had a reversible charge capacity of 795 mAh / g and an ICE of 36.3%. The material had a charge capacity retention of about 30% after 20 charge-discharge cycles at a current rate of 0.2C.

[0112] Comparative Example 3 Example 1 was repeated, except that the lithium polyacrylate was replaced with the same amount of lithium carbonate, resulting in lithium-containing negative electrode material D-3.

[0113] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Comparative Example 3. The test results showed that the material of Comparative Example 3 had a reversible charge capacity of 820 mAh / g and an ICE of 31%. The material had a charge capacity retention rate of about 10% after 10 charge-discharge cycles at a current rate of 0.2C.

[0114] Example 2 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a particle size of 120 nm and 0.04 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0115] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0116] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0117] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum degree of 100 Pa, and dried for 12 hours. The result was lithium-containing negative electrode material S-2. The median particle size and the content of each component of lithium-containing negative electrode material S-2 are shown in Table 1.

[0118] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-2 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-2 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0119] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 2. The test results showed that the material of Example 2 had a reversible charge capacity of 2812 mAh / g with an ICE of 87.6%. The material had a charge capacity retention of about 90% after 15 charge-discharge cycles at a current rate of 0.2C.

[0120] Example 3 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a diameter of 120 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0121] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0122] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 700°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0123] (4) 0.3 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum degree of 100 Pa, and dried for 12 hours. The result was lithium-containing negative electrode material S-3. The median particle size and the content of each component of lithium-containing negative electrode material S-3 are shown in Table 1.

[0124] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-3 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-3 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0125] A coin cell was fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 3. The test results showed that the material of Example 3 had a reversible charge capacity of 2760 mAh / g with an ICE of 89.3%. The material had a charge capacity retention of about 85% after 15 charge-discharge cycles at a current rate of 0.2C.

[0126] Example 4 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a diameter of 300 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0127] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0128] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 900°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0129] (4) 0.32 g of lithium alginate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum degree of 100 Pa, and dried for 12 hours. The result was lithium-containing negative electrode material S-4. The median particle size and the content of each component of lithium-containing negative electrode material S-4 are shown in Table 1.

[0130] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-4 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-4 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0131] A coin cell was fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 4. The test results showed that the material in Example 4 had a reversible charge capacity of 2720 mAh / g with an ICE of 87.9%. The material had a charge capacity retention of about 85% after 15 charge-discharge cycles at a current rate of 0.2C.

[0132] Example 5 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a diameter of 300 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0133] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0134] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0135] (4) 0.42 g of lithium carboxymethylcellulose and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum degree of 100 Pa, and dried for 12 hours. The result was lithium-containing negative electrode material S-5. The median particle size and the content of each component of lithium-containing negative electrode material S-5 are shown in Table 1.

[0136] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-5 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-5 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0137] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 5. The test results showed that the material of Example 5 had a reversible charge capacity of 2870 mAh / g with an ICE of 86.1%. The material had a charge capacity retention of about 91% after 18 charge-discharge cycles at a current rate of 0.2C.

[0138] Example 6 (1) Add 10 g of N,N-dimethylformamide to D 501 g of silicon powder having a diameter of 120 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0139] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0140] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0141] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. The resulting stirred slurry was then placed in a freeze-drying vacuum oven with a cold trap temperature of -80°C and a cavity vacuum of 100 Pa, and dried for 12 hours.

[0142] (5) The product obtained after drying in step (4) was mixed with artificial graphite in a mass ratio of 1:4. The result was a lithium-containing negative electrode material S-6 with a design capacity of 900 mAH / g. The median particle size and the content of each component of the lithium-containing negative electrode material S-6 are shown in Table 1.

[0143] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-6 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-6 had a core-shell structure, the outer surface of the core was covered with a porous carbon film and graphite, and lithium ions were inserted into the porous carbon film.

[0144] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 6. The test results showed that the material of Example 6 had a reversible charge capacity of 912 mAh / g and an ICE of 90.6%. The material had a charge capacity retention of about 96% after 100 charge-discharge cycles at a current rate of 0.2C.

