Polyester resin molded products, recycled molded products, and their manufacturing method
The polyester resin molded product with a water-soluble anchoring agent and barrier layer addresses thermal decomposition and recyclability issues, ensuring transparency and recyclability, thus reducing waste and costs.
Patent Information
- Application Number
- JP2022176138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2037-09-08
AI Technical Summary
Current high-barrier PET materials used in packaging containers face issues with thermal decomposition during extrusion, leading to gel formation and inability to be recycled, and lack transparency considerations in existing gas barrier films.
A polyester resin molded product with a water-soluble anchoring agent layer and a barrier layer, ensuring transparency and recyclability by using a polyester base sheet with a haze value of 90 to 110, and a recycled product maintaining similar properties.
The solution provides transparent and recyclable packaging containers with gas barrier properties, reducing waste and disposal costs while maintaining performance comparable to regular PET.
Smart Images

Figure 0007579834000001 
Figure 0007579834000002 
Figure 0007579834000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a polyester resin molded article having excellent transparency and recyclability, and a recycled molded article. The present invention relates to a product and a method for manufacturing the same. [Background technology]
[0002] Polyesters, such as polyethylene terephthalate (hereinafter referred to as "PET") Resins have excellent chemical and physical properties. In addition, polyester resins have excellent mechanical strength and It has excellent properties of transparency and is therefore suitable for use in packaging containers such as beverage bottles, films, and sheets. It is widely used in transportation, etc.
[0003] In packaging containers, especially food and beverage packaging containers, the contents to be stored (beverages, food, etc.) To avoid adverse effects from gases such as oxygen or water vapor in the air, or for long-term Gas barrier properties are sometimes required to prevent loss of moisture during storage. Gas barrier film with a barrier layer formed on a resin film substrate to improve barrier properties. Such a barrier layer is usually formed by bonding a resin to the film via an anchor agent (AC agent). It is formed on the surface of a film substrate. For example, Patent Document 1 discloses a method for forming a film containing a silane coupling agent. A barrier layer containing montmorillonite was formed on the surface of the PET substrate sheet via an AC agent. A gas barrier film is described.
[0004] In recent years, the consumption of polyester resin has increased. From the perspective of reducing waste, efforts are being made to reuse polyester resins. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2005-1242 Summary of the Invention [Problem to be solved by the invention]
[0006] The current high-barrier PET, which has improved gas barrier properties, is made from ethylene-vinyl alcohol copolymer It is laminated with EVAL and non-oriented polypropylene film (CPP). However, when this high-barrier PET is extruded under the same conditions as PET, it undergoes thermal decomposition and gels. Therefore, it cannot be crushed and recycled like regular PET and must be disposed of. There is no choice.
[0007] As mentioned above, when a resin film is used for a packaging container or the like, transparency is required. However, Patent Document 1 examines the transparency of the sheet, but does not examine the transparency of the container. All technical knowledge is not disclosed.
[0008] The present invention relates to a polyester resin molded article having excellent transparency and recyclability, and a recycled molded article. The present invention aims to provide a product and a method for manufacturing the same. [Means for solving the problem]
[0009] The polyester resin molded article of the present invention comprises a polyester substrate sheet layer and the polyester An anchor agent layer and a barrier layer are laminated in this order on at least one surface of a rubber-based substrate sheet layer. A molded sheet product, wherein the anchoring agent layer is formed by a water-soluble polyester-based anchoring agent. The haze value of the molded article is determined based on the polyester base sheet layer alone. The haze value of the sheet molded product is 90 to 110 relative to the value of 100. It is characterized by:
[0010] The recycled molded article of the present invention is a recycled polyester resin derived from the molded article of the present invention or the sheet. The recycled molded product is a polyester-based base sheet, and the haze value of the recycled molded product is The relative value is 90 to 110, assuming the haze value of a sheet molded product consisting of only one layer is 100. It is characterized by the fact that
[0011] The method for producing the recycled molded article of the present invention is to use recycled polyester derived from the molded article of the present invention or the sheet. The method is characterized in that it includes a step of producing a recycled molded product by molding a steric resin. . [Effects of the Invention]
[0012] The molded article of the present invention has gas barrier properties and transparency comparable to that of PET molded articles. Therefore, the molded article of the present invention is suitable for applications where transparency is required, such as packaging for food and drink. The recycled molded product of the present invention can be suitably used for containers. Therefore, the molded article of the present invention has the same transparency as ordinary PET. As a result, according to the present invention, the amount of waste molded products and This reduces waste and disposal costs and reduces the burden on the environment. DETAILED DESCRIPTION OF THE INVENTION
[0013] An embodiment of the present invention will be described below. This embodiment is an example of how the present invention is implemented. Therefore, the present invention is not limited to this embodiment.
