Crosslinkable thermoplastic resin compositions and methods for forming same, and methods for forming cured thermoplastic resins - Patents.com

Crosslinkable thermoplastic resin compositions formed from bis-benzoxazine monomers and difunctional comonomers address the limitations of traditional thermoplastics by providing high temperature resistance and adhesion to fibers, while maintaining moldability and processability, thus combining the benefits of both thermosets and thermoplastics.

JP7579883B2Active Publication Date: 2024-11-08KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022562999
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-18
Filing Date
2021-04-15
Publication Date
2024-11-08
Estimated Expiration
2041-04-15

AI Technical Summary

Technical Problem

Existing thermoplastic resins face challenges in achieving a combination of properties such as high temperature resistance, adhesion to fibers, and processability similar to thermosets, while maintaining the moldability of thermoplastics, and they often require complex temperature control and have high raw material costs.

Method used

Development of crosslinkable thermoplastic resin compositions formed by reacting bis-benzoxazine monomers with difunctional comonomers, allowing for crosslinking at elevated temperatures to achieve thermoset-like properties while remaining moldable below those temperatures, using methods like solution and melt polymerization with specific solvent systems and purification techniques to control monomer content.

Benefits of technology

The resulting benzoxazine thermoplastics exhibit improved processability and thermal stability, with the ability to be molded and remolded like thermoplastics and possess properties similar to thermosets, including high temperature resistance and adhesion to fibers, while reducing material costs and simplifying processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579883000018
    Figure 0007579883000018
  • Figure 0007579883000019
    Figure 0007579883000019
  • Figure 0007579883000020
    Figure 0007579883000020
Patent Text Reader

Abstract

The crosslinkable thermoplastic composition may include a polymer formed from the reaction of a bis-benzoxazine monomer with a difunctional comonomer having a phenolic, amine, and / or thiol functional group, wherein the polymer contains at least one crosslinkable group. A method for forming the crosslinkable thermoplastic composition may include reacting the bis-benzoxazine monomer and the difunctional comonomer to form a polymer containing at least one crosslinkable group. A method for forming a cured thermoplastic may include curing the crosslinkable thermoplastic composition by applying an external stimulus.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] 〔background〕 Thermosetting resins ("thermosets") and thermoplastic resins ("thermosets") are different classes of polymers, differentiated from one another based on their behavior in the presence of heat. Specifically, thermoplastics such as polyethylene (PE), polycarbonate (PC) and polyetheretherketone (PEEK) become flexible or moldable when heated (and solidify when cooled), whereas thermosets such as epoxies, benzoxazines and bismaleimides become irreversibly solid when cured and cannot be melted and remolded by heating. Thus, thermoplastic materials have a melting temperature (melting point) at which they begin to flow, whereas cured thermoset products can withstand higher temperatures without losing their structural integrity.

[0002] Both thermosets and thermoplastics have been used in advanced composites as building blocks for applications such as aerospace structures and interior components. Thermosets generally have a high modulus and excellent creep resistance compared to thermoplastics due to the three-dimensional network of bonds achieved during crosslinking (curing). This results in their lower elongation at break values ​​than thermoplastics, and thermosets also generally require extended cure times at temperatures ranging up to 250°C. However, many uncured thermosets have a limited shelf life and are at risk of degradation (less than 6 months for typical refrigerated storage of thermoset prepregs). Also, the cure cycle must be carefully controlled to achieve the desired cure state.

[0003] Thermoplastics, on the other hand, have the advantage of not requiring crosslinking (curing). Other advantages of thermoplastics include indefinite shelf life at room temperature (in the absence of UV radiation), short molding times, improved fire / smoke / toxicity (FST) performance, remoldability, enhanced vibration and sound damping, excellent impact damage resistance (impact toughness), ability to tailor material morphology (design flexibility), excellent shear and fracture strength, and recyclability. Thermoplastics also offer the option of fusing or welding molded subcomponents, which can reduce the weight and stress concentrations of assemblies by eliminating fasteners and adhesives. However, thermoplastics generally have significantly higher raw material costs than competing thermosets. Molding thermoplastics is also difficult. Most thermoplastic prepregs use PEEK, polyphenylene sulfide (PPS), polyimide (PI), polyetherimide (PEI), etc., which are maintained as pre-solidified dry sheets or boards and must be preheated to over 350°C to make them flexible. Often, complex temperature control tools are required to obtain optimal lamination properties of thermoplastic resins.

[0004] 〔summary〕 This Summary is provided to introduce a selection of concepts that are further described below in the Detailed Description. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.

[0005] In one aspect, embodiments disclosed herein relate to crosslinkable thermoplastic compositions comprising a polymer formed from the reaction between a bis-benzoxazine monomer and a difunctional comonomer having phenolic, amine, and / or thiol functional groups, the polymer comprising at least one crosslinkable group.

[0006] In another aspect, embodiments disclosed herein relate to a method of forming a crosslinkable thermoplastic composition comprising reacting a bis-benzoxazine monomer with a difunctional comonomer to form a polymer comprising at least one crosslinkable group.

[0007] In another aspect, the embodiments disclosed herein comprise a cured thermoplastic resin. Fat The method includes providing a crosslinkable thermoplastic resin composition and curing the crosslinkable thermoplastic resin composition by application of an external stimulus to form the cured thermoplastic resin.

[0008] Other aspects and advantages of the claimed subject matter will become apparent from the following description and the appended claims.

[0009] BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is a schematic diagram of the synthesis of a crosslinkable thermoplastic resin according to one or more embodiments.

[0010] FIG. 2 is a schematic diagram of the curing of a crosslinkable thermoplastic resin according to one or more embodiments.

[0011] FIG. 3 is a schematic diagram of the purification of a crosslinkable thermoplastic resin according to one or more embodiments.

[0012] FIG. 4 is a schematic diagram of a polymer modification strategy according to one or more embodiments of the present disclosure.

[0013] FIG. 5 is a schematic diagram of a polymer synthesis strategy described in one or more embodiments of the present disclosure.

[0014] FIG. 6A is a schematic diagram of a polymer including a curable functional group according to one or more embodiments of the present disclosure.

[0015] FIG. 6B is a schematic diagram of a cured resin according to one or more embodiments of the present disclosure.

[0016] FIG. 7A is a schematic diagram of a polymer composition including a hardenable component according to one or more embodiments of the present disclosure.

[0017] FIG. 7B is a schematic diagram of a cured resin according to one or more embodiments of the present disclosure.

[0018] 8-9 show gel permeation chromatography (GPC) data for exemplary thermoplastic compositions of one or more embodiments.

[0019] FIG. 10 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments.

[0020] FIG. 11 shows GPC data for an exemplary thermoplastic composition of one or more embodiments.

[0021] FIG. 12 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments.

[0022] FIG. 13 shows GPC data for an exemplary thermoplastic composition of one or more embodiments.

[0023] FIG. 14 is a graph showing the thermal expansion coefficient of an exemplary thermoplastic composition of one or more embodiments. 1 HNMR data is shown.

[0024] FIG. 15 shows TGA results for an exemplary thermoplastic composition of one or more embodiments.

[0025] FIG. 16 shows GPC data for an exemplary thermoplastic composition of one or more embodiments.

[0026] 17A-B are schematic diagrams of the synthesis of an exemplary crosslinkable thermoplastic resin according to one or more embodiments.

[0027] FIG. 18 is a schematic diagram of the synthesis of an exemplary crosslinkable thermoplastic resin of one or more embodiments.

[0028] FIG. 19 shows gel permeation chromatography (GPC) data for exemplary thermoplastic resin compositions of one or more embodiments: (a) PBB(120-2-30)A, (b) PBB(150-2-5)A, (c) PBB(150-2-10)A, and (d) PBB(150-2-25)A.

[0029] FIG. 20 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments.

[0030] FIG. 21 is a graphical representation of DMA results of an exemplary cured thermoplastic composition of one or more embodiments.