[0145] Example 7 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a diameter of 120 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0146] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0147] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0148] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. The resulting stirred slurry was then placed in a freeze-drying vacuum oven with a cold trap temperature of -80°C and a cavity vacuum of 100 Pa, and dried for 12 hours.

[0149] (5) The product obtained after drying in step (4) was mixed with artificial graphite in a mass ratio of 1:5. The result was a lithium-containing negative electrode material S-7 with a design capacity of 700 mAH / g. The median particle size and the content of each component of the lithium-containing negative electrode material S-7 are shown in Table 1.

[0150] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-7 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-7 had a core-shell structure, the outer surface of the core was covered with a porous carbon film and graphite, and lithium ions were inserted into the porous carbon film.

[0151] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 7. The test results showed that the material of Example 7 had a reversible charge capacity of 752 mAh / g and an ICE of 91.2%. The material had a charge capacity retention of about 96% after 150 charge-discharge cycles at a current rate of 0.2C.

[0152] Example 8 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon powder having a diameter of 120 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0153] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0154] (3) The pitch-coated silicon material obtained in step (2) above was treated by heating to 800°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon material was obtained.

[0155] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon material obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. The resulting stirred slurry was then placed in a freeze-drying vacuum oven with a cold trap temperature of -80°C and a cavity vacuum of 100 Pa, and dried for 12 hours.

[0156] (5) The product obtained after drying in step (4) was mixed with artificial graphite in a mass ratio of 1:1. The result was a lithium-containing negative electrode material S-8 with a design capacity of 1500 mAH / g. The median particle size and the content of each component of the lithium-containing negative electrode material S-8 are shown in Table 1.

[0157] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-8 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-8 had a core-shell structure, the outer surface of the core was covered with a porous carbon film and graphite, and lithium ions were inserted into the porous carbon film.

[0158] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 8. The test results showed that the material in Example 8 had a reversible charge capacity of 1512 mAh / g with an ICE of 88.9%. The material had a charge capacity retention of about 90% after 150 charge-discharge cycles at a current rate of 0.2C.

[0159] Example 9 (1) Add 10 g of N,N-dimethylformamide to D 50 1 g of silicon monoxide (SiOx, x=1) powder with a particle size of 120 nm and 0.08 g of petroleum pitch were added and ultrasonically stirred for 40 minutes.

[0160] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0161] (3) The pitch-coated silicon monoxide obtained in step (2) above was treated by heating to 750°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, carbon-coated silicon monoxide was obtained.

[0162] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon monoxide obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum degree of 100 Pa, and dried for 12 hours. The result was a lithium-containing silicon monoxide-based negative electrode material (lithium-containing silicon monoxide-based negative electrode material) S-9. The median particle size and the content of each component of the lithium-containing silicon monoxide-based negative electrode material S-9 are shown in Table 1.

[0163] The TEM image, XPS full spectrum, and Li-1s XPS spectrum of the lithium-containing silicon monoxide-based negative electrode material S-9 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing silicon monoxide-based negative electrode material S-9 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0164] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 9. The test results showed that the material of Example 9 had a reversible charge capacity of 1632 mAh / g and an ICE of 83.1%. The material had a charge capacity retention rate of about 90% after 200 charge-discharge cycles at a current rate of 0.2C.

[0165] Example 10 (1)D 50 Aluminum powder with a diameter of 100 nm and D 50 The silicon powder having a diameter of 120 nm was ball milled in a mass ratio of 4:1 under the protection of a nitrogen atmosphere for 30 minutes. The resulting mixture was calcined at 900°C for 10 hours in a nitrogen tube furnace. The resulting silicon-aluminum alloy powder (D 50 The diameter of the powder was 200 nm and the silicon content was 20% by weight. 1 g of silicon-aluminum alloy powder and 0.08 g of petroleum pitch were added to 10 g of N,N-dimethylformamide, and the mixture was subjected to ultrasonic stirring for 40 minutes.

[0166] (2) The slurry obtained after ultrasonic agitation was transferred to a 50 mL centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried (100° C. for 4 hours).