[0014] (1) Polyester resin molded products The polyester-based resin molded article according to this embodiment (hereinafter referred to as "the molded article") is made of polyester. An ester-based base sheet layer and an anchor on at least one side of the polyester-based base sheet layer. A molded sheet product in which an anchoring agent layer and a barrier layer are laminated in this order, wherein the anchoring agent layer is The layer is formed from a water-soluble polyester anchoring agent, and the haze value of the molded article is The haze value of a molded sheet consisting of only the polyester base sheet layer is set to 100. The relative value when the temperature is 90 to 110 is obtained. This molded product suppresses whitening after molding into a container and has excellent transparency. As will be described later, the molded products obtained by reusing this molded product are made from new materials. Therefore, this molded product has the same physical properties and transparency as the molded product obtained using ordinary P. It can be reused in the same way as ET.
[0015] The polyester constituting the polyester-based base sheet (hereinafter simply referred to as "base sheet") layer Polyester resins are made from polycarboxylic acids or their derivatives (esters, anhydrides, etc.) and polyalcohols. There is no limitation on the specific structure or type of the polycarboxylic acid, as long as it is a polycondensation product with coal. As the polyol, a dicarboxylic acid is usually used, and as the polyalcohol, a diol is usually used. As the polycarboxylic acid, for example, an aromatic polycarboxylic acid can be used. The polyester resin is a mixture of the polycarboxylic acid or a derivative thereof and the polyalcohol. It may also be a polycondensation product of a vinyl group-containing monomer such as styrene. The polyester resin may be a copolymer obtained by copolymerization. Polyester resins modified with epoxy resins may also be used.
[0016] Specific examples of the polyester resin include polyethylene terephthalate (PE T), polypropylene terephthalate, polybutylene terephthalate, polyethylene naphtha Polybutylene naphthalate, Polyethylene-1,2-bis(phenoxy)ethoxy cyclohexylene-4,4'-dicarboxylate, and polycyclohexylene dimethylene terephthalate The polyester resin is preferably PET.
[0017] The polyester resin may be in either a crystalline state or an amorphous state. The resin is preferably an amorphous polyester resin, more preferably an amorphous PE T. "Amorphous PET" is PET that has not crystallized like A-PET. This includes PET that is not completely crystallized, such as PET-ET and PET-G. The "PET" is preferably PET in a non-crystallized state such as A-PET.
[0018] The anchor agent (hereinafter referred to as "AC agent") layer is formed by the AC agent. This layer is formed on at least one surface and bonds the base sheet layer and the barrier layer together. The AC agent is a water-soluble polyester-based AC agent. This can prevent whitening (reduction in transparency) after the container is formed.
[0019] The water-soluble polyester AC agent is a polyester resin dissolved or dispersed in an aqueous medium. As long as the base sheet layer and the barrier layer can be bonded to each other, the specific There is no particular limitation on the composition. As described above, the water-soluble polyester AC agent contains a polyester. Not only when the steric resin is dissolved in an aqueous medium, but also when it is used in an aqueous medium as an emulsion, etc. The aqueous medium may be water or a mixture of water and alcohol (e.g., C It is a mixed medium with 1-C4 alcohol.
[0020] The polyester resin contained in the water-soluble polyester AC agent is a saturated polyester resin. The polyester resin may be a polyester or an unsaturated polyester resin. Preferably, the polyester resin has a hydroxyl group or a carboxyl group. Specific examples of the polyacrylate include polyacrylic ester and ethylene-acrylic ester. Examples of commercially available water-soluble polyester anchoring agents include: As for water-soluble polyester, "Plus Coat Z-687" manufactured by Goo Chemical Industry Co., Ltd. and "Plus Coat Z-880".
[0021] When the AC agent layer is formed, the water-soluble polyester-based AC agent may be used alone, Two or more of these may be used in combination. Alternatively, the water-soluble polyester AC agent may be used alone. However, other anchoring agents may be used in combination within the range that does not impair the effects of the present invention.
