Spun yarn and loop pile towel using the same
A spun yarn blend of non-heat-fusible and heat-fusible fibers with a three-twist structure addresses the issue of fluff shedding in towels by maintaining texture and flexibility, effectively preventing fuzz from falling off through heat-fusion.
Patent Information
- Application Number
- JP2020130661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-07-31
AI Technical Summary
Existing spun yarns for towels struggle to balance texture and fluff prevention, with conventional methods failing to effectively prevent fuzz from falling off during use.
A spun yarn blend of non-heat-fusible fibers and heat-fusible fibers, specifically a composite polyester core-sheath structure with a high-melting point core and low-melting point sheath, is used, combined with a three-twist structure to create a loop pile towel that prevents shedding through heat-fusion.
The solution maintains a good texture while significantly reducing fluff shedding, ensuring the towel remains flexible and effective over time, even after multiple washes.
Smart Images

Figure 0007579650000002 
Figure 0007579650000003 
Figure 0007579650000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a spun yarn and a loop pile towel using the same. [Background technology]
[0002] The raw yarns used for towels include single spun yarns, two-ply yarns made by twisting two single yarns together, strong twist yarns with more twists than normal yarns, and loosely twisted yarns with less twists than normal yarns. The fewer the twists of these twisted yarns, the better the texture and water absorption, but the fewer the twists, the more fuzz there is, which becomes an obstacle to weaving and makes the fuzz more likely to fall off during washing. Conversely, the more twists the raw yarn has, the greater its "strength" and "stiffness" and the less fuzz there is, but it loses the "fullness" and "smoothness" that are important for towels. For this reason, ordinary towels use around 20-count single yarns, but as this is somewhat weak in terms of strength, it is starched before weaving to suppress fuzz and compensate for the strength of the yarn. Starch, PVA (polyvinyl alcohol), etc. are used for starch, and the yarn is desizing processed after weaving. Patent Document 1 proposes a towel using spun cross-twisted yarn with a specific number of fluffs. Patent Document 2 proposes weaving a towel using wool yarn, then treating it in water to shrink it and prevent fluff from falling off. Patent Document 3 proposes weaving a towel using loosely twisted yarn made of Egyptian cotton, Indian cotton, etc., then treating it in water to shrink it and prevent fluff from falling off. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-042370 A [Patent Document 2] JP 2003-201666 A [Patent Document 3] JP 2001-346713 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above-mentioned conventional techniques are unable to effectively prevent the shedding of fluff, and further improvements are required.
[0005] In order to solve the above-mentioned problems of the conventional art, the present invention provides a spun yarn that prevents fluff from falling off while maintaining a good texture, and a loop pile towel using the same. [Means for solving the problem]
[0006] The spun yarn of the present invention is a spun yarn obtained by blending non-thermofusible fibers and thermally fusible fibers, and the ratio of the thermally fusible fibers is 1% by weight or more and less than 10% by weight when the spun yarn is used as a parameter; The heat-fusible fiber is a polyester-based composite fiber having a core-sheath structure, the core component being a high-melting point polyester and the sheath component being a low-melting point copolymer polyester, and the non-heat-fusible fiber is cotton. The yarn is a three-ply spun yarn. The yarn cross section is round, and it is a spun yarn for loop pile towels. It is characterized by:
[0007] The woven fabric of the present invention is a woven fabric containing at least the spun yarn, It is a loop pile towel with a 3-pick terry motion weave. The heat-sealing fibers are fused to prevent cotton from coming off.
[0008] The loop pile towel of the present invention is a loop pile towel containing the above-mentioned spun yarn at least in the pile yarn, It is a loop pile towel with a 3-pick terry motion weave. The loop pile towel is characterized in that the thermally fused fibers are fused to prevent the cotton from coming off. Effect of the Invention
[0009] The spun yarn of the present invention is a blend of non-thermofusible fibers and thermofusible fibers, the ratio of thermofusible fibers being 1% by weight or more and less than 10% by weight when the spun yarn is taken as the modulus, and the spun yarn is a three-ply spun yarn, so that a loop pile towel can be provided that has a good texture and prevents fluff shedding even after long-term use, and the ratio of thermofusible fibers is relatively small, so that the texture is soft and fluff shedding can be prevented even after long-term use. Also, by blending the loop yarn with a high shedding rate with thermofusible fibers and subjecting it to a fusion treatment, cotton shedding can be efficiently prevented. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1A is a schematic side view of a three-filament twisted spun yarn according to one embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view of the same. [Diagram 2] FIG. 2 is a schematic diagram of the spinning machine. [Diagram 3] FIG. 3 is a schematic explanatory diagram of the loop pile towel fabric. [Figure 4] FIG. 4 is a diagram showing the weave structure of the loop pile towel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention relates to a spun yarn, which is a blend of non-thermofusible fibers and thermofusible fibers. The blend may be any blend, such as a cotton blend or a knead blend. The two component fibers are uniformly blended by blending. The ratio of the thermofusible fibers is 1% by weight or more and less than 10% by weight, with the spun yarn as the modulus. This allows the texture to be well maintained. If the thermofusible fibers are less than 1% by weight, the effect of shedding fuzz decreases. If the thermofusible fibers are 10% by weight or more, the texture becomes rough and hard. The preferred ratio of the thermofusible fibers is 2 to 9% by weight, and more preferably 3 to 8% by weight.