[0031] FIG. 22 is a schematic diagram of the reaction between a monomer and a polymer during curing of a thermoplastic resin of one or more embodiments.

[0032] FIG. 23 is a graphical representation of GPC results of thermoplastics (powder partially dissolved in NMP) for exemplary thermoplastic compositions of one or more embodiments: (a) PDA(120-2-30)A, (b) PDA(150-2-5)A, (c) PDA(150-2-10)A, and (d) PDA(150-2-25)A.

[0033] FIG. 24 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments.

[0034] 25A-B show dynamic mechanical analysis of the storage modulus (FIG. 25A) and loss tangent (tan delta) (FIG. 25B) of an exemplary cured thermoplastic composition of one or more embodiments.

[0035] FIG. 26A is a photograph of a cured polymer composition according to one or more embodiments of the present disclosure.

[0036] FIG. 26B is a photograph of a cured polymer composition according to one or more embodiments of the present disclosure.

[0037] Detailed Description One or more embodiments of the present disclosure generally relate to crosslinkable thermoplastics that can provide a combination of properties not achievable by thermosets or thermoplastics alone. composition For example, the crosslinkable groups in the crosslinkable thermoplastic composition may form crosslinked structures by polymerization at elevated temperatures; however, below such temperatures, the crosslinkable thermoplastic resin may composition The properties of the compositions can largely mirror those of traditional thermoplastics (and can be melted / molded and remelted / molded). After crosslinking, such compositions have properties that mirror those of traditional thermoset materials (such as good adhesion to fibers and high temperature resistance).

[0038] The present disclosure also relates, in one or more embodiments, to the preparation of benzoxazine thermoplastic resins by methods including solution polymerization and melt polymerization. In particular, one or more embodiments of the present disclosure relate to one-pot solution polymerization using a solvent system in which the formed resin product has better solubility. After polymerization, depending on the desired properties of the resin, in one or more embodiments, the resin may be purified to remove unreacted monomers and oligomers, or in one or more other embodiments, the unreacted monomers and oligomers may be left in the resin to function as a plasticizer. Furthermore, multifunctional groups can also be introduced through multiple selections of available monomers, which can greatly broaden the application of the final polymer product.

[0039] Thus, one or more embodiments of the present disclosure provide benzoxazine thermoplastics having improved processability and / or thermal stability. composition In one or more embodiments, such benzoxazine thermoplastic resins are composition may contain unreacted monomers and oligomers that function as plasticizers that affect the processability of the resin. Processability and thermal stability can be improved by modifying the resin to react with at least some of the phenolic hydroxyl groups present in the resin.

[0040] Additionally, one or more embodiments of the present disclosure also relate to a benzoxazine thermoplastic comprising a polymer comprising benzoxazine ("BZ") containing monomer units and phenolic, amine, and / or thiol containing monomer units. In some embodiments, the polymer may comprise benzoxazine and phenolic, amine, and / or thiol containing monomer units. In some embodiments, the polymer may comprise ring-opened BZ containing monomer units. The polymer may be capped with a BZ end cap, such that the benzoxazine thermoplastic is crosslinkable.

[0041] The BZ-containing monomer unit can have a structure according to formula (I): [ka] In the formula, R1 may represent one or more of a hydrogen atom, a hydrocarbon group, a substituted hydrocarbon group, and a functional group. The BZ-containing monomer unit of one or more embodiments may include one or more substituents represented by R1. As used herein, the term "hydrocarbon group" may refer to a branched, linear, and / or ring-containing hydrocarbon group that may be saturated or unsaturated. The hydrocarbon group may be a primary, secondary, and / or tertiary hydrocarbon. As used herein, the term "substituted hydrocarbon group" may refer to a hydrocarbon group (as defined above) in which at least one hydrogen atom has been replaced with a non-hydrogen group to provide a stable compound. Such substituents may be selected from, but are not limited to, halo, hydroxyl, alkoxy, oxo, alkanoyl, aryloxy, alkanoyloxy, amino, alkylamino, arylamino, arylalkylamino, disubstituted amine, alkanylamino, aroylamino, aralkanoylamino, substituted alkanoylamino, substituted arylamino, substituted aralkanoylamino, thiol, alkylthio, arylthio, arylalkylthio, alkylthiono, arylthiono, arialkylthiono, alkylsulfonyl, arylsulfonyl, arylalkylsulfonyl, sulfonamido, substituted sulfonamido, nitro, cyano, carboxy, carbamyl, alkoxycarbonyl, aryl, substituted aryl, guanidine, vinyl, acetylene, acrylate, cyanate, epoxide, and heterocyclyl groups, and mixtures thereof. The functional groups may be selected from, but are not limited to, halo, hydroxyl, alkoxy, oxo, amino, amido, thiol, alkylthio, sulfonyl, alkylsulfonyl, sulfonamide, substituted sulfonamide, nitro, cyano, carboxy, carbamyl, alkoxycarbonylvinyl, acetylene, acrylate, cyanate, epoxide groups, and mixtures thereof.

[0042] R2 is not particularly limited and may represent any of the groups mentioned for R1. However, in certain embodiments, R2 may be a BZ-containing moiety. When R2 is a BZ-containing moiety, the BZ-containing monomer unit may be a bis-BZ monomer unit. The bis-BZ monomer unit may have a structure represented by formula (II): [ka] wherein R1 represents a group as described above with respect to formula (I). R1' may be the same group as R1 or a different group. R3 may represent a hydrocarbon group or a substituted hydrocarbon group. In certain embodiments, R3 may represent an aromatic group selected from, but not limited to, benzene, bibenzyl, diphenylmethane, naphthalene, anthracene, diphenyl ether, diphenyl sulfone ether, bis(phenoxy)benzene, stilbene, phenanthrene, fluorine, and substituted variants thereof. In one or more embodiments, R3 may represent a group having a molecular weight in the range of about 1 to 100,000 Da, or 1 to 10,000 Da, or 1 to 1,000 Da. In one or more embodiments, one or more ring-opening BZ-containing monomers may be used together with respect to formula (II).

[0043] In some embodiments, the polymer may include a ring-opened BZ-containing monomer unit. The BZ-containing monomer unit may have a structure represented by formula (III): [ka] wherein R1 represents a group as described above with respect to formula (I). R1' may be the same group as R1 or a different group. R4 may be selected from, but is not limited to, hydrocarbon, ether, secondary amino, amide, thioether, sulfonyl, sulfonamide, carbonyl, carbamyl, fluorenyl, alkoxycarbonyl, and mixtures thereof. In one or more embodiments, R4 may represent a group having a molecular weight ranging from about 1 to 100,000 Da, or 1 to 10,000 Da, or 1 to 1,000 Da. In one or more embodiments, one or more ring-opened BZ-containing monomers represented by formula (III) may be used in combination. In one or more embodiments, one or more ring-opened BZ-containing monomers represented by formulas (II) and (III) may be used in combination.

[0044] In one or more embodiments, the benzoxazine thermoplastic polymer may contain either a single end cap or two end caps that are crosslinkable groups. In some embodiments, these crosslinkable groups may be BZ moieties. In certain embodiments, the BZ moieties may be derived from the BZ-containing monomer units described above. Upon curing, these crosslinkable groups may crosslink multiple polymers, providing thermoset properties. In some embodiments, BZ moieties are used that are thermoset at temperatures ranging from 150-260°C, or in more specific embodiments, at temperatures below 250°C, below 225°C, or below 200°C. Low cure temperatures allow the crosslinkable thermoplastic resins of one or more embodiments to be more easily cured. composition can be readily converted into a cured structure by thermoforming using a heat press, oven, autoclave, etc. compositionThe cure temperature and other properties of the polymers are greatly influenced by the choice of monomer and the structure of the resin formed. Thus, the suitability of a given monomer depends on the rheological behavior of the desired resin, the degree of crosslinking upon curing, and the resulting tensile, mechanical, and thermal properties. As described in more detail below, the benzoxazine thermoplastic polymers may be cured by external stimuli such as UV and / or microwave curing. In some embodiments, curable groups, such as those that are UV and / or microwave curable, may be introduced into the resin to facilitate UV and / or microwave curing.

