Resin powder for three-dimensional modeling, three-dimensional modeled object, and method for producing three-dimensional modeled object
By formulating a resin powder with ethylene-propylene copolymer particles within specific parameters, the balance of tensile strength and elongation at break is achieved, enabling durable three-dimensional objects suitable for both prototyping and final products.
Patent Information
- Application Number
- JP2021514156
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-16
- Filing Date
- 2020-04-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-04-14
AI Technical Summary
Existing three-dimensional modeling methods using polypropylene resin struggle to achieve a balance between tensile strength and elongation at break, making them unsuitable for producing durable final products.
A resin powder for three-dimensional modeling is formulated with ethylene-propylene copolymer particles, specifically controlled for volume average particle diameter, ethylene content molar ratio, melt flow rate, and molecular weight, ensuring a fine crystalline structure for enhanced strength and toughness.
The solution results in a resin powder that produces three-dimensional objects with good tensile strength and excellent elongation at break, suitable for both prototyping and final product applications.
Smart Images

Figure 0007579493000003 
Figure 0007579493000004 
Figure 0007579493000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin powder for three-dimensional modeling, a three-dimensional object, and a method for producing a three-dimensional object, and in particular to a resin powder for three-dimensional modeling that uses polypropylene resin and has good tensile strength and excellent breaking elongation. [Background technology]
[0002] In recent years, various methods have been developed that allow for the relatively easy production of complex shaped three-dimensional objects. One of the methods for producing three-dimensional objects is the Powder Bed Fusion (PBF) method. Powder Bed Fusion (PBD) is a type of fusion process that is known for its high molding accuracy and high adhesive strength between laminated layers. Therefore, PBD can be used not only for producing prototypes to confirm the shape or properties of the final product, but also for manufacturing the final product.
[0003] In the powder bed fusion method, a powder material containing particles of a resin material or a metal material is spread evenly to form a thin film, and a laser is irradiated at a desired position on the thin film to selectively sinter or melt the particles contained in the powder material to bond them together (hereinafter, bonding of particles by sintering or melting is also simply referred to as "fusion bonding"). This forms one of the layers (hereinafter, simply referred to as "modeled object layer") that finely divides the three-dimensional object in the thickness direction. Further powder material is spread on the layer thus formed, and a laser is irradiated to selectively melt and bond the particles contained in the powder material to form the next modeled object layer. This procedure is repeated to build up the modeled object layers, and a three-dimensional object of the desired shape is produced.
[0004] For the particles contained in the powder material, a resin material such as polyamide may be used from the viewpoints of ease of handling and wide range of applicable targets. In particular, polyamide 12 can be suitably used since it has a relatively low melting point among polyamides, a small thermal shrinkage rate, and low water absorption among polyamides (see, for example, Patent Document 1).
[0005] However, in recent years, in addition to prototyping, there has been an increasing demand to use the molded objects as final products, and in particular, there has been an increasing demand to use polypropylene resin, which has a distinctive elongation at break. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 6402810 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a resin powder for 3D modeling, which uses polypropylene resin and has good tensile strength and excellent breaking elongation, a 3D modeled object, and a method for producing a 3D modeled object. [Means for solving the problem]
[0008] In the course of investigating the causes of the above problems in order to solve the above problems, the present inventors discovered that by specifying the volume average particle size, ethylene molar ratio, and melt flow rate of ethylene-propylene copolymer particles within specific ranges, it is possible to provide a resin powder for three-dimensional modeling using a polypropylene resin, which has good tensile strength and excellent elongation at break, and thus arrived at the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0009] 1. A resin powder for three-dimensional modeling, Contains ethylene-propylene copolymer particles, The ethylene-propylene copolymer particles have a volume average particle size within the range of 5 to 200 μm; The ethylene-propylene copolymer particles have an ethylene content molar ratio (ethylene / (ethylene+propylene)), 0.01~0.025 is within the range The weight average molecular weight of the ethylene-propylene copolymer particles is within a range of 260,000 to 330,000; and, A resin powder for three-dimensional modeling, having a melt flow rate (MFR) in the range of 3 to 40 g / 10 min at 230°C.
[0010] 2. The melting point is within the range of 100 to 160°C, and 2. The resin powder for three-dimensional modeling according to claim 1, which satisfies the relationship of the following formula (1): Formula (1): (melting point temperature-recrystallization temperature)≧10°C
[0011] 3. A resin powder for three-dimensional modeling as described in claim 1 or 2, in which the number of particles having an average particle size 0.15 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn).
[0012] 4. A resin powder for three-dimensional modeling according to any one of claims 1 to 3, wherein the number of particles having an average particle size 0.41 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn).
[0013] 5. A three-dimensional object formed using a resin powder for three-dimensional modeling, 5. A three-dimensional object which is a sintered or molten body of the resin powder for three-dimensional object production according to any one of claims 1 to 4.
[0014] 6. A method for producing a three-dimensional object using a resin powder for three-dimensional modeling, comprising the steps of: A method for producing a three-dimensional object by a powder bed fusion method using the resin powder for three-dimensional modeling according to any one of items 1 to 4.
[0015] 7. Forming a thin layer of the resin powder for three-dimensional modeling; a step of selectively irradiating the formed thin layer with a laser beam to form a model layer in which resin particles contained in the resin powder for three-dimensional modeling are sintered or melt-bonded; 7. The method for producing a three-dimensional object according to claim 6, further comprising: a step of repeating the step of forming the thin layer and the step of forming the object layer in this order a number of times to stack the object layers. Effect of the Invention
[0016] According to the above-mentioned means of the present invention, it is possible to provide a resin powder for three-dimensional modeling, a three-dimensional model, and a method for producing a three-dimensional model, which use a polypropylene resin and have good tensile strength and excellent breaking elongation. Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. In general, the larger the crystal portion of a crystalline resin, the greater the force acting on the crystal interface, making it more brittle. Therefore, in order to maintain strength while increasing toughness, it is necessary to disperse the force by making the crystals finer and increasing the number of interfaces, but it has been found that simply powdering polypropylene resin makes it difficult to achieve the desired fineness, and sufficient strength and toughness cannot be obtained. In the course of investigation to solve this problem, it was discovered that the desired strength and toughness could be obtained by copolymerizing ethylene with a propylene polymer. That is, in the resin powder for three-dimensional modeling of the present invention, ethylene-propylene copolymer particles are contained, and the ethylene content molar ratio, volume average particle size, and melt flow rate of the ethylene-propylene copolymer particles are set within specific ranges, thereby making it possible to refine the crystals, and as a result, it is possible to obtain a resin powder for three-dimensional modeling using polypropylene resin, which has good tensile strength and excellent elongation at break. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a side view showing a schematic configuration of a three-dimensional object forming apparatus according to an embodiment of the present invention; [Diagram 2]FIG. 1 is a diagram showing a main part of a control system of a three-dimensional object forming apparatus according to an embodiment of the present invention DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The resin powder for three-dimensional modeling of the present invention contains ethylene-propylene copolymer particles, and the ethylene-propylene copolymer particles have a volume average particle size in the range of 5 to 200 μm, an ethylene molar ratio (ethylene / (ethylene+propylene)) in the ethylene-propylene copolymer particles in the range of 0.001 to 0.04, and a melt flow rate (MFR) in the range of 3 to 40 g / 10 min at 230°C. This feature is a technical feature common to or corresponding to each of the following embodiments.
[0019] In an embodiment of the present invention, the melting point is within the range of 100 to 160°C and satisfies the relationship of formula (1) ((melting point temperature-recrystallization temperature)≧10°C), which is the temperature range required to suppress distortion of the object in the powder additive manufacturing method.
[0020] It is preferable that the number of particles having an average particle size 0.15 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn), since particles having an average particle size 0.15 times the number average particle size (Mn) are arranged between particles having the above number average particle size (Mn), thereby making it possible to make the crystals finer and increasing toughness while maintaining strength.
[0021] In addition, it is preferable that the number of particles having an average particle size 0.41 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn), since particles having an average particle size 0.41 times the number average particle size (Mn) are arranged between particles having the above number average particle size (Mn), thereby making it possible to make the crystals finer and increasing toughness while maintaining strength.
[0022] The three-dimensional object of the present invention is a three-dimensional object formed by using the resin powder for three-dimensional modeling, and is a sintered body or a molten body of the resin powder for three-dimensional modeling. This makes it possible to obtain a three-dimensional object substantially made of polypropylene resin, which has good tensile strength and excellent breaking elongation.