[0012] The non-thermal fusion fiber of the present invention is a fiber having a higher melting point, softening point or decomposition temperature than the thermal fusion fiber, and is a fiber with a ratio of 90 to 99% by weight when the spun yarn is used as a parameter. The non-thermal fusion fiber constituting the spun yarn may be a single fiber or a combination of two or more fibers. The non-thermal fusion fiber is preferably a cellulose fiber. The cellulose fiber is preferably at least one selected from natural cellulose fibers and regenerated cellulose fibers, and more preferably natural cellulose fibers. Natural cellulose fibers include cotton, hemp, bamboo, etc., and regenerated cellulose fibers include normal rayon, Bembell rayon, solvent-based rayon, lyocell, cupra, etc. Examples of blends of cellulose fibers and non-cellulose fibers include cotton and polyester, cotton and vinylon, etc., and blends of cotton and rayon are considered for cellulose fibers. The blend ratio of these fibers can be changed depending on the use.
[0013] The cotton that can be used in the present invention may be any type of cotton, including American cotton such as Supima cotton and San Joaquin cotton, Egyptian cotton such as Giza cotton, Indian cotton, Chinese cotton such as Xinjiang cotton, and Sea Island cotton.
[0014] In the present invention, the spun yarn is a three-strand twisted spun yarn. Compared with a yarn made from two rovings, this three-strand twisted spun yarn has less fuzz, good yarn uniformity, and is rounded in the longitudinal direction, and the yarn does not have diffuse reflection, so the fabric is neat and firm. Even if the yarn is a relatively thick count, the cross section of the yarn is rounded and uniform.
[0015] The heat-sealing fiber is preferably a composite fiber having a polyester-based core-sheath structure, and the core component is preferably a composite fiber having a high melting point polyester and the sheath component is preferably a low melting point copolymerized polyester. Polyester-based composite fibers have stiffness and quick drying properties. In addition, in the case of a core-sheath structure, the core component maintains the fiber shape, and the sheath component melts and is used for fusion, so that the texture can be kept soft. The high melting point polyester core component is preferably polytrimethylene terephthalate (PTT) or polyethylene terephthalate (PET, melting point 250 to 260°C), and may be a polyester copolymerized with 5-sodium sulfoisophthalate of a cationic dye-dyeable type. The low melting point copolymerized polyester sheath component preferably has a melting point 40°C or more lower than that of PET, and more preferably 45°C or more lower. An example of such a composite fiber having a polyester-based core-sheath structure is the product name "Safmet" manufactured by Toray Industries, Inc.
[0016] The spun yarn has a British count of 10 to 100, preferably 14 to 50. The twist coefficient K, as shown in the following formula, is preferably 1.0 to 8.0, more preferably 1.5 to 7.0. K=t / √S Where t: number of twists per inch (2.54 cm), S: British count (multiples of 840 yards (0.9144 m) at a standard weight of 1 pound (0.4536 kg)). The yarn count in the above range is suitable for loop pile towels, and the twist factor K in the above range can maintain a good texture. The English count can be converted to the internationally used tex count by the formula 590.5413 / English count.
[0017] The spun yarn can be used for loop pile towels, and is also suitable for clothing, socks, rugs, bedding, etc.
[0018] The woven or knitted fabric of the present invention contains the above-mentioned triple-twisted spun yarn in the yarn constituting the woven or knitted fabric, and after making the woven or knitted fabric, heat treatment is performed to fuse the heat-fusible fibers. The heat treatment may be performed on the spun yarn before the process of making the woven or knitted fabric. The heat treatment temperature is preferably in the range of not less than the melting point (Tm) or softening point (Sp) of the low melting point fiber of the heat-fusible fiber, and not more than about the melting point or softening point +20°C.