[0045] In one or more embodiments, the benzoxazine thermoplastic resins of the present disclosure composition may generally comprise a polymer including a difunctional monomer, such as a monomer having a functional group selected from a phenolic functional group, an amine functional group, and a thiol functional group.

[0046] In one or more specific embodiments, the polymer may include a phenol-containing monomeric unit. The phenol-containing monomeric unit in one or more embodiments may have a structure represented by formula (IV): [ka] R5 is not particularly limited and can represent one or more of a hydrogen atom, a hydrocarbon group, a substituted hydrocarbon group, a hydroxyl group, and a functional group. The phenol-containing monomer unit of one or more embodiments can include one or more substituents represented by R5. For example, in certain embodiments, the phenol-containing monomer represented by formula (IV) can be a benzenediol (catechol, resorcinol, or hydroquinone), or a substituted benzenediol (including 2-methylresorcinol, 2-ethylresorcinol, 4-methylcatechol, etc., and alkoxylated derivatives thereof in which the alkyl group is replaced by an alkoxy group).

[0047] In certain embodiments, R5 may be a phenol-containing moiety. In one or more embodiments, one or more phenol-containing monomers represented by formula (IV) may be used in combination. When R5 is a phenol-containing moiety, the phenol-containing monomer unit may be a bisphenol monomer unit. The bisphenol monomer unit may have a structure represented by formula (V): [ka] wherein R7 represents a group as described above for R5. R7' may be the same group as R7 or a different group. R6 may represent a hydrocarbon group or a substituted hydrocarbon group. The bisphenol monomers of one or more embodiments include 2,2'-bis(4-hydroxyphenyl)propane (bisphenol A), 2,2'-bis(4-hydroxyphenyl)butane (bisphenol B), 1,1'-bis(4-hydroxyphenyl)ethane (bisphenol E), 2,2'-bis(4-hydroxy-3-isopropylphenyl)propane (bisphenol G), bis(4-hydroxyphenyl)methane (bisphenol F), 2,2'-bis(4-hydroxyphenyl)hexafluoropropane (bisphenol AF), 4,4' -(1-phenylethylidene)bisphenol (bisphenol AP), 4,4'-cyclohexylidene bisphenol (bisphenol Z), bis(4-hydroxyphenyl)sulfone (bisphenol S), 4,4'-(9-fluorenylidene)diphenol (bisphenol FL), 4,4'-(1,3-phenylenediisopropylidene)bisphenol (bisphenol M), 4,4'-(1,4-phenylenediisopropylidene)bisphenol (bisphenol P), and substituted derivatives thereof. In certain embodiments, the bisphenol monomer may be one or more of 3,3'-dimethylbisphenol A (bisphenol C), 3,3'-diallylbisphenol A, and 2,2'-bis(2-hydroxy-5-biphenylyl)propane (bisphenol PH). In one or more embodiments, one or more bisphenol-containing monomers represented by formula (V) may be used in combination. In one or more embodiments, one or more phenol- or bisphenol-containing monomers represented by formulas (IV) and (V) may be used in combination.

[0048] As mentioned above, in one or more embodiments, the polymer of the present disclosure may include a difunctional monomer containing an amine group, or a diamine such as an aromatic diamine, a silicon-based diamine, an alkyl diamine, and a polyether amine. The diamines described in the present disclosure include aromatic diamine compounds having 6 to 27 carbon atoms, such as bis[4-(3-aminophenoxy)phenyl]sulfone (BAPS-m), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS-p), 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene (2,4-TDA), 4,4'-diaminodiphenylmethane (MDA), 4,4'-diaminodiphenylether (ODA), 3,4'-diaminodiphenylmethane (DMD), 4,4'-diaminodiphenylether (ODA), 4,4'-diaminodiphenylmethane (DMD), 4,4'-diaminodiphenylether (ODA), 4,4'-diaminodiphenylmethane (DMD), 4,4'-diaminodiphenylether (DMD ... diaminodiphenyl ether (DPE), 3,3'-dimethyl-4,4'-diaminobiphenyl (TB), 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl (TFMB), 3,7-diamino-dimethyldibenzothiophene-5,5-dioxide (TSN), 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-bis(4-aminophenyl)sulfide (ASD), 4,4' -Diaminodiphenylsulfone (ASN), 4,4'-diaminobenzanilide (DABA), 1,n-bis(4-aminophenoxy)alkane (n = 3, 4 or 5, DAnMG), 1,3-bis(4-aminophenoxy)-2,2-dimethylpropane (DANPG), 1,2-bis[2-(4-aminophenoxy)ethoxy]ethane (DA3EG), 1,5-bis(4-aminophenoxy)pentane (DA5MG), 1,3-bis(4-aminophenoxy)propane (DA3MG), 9,9 -Bis(4-aminophenyl)fluorene (FDA), 5(6)-amino-1-(4-aminomethyl)-1,3,3-trimethylindane, 1,4-bis(4-aminophenoxy)benzene (TPE-Q or APB-144), 1,3-bis(4-aminophenoxy)benzene (TPE-R or APB-134 or RODA), 1,3-bis(3-aminophenoxy)benzene (APB or APB-133)), 4,4'-bis(4-aminophenoxy)biphenyl (BAPB), 4,4'-Bis(3-aminophenoxy)biphenyl, 2,2-bis(4-aminophenoxyphenyl)propane (BAPP), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (HFBAPP), 3,3'-dicarboxy-4,4'-diaminodiphenylmethane (MBAA), 4,6-dihydroxy-1,3-phenylenediamine (known as 4,6-diaminoresorcinol), 3,3'-dihydroxy-4,4'-diaminobiphenyl (HAB) and 3,3',4,4'-tetraaminobiphenyl (TAB); aliphatic compounds with 6 to 24 carbon atoms. or alicyclic diamine compounds such as 1,6-hexamethylenediamine (HMD), 1,8-octamethylenediamine (OMDA), 1,9-nonamethylenediamine, 1,12-dodecamethylenediamine (DMDA), 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 4,4'-dicyclohexylmethanediamine and cyclohexanediamine; and silicone-based diamine compounds such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and polydimethylsiloxane (PDMS). Other embodiments may include aromatic diamines (VI) or (VII) (wherein each R, 3 is independently selected from H, CH or a halogen, and n is an integer from 1 to 7), and one or more flexible comonomers may be used, including alkyl diamines such as hexamethylenediamine (VII): [ka]

[0049] In one or more embodiments, the polymers of the present disclosure may include a difunctional monomer that includes a thiol group. The thiol-containing monomer has the general formula HS-R 8 -SH(wherein, R 8 may represent a hydrocarbon group or a substituted hydrocarbon group, including an alkyl or aromatic backbone, optionally substituted with alkyl and / or aromatic pendant groups.

[0050] As shown by the general reaction scheme in FIG. 1, the polymer represented by the benzoxazine thermoplastic of one or more embodiments may include a ring-opened benzoxazine structure 3 resulting from the reaction of bis-BZ 1 with benzenediol 2. Although the embodiment shown in FIG. 1 illustrates a solution polymerization, melt polymerization methods may also be used to form the ring-opened benzoxazine structure 3. As shown in FIG. 2, the benzoxazine thermoplastic 3 having terminal BZ groups may be cured to obtain a crosslinked structure 4. Specifically, including a greater molar amount of difunctional benzoxazine monomer compared to the comonomer may result in a greater number of terminal benzoxazine groups, as shown in FIG. 2, allowing for subsequent crosslinking to occur. Thus, in one or more embodiments, in a solution polymerization method, the molar ratio between the difunctional benzoxazine monomer and the difunctional comonomer may range from 1:1 to 2:1, for example, with a lower limit of any of 1:1, 1.2:1, or 1.5:1 to an upper limit of any of 1.5:1, 1.75:1, or 2:1, and any lower limit may be used in combination with any upper limit.