[0023] In the method for producing a three-dimensional object of the present invention, a three-dimensional object is produced by a powder bed fusion method using the resin powder for three-dimensional object production. The method for producing a three-dimensional object of the present invention preferably includes the steps of forming a thin layer of the resin powder for three-dimensional modeling, selectively irradiating the formed thin layer with laser light to form a model layer in which resin particles contained in the resin powder for three-dimensional modeling are sintered or melt-bonded, and repeating the steps of forming the thin layer and forming the model layer multiple times in this order to laminate the model layers. This makes it possible to obtain a three-dimensional object that is substantially made of polypropylene resin and has good tensile strength and excellent elongation at break, and also makes it possible to obtain a three-dimensional object with high modeling precision and high adhesive strength between the laminated layers.
[0024] The present invention, its components, and embodiments for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as lower and upper limits.
[0025] [Resin powder for three-dimensional modeling of the present invention] The resin powder for 3D modeling of the present invention contains ethylene-propylene copolymer particles, and the ethylene-propylene copolymer particles have a volume average particle size in the range of 5 to 200 μm, an ethylene molar ratio (ethylene / (ethylene+propylene)) in the ethylene-propylene copolymer particles in the range of 0.001 to 0.04, and a melt flow rate (MFR) in the range of 3 to 40 g / 10 min at 230° C. The resin powder for 3D modeling of the present invention may contain other types of resin particles within the range that does not impair the effects of the present invention.
[0026] [Ethylene-propylene copolymer particles] <Volume average particle size> The ethylene-propylene copolymer particles (hereinafter also referred to as copolymer particles) according to the present invention have a volume average particle size within the range of 5 to 200 μm, more preferably within the range of 20 to 100 μm.
[0027] (Measurement method) The volume average particle size (Mv) of the ethylene-propylene copolymer particles was measured by a particle size distribution analyzer (Microtrac MT3300EXII, manufactured by Microtrac Bell Co., Ltd.) using the particle refractive index of each powder and a dry (air) method without using a solvent. The particle refractive index was set to 1.5. The measurement procedure was as follows: 0.1 g of particles was added to 0.2 g of a surfactant (Emeral E-27C, manufactured by Kao Corporation) and 30 mL of water, and ultrasonic dispersion was performed for 10 minutes.
[0028] The volume average particle size of the ethylene-propylene copolymer particles can be adjusted, for example, by subjecting the ethylene-propylene copolymer particles to a pulverization treatment by a pulverization method such as a mechanical pulverization method or a wet pulverization method, or by subjecting the ethylene-propylene copolymer particles to a particle spheronization treatment.
[0029] <Ethylene molar ratio> The ethylene-propylene copolymer particles have an ethylene molar ratio (ethylene / (ethylene+propylene)) within a range of 0.001 to 0.04, and more preferably within a range of 0.05 to 0.03. As a means for controlling the ethylene-containing molar ratio within the above range, it can be controlled by adjusting the gas composition (ethylene-containing molar ratio) in a gas phase polymerization vessel during synthesis of the copolymer particles, as described later.
[0030] (Measurement method) The ethylene molar ratio in the copolymer particles was measured by dissolving 100 mg of the copolymer particles in a mixture of deuterated benzene and deuterated o-dichlorobenzene (deuterated benzene / deuterated o-dichlorobenzene = 3 / 1) at 120°C. 13Perform C-NMR measurement (quantitative mode). Measurement equipment: JEOL ECZ400 Measurement frequency: 13C 100MHz Pulse condition: X_90_width = 11.76μs Number of times accumulated: 1024
[0031] <Melt flow rate> The melt flow rate (MFR) of the resin powder for three-dimensional modeling of the present invention at 230° C. is within the range of 3 to 40 g / 10 min, and more preferably within the range of 5 to 35 g / 10 min.
[0032] (Measurement method) The melt flow rate is a value measured in accordance with JIS K7210 Method A under conditions of 230° C. and a load of 2.16 kg.
[0033] The melt flow rate can be controlled within the above range by adjusting the ethylene molar ratio and the weight average molecular weight (Mw) of the ethylene-propylene copolymer particles. The weight average molecular weight of the ethylene-propylene copolymer particles is preferably within a range of 300,000 to 400,000, and more preferably within a range of 300,000 to 350,000.
[0034] The weight average molecular weight was calculated from the molecular weight distribution in terms of polystyrene (PS) by gel permeation chromatography (GPC). The conditions for the analysis method are as follows. Equipment: Agilent PL-GPS220 Column: Agilent PLgel Olexis x 2 + Guard Dissolving solution: o-dichlorobenzene Temperature: 145℃ Concentration: 0.1wt / vol% Flow rate: 1.0mL / min Pretreatment: Hot filtration (0.5 μm pore size filter) Solubility: Completely soluble Detector: Differential refractometer (RI)
[0035] <Melting point> It is essential in the powder additive manufacturing method that the melting point of the resin powder for three-dimensional modeling according to the present invention is within the range of 100 to 160° C. and that the relationship of the following formula (1) is satisfied. Formula (1): (melting point temperature-recrystallization temperature)≧10°C The melting point is more preferably within the range of 120 to 150° C. Also, it is more preferable that (melting point temperature-recrystallization temperature)≧15° C.
[0036] (Measurement method) The melting point and the recrystallization temperature were measured as follows. According to the measurement method of ISO 3146 (Method for measuring plastic transition temperature, JIS K7121), a differential scanning calorimeter (DSC7000X, Hitachi High-Tech Science Corporation) was used to measure the endothermic peak by raising the temperature to 30°C higher than the melting point at 10°C / min. The melting point is the endothermic peak temperature. Then, the temperature was lowered to -30°C or lower at 10°C / min, and the recrystallization peak was measured. The recrystallization temperature is the exothermic peak temperature.
[0037] <Number average particle size> In the resin powder for three-dimensional modeling of the present invention, the number of particles having an average particle size 0.15 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is preferably equal to or greater than the number of particles having the number average particle size (Mn). In other words, when the number of particles having the number average particle size (Mn) is M1 and the number of particles having an average particle size 0.15 times the number average particle size (Mn) is M2, it is preferable that M1 / M2 is 0.5 or less. It is also preferred that the number of particles having an average particle size 0.41 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn). In other words, when the number of particles having an average particle size 0.41 times the number average particle size (Mn) is defined as M3, it is preferred that M1 / M3 is 0.5 or less. As a result, particles having an average particle size that is 0.15 or 0.41 times the number average particle size (Mn) are arranged between particles having the above number average particle size (Mn), making it possible to make the crystals finer and increasing toughness while maintaining strength.
[0038] (Measurement method) The number-average particle size (Mn) of the copolymer particles was measured by a particle size distribution analyzer (Microtrac MT3300EXII, manufactured by Microtrac-Bell Co., Ltd.) using the particle refractive index of each powder by a dry (air) method without using a solvent. The particle refractive index was set to 1.5.
[0039] [Preparation of resin powder for 3D modeling] The resin powder for three-dimensional modeling of the present invention can be produced by synthesizing the ethylene-propylene copolymer particles and then subjecting the ethylene-propylene copolymer particles to a pulverization treatment by a pulverization method such as a mechanical pulverization method or a wet pulverization method, or a particle spheronization treatment.
[0040] <Synthesis of ethylene-propylene copolymer> The ethylene-propylene copolymer contained in the resin powder for 3D modeling of the present invention can be synthesized, for example, by polymerizing propylene using an olefin polymerization catalyst containing the following solid titanium catalyst component (I) and organometallic compound catalyst component (II), and then copolymerizing propylene with ethylene. The catalyst components (I) and (II) and the polymerization method will be described below.
[0041] (Solid titanium catalyst component (I)) The solid titanium catalyst component (I) preferably contains titanium, magnesium, a halogen, and, if necessary, an electron donor. Any known solid titanium catalyst component can be used as the solid titanium catalyst component (I) without any restrictions. An example of a method for producing the solid titanium catalyst component (I) is shown below.