[0019] The woven or knitted fabric of the present invention can be used as yarn for towels, sock linings, innerwear, outerwear, and denim. Towel fabrics include gauze, waffle, cut pile, loop pile, etc. The woven or knitted fabric of the present invention can be preferably used for loop pile towels and socks.
[0020] The loop pile towel of the present invention contains the above-mentioned three-ply spun yarn at least in the loop yarn, and is woven into a loop pile fabric, which is then heat-treated to fuse the heat-fusible fibers. The heat treatment temperature is preferably in the range of not less than the melting point (Tm) or softening point (Sp) of the low-melting fiber of the heat-fusible fiber, and not more than about the melting point or softening point +20°C. Fusion does not occur below the above temperature, and cotton tends to be damaged if the temperature exceeds the above temperature. The heat treatment may be performed in the state of yarn (for example, in the state of being wound around a cheese) or after the fabric is produced. After the above-mentioned three-ply spun yarn is woven into a loop pile fabric, bleaching, dyeing, washing, drying, and the like can be performed using conventional methods. Since the loop yarn protrudes, the feathers have a high shedding rate, but by blending the loop yarn with heat-fusible fibers and performing a fusion treatment, the shedding of cotton can be efficiently prevented.
[0021] The weight of loop pile towels varies depending on factors such as the amount of pile and the thickness of the fabric. The weight per unit area of this loop pile towel is 130 to 700 g / m 2 More preferably, the weight of a bath towel is 400 to 600 g / m 2 , 130~200g / m for face towels 2 The above weight is sufficient for forming the pile and provides a good feel when used.
[0022] The cotton removal rate of the loop pile towel is preferably 0.2% by weight or less, calculated from the fluff removed by washing in a fully automatic domestic washing machine. This fluff removal test method is a method implemented by the Osaka Industrial Technology Research Institute, a local independent administrative institution, and will be described in detail later.
[0023] The three-ply spun yarn of the present invention can be used for any or all of the pile yarn, warp yarn (ground yarn) and weft yarn (ground yarn). It is particularly preferable to use it for pile yarn that is easy to remove cotton. The warp yarn (ground yarn) and weft yarn (ground yarn) may be spun cotton yarn, a blend of cotton and other fibers, or in some cases, a spun yarn of other fibers. Examples of other fibers include polyester fiber, rayon fiber, acrylic fiber and wool fiber. The blending ratio can be any ratio. The count of the warp yarn (ground yarn) and weft yarn (ground yarn) is 10 to 100 in English count, and the twist coefficient K shown in the above formula is preferably 1.0 to 8.0, more preferably 1.5 to 7.0.
[0024] The following description will be given with reference to the drawings. In the following drawings, the same reference numerals indicate the same objects. Fig. 1A is a schematic side view of a three-filament twisted spun yarn 1 according to one embodiment of the present invention, and Fig. 1B is a schematic cross-sectional view of the same. This three-filament twisted spun yarn 1 is a yarn in which spun yarn components 1a, 1b, and 1c are twisted together, and the cross section is nearly round as shown in Fig. 1B. The twist direction may be either S twist or Z twist. Usually, the twist direction of spun yarn components 1a, 1b, and 1c and the twist direction of three-filament twisted spun yarn 1 are the same.
[0025] FIG. 2 is a schematic diagram of the spinning machine 2. The spinning machine 2 is a ring spinning machine, and is composed of a drafting device 20 from the back rollers 7, 8 to the front rollers 14, 15, and a twisting winding device 21 from the front rollers 14, 15 to the traveler 18. The drafting device 20 drafts (stretches) the roving yarn to make it thinner. The twisting winding device 21 twists the drafted roving yarn in three in the same direction while giving it a twist, and winds the resulting yarn on a bobbin. When three roving yarns 3, 4, 5 are supplied from a bobbin (not shown) through one trumpet guide 6 having holes for dispersing the fiber bundles of the three roving yarns, the roving yarns 3, 4, 5 are introduced between the upper and lower back rollers 7, 8, respectively, and passed through at a predetermined speed. Here, the trumpet guide 6 has three holes provided at equal intervals in a row. The shape of the holes is wide at the entrance side, gradually narrows, and becomes a narrow groove of the same width at the exit side. The hole spacing is set appropriately depending on the count. For example, for counts thicker than British cotton count 30, a hole spacing of 3 to 5 mm is appropriate.