[0051] Crosslinkable thermoplastic resin according to one or more embodiments of the present disclosure composition may include one or more polymers. In one or more embodiments, two or more crosslinkable thermoplastic resins may be blended by mixing in the melt or in solution. In one or more embodiments, two or more monomers may be used together and copolymerized in the polymer.

[0052] The crosslinkable thermoplastic resin according to one or more embodiments of the present disclosure Fat In some embodiments, the crosslinkable thermoplastic resin may have a weight average molecular weight (Mw) in the range of about 1 to 1,000 kilodaltons (kDa). Fatty The Mw may be a range having a lower limit of one of 1, 5, 10, 20, 30, 50, 100, 150, 200, 250, and 300 kDa and an upper limit of one of 20, 30, 50, 100, 150, 200, 250, 500, 750, and 1000 kDa, any lower limit may be paired with any upper limit.

[0053] The crosslinkable thermoplastic resin according to one or more embodiments of the present disclosure Fat In some embodiments, the crosslinkable thermoplastic resin may have a number average molecular weight (Mn) in the range of about 1 to 100 kDa. Fatty Mn may be a range having a lower limit of one of 1, 5, 10, 20, 30, 50, and 70 kDa and an upper limit of one of 20, 30, 50, 70, and 100 kDa, any lower limit may be paired with any upper limit.

[0054] The crosslinkable thermoplastic resin according to one or more embodiments of the present disclosure Fat The crosslinkable thermoplastic resin may have a polydispersity index (Mw / Mn) ranging from about 1 to 5. In some embodiments, the crosslinkable thermoplastic resin may have a polydispersity index (Mw / Mn) ranging from about 1 to 5. Fatty The polydispersity index may be a range having a lower limit of one of 1, 2, 3, and 4 and an upper limit of one of 2, 3, 4, and 5, and any lower limit may be paired with any upper limit.

[0055] As mentioned above, the crosslinkable thermoplastic resin composition The melt viscosity of the crosslinkable thermoplastic resin may vary, for example, depending on the monomer selection, polymerization conditions, and structure of the resin formed. In one or more embodiments, at a temperature of 140° C., composition may have a melt viscosity of 50,000 Pa.s or less, 20,000 Pa.s or less, 10,000 Pa.s or less, 5,000 Pa.s or less, 4,000 Pa.s or less, 3,000 Pa.s or less, 2,000 Pa.s or less, or 1,000 Pa.s or less. In some embodiments, the crosslinkable thermoplastic resin composition may be a range having a lower limit of one of 1, 50, 100, 250, 500, 750, 1000, 2000, 3000, 4000, 5000, and 6000 Pa.s and an upper limit of one of 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 10000, 20000, 40000, or 50000 Pa.s, any lower limit may be paired with any upper limit.

[0056] In one or more embodiments, the polymer can be obtained by solution polymerization using a solvent (or solvent mixture) having a boiling point above 75° C. under one atmosphere. Such solvents and solvent mixtures include, but are not limited to, ethyl acetate, 2-methoxyethanol, dimethylformamide (DMF), N-methylpyrrolidone (NMP), butyl acetate, and a mixture of 2-methoxyethanol / tetrahydrofuran (THF). In one or more embodiments, the solvent can be selected based on the solubility of the monomer (especially the difunctional benzoxazine) to achieve a solution with at least 20% solids at room temperature. Advantageously, as found by the inventors, while conventional benzoxazine polymerization occurs in a solvent such as methanol to dissolve the monomer in the solvent, the use of the solvents described herein can provide better solubility of the resulting polymer, thus allowing for the synthesis of higher molecular weight resins. It is further envisioned that the solvent may be a blend of solvents having a boiling point higher than 75° C. used in combination with a solvent having a boiling point lower than 75° C., where the solvent having a boiling point higher than 75° C. is used in an amount ranging from 50 to 100% by volume, and the solvent having a boiling point lower than 75° C. is used in an amount ranging from 0 to 50% by volume. Such solvents having a boiling point lower than 75° C. may include, for example, methanol, ethanol, and the like.

[0057] Thus, in one or more embodiments, synthesis can occur by adding the difunctional benzoxazine monomer and the difunctional comonomer in a solvent (or blend of solvents) such as those described herein, and heating the mixture to a temperature ranging from 45° C. to the boiling point of the solvent for a reaction time that can range from 1 hour to 120 hours, depending on the reaction temperature used.

[0058] Furthermore, one-pot synthesis may also allow for simplified purification (compared to traditional multi-step purification), since the resulting resin may remain soluble in the solvent. Specifically, if purification is desired, after completion of the reaction (and after the reactants have cooled to room temperature), the solution may be directly mixed with a purification solvent, as shown in FIG. 3, and the high molecular weight components (polymers) may precipitate from the solution, while the unreacted monomers and oligomers may remain in the solution. Such purification solvents may be selected from, but are not limited to, methanol, ethanol, propanol, isopropanol, n-hexane, cyclohexane, and mixtures thereof. Following such precipitation, the solid resin may be recovered by filtration and dried, such as in a vacuum oven. Thus, in one or more embodiments, the purified resin may have an unreacted monomer and oligomer content of less than 5% by weight, less than 2% by weight, less than 1% by weight, or less than 0.5% by weight.

[0059] In one or more embodiments, the polymer may be obtained by melt polymerization. In some embodiments, melt polymerization may be used to synthesize the polymer since no solvent is required, the reaction time is significantly reduced compared to solution phase polymerization, it is suitable for a variety of monomer selections, and it can be applied to in situ prepreg processes.

[0060] In one or more embodiments of the melt polymerization, the ramp rate can vary from about 0.5 to 5° C. / min. In some embodiments, the ramp rate can be a range having a lower limit of one of 0.5, 1.0, 1.5, 2.0, 2.5, 3.0° C. / min and an upper limit of one of 2.0, 2.5, 3.0, 4.0, and 5.0° C. / min, any lower limit may be paired with any upper limit.

[0061] The melt polymerization of one or more embodiments may have a final temperature in the range of about 120-180° C. In some embodiments, the melt polymerization may have a final temperature in the range having a lower limit of one of 120, 125, 130, 135, 140, 145, 150, and 160° C. and an upper limit of one of 140, 145, 150, 155, 160, 165, 170, 175, and 180° C., any lower limit may be paired with any upper limit.

[0062] The melt polymerization of one or more embodiments may have a final temperature hold time ranging from about 2 to 30 minutes, in some embodiments, the melt polymerization may have a final temperature hold time ranging from a lower limit of one of 2, 3, 4, 5, 6, 8, 10, and 12 minutes, and an upper limit of one of 3, 5, 7, 9, 10, 12, and 15, 20, 30 minutes, any lower limit may be paired with any upper limit.

[0063] The melt polymerization of one or more embodiments may be carried out for a total time ranging from about 60 to 180 minutes, in some embodiments, the melt polymerization may be carried out for a total time ranging from a lower limit of one of 60, 70, 80, 90, 100, 120, 140, and 160 minutes and an upper limit of one of 80, 100, 120, 140, 150, 160, 170, and 180 minutes, any lower limit may be paired with any upper limit.

[0064] In one or more embodiments, the melt polymerization may include a molar ratio (benzoxazine monomer to phenol-containing monomer) of 1:10 to 10:1 of benzoxazine monomer to phenol-containing monomer. In some embodiments, the molar ratio of benzoxazine monomer to phenol-containing monomer may be a range having a lower limit of one of 1:10, 1:8, 1:5, 1:3, 1:2, 1:1, and 2:1, and an upper limit of one of 1:2, 1:1, 2:1, 3:1, 5:1, 8:1, and 10:1, with any lower limit paired with any upper limit.