[0042] In preparing the solid titanium catalyst component (I) according to the present invention, a magnesium compound and a titanium compound are preferably used. Specific examples of the magnesium compound include known magnesium compounds such as magnesium halides, such as magnesium chloride and magnesium bromide; alkoxymagnesium halides, such as methoxymagnesium chloride, ethoxymagnesium chloride and phenoxymagnesium chloride; alkoxymagnesium, such as ethoxymagnesium, isopropoxymagnesium, butoxymagnesium and 2-ethylhexoxymagnesium; aryloxymagnesium, such as phenoxymagnesium; and magnesium carboxylates, such as magnesium stearate.
[0043] These magnesium compounds may be used alone or in combination of two or more kinds. Furthermore, these magnesium compounds may be complex compounds or complex compounds with other metals, or mixtures with other metal compounds.
[0044] Among these, magnesium compounds containing halogen are preferred, and magnesium halides, especially magnesium chloride, are preferably used.Other than these, alkoxymagnesium such as ethoxymagnesium are also preferably used.The magnesium compound may be derived from other substances, for example, those obtained by contacting an organomagnesium compound such as a Grignard reagent with a titanium halide, a silicon halide, a halogenated alcohol, etc.
[0045] The titanium compound may, for example, be a tetravalent titanium compound represented by the following formula: Ti(OR) g X 4-g [In the formula, R represents a hydrocarbon group, X represents a halogen atom, and g is 0≦g≦4.]
[0046] More specifically, examples of the titanium tetrahalides include TiCl4, TiBr4, etc.; alkoxy titanium trihalides such as Ti(OCH3)Cl3, Ti(OC2H5)Cl3, Ti(On-C4H9)Cl3, Ti(OC2H5)Br3, Ti(O-isoC4H9)Br3, etc.; alkoxy titanium dihalides such as Ti(OCH3)2Cl2, Ti(OC2H5)2Cl2, etc.; alkoxy titanium monohalides such as Ti(OCH3)3Cl, Ti(On-C4H9)3Cl, Ti(OC2H5)3Br, etc.; and tetraalkoxy titanium such as Ti(OCH3)4, Ti(OC2H5)4, Ti(OC4H9)4, Ti(O-2-ethylhexyl)4, etc.
[0047] Among these, titanium tetrahalides are preferred, and titanium tetrachloride is particularly preferred. These titanium compounds may be used alone or in combination of two or more.
[0048] Examples of the magnesium compounds and titanium compounds include those described in detail in JP-A-57-63310 and JP-A-5-170843.
[0049] Specific preferred methods for preparing the solid titanium catalyst component (I) used in the present invention include the following methods (P-1) to (P-4). (P-1): A method in which a solid adduct consisting of an electron donor component (a) such as a magnesium compound and an alcohol is contacted with an electron donor component (b) described below and a liquid titanium compound in a suspended state in the presence of an inert hydrocarbon solvent. (P-2): A method in which a solid adduct consisting of a magnesium compound and an electron donor component (a), an electron donor component (b), and a liquid titanium compound are contacted in separate batches. (P-3): A method in which a solid adduct consisting of a magnesium compound and an electron donor component (a), an electron donor component (b), and a liquid titanium compound are contacted in a suspended state in the presence of an inert hydrocarbon solvent, and the contact is carried out in multiple batches. (P-4): A method of contacting a liquid magnesium compound consisting of a magnesium compound and an electron donor component (a), a liquid titanium compound, and an electron donor component (b).
[0050] The reaction temperature is preferably in the range of -30 to 150°C, more preferably -25 to 130°C, and further preferably -25 to 120°C. The production of the solid titanium catalyst component can be carried out in the presence of a known medium, if necessary. Examples of the medium include aromatic hydrocarbons having a slight polarity, such as toluene, and known aliphatic and alicyclic hydrocarbon compounds, such as heptane, octane, decane, and cyclohexane. Among these, aliphatic hydrocarbons are preferred.
[0051] The electron donor component (a) used to form the solid adduct or liquid magnesium compound is preferably a known compound capable of solubilizing the magnesium compound in a temperature range of about room temperature to 300° C., such as alcohols, aldehydes, amines, carboxylic acids, and mixtures thereof. Examples of these compounds include those described in detail in JP-A-57-63310 and JP-A-5-170843.
[0052] More specifically, examples of the alcohol capable of solubilizing the magnesium compound include aliphatic alcohols such as methanol, ethanol, propanol, butanol, isobutanol, ethylene glycol, 2-methylpentanol, 2-ethylbutanol, n-heptanol, n-octanol, 2-ethylhexanol, decanol, and dodecanol; alicyclic alcohols such as cyclohexanol and methylcyclohexanol; aromatic alcohols such as benzyl alcohol and methylbenzyl alcohol; and aliphatic alcohols having an alkoxy group such as n-butyl cellosolve.
[0053] Examples of the carboxylic acid include organic carboxylic acids having 7 or more carbon atoms, such as caprylic acid and 2-ethylhexanoic acid. Examples of the aldehyde include aldehydes having 7 or more carbon atoms, such as capric aldehyde and 2-ethylhexyl aldehyde.
[0054] Examples of the amine include amines having 6 or more carbon atoms, such as heptylamine, octylamine, nonylamine, laurylamine, and 2-ethylhexylamine.
[0055] As the electron donor component (a), the above-mentioned alcohols are preferred, and in particular, ethanol, propanol, butanol, isobutanol, hexanol, 2-ethylhexanol, decanol, and the like are preferred.
[0056] The composition ratio of magnesium to the electron donor component (a) in the resulting solid adduct or liquid magnesium compound varies depending on the type of compound used and cannot be generally defined, but the amount of the electron donor component (a) per mole of magnesium in the magnesium compound is preferably 2 moles or more, more preferably 2.3 moles or more, and even more preferably 2.7 moles or more and 5 moles or less.
[0057] Particularly preferred examples of the electron donor that may be used as necessary in the solid titanium catalyst component (I) used in the present invention include aromatic carboxylic acid esters and / or compounds having two or more ether bonds via a plurality of carbon atoms (hereinafter also referred to as "electron donor component (b)").
[0058] As the electron donor component (b), known aromatic carboxylic acid esters and polyether compounds that have been preferably used in conventional olefin polymerization catalysts, such as the compounds described in JP-A-5-170843 and JP-A-2001-354714, can be used without limitation.
[0059] Specific examples of the aromatic carboxylate include aromatic carboxylate monoesters such as benzoates and toluates, as well as aromatic polyvalent carboxylates such as phthalates. Among these, aromatic polyvalent carboxylates are preferred, and phthalates are more preferred. As the phthalates, alkyl phthalates such as ethyl phthalate, n-butyl phthalate, isobutyl phthalate, hexyl phthalate, and heptyl phthalate are preferred, and diisobutyl phthalate is particularly preferred.
[0060] More specifically, the polyether compound may be a compound having a structure represented by the following formula (1).
[0061] [ka]
[0062] In the above formula (1), m is an integer of 1≦m≦10, more preferably an integer of 3≦m≦10; R 11 ~R 36 are each independently a hydrogen atom or a substituent having at least one element selected from carbon, hydrogen, oxygen, fluorine, chlorine, bromine, iodine, nitrogen, sulfur, phosphorus, boron and silicon.
[0063] When m is 2 or more, there are multiple R 11 and R 12 may be the same or different. Any R 11 ~R 36 , preferably R 11 and R 12 may combine together to form a ring other than a benzene ring.
[0064] Specific examples of such compounds include mono-substituted dialkoxypropanes such as 2-isopropyl-1,3-dimethoxypropane, 2-s-butyl-1,3-dimethoxypropane, and 2-cumyl-1,3-dimethoxypropane; 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3 -Dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-diethoxypropane, 2,2-diisobutyl-1,3-dibutoxypropane, 2,2-di-s-butyl-1,3-dimethoxypropane, 2,2-dineopentyl-1,3-dimethoxypropane, 2-isopropyl -2-isopentyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and other 2-substituted dialkoxypropanes; 2,3-dicyclohexyl-1,4-diethoxybutane, 2,3-dicyclohexyl-1,4-diethoxybutane, 2,3-diisopropyl-1,4-diethoxybutane, 2,4-diphenyl-1,5-dimethoxypentane, 2,5-diphenyl-1,5-dimethoxyhexane, 2,4-di Examples include dialkoxyalkanes such as isopropyl-1,5-dimethoxypentane, 2,4-diisobutyl-1,5-dimethoxypentane, and 2,4-diisoamyl-1,5-dimethoxypentane; and trialkoxyalkanes such as 2-methyl-2-methoxymethyl-1,3-dimethoxypropane, 2-cyclohexyl-2-ethoxymethyl-1,3-diethoxypropane, and 2-cyclohexyl-2-methoxymethyl-1,3-dimethoxypropane.