[0022] The AC agent layer is usually formed by applying an AC agent to the surface of the base sheet layer and then drying it. The coating and drying methods and conditions are not particularly limited, and As the coating method, specifically, a well-known method such as gravure coating can be used. The drying method may be a conventional wet coating method. Examples include drying and infrared irradiation.
[0023] The amount of the AC agent to be applied is as small as possible to bond the barrier layer and the base sheet layer. The amount of application is not particularly limited, and depends on the type of the AC agent and the amount of application of the barrier layer and the base sheet. The coating amount can be set to an appropriate range depending on the configuration of the coating layer. If so, the solid content is 0.05 to 5 g / m 2 , preferably 0.1 to 2 g / m 2 It can be said that When the coating amount is within the above range, excellent adhesion can be achieved and the drying time can be shortened. This is preferable because it can be done easily.
[0024] The barrier layer is formed on the outer side of the AC agent layer (the surface of the AC agent layer, which is adjacent to the base sheet layer) The specific structure of the laminate is not particularly limited as long as it has gas barrier properties. Specific examples of the material for forming the barrier layer include resins, metal oxides, and the like. substances (aluminum oxide, silicon oxide, magnesium oxide, etc.) or inorganic compounds (aluminum nitride Examples of the thin film include a thin film of a nitride such as silicon nitride, a carbide such as silicon carbide, etc. The barrier layer is preferably a barrier layer formed of a resin. There is no limitation. Specific examples of the resin include polyvinylidene chloride resin, polyvinyl Examples include alcohol resins and ethylene vinyl alcohol copolymers.
[0025] The barrier layer may contain other components. In the case of a rear layer, specific examples of the other components include layered inorganic compounds. Layered minerals and silicates are included. By including layered silicates, gas barrier properties are improved. Specific examples of the layered silicate include hydrous silicate. silicates (phyllosilicate minerals, etc.), kaolinite group clay minerals (halloysite, kaolinite, etc.) antigorite group clay minerals (antigorite, endelite, dickite, nacrilite, etc.) gorite, chrysotile, etc.), smectite clay minerals (montmorillonite, beidelite, etc.) nontronite, saponite, hectorite, sauconite, stevensite, etc.) Vermiculite clay minerals (such as vermiculite), mica or mica clay minerals (such as white clouds) Examples include quartz, phlogopite, mica such as margarite, tetrasilicic mica, and taeniolite. These may be natural minerals or synthetic compounds. As the layered inorganic compound, layered silica is preferably used. More preferably, it is a montmorillonite.
[0026] The method for forming the barrier layer is not particularly limited. The barrier layer can be formed by a known method depending on the type of material. When the barrier layer is formed by the resin solution or dispersion (if necessary, a pre-formed layer may be added to the medium), The layered inorganic compound may be included.) is applied to the surface of the AC agent layer, and then dried. The coating and drying methods and conditions are not particularly limited. A known method can be used. Specific examples of the coating method include gravure coating. The drying method specifically includes a conventional wet coating method. These include air drying and infrared irradiation.
[0027] The sheet may have other layers as needed. For example, to improve waterproofing, The outer side of the barrier layer (the side of the surface of the barrier layer that is not in contact with the AC agent layer) A waterproof protective layer can be provided on the surface of the substrate. There is no particular limitation on the type of the waterproof protective layer. Specific examples of the waterproof protective layer include a protective layer having an acrylic resin as a base material. can be done.
[0028] There is no particular limitation on the method for producing the sheet. The AC agent is applied to the surface of the polyester resin constituting the composition and dried to form the AC agent. Then, a barrier agent is applied to the outside of the AC agent layer and dried to form a pre-coated layer. The barrier layer can be formed as described above.
[0029] There is no particular limitation on the thickness of the sheet or the layers constituting the sheet. The thickness of the sheet can be determined appropriately as needed. The thickness of the base sheet layer is usually 0.1 to 1 mm.
[0030] Each layer constituting the sheet may be formed as necessary within the range that does not significantly impair transparency and recyclability. If necessary, other components may be contained. For example, the base sheet layer may contain polyester. The resin may contain other resins other than the resin. Additives used in the resin sheet, such as flame retardants, ultraviolet absorbers, fluorescent whitening agents, Antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, and Antibacterial agents are included.