[0065] The melt polymerization of one or more embodiments may include mixing monomers by solvent or melt mixing. In one or more embodiments, the melt polymerization includes, but is not limited to, heating, which may be performed using an oven, an extruder, a hot plate, a hot press, an autoclave, and the like. In one or more embodiments, the melt polymerization may be performed under, but is not limited to, standard atmospheric pressure, vacuum, and an inert atmosphere, such as argon or nitrogen gas. In one or more embodiments, the melt polymerization by heating may be performed under, but is not limited to, air, and a supply of an inert gas, such as argon or nitrogen.

[0066] As mentioned above, solution-based synthesis methods can also provide the same chemical structure as ring-opened benzoxazine thermoplastics. The synthesis method can be selected based on the reactivity and solubility of the monomers used. For example, for some highly reactive bisphenol monomers such as cresol, the solution method can achieve similar results as the melt polymerization method, but for monomers such as 3,3'-dimethylbisphenol A and 3,3'-diallylbisphenol A, the solution method cannot provide the same molecular weight and final mechanical and thermal properties. Therefore, the choice of synthesis route can also depend on the desired properties of the resin.

[0067] In embodiments in which the resin is purified after solution polymerization, after purification, the purified crosslinked benzoxazine resin of the present disclosure may have a weight average molecular weight (Mw) in the range of about 1 to 1,000 kilodaltons (kDa) and a number average molecular weight (Mn) in the range of about 1 to 100 kDa. The Mw of the purified crosslinked benzoxazine resin may have a lower limit of one of 1, 5, 10, 20, 30, 50, 100, 150, 200, 250, and 300 kDa, and an upper limit of one of 20, 30, 50, 100, 150, 200, 250, 500, 750, and 1000 kDa, any lower limit may be paired with any upper limit. The Mn of the purified crosslinked benzoxazine resin can have a lower limit of any of 1, 2, 5, 10, 20, 30, 50, or 70 kDa, and an upper limit of any of 20, 30, 50, 70, or 100 kDa, and any lower limit can be used in combination with any upper limit.

[0068] However, one or more embodiments relate to a resin composition that may maintain the inclusion of at least a portion of the unreacted monomers and oligomers formed during synthesis, where it may be desirable to have a resin composition with a lower melt viscosity than the purified resin product. In a solution polymerization process, the post-synthesis solution may be treated by solvent evaporation to obtain a resin containing the monomers and oligomers. In particular, the inventors have found that the presence of unreacted monomers and oligomers may function as a plasticizer, breaking the hydrogen bonds formed between polymer chains, thereby improving the processability of the resin. Thus, in one or more embodiments of the present disclosure, the resin composition may include benzoxazine polymers, oligomers, and unreacted monomers. For example, the resin composition may have a polymer content ranging from one of 30, 40, 50, or 75% by weight lower limit and one of 50, 60, 70, 80, or 90% by weight upper limit, any lower limit may be paired with any upper limit. The resin composition according to one or more embodiments of the present disclosure may have an unreacted monomer content of 25% by weight (wt%) or less, 15% by weight or more, 10% by weight or more, or 5% by weight or more. The resin composition according to one or more embodiments of the present disclosure may have an oligomer content of 25% by weight (wt%) or less, 15% by weight or more, 10% by weight or more, or 5% by weight or more.

[0069] Benzoxazine thermoplastic resins according to one or more embodiments of the present disclosure composition may be free of unreacted monomer content. In one or more embodiments, any unreacted monomer may be removed from the polymer by a purification method. The purification method may include dissolving the resin in THF and then adding a solvent such as methanol to precipitate the polymer.

[0070] The benzoxazine thermoplastic resin according to one or more embodiments of the present disclosure may include units derived from benzoxazine monomers in an amount ranging from 0 to 40% by weight. In some embodiments, the benzoxazine thermoplastic resin may include units derived from benzoxazine monomers in an amount ranging from 0, 0.5, 1, 2, 5, 10, 20, and 30% by weight, with a lower limit of 0, 0.5, 1, 2, 5, 10, 20, 30, and 40% by weight, with any lower limit paired with any upper limit.

[0071] The benzoxazine thermoplastic resin according to one or more embodiments of the present disclosure may include units derived from a difunctional comonomer in an amount ranging from 0 to 40% by weight. In some embodiments, the benzoxazine thermoplastic resin may include units derived from a difunctional comonomer in an amount ranging from 0, 0.5, 1, 2, 5, 10, 20, and 30% by weight, with an upper limit of 1, 2, 5, 10, 20, 30, and 40% by weight, with any lower limit paired with any upper limit.

[0072] Such a resin composition may have a minimum melt viscosity in the range of 1 to 5000 Pa.s. For example, the resin composition may have a minimum melt viscosity having a lower limit of any of 1, 5, 10, 50, 100, 500, or 1000 Pa.s and an upper limit of any of 1000, 2000, 3000, 4000, or 5000 Pa.s, and any lower limit may be used in combination with any upper limit.

[0073] In one or more other embodiments, the processability and thermal stability of the benzoxazine resin of the present disclosure may also be improved by modifying at least a portion of the phenolic hydroxyl groups present in the resin. Such modification may be by acetylation of at least a portion of the phenolic hydroxyl groups. For example, in one or more embodiments, the portion of the phenolic hydroxyl groups modified may vary at a lower limit of any of 10, 20, 30, 40, or 50 percent, and at an upper limit of the range of 40, 50, 60, 70, 80, 90, or 100 percent, and any lower limit may be used in combination with any upper limit.

[0074] In one or more embodiments, the purified resin may be redissolved in a polar aprotic solvent, including but not limited to THF, DMF, or NMP, and reacted with a modifier, such as an acetylating agent. However, other modifications of the phenolic group with other functional groups are also contemplated to be within the scope of the present disclosure. Such modifications may be by nucleophilic substitution or condensation reactions to form ether derivatives, acrylate / methacrylate derivatives, oxirane derivatives, carbamate derivatives, phosphate derivatives, glycolipid derivatives, ester derivatives, polyethoxylate derivatives, or benzoxazine ring structures. Examples of acetylating agents include, but are not limited to, acetic anhydride or acyl halides. Other modifiers include those present in Lochab et al., RSC Adv. 2014, 4, 21712 at 21730, which is incorporated herein by reference in its entirety. Additionally, it is contemplated that a neutralizing agent, such as sodium bicarbonate, may be added to neutralize any released acid to reduce premature ring opening of the terminal BZ group during acetylation.

[0075] In one or more embodiments, the modified benzoxazine resin, such as the acetylated benzoxazine resin, may have a minimum melt viscosity in the range of 1 to 5000 Pa.s. For example, the resin composition may have a minimum melt viscosity having a lower limit of any of 1, 5, 10, 50, 100, 500, or 1000 Pa.s and an upper limit of any of 1000, 2000, 3000, 4000, or 5000 Pa.s, and any lower limit may be used in combination with any upper limit.

[0076] After modification, the modified benzoxazine resins of the present disclosure may have a weight average molecular weight (Mw) in the range of about 1 to 1,000 kilodaltons (kDa) and a number average molecular weight (Mn) in the range of about 1 to 100 kDa. The Mw of the modified benzoxazine resin may have a lower limit of one of 1, 5, 10, 20, 30, 50, 100, 150, 200, 250, and 300 kDa and an upper limit of one of 20, 30, 50, 100, 150, 200, 250, 500, 750, and 1000 kDa, any lower limit may be paired with any upper limit. The Mn of the modified benzoxazine resin may have a lower limit of any of 1, 2, 5, 10, 20, 30, 50, or 70 kDa, and an upper limit of any of 20, 30, 50, 70, or 100 kDa, and any lower limit can be used in combination with any upper limit.