[0065] Of these, 1,3-diethers are preferred, and 2-isopropyl-2-isobutyl-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, and 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane are particularly preferred.
[0066] These compounds may be used alone or in combination of two or more.
[0067] In the solid titanium catalyst component (I) used in the present invention, the halogen / titanium (atomic ratio) (i.e., the number of moles of halogen atoms / the number of moles of titanium atoms) is 2 to 100, preferably 4 to 90, and in the electron donor component (a) and the electron donor component (b), the electron donor component (a) / titanium atom (molar ratio) is 0 to 100, preferably 0 to 10, and the electron donor component (b) / titanium atom (molar ratio) is 0 to 100, preferably 0 to 10.
[0068] The magnesium / titanium (atomic ratio) (ie, the number of moles of magnesium atoms / the number of moles of titanium atoms) is 2-100, and preferably 4-50.
[0069] As more detailed preparation conditions for the solid titanium catalyst component (I), except for the use of the electron donor component (b), for example, the conditions described in EP585869A1 (European Patent Application Publication No. 0585869) and JP-A-5-170843 can be preferably used.
[0070] Next, the organometallic compound catalyst component (II) containing a metal element selected from Groups 1, 2 and 13 of the periodic table will be described.
[0071] (Organometallic compound catalyst component (II)) As the organometallic compound catalyst component (II), compounds containing a Group 13 metal, for example, organoaluminum compounds, complex alkylates of a Group 1 metal and aluminum, organometallic compounds of a Group 2 metal, etc. can be used. Among these, organoaluminum compounds are preferred.
[0072] Specifically, as the organometallic compound catalyst component (II), the organometallic compound catalyst components described in known documents such as the above-mentioned EP585869A1 can be cited as preferred examples.
[0073] As long as the object of the present invention is not impaired, in addition to the above electron donor component (a) and electron donor component (b), a known electron donor component (c) may be used in combination. Preferably, an organosilicon compound can be cited as such an electron donor component (c). Examples of such an organosilicon compound include compounds represented by the following formula. R n Si(OR′) 4-n [In the formula, R and R′ represent hydrocarbon groups. n is an integer of 0 < n < 4.]
[0074] Specific examples of the organosilicon compound represented by the above formula include diisopropyldimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldiethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, t-butyltriethoxysilane, phenyltriethoxysilane, cyclohexyltrimethoxysilane, cyclopentyltrimethoxysilane, 2-methylcyclopentyltrimethoxysilane, cyclopentyltriethoxysilane, dicyclopentyldimethoxysilane, dicyclopentyldiethoxysilane, tricyclopentylmethoxysilane, dicyclopentylmethylmethoxysilane, dicyclopentylethylmethoxysilane, cyclopentyldimethylethoxysilane, etc.
[0075] Of these, vinyltriethoxysilane, diphenyldimethoxysilane, dicyclohexyldimethoxysilane, cyclohexylmethyldimethoxysilane, and dicyclopentyldimethoxysilane are preferably used.
[0076] Further, the silane compounds represented by the following formula, which are described in WO 2004 / 016662, are also preferred examples of the organosilicon compounds. Si(OR a )3(NR b R c )
[0077] In the formula, R a is a hydrocarbon group having 1 to 6 carbon atoms, R a Examples of the alkyl group include unsaturated or saturated aliphatic hydrocarbon groups having 1 to 6 carbon atoms, and particularly preferably hydrocarbon groups having 2 to 6 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, and a cyclohexyl group, and among these, an ethyl group is particularly preferred.
[0078] R b is a hydrocarbon group having 1 to 12 carbon atoms or hydrogen, R b Examples of the aryl group include hydrogen and unsaturated or saturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms. Specific examples include a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group. Among these, an ethyl group is particularly preferred.
[0079] R c is a hydrocarbon group having 1 to 12 carbon atoms, R cExamples of the aryl group include hydrogen and unsaturated or saturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms. Specific examples include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, an iso-butyl group, a sec-butyl group, an n-pentyl group, an iso-pentyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, and an octyl group. Among these, an ethyl group is particularly preferred.
[0080] Specific examples of the compound represented by the above formula include dimethylaminotriethoxysilane, diethylaminotriethoxysilane, diethylaminotrimethoxysilane, diethylaminotriethoxysilane, diethylaminotri-n-propoxysilane, di-n-propylaminotriethoxysilane, methyl n-propylaminotriethoxysilane, t-butylaminotriethoxysilane, ethyl n-propylaminotriethoxysilane, ethyl iso-propylaminotriethoxysilane, and methylethylaminotriethoxysilane.
[0081] Further, other examples of the organosilicon compound include compounds represented by the following formula: RNSi(OR a )3 In the formula, RN represents a cyclic amino group. Examples of the cyclic amino group include a perhydroquinolino group, a perhydroisoquinolino group, a 1,2,3,4-tetrahydroquinolino group, a 1,2,3,4-tetrahydroisoquinolino group, and an octamethyleneimino group.
[0082] Specific examples of the compound represented by the above formula include (perhydroquinolino)triethoxysilane, (perhydroisoquinolino)triethoxysilane, (1,2,3,4-tetrahydroquinolino)triethoxysilane, (1,2,3,4-tetrahydroisoquinolino)triethoxysilane, and octamethyleneiminotriethoxysilane. These organosilicon compounds can also be used in combination of two or more.
[0083] Ethylene-propylene copolymers can be synthesized by polymerizing propylene in the presence of the above-mentioned olefin polymerization catalyst and then copolymerizing propylene and ethylene, or by polymerizing propylene in the presence of a prepolymerization catalyst obtained by prepolymerization and then copolymerizing propylene and ethylene.
[0084] The prepolymerization is carried out by prepolymerizing an olefin in an amount of usually 0.1 to 1000 g, preferably 0.3 to 500 g, and particularly preferably 1 to 200 g, per 1 g of the olefin polymerization catalyst. In the preliminary polymerization, a catalyst can be used at a higher concentration than that in the main polymerization system. The concentration of the solid titanium catalyst component (I) in the prepolymerization is usually about 0.001 to 200 millimoles, preferably about 0.01 to 50 millimoles, and particularly preferably 0.1 to 20 millimoles, calculated as titanium atom per liter of the liquid medium.
[0085] The amount of the organometallic compound catalyst component (II) in the prepolymerization may be such that usually 0.1 to 1000 g, preferably 0.3 to 500 g, of polymer is produced per gram of the solid titanium catalyst component (I), and usually about 0.1 to 300 mol, preferably about 0.5 to 100 mol, particularly preferably 1 to 50 mol, per mol of titanium atom in the solid titanium catalyst component (I).
[0086] In the preliminary polymerization, the above-mentioned electron donor component and the like can be used as necessary. In this case, these components are used in an amount of usually 0.1 to 50 mol, preferably 0.5 to 30 mol, and more preferably 1 to 10 mol, per 1 mol of titanium atom in the above-mentioned solid titanium catalyst component (I).
[0087] The prepolymerization can be carried out under mild conditions by adding an olefin and the above-mentioned catalyst components to an inert hydrocarbon medium. In this case, specific examples of the inert hydrocarbon medium used include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, cycloheptane, methylcycloheptane, and cyclooctane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride and chlorobenzene; and mixtures thereof. Among these inert hydrocarbon media, it is particularly preferable to use an aliphatic hydrocarbon. When an inert hydrocarbon medium is used, it is preferable to carry out the prepolymerization in a batch manner.
[0088] On the other hand, the prepolymerization can be carried out using the olefin itself as a solvent, or in the substantial absence of a solvent, in which case it is preferred to carry out the prepolymerization continuously.
[0089] The olefin used in the prepolymerization may be the same as or different from the olefin used in the main polymerization described below, but is preferably propylene. The temperature during the prepolymerization is usually in the range of -20 to +100°C, preferably -20 to +80°C, and more preferably 0 to +40°C.