[0167] (3) The pitch-coated silicon-aluminum alloy obtained in step (2) above was treated by heating to 750°C at a rate of 5°C / min in a tubular furnace and maintaining it for 30 minutes under a nitrogen atmosphere. After naturally cooling to room temperature, a carbon-coated silicon-aluminum alloy was obtained.

[0168] (4) 0.15 g of lithium polyacrylate and the carbon-coated silicon-aluminum alloy obtained in step (3) above were added to 3 mL of deionized water and stirred at room temperature for 12 hours. Next, the slurry obtained after stirring was placed in a freeze-drying vacuum oven with a cooling trap temperature of -80°C and a cavity vacuum of 100 Pa, and dried for 12 hours. The result was a lithium-containing silicon-aluminum-based negative electrode material (lithium-containing silicon-aluminum-based negative electrode material) S-10. The median particle size and the content of each component of the lithium-containing silicon-aluminum-based negative electrode material S-10 are shown in Table 1.

[0169] The TEM image, XPS full spectrum, and Li-1s XPS spectrum of the lithium-containing silicon-aluminum-based negative electrode material S-10 were similar to those in Figures 1 to 3. This indicated that the obtained lithium-containing silicon-aluminum-based negative electrode material S-10 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0170] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 10. The test results showed that the material of Example 10 had a reversible charge capacity of 721 mAh / g and an ICE of 84.1%. The material had a charge capacity retention of about 90% after 200 charge-discharge cycles at a current rate of 0.2C.

[0171] Example 11 Example 1 was repeated, except that the petroleum pitch was replaced with the same amount of coal tar pitch. The result was lithium-containing negative electrode material S-11. The median particle size and the content of each component of the lithium-containing negative electrode material S-11 are shown in Table 1.

[0172] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-11 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-11 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0173] A coin cell was fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 11. The test results showed that the material of Example 11 had a reversible charge capacity of 2932 mAh / g and an ICE of 88.7%. The material had a charge capacity retention of about 85% after 30 charge-discharge cycles at a current rate of 0.2C.

[0174] Example 12 Example 1 was repeated, except that the lithium polyacrylate was replaced with the same amount of lithium polymethacrylate. The result was lithium-containing negative electrode material S-12. The median particle size and the content of each component of the lithium-containing negative electrode material S-12 are shown in Table 1.

[0175] The TEM image, XPS full spectrum, and Li-1s XPS spectrum of the lithium-containing negative electrode material S-12 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-12 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0176] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 12. The test results showed that the material of Example 12 had a reversible charge capacity of 2895 mAh / g and an ICE of 87.1%. The material had a charge capacity retention of about 85% after 30 charge-discharge cycles at a current rate of 0.2C.

[0177] Example 13 Example 1 was repeated, except that the lithium polyacrylate was replaced with the same amount of lithium polymaleate. The result was lithium-containing negative electrode material S-13. The median particle size and the content of each component of the lithium-containing negative electrode material S-13 are shown in Table 1.

[0178] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-13 were the same as those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-13 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0179] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 13. The test results showed that the material of Example 13 had a reversible charge capacity of 2925 mAh / g and an ICE of 86.8%. The material had a charge capacity retention of about 85% after 30 charge-discharge cycles at a current rate of 0.2C.

[0180] Example 14 Example 1 was repeated, except that the lithium polyacrylate was replaced with the same amount of lithium polyfumarate. The result was lithium-containing negative electrode material S-14. The median particle size and the content of each component of the lithium-containing negative electrode material S-14 are shown in Table 1.

[0181] The TEM image, XPS full spectrum and Li-1s XPS spectrum of the lithium-containing negative electrode material S-14 were similar to those in Figures 1 to 3, respectively. This indicated that the obtained lithium-containing negative electrode material S-14 had a core-shell structure, the outer surface of the core was covered with a porous carbon film, and lithium ions were inserted into the porous carbon film.

[0182] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with the material obtained in Example 14. The test results showed that the material of Example 14 had a reversible charge capacity of 2963 mAh / g and an ICE of 86.5%. The material had a charge capacity retention of about 85% after 30 charge-discharge cycles at a current rate of 0.2C.