[0077] In some embodiments, the substituents may be introduced as pendant groups by chemical reaction of an organic compound with the phenolic hydroxyl groups in the polymer structure of the benzoxazine thermoplastic. Methods by which the substituents may be introduced include, but are not limited to, reaction in solution, melt reaction using an extruder, oven, hot press, or autoclave. For example, to introduce the substituents, the organic compound may include, but is not limited to, anhydrides, dianhydrides, carboxylic acid halides, or other functional groups that can react with the phenolic hydroxyl groups. For example, the substituents introduced as side pendants of the polymer may include, but are not limited to, acetyl groups, phenyl groups, or other hydrocarbon groups. For substitution, one or more organic compounds may be used alone or in combination. The introduction of the substituents may not be completely achieved for all hydroxyl groups in the polymer. In one or more embodiments, the introduction of the substituents may be 20% or more, 50% or more, or 70% or more of all hydroxyl groups in the polymer structure of the benzoxazine thermoplastic.

[0078] Benzoxazine Thermoplastic Resin composition can be cured (crosslinked) in a variety of ways, including but not limited to, cure cycles, solution casting, hot melt pressing, etc., including by an external stimulus selected from heat, UV radiation, microwave radiation, moisture, etc. In some embodiments, one of these external stimuli is a benzoxazine thermoplastic. composition In some embodiments, two or more stimuli may be used simultaneously. In some embodiments, the benzoxazine thermoplastic resin compositionTwo or more external stimuli may be used separately to purposefully create an initial partially cured (pre-cured) intermediate of 100° C., which is then fully cured under application of a final stimulus after application of one or more stimuli. In some embodiments, the choice of cure mechanism may be determined by the type of article and the manner in which the resin is to be used, e.g., impregnating (such as to form prepregs in composite fibers), composites, adhesives, coatings, etc. For example, prior to curing, the resin may be pre-cured to a glass transition temperature (T g ) but lower than the curing temperature to form a crosslinkable thermoplastic resin composition The resin may be melt processed into its desired form and then cured to crosslink and solidify the resin.

[0079] In one or more embodiments, the crosslinkable thermoplastic resin composition may contain groups that crosslink with each other under application of an external stimulus. In one or more embodiments, the phenol-containing monomer may contain one or more groups that are crosslinkable by one or more of the aforementioned external stimuli. In some embodiments, the crosslinkable groups are pendant groups that are formed into a crosslinkable thermoplastic resin by chemical reaction with the hydroxyl groups of the phenol. composition The crosslinkable groups can be introduced into the polymer structure of the crosslinkable thermoplastic resin. The crosslinkable groups can be introduced by a solvent-free reaction, for example, but not limited to, a melt reaction using an extruder, an oven, a hot press, or an autoclave. In some embodiments, the crosslinkable groups can react with each other to form a crosslinked structure by an external stimulus as described above, such as one selected from heat, ultraviolet radiation, microwave radiation, moisture, and the like. In some embodiments, these external stimuli can be introduced into the polymer structure of the crosslinkable thermoplastic resin. composition In some embodiments, these crosslinkable thermoplastic resins may be used independently to cure the composition Two or more stimuli may be used simultaneously to cure the crosslinkable thermoplastic resin before it is fully cured. composition Two or more external stimuli may be used separately to purposefully create a partially cured (pre-cured) intermediate of In some embodiments, compounds having these external stimuli are used as crosslinkers to crosslink the crosslinkable thermoplastic resin. In the composition They may be used together to cure. For example, heat-activated crosslinking groups may include, but are not limited to, epoxy, benzoxazine, nitrile, bismaleimide, citraconimide, and other unsaturated hydrocarbon groups, such as nadic imide, phenylethynyl, phenylethynyl imide, and the like. UV-activated crosslinking groups may include, but are not limited to, acrylic, methacrylic, cinnamic, aryl azide, and other unsaturated hydrocarbon groups. In some embodiments, these crosslinking groups may be used independently. In some embodiments, two or more crosslinking groups may be used together. Also, for example, microwave radiation-activated crosslinking groups may include, but are not limited to, epoxy and other unsaturated hydrocarbon groups. These crosslinking groups may be used independently or together. Also, moisture-activated crosslinking groups may include, but are not limited to, cyanoacrylate, isocyanate, and alkoxysilane. These crosslinking groups may be used with a catalyst to accelerate the curing reaction. These crosslinkable groups can be cured with a catalyst, which can include inorganic salts, organic compounds, or combinations thereof.

[0080] In one or more embodiments, the thermoplastic resin composition may include functional groups that can be cured (crosslinked) via UV and / or microwave treatment (referred to herein as "curable functional groups"). Suitable curable functional groups include functional groups that are microwave and / or UV curable. These are functional groups that, upon exposure to UV and / or microwave radiation, cause the thermoplastic resin compositionThis means that crosslinking is induced in the thermoplastic composition. In the case of microwave radiation, the curable functional groups can absorb the radiation to induce crosslinking. For example, for compounds that are microwave curable, they may include polar functional groups. Such functional groups can thus absorb the radiation and convert it to heat to induce curing of the thermoplastic composition. In the case of UV radiation, the photoinitiator can absorb the UV radiation and generate radicals and / or ions that attack the curable functional groups and induce crosslinking. For a compound to be UV curable, the compound may include functional groups that can be attacked by the radicals and / or ions generated by one or more photoinitiators to form covalent bonds with other functional groups. In one or more embodiments, curing may involve reaction of other functional groups present in the thermoplastic composition, including, but not limited to, benzoxazine rings that may open upon curing. The reaction is induced by heat generated by the curable functional groups or by the radicals and / or ions generated by the photoinitiator.

[0081] In one or more embodiments, the curable functional group is a polar group suitable for absorbing microwave radiation. Examples of suitable polar functional group types include, but are not limited to, carboxylic acids, amides, alcohols, esters, aldehydes, and ketones.

[0082] In one or more embodiments, the curable functional group is "UV-sensitive". This means that it is a functional group that can be attacked by radicals and / or ions generated by one or more photoinitiators. Such functional groups can then form covalent bonds (crosslinks) with other functional groups. Examples of types of UV-sensitive functional groups can include, but are not limited to, functional groups with activated double bonds, such as acrylic groups, methacrylic groups, styrene groups, and vinylpyrrolidone groups.

[0083] In one or more embodiments, the curable functional group may be attached to the thermoplastic polymer. This may occur by modifying the thermoplastic polymer with a curing component having such a curable functional group, or by polymerizing a monomer having such a curable functional group, i.e., by synthesizing the polymer. In such an embodiment, the curable functional group is an internal component, i.e., covalently bonded to the polymer. Furthermore, it is also envisioned that the polymer can be combined with an external curing component that does not react with the polymer until triggered by microwave or UV curing.

[0084] Thus, in one or more other embodiments, the curing component (prior to reaction with the polymer) may include multiple functional groups, including a curable functional group and at least one functional group that is reactive such that it can bond to the thermoplastic polymer. In such embodiments, the curing component (prior to reaction with the polymer) may function as a precursor to form a polymer with internal curable functional groups. Thus, in addition to polar and / or UV-sensitive functional groups, the curing component may include a number of functional groups that can be combined with the thermoplastic polymer to form a polymer having internal curable functional groups. To fat The curable functional group may also include at least one reactive functional group that is reactive to the curable functional group. Furthermore, in addition to the functional group that is bound to the polymer prior to microwave-induced and / or UV-induced curing, the curable component may also optionally include at least one additional reactive functional group that is reactive to microwave-induced and / or UV-induced curing. That is, in one or more embodiments that include at least one additional reactive functional group, the curable component that serves as a raw material (before binding to the polymer, or before binding to the monomer if the curable functional group is incorporated by a polymer synthesis mechanism) may have at least two reactive groups, such that upon initial reaction with the polymer or monomer, at least one reactive group remains in the curable functional group. Furthermore, while the curable functional group may include one of such additional reactive functional groups, it is also envisioned that the curable functional group may include at least two of such additional reactive functional groups, such that such additional reactive functional groups may provide additional crosslinking.