[0090] Next, the main polymerization, which is carried out after or without passing through preliminary polymerization, will be described. This polymerization is divided into a process for producing a propylene polymer component and a process for producing an ethylene-propylene copolymer rubber component. The preliminary polymerization and the main polymerization can be carried out by any of liquid phase polymerization methods such as bulk polymerization, solution polymerization, and suspension polymerization, or gas phase polymerization methods. The preferred process for producing the propylene polymer component is liquid phase polymerization such as bulk polymerization and suspension polymerization, or gas phase polymerization methods. The preferred process for producing the propylene-ethylene copolymer rubber component is liquid phase polymerization such as bulk polymerization and suspension polymerization, or gas phase polymerization methods, and more preferred is gas phase polymerization methods.
[0091] When the main polymerization is carried out in the form of a slurry polymerization reaction, the reaction solvent may be the inert hydrocarbon used in the above-mentioned preliminary polymerization, or an olefin which is liquid at the reaction temperature and pressure.
[0092] In this polymerization, the solid titanium catalyst component (I) is usually used in an amount of about 0.0001 to 0.5 millimoles, preferably about 0.005 to 0.1 millimoles, calculated as titanium atoms per 1 liter of polymerization volume. The organometallic compound catalyst component (II) is usually used in an amount of about 1 to 2000 moles, preferably about 5 to 500 moles, per mole of titanium atoms in the prepolymerized catalyst component in the polymerization system. The electron donor component, if used, is used in an amount of 0.001 to 50 moles, preferably 0.01 to 30 moles, particularly preferably 0.05 to 20 moles, per mole of the organometallic compound catalyst component (II).
[0093] If this polymerization is carried out in the presence of hydrogen, the molecular weight of the resulting polymer can be adjusted (reduced), and a polymer with a high melt flow rate can be obtained. The amount of hydrogen required to adjust the molecular weight varies depending on the type of production process used, the polymerization temperature, and the pressure, so it can be adjusted appropriately. In the process of producing the propylene polymer component, the MFR can be adjusted by adjusting the polymerization temperature and the amount of hydrogen. Also, in the process of producing the ethylene-propylene copolymer rubber component, the intrinsic viscosity can be adjusted by adjusting the polymerization temperature, pressure, and the amount of hydrogen.
[0094] In this polymerization, the polymerization temperature of the olefin is usually about 0 to 200° C., preferably about 30 to 100° C., and more preferably 50 to 90° C. The pressure (gauge pressure) is usually normal pressure to 100 kgf / cm. 2 (9.8MPa), preferably about 2 to 50 kgf / cm 2 (0.20 to 4.9 MPa). In the process for producing ethylene-propylene copolymer, polymerization can be carried out in any of batch, semi-continuous, and continuous modes. Furthermore, the reactor shape can be either tubular or tank type. Furthermore, polymerization can be carried out in two or more stages by changing the reaction conditions. In this case, tubular and tank types can be combined.
[0095] In addition, in order to obtain the ethylene-propylene copolymer according to the present invention, the ethylene molar ratio ("ethylene / (ethylene + propylene)") of the gas composition is controlled. The ethylene molar ratio (ethylene / (ethylene+propylene)) is preferably controlled within a range of 0.001 to 0.04, preferably 0.005 to 0.035, and more preferably 0.07 to 0.03.
[0096] The ethylene-propylene copolymer particles obtained above are subjected to a pulverization process by a pulverization method such as a mechanical pulverization method or a wet pulverization method, or a particle spheroidization process to produce a resin powder for three-dimensional modeling. By such a process, a resin powder for three-dimensional modeling can be produced in which the volume average particle size of the ethylene-propylene copolymer particles is within the range of 5 to 200 μm.
[0097] <Mechanical grinding method> In the mechanical milling method, the ethylene-propylene copolymer particles are mechanically milled to produce particles with the desired average particle size. Using the mechanical milling method, particles can be produced in the following manner. The ethylene-propylene copolymer particles may be crushed after freezing or at room temperature. Mechanical crushing can be performed by known devices for crushing thermoplastic resins. Examples of such devices include hammer mills, jet mills, ball mills, impeller mills, cutter mills, pin mills, and twin-shaft crushers.
[0098] In the mechanical crushing method, the ethylene-propylene copolymer particles may fuse together due to frictional heat generated from the ethylene-propylene copolymer particles during crushing, and particles of the desired particle size may not be obtained. Therefore, it is preferable to cool and embrittle the ethylene-propylene copolymer particles using liquid nitrogen or the like before crushing them. In the mechanical grinding method, the average particle size of the produced particles can be adjusted to the desired range (volume average particle size: 5 to 200 μm) by appropriately adjusting the amount of solvent relative to the ethylene-propylene copolymer particles, or the grinding method or speed.
[0099] The desired particle size achieved by pulverization is determined by the operation time of the apparatus, and is preferably within the range of 5 to 45 hours. Specifically, it is preferable to cool the ethylene-propylene copolymer particles to about -150°C with liquid nitrogen and pulverize them with the above-mentioned pulverizer so that the volume average particle size falls within the range of 5 to 200 µm.
[0100] <Wet grinding method> In the wet grinding method, ethylene-propylene copolymer particles are dissolved in a solvent by heating and stirring, the resin solution obtained by the dissolution is cooled while stirring, and the resin slurry obtained by cooling is dried in vacuum while stirring to grind the resin slurry, thereby producing particles having a desired average particle size. Specifically, the method described in JP-A-3-12428 can be mentioned.
[0101] <Particle spheroidization treatment> The particle spheroidization treatment can be carried out by applying a mechanical impact force, for example, using a mechanical impact grinder such as the Kryptron System (manufactured by Kawasaki Heavy Industries, Ltd.) or Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.). Another method is to apply mechanical impact force to the ethylene-polypropylene copolymer particles by centrifugal force using rapidly rotating blades to press the ethylene-polypropylene copolymer particles against the inside of a casing, using forces such as compression and friction, as in devices such as the Mechanofusion System (manufactured by Hosokawa Micron Corporation) and Hybridization System (manufactured by Nara Machinery Works).
[0102] <Other ingredients> The resin powder for three-dimensional modeling of the present invention may further contain other materials, such as a laser absorber and a flow agent, within the scope of not significantly impeding the dense packing of the ethylene-propylene copolymer particles when melt-bonding and forming a thin layer by laser irradiation, which will be described later, and not significantly decreasing the accuracy of the three-dimensional model.
[0103] (Laser absorber) From the viewpoint of converting the light energy of the laser into heat energy more efficiently, the resin powder for three-dimensional modeling may further contain a laser absorbent. The laser absorbent may be any material that absorbs a laser having a wavelength to be used and generates heat. Examples of such laser absorbents include carbon powder, nylon resin powder, pigments, and dyes. These laser absorbents may be used alone or in combination of two types.
[0104] The amount of the laser absorbent can be appropriately set within a range that facilitates melting and bonding of the copolymer particles, and can be, for example, greater than 0% by mass and less than 3% by mass relative to the total mass of the resin powder for three-dimensional modeling.
[0105] (Flow Agent) From the viewpoint of further improving the flowability of the resin powder for 3D printing and facilitating the handling of the powder for 3D printing when producing a 3D object, the resin powder for 3D printing may further contain a flow agent. The flow agent may be any material having a small coefficient of friction and self-lubricating properties. Examples of such flow agents include silicon dioxide and boron nitride. These flow agents may be used alone or in combination. Even if the flow agent increases the fluidity of the resin powder for three-dimensional modeling, the copolymer particles are less likely to be charged, and the copolymer particles can be packed more densely when a thin film is formed.
[0106] The amount of the flow agent can be appropriately set within a range in which the fluidity of the resin powder for 3D modeling is improved and sufficient melt-bonding of the copolymer particles occurs, and can be, for example, greater than 0% by mass and less than 2% by mass relative to the total mass of the resin powder for 3D modeling.
[0107] The resin powder for three-dimensional modeling of the present invention can be produced by synthesizing the ethylene-propylene copolymer particles, and stirring and mixing the synthesized particles with materials other than the copolymer particles, as necessary.
[0108] [Three-dimensional object] The three-dimensional object of the present invention is a three-dimensional object formed using a resin powder for three-dimensional modeling, and is a sintered body or a molten body of the resin powder for three-dimensional modeling. The three-dimensional object of the present invention can be produced by the powder bed fusion method (PBF method) described below using the above-mentioned resin powder for three-dimensional modeling.