[0183] Example 15 1) 10 g of N,N-dimethylformamide and 0.272 g of phytic acid were mixed to form a solution. 0.54 g of silicon powder (D 50 = 100 nm) was added to the solution. The mixture was heated to 40°C under stirring and maintained for 60 minutes. After reaction, the solid powder was vacuum filtered, washed and dried under vacuum at 80°C for 4 hours.

[0184] 2) The solid was heated in a tube furnace at a first heating rate of 5° C. / min to 480° C., then at a second heating rate of 2° C. / min to 620° C., and maintained at 620° C. for 3 hours. After cooling to room temperature, the resulting product was named phosphorus-coated silicon-containing material S-15-1.

[0185] 3) 1.5 g of phosphorus-coated silicon-containing material S-15-1 and 0.18 g of petroleum pitch were added to 15 g of N,N-dimethylformamide and ultrasonically stirred for 60 minutes. The slurry obtained after ultrasonic stirring was transferred to a centrifuge tube and centrifuged at 5000 rpm for 5 minutes. The solid at the bottom was collected and dried at 100°C for 4 hours to obtain pitch-coated S-15-1.

[0186] 4) The pitch-coated S-15-1 was treated in a tube furnace by heating to 800°C at a rate of 5°C / min and maintaining for 30 minutes under nitrogen atmosphere. After natural cooling to room temperature, the carbon-coated S-15-1 was obtained.

[0187] 5) 0.188g of lithium polyacrylate and carbon-coated S-15-1 was added to 5mL of deionized water and stirred at room temperature for 12 hours. The resulting slurry was then placed in a freeze-drying vacuum oven with a cold trap temperature of -80°C and a cavity vacuum of 100Pa and dried for 12 hours. The result was anode material S-15.

[0188] Coin cells were fabricated and tested for electrical properties as outlined in Example 1, except that the lithium-containing anode material S-1 was replaced with material S-15 obtained in Example 15. The test results showed that the material of Example 15 had a reversible charge capacity of 3480 mAh / g with an ICE of 91.2%. The material had a charge capacity retention of 94.8% after 30 charge-discharge cycles at a current rate of 0.2C.

[0189] [Table 1]

[0190] From the above examples and results, it can be seen that the anode material of the present disclosure has improved reversible charge capacity. When used in a lithium ion battery, the anode material of the present disclosure can improve the energy density of the lithium battery. More importantly, it can be seen that the anode material of the present disclosure simultaneously improves the initial coulombic efficiency and the cycle charge capacity retention rate, especially the cycle charge capacity retention rate over a long period of time.

[0191] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited thereto. In addition, within the technical scope of the present invention, various simple modifications, including combinations of various technical features in a more suitable manner than others, may be made into the embodiments of the present invention. These simple modifications and combinations should also be regarded as the contents disclosed in this specification and should be regarded as the contents within the protection scope of the present disclosure.

Claims

1. A negative electrode material, The negative electrode material has a core-shell structure, the core comprises a silicon-containing material; The shell comprises an organic lithium salt and a porous carbon membrane, and at least a portion of the lithium ions are intercalated into the porous carbon membrane.

2. 10. The negative electrode material of claim 1, further comprising a phosphorus-containing coating layer between the core and the shell.

3. The phosphorus-containing coating layer comprises a polymer having a polycyclic aromatic hydrocarbon structural segment, or 3. The negative electrode material of claim 2, wherein the phosphorus-containing coating layer is made from phytic acid.

4. 2. The negative electrode material according to claim 1, wherein the organic lithium salt is present in an amount of 5 to 34 wt%, the silicon-containing material is present in an amount of 65 to 90 wt%, and the porous carbon membrane is present in an amount of 1 to 10 wt%, based on the total amount of the negative electrode material.

5. The negative electrode material of claim 4, wherein the negative electrode material further comprises graphite.

6. The negative electrode material of claim 5, wherein the graphite is present in the core and / or the shell.

7. The negative electrode material described in claim 5, wherein the mass ratio of the total amount of the silicon-containing material, the organic lithium salt, and the porous carbon film to the amount of the graphite is 1:1 to 10.