[0085] In one or more embodiments, the reactive functional group is one that can bond to and / or crosslink with a thermoplastic polymer. Examples of types of functional groups suitable for use as reactive functional groups include, but are not limited to, phenols, amines, thiols, ethers, esters, acrylates, oxiranes, carbamates, phosphorylates, glycolipids, polyethoxylates, benzoxazines, and derivatives thereof.

[0086] It is further understood that the functional groups that absorb microwave radiation or are UV sensitive may also be reactive functional groups, such that when triggered by radiation, the groups crosslink the polymer.

[0087] It is also envisioned that radiation may induce a combination of reactions involving the curable functional groups themselves and other functional groups that do not absorb radiation and convert it to heat.

[0088] However, as mentioned above, if the curing component does not contain two reactive functional groups (and the curable functional groups attached to the polymer do not contain at least one reactive functional group), the polymer can still be crosslinked by including other reactive groups, such as reactive endcaps. The reaction can be induced by heat generated from microwaves or by radicals and / or ions released by the photoinitiator after UV radiation. In one or more embodiments, the polymer may include benzoxazine endcaps whose cure can be induced by microwave radiation. It is further contemplated that the resin composition may include both reactive endcaps and curable functional groups that contain reactive functional groups.

[0089] Examples of reactive functional groups include, but are not limited to, epoxides, thiols, amines and carboxylic acids. Examples of compounds that contain such reactive functional groups and can be curing components can include, but are not limited to, epichlorohydrin, Ceroxide 2021P (7-oxabicyclo[4.1.0]heptan-4-yl 2-(7-oxabicyclo[4.1.0]heptan-4-yl)acetate), YDF-170 (diglycidyl ether bisphenol A epoxy oligomer), methacrylic anhydride, and 1,1,1-tris(4-hydroxyphenyl)ethane, 4,4'-oxydianiline.

[0090] The curable functional groups of the present disclosure can be incorporated into the thermoplastic composition using a variety of suitable strategies. In one or more embodiments, the curable functional groups may be covalently bonded to the thermoplastic polymer, and thus the polymer includes internal curable functional groups. In other embodiments, the curable functional groups are not covalently bonded to the thermoplastic polymer, but rather are present in an external curing component that is mixed with the polymer and is curable, particularly by microwave radiation. In such embodiments, the polymer does not react with or bond to the external curing component until curing is induced by microwave or UV radiation. It is further envisioned that polymers with internal curable functional groups can be combined with an external curing component and cured.

[0091] As noted above, in embodiments in which the polymer has a curable functional group, which is covalently bonded to the thermoplastic polymer (i.e., an internal curable functional group), the curable group may be introduced by covalently bonding directly to the thermoplastic polymer or by selecting at least one monomer that contains the curable functional group for use in a monomer mixture that is then polymerized to form the thermoplastic polymer.

[0092] In the embodiment induced by UV radiation, at least one photoinitiator is also generally present. Photoinitiators are compounds that can convert UV radiation into chemical energy in the form of radicals and / or ions. Types of photoinitiators can include, but are not limited to, benzoin ethers, benzil ketals, α-dialkoxyacetophenones, α-hydroxyalkylphenones, α-aminoalkylphenones, acylphosphine oxides, benzophenones / amines, thioxanthones / amines, and titanocenes.

[0093] A schematic diagram of an embodiment of attaching a hardenable group to a polymer such that the polymer comprises an internal hardenable functional group is shown in FIG. 4. In FIG. 4, a thermoplastic polymer 402 comprises a polymer backbone 404 and optional end caps 406. The polymer is modified such that a hardenable functional group 408 is covalently attached to the thermoplastic polymer 402 (indicated by the arrows), such that the polymer comprises an internal hardenable functional group. In the embodiment shown in FIG. 4, the hardenable functional group 408 is covalently attached to the polymer backbone 404. In some embodiments, the hardenable group may be covalently attached to the end caps. In some embodiments, the hardenable group may be covalently attached to the polymer backbone and the end caps. As can be appreciated by one of ordinary skill in the art, the amount of internal hardenable groups attached to the polymer may be adjusted to adjust the amount of crosslinking in the cured polymer.

[0094] In one or more embodiments, a thermoplastic resin containing benzoxazine functionality may be utilized as the thermoplastic polymer to which the curable functional group may be attached. In some embodiments, the thermoplastic polymer may include a ring-opened benzoxazine having phenol functionality. An example of a ring-opened benzoxazine thermoplastic polymer is shown as structure (1). [ka]

[0095] According to one or more embodiments of the present disclosure, the polymer backbone of structure (IX) can be modified with a curing component such as epichlorohydrin or methacrylic anhydride to form a polymer containing internal curable functional groups such as epoxide or acrylic groups. In particular, the curing component can react with the phenolic functional groups in structure (IX). When the ring-opened benzoxazine shown in structure (IX) is modified with methacrylic anhydride, the methacrylic anhydride reacts with the phenolic functional groups to form the polymer shown in structure (X). [ka]

[0096] The polymers shown in Structure (X) can be cured by UV treatment (in the presence of a photoinitiator) due to the presence of curable functional groups, particularly UV-sensitive groups. As shown, these internal functional groups are covalently attached to the polymer backbone. Furthermore, as can be appreciated, depending on the amount of curing component reacted with the polymer shown in Structure (XI), a portion of the resin can include repeat units of Structure (XI) along with other repeat units of Structure (X). In one or more embodiments, such structures can be endcapped with benzoxazine groups.

[0097] When the ring-opened benzoxazine shown in structure (IX) is modified with epichlorohydrin, the epichlorohydrin reacts with the phenol functionality to form a polymer shown in structure (XI). [ka]

[0098] The polymers shown in Structure (XI) can be cured by microwave treatment due to the presence of polar curable functional groups. As shown, these internal functional groups are covalently attached to the polymer backbone. Furthermore, as can be appreciated, depending on the amount of curing component reacted with the polymer shown in Structure (IX), a portion of the resin can include repeat units of Structure (IX) along with other repeat units of Structure (XI). In one or more embodiments, such structures can be endcapped with benzoxazine groups.

[0099] In one or more embodiments, curable functional groups may be incorporated into a thermoplastic composition by selecting at least one monomer that includes a curable functional group for use in a monomer mix, which is then polymerized to form a thermoplastic polymer. A schematic of this strategy is shown in Figure 5. In the embodiment shown in Figure 5, some of the monomers 504 include a curable group 508. The resulting mixture is then polymerized (indicated by the arrows) to form a thermoplastic polymer 502 that includes the curable group 508 as an internal curable functional group. The polymer 502 includes optional end caps 506 that are curable functional groups.

[0100] In one or more embodiments, the curable functional groups may be present in the thermoplastic composition by blending an external curing component containing the curable functional groups with the thermoplastic composition. In such embodiments, the curable functional groups are not covalently bonded to the thermoplastic polymer, but are present on the external curing component combined with the polymer. Instead, in some embodiments, the curable functional groups in the external curing component absorb microwave radiation and heat the polymer. In such cases, the curable groups may also contain reactive functional groups, and the heating generated by the microwave radiation may also crosslink the thermoplastic polymer with the curable functional groups to form a cured (crosslinked) polymer. In one or more embodiments, the curable groups may be replaced by polar non-curable groups. In such cases, the polar non-curable groups absorb the microwave radiation and convert it to heat, aiding in the curing of the thermoplastic polymer. In some embodiments, the photoinitiator absorbs UV radiation and generates radicals and / or ions that attack the curable functional groups present on the curing component, which then covalently bond to other functional groups in the polymer.

[0101] A schematic diagram of a crosslinkable benzoxazine thermoplastic polymer having curable groups covalently bonded to the polymer as internal curable groups is shown in Figure 6A. The curable groups on the polymer are shown as circles and the thermoplastic polymer is shown as lines. A schematic diagram of the cured resin of the composition shown in Figure 6A is shown in Figure 6B.