[0109] [How to create a three-dimensional object] The method for producing a three-dimensional object of the present invention can be carried out in the same manner as in the conventional powder bed fusion method, except that the resin powder for three-dimensional object production is used. Specifically, the method for producing a three-dimensional object of the present invention includes the steps of: (1) forming a thin layer of the resin powder for three-dimensional modeling; (2) selectively irradiating the preheated thin layer with laser light to form a modeled object layer in which ethylene-propylene copolymer particles contained in the resin powder for three-dimensional modeling are melt-bonded; and (3) repeating steps (1) and (2) in this order multiple times to laminate the modeled object layers. By step (2), one of the layers of the three-dimensional object is formed, and by repeating steps (1) and (2) in step (3), the next layer of the three-dimensional object is laminated to produce a final three-dimensional object. The method for producing a three-dimensional object of the present invention may further include a step (4) of preheating the thin layer of the resin powder for three-dimensional modeling that is formed, at least prior to step (2).
[0110] <Step of forming a thin layer made of resin powder for three-dimensional modeling (step (1))> In this step, a thin layer of the resin powder for three-dimensional modeling is formed. For example, the resin powder for three-dimensional modeling supplied from a powder supply unit is spread evenly on the modeling stage by a recoater. The thin layer may be formed directly on the modeling stage, or may be formed so as to be in contact with the resin powder for three-dimensional modeling that has already been spread or the modeling object layer that has already been formed.
[0111] The thickness of the thin layer can be set according to the thickness of the modeling layer. The thickness of the thin layer can be set arbitrarily according to the accuracy of the three-dimensional model to be produced, but is usually within the range of 0.01 to 0.30 mm. By setting the thickness of the thin layer to 0.01 mm or more, it is possible to prevent the copolymer particles of the lower layer from being melted and bonded by the laser irradiation for forming the next layer, or the modeling layer of the lower layer from being remelted. By setting the thickness of the thin layer to 0.30 mm or less, the energy of the laser can be transmitted to the lower part of the thin layer, and the copolymer particles contained in the resin powder for three-dimensional modeling that constitutes the thin layer can be sufficiently melted and bonded throughout the entire thickness direction. From the above viewpoints, the thickness of the thin layer is more preferably within the range of 0.01 to 0.10 mm. Also, from the viewpoints of more sufficiently melting and bonding the copolymer particles over the entire thickness direction of the thin layer and making it more difficult for cracks to occur between the laminated layers, it is preferable to set the thickness of the thin layer so that the difference from the beam spot diameter of the laser described below is within 0.10 mm.
[0112] <Step (2) of forming a model layer by melt-bonding ethylene-propylene copolymer particles> In this process, a laser is selectively irradiated to the positions of the formed thin layer where the model layer is to be formed, and the copolymer particles at the irradiated positions are melted and bonded. As a result, adjacent copolymer particles melt together to form a fused body, which becomes the model layer. At this time, the copolymer particles that receive the energy of the laser are also melted and bonded to the already formed layers, so that adhesion between adjacent layers also occurs.
[0113] The wavelength of the laser may be set within a range where the wavelength corresponding to the energy required for vibration, rotation, etc. of the constituent molecules of the copolymer particle is absorbed. At this time, it is preferable to make the difference between the wavelength of the laser and the wavelength at which the absorption rate is highest small, but since the resin can absorb light in various wavelength ranges, it is preferable to use a laser with a wide wavelength range such as a CO2 laser. For example, the wavelength of the laser is preferably within the range of 0.8 to 12 μm.
[0114] For example, the power of the laser output may be set within a range in which the copolymer particles are sufficiently melted and bonded at the laser scanning speed described below, and specifically, may be within a range of 10 to 100 W. From the viewpoint of reducing the laser energy, reducing the production cost, and simplifying the configuration of the production apparatus, the power of the laser output is preferably 60 W or less, and more preferably 40 W or less.
[0115] The scanning speed of the laser may be set within a range that does not increase the manufacturing cost and does not make the device configuration excessively complicated. Specifically, the scanning speed is preferably within a range of 20,000 mm / sec, more preferably within a range of 1,000 to 18,000 mm / sec, even more preferably within a range of 2,000 to 15,000 mm / sec, even more preferably within a range of 3 to 80 mm / sec, and even more preferably within a range of 3 to 50 mm / sec.
[0116] The diameter of the laser beam can be appropriately set depending on the precision of the three-dimensional object to be produced.
[0117] <Step of stacking thin layers of the formed resin powder for 3D modeling (step (3))> In this process, steps (1) and (2) are repeated to stack layers of the object formed in step (2). By stacking the layers of the object, a desired three-dimensional object is produced.
[0118] <Step (4) of preheating the formed thin layer of resin powder for 3D modeling> In this step, the thin layer of the resin powder for three-dimensional modeling is preheated prior to step (2) For example, the surface temperature of the thin layer (standby temperature) can be heated to 15°C or lower, preferably 5°C or lower, higher than the melting point of the copolymer particles by using a heater or the like.
[0119] <Other> From the viewpoint of preventing a decrease in the strength of the three-dimensional object due to oxidation of the copolymer particles during melt bonding, it is preferable to carry out at least the step (2) under reduced pressure or in an inert gas atmosphere. -2 Pa or less, and -3 It is more preferable that the pressure is 0.1 Pa or less. Examples of inert gases that can be used in the present invention include nitrogen gas and rare gases. Among these inert gases, nitrogen (N2) gas, helium (He) gas, or argon (Ar) gas is preferred from the viewpoint of availability. From the viewpoint of simplifying the production process, it is preferable to carry out all of steps (1) to (3) (when step (4) is included, all of steps (1) to (4)) under reduced pressure or in an inert gas atmosphere.
[0120] <3D modeling device> The 3D modeling apparatus according to the present invention may have the same configuration as a known apparatus for producing a 3D object by powder bed fusion bonding, except that the resin powder for 3D modeling is used. Specifically, as shown in FIG. 1, which is a side view showing a schematic configuration of the 3D modeling apparatus 100, the 3D modeling apparatus 100 includes a modeling stage 110 located within the opening, a thin film forming unit 120 which forms a thin film of resin powder for 3D modeling, containing the ethylene-propylene copolymer particles, on the modeling stage, a laser irradiation unit 130 which irradiates the thin film with a laser to form a modeled object layer in which the copolymer particles are melted and bonded, a stage support unit 140 which supports the modeling stage 110 so that its position in the vertical direction can be changed, and a base 145 which supports the above-mentioned units.
[0121] 2 showing the main parts of the control system, the three-dimensional modeling apparatus 100 may include a control unit 150 that controls the thin film forming unit 120, the laser irradiation unit 130, and the stage support unit 140 to repeatedly form and stack the above-mentioned modeled object layers, a display unit 160 for displaying various information, an operation unit 170 including a pointing device for receiving instructions from a user, a storage unit 180 for storing various information including a control program executed by the control unit 150, and a data input unit 190 including an interface for transmitting and receiving various information such as three-dimensional modeling data to and from an external device. A computer device 200 for generating data for three-dimensional modeling may be connected to the three-dimensional modeling apparatus 100.
[0122] On the modeling stage 110, a modeling material layer is formed by forming a thin layer by the thin film forming unit 120 and irradiating a laser by the laser irradiation unit 130, and a three-dimensional object is formed by stacking these modeling material layers.
[0123] The thin film forming unit 120 can be configured, for example, to include an opening whose edge is horizontally on approximately the same plane as the edge of the opening through which the modeling stage 110 rises and falls, a powder material storage unit extending vertically downward from the opening, and a powder supply unit 121 equipped with a supply piston provided at the bottom of the powder material storage unit and rising and falling within the opening, as well as a recoater 122a that spreads the supplied powder material evenly on the modeling stage 110 to form a thin layer of powder material.
[0124] In addition, the powder supply unit 121 may be configured to include a powder material storage unit provided vertically above the modeling stage 110, and a nozzle, and to eject resin powder for three-dimensional modeling on the same plane horizontally as the modeling stage.
[0125] The laser irradiation unit 130 includes a laser light source 131 and a galvanometer mirror 132a. The laser irradiation unit 130 may include a lens (not shown) for adjusting the focal length of the laser to the surface of the thin layer. The laser light source 131 may be any light source that emits a laser of the above wavelength with the above output. Examples of the laser light source 131 include a YAG laser light source, a fiber laser light source, and a CO2 laser light source. The galvanometer mirror 132a may be composed of an X mirror that reflects the laser emitted from the laser light source 131 and scans the laser in the X direction and a Y mirror that scans the laser in the Y direction.