[0031] The molded product can be obtained by molding the sheet. There is no particular limitation on the molding method. As the molding method, there is no known molding method generally adopted for polyester resins. Specifically, for example, vacuum molding (plug-assist molding, etc.), injection molding, ultra-high Rapid injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, and heat-insulating molds. Molding methods used, molding methods using rapid heating molds, foam molding (including supercritical fluids), Cert molding, IMC (in-mold coating molding) molding method, extrusion molding method, sheet molding Examples of methods include thermoforming, rotational molding, lamination molding, press molding, and blow molding. The molding conditions are not particularly limited and can be appropriately determined as needed.
[0032] The haze value of this molded product is calculated by setting the haze value of a molded product consisting of only the base sheet layer at 100. The relative value when the temperature is 90 to 110, preferably 92 to 108, and more preferably 95 to 105 The "haze value of the molded article consisting of only the base sheet layer is 90 to 110" means the The same method as this molded product was used except that a sheet consisting of only the base sheet layer was used instead of the above sheet. The haze value of the molded product obtained by this method is 100, and the relative value is 90 to 110. The haze value is a value measured in accordance with JIS K 7136. As long as the above condition is satisfied, there is no particular limitation on the specific range of the haze value of the molded product. The value is usually 10% or less, preferably 8% or less, and more preferably 5% or less.
[0033] There are no particular limitations on the shape, dimensions, or specific uses of this molded product. , packaging containers, for example, food and drink packaging containers. It includes not only the entire container but also a part of the container. For example, the "container" includes not only the main body of the container but also a part of the container. This also includes the lid of the container.
[0034] (2) Recycled molded products and their manufacturing methods The recycled molded product according to this embodiment (hereinafter referred to as the "recycled molded product") is a product obtained by reusing the recycled molded product or the previous product. A recycled molded product made of recycled polyester resin derived from the sheet, The haze value of a molded sheet consisting of only the polyester base sheet layer is 10 The relative value when set to 0 is 90 to 110. The method (hereinafter referred to as "the method") is a method for producing recycled polyester from the molded product or the sheet. The recycled molded product is manufactured by molding a new plastic resin. The physical properties (e.g., IV value, flexural modulus and tensile strength) of the molded product obtained using the material are the same as those of the molded product obtained using the material. In this method, the recycled polyester has strength such as tensile modulus and transparency. The resin can be recycled in the same way as regular PET, resulting in a reduction in waste material. This reduces the burden on the environment and also reduces the production costs of polyester resin. This is preferable because it can
[0035] The recycled polyester resin may be prepared in the form of a product or a sheet. The method is not particularly limited. The recycled polyester resin may be, for example, The recycled polyester resin can be prepared by crushing the recycled polyester resin. For example, when manufacturing the molded product or the sheet, Scrap materials from the sheet (for example, scrap materials generated during container molding) can be used.
[0036] The recycled polyester resin is molded to produce the recycled molded product. There is no particular limitation on the type of resin. Usually, the recycled polyester resin or other resins and and / or other ingredients are kneaded using a conventional kneader, roll, mixer or extruder, Next, known molding methods such as extrusion molding, injection molding, calendar molding, blow molding, vacuum molding, and pressure molding are used. A resin sheet is produced by the molding method described above, and the resin sheet is then molded into, for example, the molded product shown in the section on the present invention. By molding using the molding method described above, the recycled molded product can be manufactured. There are no particular limitations on the specific conditions (for example, temperature and time) in the process. It can be determined appropriately as needed.
[0037] In the present recycled molded product and method, in addition to the recycled polyester resin, other materials may be used as needed. For example, the other resin may be a polyester resin. Resins, especially virgin polyester resins, can be used. In addition, the other components may be the same as those described in the section on the molded product. When other resins are used in combination, the ratio of the recycled polyester resin to the other resins is not particularly important. For example, the total mass of the recycled polyester resin and the other resin is 100%. In the mass %, the proportion of the recycled polyester resin can be 10 to 70 mass %.
[0038] The haze value of this recycled molded product is calculated by dividing the haze value of a molded product consisting of only the base sheet layer by 100. The relative value when 05. In addition, "a haze value of 90 to 110 for a molded article consisting of only the base sheet layer" means The recycled molded product is obtained in the same manner as the present recycled molded product, except that a sheet consisting of only the base sheet layer is used. The haze value of the molded article is set to 100, and the relative value is 90 to 110. The haze value is a value measured in accordance with JIS K 7136. As long as the above conditions are met, Therefore, there is no particular limitation on the specific range of the haze value of this recycled molded product. is usually 10% or less, preferably 8% or less, and more preferably 5% or less.