8. 2. The negative electrode material according to claim 1, wherein the median particle size is 0.1 to 20 μm.

9. The organic lithium salt is at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose, and lithium alginate, or The silicon-containing material is elemental silicon, SiO x (wherein 0.6<x<1.5) and at least one selected from the group consisting of a silicon-containing alloy; and the silicon-containing alloy is at least one selected from the group consisting of a silicon-aluminum alloy, a silicon-magnesium alloy, a silicon-zirconium alloy, and a silicon-boron alloy.

10. A method for producing a negative electrode material, comprising the steps of: (1) mixing a silicon source and a carbon source and then calcining the mixture; (2) mixing the fired product obtained in the step (1) with an organic lithium salt; and (3) A step of subjecting the material obtained by mixing in the step (2) to vacuum freeze-drying.

11. The silicon source is elemental silicon, SiO x wherein 0.6<x<1.5, and at least one selected from the group consisting of a silicon-containing alloy, wherein the silicon-containing alloy is at least one selected from the group consisting of a silicon-aluminum alloy, a silicon-magnesium alloy, a silicon-zirconium alloy, and a silicon-boron alloy; or The carbon source is at least one selected from the group consisting of petroleum pitch, coal tar pitch, natural pitch and modified pitch; or The method of claim 10, wherein the mass ratio of the silicon source to the carbon source is 1:(0.04-0.12).

12. The method according to claim 10, wherein the mixing in step (1) comprises adding the silicon source and the carbon source to an organic solvent and ultrasonically stirring the organic solvent.

13. The organic solvent is at least one selected from the group consisting of N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone, or The method of claim 12, wherein the calcination is carried out at a temperature of 600-1000° C. under an inert atmosphere for a period of 10-240 minutes.

14. The organic lithium salt is at least one selected from the group consisting of lithium polyacrylate, lithium polymethacrylate, lithium polymaleate, lithium polyfumarate, lithium carboxymethylcellulose, and lithium alginate, or The organic lithium salt is used in an amount of 0.05 to 0.5 parts by weight per part by weight of the silicon source, or The method according to claim 12, wherein the mixing in step (2) includes adding the fired product obtained in step (1) and the organic lithium salt to the solvent and stirring for 4 to 48 hours.

15. The method according to claim 14, wherein the vacuum freeze-drying step (3) is carried out at a temperature of −65° C. or lower and a vacuum degree of 120 Pa or lower for 4 to 48 hours.

16. The method further comprises adding graphite in the step (1) and / or the step (2), The method according to any one of claims 10 to 15, further comprising a step (4) of mixing the product obtained in the vacuum freeze drying of step (3) with graphite.

17. The method according to claim 16, wherein graphite is used in an amount of 1 to 15 parts by weight per 1 part by weight of the product obtained in the vacuum freeze-drying of step (3).

18. The method further includes a step of forming a phosphorus-containing coating layer prior to step (1) by a method including the steps of: (a) contacting the silicon source, the phosphorus source and a solvent at 30-80° C. to graft the phosphorus source onto the surface of the silicon source; and (b) subjecting the resulting product to baking at an elevated temperature to convert the phosphorus source surrounding the silicon source into a phosphorus-containing coating layer comprising a polymer having a polycyclic aromatic hydrocarbon structural segment; The temperature-raising firing is heating at a first temperature between 400 and 500° C. at a first heating rate; heating to a second temperature of 600-800° C. at a second heating rate, the second heating rate being lower than the first heating rate; and maintaining at the second temperature.

19. The phosphorus source is phytic acid; or The solvent is at least one selected from the group consisting of toluene, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; or The temperature-raising firing is heating to a first temperature of 450-500° C. at a first heating rate of 1-10° C. / min; then heating to a second temperature of 600-650° C. at a second heating rate of 1-5° C. / min; and maintaining at the second temperature for 1 to 8 hours.

Citation Information

Patent Citations

  • Negative electrode active material, mixed negative electrode active material substance, and method for producing negative electrode active material

    WO2018061536A1

  • Secondary battery, battery pack, electric vehicle, electric tool and electronic device

    WO2018146865A1