[0126] The stage support unit 140 supports the modeling stage 110 so that its vertical position can be variably adjusted. In other words, the modeling stage 110 is configured to be precisely movable in the vertical direction by the stage support unit 140. Various configurations can be adopted for the stage support unit 140, and for example, it can be configured with a holding member that holds the modeling stage 110, a guide member that guides the holding member in the vertical direction, and a ball screw that engages with a screw hole provided in the guide member.
[0127] The control unit 150 controls the overall operation of the 3D object forming apparatus 100 during the operation of forming the 3D object.
[0128] The control unit 150 may also include a hardware processor such as a central processing unit, and may be configured to convert the three-dimensional printing data acquired by the data input unit 190 from the computer device 200 into a plurality of slice data sliced thinly in the stacking direction of the printing material layers. The slice data is printing data for each printing material layer for printing a three-dimensional object. The thickness of the slice data, i.e., the thickness of the printing material layer, corresponds to the distance (layer pitch) corresponding to the thickness of one printing material layer.
[0129] The display unit 160 can be, for example, a liquid crystal display or a monitor.
[0130] The operation unit 170 can include, for example, a keyboard and a pointing device such as a mouse, and may be provided with various operation keys such as a numeric keypad, an execution key, and a start key.
[0131] The storage unit 180 can include various storage media such as a ROM, a RAM, a magnetic disk, a HDD, and an SSD.
[0132] The 3D modeling apparatus 100 may include a pressure reducing unit (not shown) such as a pressure reducing pump that reduces the pressure inside the apparatus under the control of the control unit 150, or an inert gas supply unit (not shown) that supplies an inert gas into the apparatus under the control of the control unit 150. The 3D modeling apparatus 100 may also include a heater (not shown) that heats the inside of the apparatus, particularly the upper surface of the thin layer of resin powder for 3D modeling, under the control of the control unit 150.
[0133] <Example of 3D modeling using 3D modeling device 100> The control unit 150 converts the 3D modeling data acquired by the data input unit 190 from the computer device 200 into a plurality of slice data pieces obtained by thinly slicing the modeling material layers in the stacking direction. After that, the control unit 150 controls the following operations in the 3D modeling apparatus 100.
[0134] The powder supply unit 121 drives a motor and a drive mechanism (neither shown) in accordance with the supply information output from the control unit 150, moves the supply piston vertically upward (in the direction of the arrow in the figure), and extrudes the resin powder for three-dimensional modeling onto the same horizontal plane as the modeling stage.
[0135] Thereafter, the recoater driving unit 122 moves the recoater 122a horizontally (in the direction of the arrow in the figure) in accordance with the thin film formation information output from the control unit 150, transports the resin powder for three-dimensional modeling to the modeling stage 110, and presses the powder material so that the thickness of the thin layer is the same as the thickness of one layer of the modeled object.
[0136] Thereafter, the laser irradiation unit 130 emits a laser from the laser light source 131 in accordance with the laser irradiation information output from the control unit 150, in accordance with an area on the thin film that constitutes a three-dimensional object in each slice data, and scans the laser by driving the galvanometer mirror 132a by the galvanometer mirror driving unit 132. The ethylene-propylene copolymer particles contained in the resin powder for three-dimensional object formation are melted and bonded by the laser irradiation, and a modeling layer is formed.
[0137] Thereafter, the stage support unit 140 drives a motor and a drive mechanism (neither shown) in accordance with the position control information output from the control unit 150, and moves the modeling stage 110 vertically downward (in the direction of the arrow in the figure) by the layer pitch.
[0138] The display unit 160, under the control of the control unit 150 as necessary, displays various information and messages that should be recognized by the user. The operation unit 170 accepts various input operations by the user and outputs operation signals corresponding to the input operations to the control unit 150. For example, the virtual three-dimensional object to be formed is displayed on the display unit 160 to check whether a desired shape is formed, and if the desired shape is not formed, corrections may be made from the operation unit 170.
[0139] The control unit 150 stores data in the storage unit 180 or retrieves data from the storage unit 180 as necessary. By repeating these operations, layers of the object are stacked to produce a three-dimensional object. EXAMPLES
[0140] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0141] [Preparation of resin powder 1 for 3D modeling] <Synthesis of ethylene-propylene copolymer particles 1> (1) Preparation of solid titanium catalyst component 952 g of anhydrous magnesium chloride, 4420 mL of decane, and 3906 g of 2-ethylhexyl alcohol were heated at 130° C. for 2 hours to obtain a homogeneous solution. 213 g of phthalic anhydride was added to this solution, and the mixture was stirred and mixed at 130° C. for another hour to dissolve the phthalic anhydride. The homogeneous solution thus obtained was cooled to 23° C., and then 750 mL of this homogeneous solution was added dropwise over one hour to 2000 mL of titanium tetrachloride kept at −20° C. After the dropwise addition, the temperature of the resulting mixture was raised to 110° C. over four hours, and when it reached 110° C., 52.2 g of diisobutyl phthalate (DIBP) was added, and the mixture was kept at the same temperature for another two hours with stirring. Next, the solid portion was collected by hot filtration, resuspended in 2750 mL of titanium tetrachloride, and then heated again for 2 hours at 110° C. After heating was completed, the solid portion was collected again by hot filtration and washed with decane and hexane at 110° C. until no titanium compounds were detected in the washings. The solid titanium catalyst component prepared as above was stored as a hexane slurry, and a portion of it was dried to examine the catalyst composition. The solid titanium catalyst component contained titanium in the amounts of 2 mass%, chlorine in the amount of 57 mass%, magnesium in the amount of 21 mass%, and DIBP in the amount of 20 mass%.
[0142] (2) Preparation of prepolymerization catalyst 87.5 g of the solid titanium catalyst component, 99.8 mL of triethylaluminum, 28.4 mL of diethylaminotriethoxysilane, and 12.5 L of heptane were charged into a 20 L autoclave equipped with a stirrer, and 875 g of propylene was charged while maintaining the internal temperature at 15 to 20°C, and the reaction was carried out for 100 minutes while stirring. After the polymerization was completed, the solid component was allowed to settle, and the supernatant was removed and washed with heptane twice. The obtained prepolymerization catalyst was resuspended in purified heptane, and the concentration of the solid catalyst component was adjusted to 0.7 g / L with heptane.
[0143] (3) Main Polymerization To a jacketed circulation type tubular polymerization reactor having an internal volume of 58 L, propylene was continuously fed at 40 kg / h, hydrogen at 123 NL / h, the catalyst slurry produced in (2) at 0.30 g / h as a solid catalyst component, triethylaluminum at 2.1 mL / h, and diethylaminotriethoxysilane at 0.88 mL / h, and polymerization was carried out in a liquid-filled state in which no gas phase was present. The temperature of the tubular polymerization reactor was 70°C, and the pressure was 3.3 MPa / G. The obtained slurry was sent to a 100 L vessel polymerization reactor equipped with a stirrer, and further polymerization was carried out. Propylene was fed to the polymerization reactor at 15 kg / hr, and hydrogen was fed to the polymerization reactor so that the hydrogen concentration in the gas phase was 3.3 mol%. Polymerization was carried out at a polymerization temperature of 70°C and a pressure of 3.1 MPa / G. The obtained slurry was transferred to a 2.4 L liquid transfer tube, where it was gasified and subjected to gas-solid separation. After that, the polypropylene homopolymer powder was sent to a 480 L gas-phase polymerization reactor, where ethylene-propylene copolymerization was carried out. Propylene, ethylene, and hydrogen were continuously fed into the gas phase polymerization reactor so that the gas composition in the reactor was ethylene / (ethylene + propylene) = 0.01 (ethylene molar ratio) and hydrogen / ethylene = 0.10 (molar ratio). After polymerization at a polymerization temperature of 70°C and a pressure of 1.2 MPa / G, the particles were dried in vacuum at 80°C to obtain ethylene-propylene copolymer particles 1.
[0144] <Mechanical crushing process> The ethylene-propylene copolymer particles 1 obtained above were cooled to about -150°C with liquid nitrogen and pulverized with a pulverizer (Rinrex Mill) until the volume average particle size reached 80 μm.