[0026] Next, the roving is passed between the second rollers 9, 10 having upper and lower aprons 11, 12. Here, the fiber bundle is gripped and weighted, and drafted while being controlled so as to prevent draft unevenness. The three rovings that have passed through the aprons 11, 12 are then passed through recesses provided in the collector 13, respectively, to maintain an appropriate distance between them. The rovings pass through three grooves provided in the collector 13, and are guided to the last rollers (front rollers 14, 15). The three grooves are formed continuously, and each is wide at the inlet side, gradually narrowing, and narrow at the outlet side, but of the same width. The collector 13 is installed near the front rollers 14, 15. The purpose of using the collector 13 is to prevent the fiber bundles from overlapping when the rovings pass through the draft device, and to combine the fleece 16 that comes out of the front rollers 14, 15 into one without breaking it.
[0027] Next, the three rovings are passed between upper and lower front rollers 14, 15 and drafted to form a thin layered fleece 16. The fleece 16 emerging from the front rollers 14, 15 is then passed through a snell wire 17. Next, the fleece 16 is ring spun by a traveler 18, twisting it once per revolution of the traveler, and the resulting yarn (spun pipe yarn) is wound around a pipe bobbin 19. In this manner, a three-strand twisted spun yarn is produced.
[0028] FIG. 3 is a schematic diagram of the loop pile towel fabric 22. The loop pile towel fabric 22 is composed of pile yarns 23, warp yarns (ground yarns) 24, and weft yarns (ground yarns) 25, and the pile yarns 23 form loop piles while being fixed to a ground weave composed of the warp yarns (ground yarns) 24 and weft yarns (ground yarns) 25. The three-strand spun yarn of the present invention can be used for any or all of the pile yarns 23, warp yarns (ground yarns) 24, and weft yarns (ground yarns) 25. It is particularly preferable to use it for the pile yarns 23, which are easily removed from the cotton. The loop pile towel fabric 22 is cut to a predetermined size, and the ends are processed to make a towel. In the case of a bath towel, the size is, for example, 70 cm vertically and 140 cm horizontally.
[0029] Figure 4 shows the weave of a loop pile towel. This weave is a three-pick terry motion, with the pile yarns crossing once for every three wefts. The warp yarns are arranged in an alternating pattern of ground yarns G and pile yarns P. In Figure 4, black and cross marks indicate floating yarns, and white indicates sinking yarns. EXAMPLES
[0030] The present invention will be specifically described below using examples, but the present invention is not limited to the following examples. <Lifting test method> The fluffing test method was conducted by the Osaka Industrial Technology Research Institute, a local independent administrative institution. (1) Sample: one towel. (2) Washing machine used: Fully automatic household washing machine, high water level, detergent used, standard wash cycle. Washing tests were conducted with and without fabric softener. (3) Collection of fuzz: Filter the fuzz from the lint filter in the washing machine and from the drainage water using a 150 μm mesh sieve. (4) Weighing: The collected fluff was pre-dried at 50°C, and then left to stand under standard conditions (20°C, 65% RH) until stable and then weighed. (5) Calculate using the following formula. Washing cotton removal rate (%) = [weight of cotton removed by washing (g) / towel weight before washing (g)] x 100
[0031] Example 1 <Raw fiber> 1 Pile yarn (1) Cotton The cotton used is Supima cotton. (2) Heat-sealing fibers The heat-sealing fiber used was a polyester-based core-sheath composite fiber, trade name "Safmet" T-9611 (fineness 2.2 decitex, fiber length 38 mm) manufactured by Toray Industries, Inc. This fiber has a strength of 3.4 cN / decitex and a breaking elongation of 39%. <Spun yarn manufacturing> 95% by mass of cotton and 5% by mass of heat-meltable fibers were mixed in a carding machine to form a web, a sliver, and a roving, which were then spun and twisted in a ring spinning machine as shown in Figure 2 to produce a three-ply twisted spinned yarn with an English cotton count of 20 (fineness: 29.5 tex), a twist rate of 15.65 turns / inch, Z twist, and a twist factor K of 3.5. This three-ply twisted spinned yarn was used as a single yarn and arranged as a pile yarn in the warp. 2. Ground thread (1) The warp yarn (ground yarn) was a ring-spun yarn made of 100% cotton by mass, British cotton count 16 (fineness: 36.9 tex), twist number 13.2 turns / inch, Z twist, twist factor K = 3.3. This spun yarn was used as a single yarn. (2) The weft (ground yarn) was a ring-spun yarn made of 100% cotton by mass, British cotton count 20 (fineness: 29.5 tex), twist number 14.8 turns / inch, Z twist, twist factor K=3.3. This spun yarn was used as a single yarn. <Textile manufacturing> A towel loom was used to manufacture the loop pile fabric shown in Figures 3 and 4. The pile yarn 23 was fed at a rate of six times that of the warp yarn (ground yarn) 24. In this way, a pile fabric with a warp density of 32 threads / inch and a weft density of 55 threads / inch was manufactured. After scouring and bleaching, this pile fabric was heat-treated in a tenter at a temperature of 190°C for 2 minutes to fuse the heat-fusible fibers. The mass per unit area (basis weight) of this fabric was 490g / m 2 It was. <Evaluation> The cotton removal rate was measured using the above-mentioned fluffing test method. As a result, the cotton removal rate of the sample with fabric softener added during washing was 0.06%, and the cotton removal rate of the sample without fabric softener was 0.05%.