[0039] The recycled molded product is obtained by molding the recycled polyester resin, and has no haze. As long as the values are within the above ranges, there are no particular limitations on the specific structure. It may be a single-layer structure or a multi-layer structure containing two or more layers. There are no particular limitations on the type and specific uses. For these, the explanation in the section on molded products is appropriate. do. [Example]
[0040] The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to the embodiments shown in the examples. The embodiments of the present invention may be modified in various ways within the scope of the present invention depending on the purpose, application, etc. It is possible.
[0041] 1. Evaluation of transparency and gas barrier properties of molded products (1) Container manufacturing <Example> The following components were used as raw materials. The IV values (d The viscosity (l / g) was measured in accordance with JIS K 7367-5. A mixed solvent of 1,1,2,2-tetrachloroethane (weight ratio 3 / 1) was used. (A) A-PET: PET resin "YS-H01" manufactured by Hainan Yisheng Petrochemical Co., Ltd., China (IV value = 0. 78dl / g, thickness 0.85mm) (B) Water-soluble polyester AC agent; "Pluscoat Z-687" manufactured by Goo Chemical Co., Ltd. "Plus Coat Z-880". When using, the AC agent is diluted with isopropyl alcohol by mass. The mixture was diluted with alcohol and water (2:1) (AC agent:diluent ratio of 16:84 by mass). (C) Barrier agent: "EXCEIER" (containing montmorillonite) manufactured by Sumitomo Chemical Co., Ltd. (D) Protective agent: "Stiply" manufactured by Osaka Printing Ink Co., Ltd. When used, the protective agent is diluted with a diluent (Stiply). The protective agent was diluted with a diluent (protectant:diluent=1:1 by mass).
[0042] The A-PET was subjected to a corona discharge treatment, and then printed on a gravure plate (6-zone printing machine). The AC agent, barrier agent, and protective agent were applied in this order to the corona discharge treated surface of the A-PET. The sheet was then coated with the AC agent layer, the barrier layer, and the protective layer, and dried to produce a sheet. The specific application and drying conditions are shown in Table 1.
[0043] [Table 1]
[0044] The sheet obtained by the above method is thermoformed into a container (container size) by vacuum pressure forming. Specifically, a convex part called a plug was manufactured. By using a resin mold in combination with the resin sheet, the resin is softened by heating and pressed with a plug. The inner shape of the container is given to the grease sheet to correspond to the outer shape of the plug, and then the cavity The bottom and sides of the container are formed by vacuuming the mold. The upper heater temperature is 375°C and the lower heater temperature is 395°C.
[0045] <Comparative Example 1> Instead of the AC agent used in the examples, a polyethyleneimine-based AC agent ("AD-3" manufactured by Toyo-Morton Co., Ltd.) was used. 72MW and Seikadyne 4100 manufactured by Dainichi Seika Chemicals Co., Ltd.) and the mixture of the AC agent and the diluent The dilution ratio was 1:6 (AD-372MW: diluent) and 1:9 (Seikadyne 410 A container was produced in the same manner as in Example 1, except that the ratio of the cellulose acetate to diluent was changed to 1:9.
[0046] <Comparative Example 2> Instead of the sheet of the example, a sheet made of A-PET of the example was used, and the same A container was manufactured by the method.
[0047] (2) Performance evaluation The haze value and oxygen permeability of the containers of the example and comparative examples 1 and 2 were measured by the following methods. The haze values of the sheets produced in Example 1 and Comparative Example 1 and the A-PET were also measured. The results are shown in Table 2 below.
[0048] (I) Haze value Measurement was carried out in accordance with JIS K 7136.
[0049] (II) Oxygen permeability According to JIS K7126 A method, an oxygen permeability measuring device (Illinois Corporation, "8001 The measurement was carried out under the condition of an atmosphere of 23°C.
[0050] [Table 2]
[0051] As can be seen from Table 2, in Comparative Example 1, in which a polyethyleneimine-based AC agent was used as the AC agent, the sheet and The container became cloudy and transparency was reduced. On the other hand, the haze value of the container of the example was 4. The haze value is 0.3%, which is a relative value when the haze value of the A-PET molded product (Comparative Example 2) is set to 100. The oxygen permeability of the containers of the examples was 90 to 110, and the transparency was maintained at the same level. The gas permeability was 0.06 cc / pack / day, which was superior to that of the A-PET molded product (Comparative Example 2). From these results, it can be seen that the containers of the examples have the following properties compared to Comparative Examples 1 and 2: It is clear that the film has excellent transparency and gas barrier properties.