[0145] <Particle spheroidization treatment> After the pulverization, the particles were subjected to a spheroidizing treatment. Specifically, the ethylene-propylene copolymer particles 1 were subjected to a mechanical impact force by hybridization to be spheroidized, and a resin powder 1 for three-dimensional modeling containing the ethylene-propylene copolymer particles 1 was obtained.
[0146] The volume average particle size, ethylene molar ratio, melt flow rate, and weight average molecular weight (Mw) of the ethylene-propylene copolymer particles 1 of the obtained resin powder 1 for three-dimensional modeling were measured, and the volume average particle size was 80 μm, the ethylene molar ratio was 0.01, the melt flow rate was 30 g / 10 min, and the weight average molecular weight (Mw) was 280,000. The number average particle size (Mn) of the ethylene-propylene copolymer particles was measured, and the number of particles (M2) having an average particle size 0.15 times the number average particle size (Mn) and the ratio (M1 / M2) of the number of particles (M1) having the number average particle size (Mn) were calculated. Furthermore, the number of particles (M3) having an average particle size 0.41 times the number average particle size (Mn) of the ethylene-propylene copolymer particles and the ratio (M1 / M3) of the number of particles (M1) having the number average particle size (Mn) were calculated and shown in the table below. The volume average particle size, ethylene molar ratio, melt flow rate, weight average molecular weight (Mw) and number average particle size (Mn) were measured by the methods described above. The resin powders 2 to 9 for 3D modeling prepared below were also measured in the same manner. For the number average particle size (Mn), the concentration index (Diffraction Volume) in the particle size distribution measuring device (Microtrac MT3300EXII, manufactured by Microtrac-Bell Co., Ltd.) was set to 0.8. Furthermore, the melting point of the obtained Resin Powder 1 for 3D modeling was measured by the above-mentioned method, and the value of (melting point temperature-recrystallization temperature) was calculated and shown in the following table.
[0147] [Preparation of resin powders 2 to 9 for 3D modeling] Resin powders 2 to 9 for 3D modeling were prepared in the same manner, except that in the preparation of resin powder 1 for 3D modeling, the powder was pulverized so that the volume average particle size in the mechanical pulverization process was as shown in the table below, and the ethylene-containing molar ratio in the gas phase polymerization reactor was as shown in the table below. In addition, for the resin powder 2 for 3D modeling, the polymerization temperature was changed from 70°C in the production of the resin powder 1 for 3D modeling to 80°C. Similarly to Resin Powder 1 for 3D Modeling, Resin Powders 2 to 9 were also measured for volume average particle size, ethylene molar ratio, melt flow rate, weight average molecular weight (Mw), melting point, and the like, and the results are shown in the table below.
[0148] [Creation of 3D objects 1-9] A 3D modeling device (Aspect (RaFaEl300)) was used to model the object on the modeling stage. The prepared resin powder for three-dimensional modeling was spread at a constant recoating speed (160 mm / s) to form a thin layer with a thickness of 0.1 mm. This thin layer was irradiated with laser light from a CO2 laser equipped with a galvanometer scanner for CO2 laser wavelengths in an area of 300 mm length x 300 mm width under the following conditions to produce a modeling layer. Thereafter, the resin powder for three-dimensional modeling was further spread on the modeling layer, and laser light was irradiated to laminate the modeling layer. These steps were repeated to produce three-dimensional models (laminated bodies of modeling layers) 1 to 9. Laser light emission conditions Laser power: 30W Laser light wavelength: 10.6μm Beam diameter: 300μm at the surface of the thin layer Laser light scanning conditions Scanning speed: 10000mm / sec Number of lines: 1 line
[0149] [evaluation] <Modeling Possibility> It was confirmed whether or not a three-dimensional object was obtained by the above-mentioned "production of a three-dimensional object".
[0150] <Elongation at break> The breaking elongation of the obtained three-dimensional object was measured using a Tensilon universal material testing machine RTC-1250 (manufactured by A&D Co., Ltd.). The measurement conditions were set as follows, and the breaking distance was taken as the breaking elongation, and the evaluation was made based on the presence or absence of a yield point. (If destruction occurred before the yield point, it was considered that there was no yield point.) Tensile test specimen: Shape conforming to JIS K7161 Tensile speed: 50mm / s Chuck distance: 115mm Gauge length: 100mm
[0151] <Tensile modulus> The tensile modulus of elasticity of the obtained three-dimensional object was measured using a Tensilon universal material testing machine RTC-1250 (manufactured by A&D Co., Ltd.). The measurement conditions were set as follows. The tensile modulus of elasticity was determined by linear regression between strains of 0.05 and 0.25%. It was determined that there was no practical problem when the value showed 80% or more of the tensile modulus of elasticity of Comparative Example 1 (1450 MPa) (i.e., 1160 MPa or more). Tensile test specimen: Shape conforming to JIS K7161 Tensile speed: 1mm / s Chuck distance: 115mm Gauge length: 100mm
[0152] [Table 1]
[0153] As is clear from the above results, the resin powder for 3D modeling of the present invention is capable of producing 3D objects and is also favorable in terms of tensile modulus and breaking elongation compared to the resin powder for 3D modeling of the comparative example. [Industrial Applicability]
[0154] INDUSTRIAL APPLICABILITY The present invention can be utilized for a resin powder for three-dimensional modeling, a three-dimensional model, and a method for producing a three-dimensional model, which use a polypropylene resin and have good tensile strength and excellent breaking elongation. [Explanation of symbols]
[0155] 100 Three-dimensional modeling equipment 110 Modeling Stage 120 Thin film forming section 121 Powder supply section 122 Recoater drive unit 122a Recoater 130 Laser irradiation unit 131 Laser Light Source 132 Galvano mirror drive unit 132a Galvano Mirror 140 Stage support 145 Base 150 Control section 160 Display section 170 Operation section 180 Storage section 190 Data Entry Section 200 Computer Equipment
Claims
1. A resin powder for three-dimensional modeling, Contains ethylene-propylene copolymer particles, The ethylene-propylene copolymer particles have a volume average particle size in the range of 5 to 200 μm; the ethylene-propylene copolymer particles have an ethylene molar ratio (ethylene / (ethylene+propylene)) in the range of 0.01 to 0.025; The weight average molecular weight of the ethylene-propylene copolymer particles is within a range of 260,000 to 330,000; and A resin powder for three-dimensional modeling, having a melt flow rate (MFR) in the range of 3 to 40 g / 10 min at 230°C.
2. The melting point is within the range of 100 to 160°C, and The resin powder for three-dimensional object formation according to claim 1 , which satisfies the following formula (1): Formula (1): (melting point temperature-recrystallization temperature)≧10° C.
3. 3. The resin powder for three-dimensional modeling according to claim 1 or claim 2, wherein the number of particles having an average particle size 0.15 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn).
4. 4. The resin powder for three-dimensional modeling according to claim 1, wherein the number of particles having an average particle size 0.41 times the number average particle size (Mn) of the ethylene-propylene copolymer particles is equal to or greater than the number of particles having the number average particle size (Mn).
5. A three-dimensional object formed using a resin powder for three-dimensional modeling, A three-dimensional object which is a sintered body or a molten body of the resin powder for three-dimensional object production according to any one of claims 1 to 4.
6. A method for producing a three-dimensional object using a resin powder for three-dimensional modeling, comprising the steps of: A method for producing a three-dimensional object by a powder bed fusion method, using the resin powder for three-dimensional object production according to any one of claims 1 to 4.
7. forming a thin layer of the resin powder for three-dimensional modeling; a step of selectively irradiating the formed thin layer with a laser beam to form a model layer in which resin particles contained in the resin powder for three-dimensional modeling are sintered or melt-bonded; The method for producing a three-dimensional object according to claim 6 , further comprising: repeating the step of forming the thin layer and the step of forming the object layer in this order a number of times to stack the object layers.
Citation Information
Patent Citations
Polypropylene powder for selective laser sintering and preparation thereof
CN107304270A
The deburring method of running steel
JP1989002810A
Resin powder for stereoscopic shaping, stereoscopic shaping apparatus, production method for stereoscopic shaping article, and resin powder
JP2019001154A
Three-dimensional (3D) printing method
WO2016068899A1
Polypropylene for additive manufacturing (3d printing)
WO2018041839A1