[0032] Example 2 Except for using San Joaquin cotton instead of Supima cotton as the pile yarn, the same experiment was carried out as in Example 1. When this pile fabric was washed with fabric softener, the cotton removal rate was 0.12%, and when no fabric softener was used, the cotton removal rate was 0.11%.
[0033] Comparative Example 1 Except for not adding heat-fusible fibers to the pile yarn, the same procedure was carried out as in Example 1. When this pile fabric was washed, the sample to which fabric softener was added had a cotton removal rate of 0.27%, while the sample without fabric softener had a cotton removal rate of 0.23%. The above results are summarized in Table 1.
[0034] [Table 1]
[0035] As is clear from Table 1, the cotton removal rate was significantly reduced by adding 5% by mass of heat-fusible fibers to the pile yarn in Examples 1 and 2. When the texture was evaluated by sensory testing, the pile woven fabrics of Examples 1 and 2 were soft and equivalent to the comparative example. [Industrial Applicability]
[0036] The spun yarn of the present invention is also suitable for use in loop pile towels (bath towels, face towels, towel handkerchiefs, sports towels, bathrobes), clothing, socks, rugs, bedding, and the like. [Explanation of symbols]
[0037] 1 3-ply spun yarn 1a, 1b, 1c Spun yarn components 2 spinning machine 3,4,5 Coarse thread 6 Trumpet Guide 7,8 Back roller 9,10 Second Roller 11,12 Apron 13 Collector 14,15 Front roller 16 Fleece 17 Snell Wire 18 Traveler 19 Thread bobbin 20 Draft device 21 Twisting winding device 22 Loop pile towel fabric 23 Pile yarn 24 Warp threads (ground threads) 25 Weft thread (ground thread)
Claims
1. A spun yarn obtained by blending non-thermofusible fibers and thermally fusible fibers, The ratio of the heat-fusible fiber is 1% by weight or more and less than 10% by weight when the spun yarn is used as a parameter; The heat-sealing fiber is a polyester-based composite fiber having a core-sheath structure, the core component being a high-melting point polyester and the sheath component being a low-melting point copolymer polyester, The non-thermofusible fiber is cotton, The spun yarn is a three-ply spun yarn, has a round cross section, and is a spun yarn for loop pile towels.
2. 2. The spun yarn according to claim 1, wherein the spun yarn has an English count of 10 to 100.
3. 3. The spun yarn according to claim 1, wherein the twist coefficient K of the spun yarn is 1.0 to 8.0, as represented by the following formula: K = t / √S Where t: number of twists per inch (2.54 cm), S: British yarn count.
4. The spun yarn according to any one of claims 1 to 3, wherein the spun yarn is a spun yarn for a loop pile towel having a three-pick terry motion weave.
5. The woven fabric comprising at least the spun yarn according to any one of claims 1 to 4 is a loop pile towel of a three-pick terry motion woven fabric, A woven fabric characterized in that heat-fusible fibers are fused and the fabric is prevented from coming off.
6. A loop pile towel comprising at least a pile yarn containing the spun yarn according to any one of claims 1 to 4, The towel is a loop pile towel made of a 3-pick terry motion fabric. The loop pile towel is characterized in that heat-fusible fibers are fused to the loop pile towel, thereby preventing the cotton from coming off.
Citation Information
Patent Citations
Spun yarn
JP1985181331A
Span yarn for machine sewing thread
JP1997228174A
Sheath-core structure srun yarn and woven or knitted fabric thereerom
JP2001123351A
Towel handkerchief
JP2001346713A
Method for preventing falling off of pile yarn of towel cloth
JP2003201666A