[0052] 2.Recyclability evaluation (1) Manufacturing recycled sheets The waste material generated during the molding of the container in the above example was crushed and recycled into polyester resin. In addition to the above-mentioned crushed PET, the following materials were used as raw materials for the recycled sheet: The following components were used: (A) A-PET (new material): PET resin manufactured by Hainan Yisheng Petrochemical Co., Ltd., China, used in the above examples. YS-H01 (B) Lubricant MB: Toyobo "RE555" (polyester with an intrinsic viscosity of 0.62 dl / g) Fine particles made by mixing 7000 ppm of spherical silica with an average particle size of 2.4 μm into the resin during polymerization. (See JP-A-2008-30282) (C) Black pigment: "APET-BK-3216" manufactured by Nikko Bix Co., Ltd.
[0053] A mixture of 94% by mass of A-PET (new material) and 6% by mass of MB lubricant was prepared to form the surface layer. The crushed PET, A-PET (new material), and black pigment were mixed in the ratios shown in Table 3. A mixture for forming a core layer was prepared. The mixture for forming the core layer and the mixture for forming the surface layer were mixed together in 2 portions. The material is fed into a screw extruder and melt-kneaded and extruded at a processing temperature of 280°C. Recycled sheets (sheets 1 and 2) were prepared. The recycled sheets had a thickness of 0.35 mm and a layer structure. It is two types and three layers (layer ratio: skin layer / core layer / skin layer = 4% / 92% / 4%).
[0054] A mixture of 94% by mass of A-PET (new material) and 6% by mass of MB lubricant was prepared to form the surface layer. The crushed sheet was mixed with A-PET (new material) in the ratio shown in Table 4 to form a core layer. A mixture for forming a core layer and a mixture for forming a surface layer were prepared. Recycled sheets (sheets 3 to 5) for transparency evaluation were prepared in the same manner as above. The sheet is 0.30 mm thick and has a layer structure of two types and three layers (layer ratio: skin layer / core layer / skin layer = 4% / 92% / 4%).
[0055] (2) Performance evaluation of recycled sheets Using the above-mentioned sheets 1 and 2, the IV value, flexural modulus, tensile modulus, The DuPont impact strength was measured. As a control, a sample containing no crushed PET in the core layer was used. The performance of the sheet was also evaluated, and the results are shown in Table 3. (A) IV value: Measured using the same method as that for A-PET (new material). (B) Flexural modulus: JIS (Japanese Industrial Standard) K7171, Shimadzu Corporation Using an autograph manufactured by , the measurement conditions were: distance between supports: 30 mm, bending speed: 20 mm / min Measured. (C) Tensile modulus: measured in accordance with JIS K7127. (D) DuPont impact strength: measured in accordance with JIS K7124.
[0056] [Table 3]
[0057] The haze values of the sheets 3 to 5 were measured in accordance with JIS K 7136. As a control, the transparency haze value of A-PET (new material) having the same thickness as the sheet was measured. The results are shown in Table 4.
[0058] [Table 4]
[0059] From Tables 3 and 4, the recycled sheet has the same level of durability as the sheet made of A-PET (new material). From these results, the container of the above example or the sheet constituting it was found to be strong and transparent. It can be seen that PET can be suitably used as a recycled material, just like regular PET.
Claims
[Claim 1] A method for producing a recycled molded product by molding recycled polyester resin derived from a molded product or sheet, The method for producing a recycled molded product is characterized in that the molded product or sheet is a sheet comprising a polyester-based base sheet layer and an anchor agent layer and a barrier layer laminated in this order on at least one side of the polyester-based base sheet layer, or a molded product molded from the sheet, wherein the anchor agent layer is a layer formed from a water-soluble polyester-based anchor agent, the barrier layer is a barrier layer formed from a resin containing layered silicate, and the molded product has a haze value of 90 to 110 in relative value when the haze value of a molded product of a sheet consisting of only the polyester-based base sheet layer is taken as 100.
Citation Information
Patent Citations
Gas-barrier film and packaging material using the film
JP2005001242A
Polyester film
JP2005097560A