[0102] A schematic diagram of a crosslinkable benzoxazine thermoplastic polymer having external curable groups that are not covalently bonded to the polymer is shown in Figure 7A. The curable components containing the curable groups are shown as circles and the thermoplastic polymer is shown as a line. A schematic diagram of the cured resin of the composition shown in Figure 7A is shown in Figure 7B.

[0103] The compositions of the present disclosure may be cured by microwave and / or UV treatment. As can be understood by one skilled in the art, suitable conditions for microwave and UV treatment can be selected based on the properties of the material to be cured and based on the desired properties of the cured material.

[0104] The compositions disclosed herein may be cured by microwave treatment at a suitable time, frequency and power. In one or more embodiments, the microwave treatment time may be from 1 minute to 60 minutes. The microwave treatment time may have a lower limit of one of 1 minute, 5 minutes, 10 minutes, 15 minutes and 20 minutes, and an upper limit of one of 30 minutes, 45 minutes, 50 minutes, 55 minutes and 60 minutes, where any lower limit may be combined with any mathematically consistent upper limit. In one or more embodiments, the microwave treatment frequency may be from 0.3 to 300 GHz, and the microwave treatment power may be from 100 W to 100 kW.

[0105] The compositions disclosed herein may be cured by UV treatment at a suitable time, wavelength and power. In one or more embodiments, the UV treatment time may be from 5 seconds to 2 hours. The UV treatment time may have lower limits of 5 seconds, 10 seconds, 30 seconds, 60 seconds, 90 seconds and 5 minutes, and upper limits of one of 10 minutes, 20 minutes, 30 minutes, 60 minutes, 90 minutes and 120 minutes. Here, any lower limit may be paired with any mathematically consistent upper limit. In some embodiments, the UV treatment wavelength is less than 400 nm. In one or more embodiments, the UV treatment power may be from 10 W to 1 kW. Such treatment may result in a crosslinked structure determined by the curable functional groups.

[0106] The compositions and methods disclosed herein may be particularly useful compared to conventional thermal curing of resins, since UV and microwave curing may require shorter curing times, less energy input for curing, and more flexibility in processing the composition.For example, microwave curing may allow for independent post-cure strategies, and UV curing may allow easier processing in surface coating and UV patterning applications.

[0107] In one or more embodiments, the crosslinkable benzoxazine resin may be compounded with additives and reinforcing agents made from thermoplastics, thermosets, inorganic salts, organic compounds, and the like. Compounding may be done by powder dry mixing, melt mixing, or mixing in solution. The shapes of both additives and reinforcing agents may include, but are not limited to, particles, plates, fibers, and the like. In one or more embodiments, the crosslinkable benzoxazine resin may be reinforced with fibers. Reinforcement may be done by solution coating, melt coating, impregnation, and the like. The shapes of the reinforcing fibers may include, but are not limited to, single filaments such as short fibers, continuous fibers, blended fibers (yarns), tows, woven fabrics, bundles, sheets, knits, and the like to make prepregs for molding fiber reinforced composites. The continuous fibers may further be in any of the following configurations: unidirectional, multidirectional, nonwoven, woven, knitted, stitched, wound, and braided configurations, as well as swirl mat, felt mat, and chopped fiber mat configurations. The fiber composition may be varied to achieve the desired properties of the final composite structure. Exemplary fiber materials may include, but are not limited to, glass, carbon, graphite, aramid, quartz, polyethylene, polyester, poly-p-phenylene-benzobisoxazole (PBO), boron, polyamide, graphite, silicon carbide, silicon nitride, and combinations thereof. One or more additives, toughening agents, and reinforcing agents may be added to a crosslinkable thermoplastic resin. composition For example, one or more thermoplastic resins can be blended with the crosslinkable benzoxazine resin. Such thermoplastic resins include, but are not limited to, PEEK, PPS, PEI, PC, polysulfone, and the like. In another example, one or more thermosets can be blended with the crosslinkable thermoplastic resin. composition and thermally co-cured. Such thermosets may include, but are not limited to, epoxies, benzoxazines, bismaleimides, cyanate esters, and the like. Thermoplastics and thermosets may be crosslinked with the crosslinkable thermoplastic resins of the present disclosure. compositionIn one or more embodiments, inorganic salts, organic compounds, and any combination thereof can be used in combination with crosslinkable thermoplastic resins to lower the cure temperature and control the melt viscosity. composition For example, the organic compound may contain functional groups such as, but not limited to, amino groups, imidazole groups, carboxyl groups, hydroxyl groups, and sulfonyl groups.

[0108] The crosslinkable benzoxazine resin may be in the form of, but is not limited to, a powder, a film, a chunk, a fiber, etc. The film, the chunk, and the fiber are crosslinkable thermoplastic resins. composition The molded article can be thermally produced by casting or pressing using a powder or solution of the above. The molded article can be thermally remolded by casting or pressing at a lower temperature when crosslinking is initiated. The molded article can be remolded by casting or pressing when using a partially cured crosslinkable benzoxazine resin.

[0109] In one or more embodiments, the crosslinkable benzoxazine resin may be thermally cured at a temperature range of about 120-260° C. The crosslinkable benzoxazine resin may be subjected to longer cure times at the lower end of the temperature range and shorter times at the higher end of the temperature range based on the desired application. In some embodiments, the cure temperature of the crosslinkable benzoxazine resin may be in a range having a lower limit of one of 120, 130, 140, 150, 160, and 180° C. and an upper limit of one of 160, 170, 180, 190, 200, 220, 240, and 260° C., with any lower limit paired with any upper limit.

[0110] In one or more embodiments, the crosslinkable benzoxazine resin may be heat cured for a time period ranging from 30 minutes to 5 hours. In some embodiments, the curing conditions may include several successive steps.

[0111] In one or more embodiments, the crosslinkable benzoxazine resin has a pre-cure T in the range of about 80-120° C. g For example, a crosslinkable thermoplastic resin may be used. composition is a range of T before curing having a lower limit of 80, 90, 100, or 110°C and an upper limit of 90, 100, 110, or 120°C. g and any lower limit can be used in combination with any upper limit.

[0112] In one or more embodiments, the crosslinkable benzoxazine resin has a T after curing in the range of about 110 to 250° C. g For example, the crosslinkable benzoxazine resin may have a T after curing in a range having lower limits of 110, 130, 150, 170, and 190° C. and upper limits of 140, 160, 180, and 250° C. g and any lower limit can be used in combination with any upper limit.

[0113] In one or more embodiments, the T of the crosslinkable benzoxazine resin before curing g value and T after curing g The difference between the T values ​​before curing may be 20° C. or more, 50° C. or more, or 70° C. or more. For example, the crosslinkable benzoxazine resin may have a difference between the T values ​​before curing in a range having a lower limit of 20, 25, 30, 40, 50, 60, and 70° C. and an upper limit of 40, 50, 60, 70, and 90° C. g value and T after curing g The difference may have a value, and any lower limit may be used in combination with any upper limit. This difference may allow for melt processing of the resin before it hardens.

[0114] In one or more embodiments, the cured crosslinkable benzoxazine resin has a 5% decomposition temperature, Td, according to ASTM E1131, of 200° C. or more, 250° C. or more, or 300° C. or more, 350° C. or more, or 400° C. or more. 5%For example, the cured crosslinkable benzoxazine resin may have a Td in the range having a lower limit of any of 200, 225, 250, 275, 300, 325, 350, 375, 400, and 425° C. and an upper limit of any of 300, 350, 375, 400, 425, and 450° C. 5% Any lower limit may be used in combination with any upper limit.

[0115] In one or more embodiments, the cured crosslinkable benzoxazine resin may have an elastic modulus in the range of about 2.0 to 4.0 GPa according to ASTM D 1708. For example, the cured crosslinkable benzoxazine resin may have an elastic modulus in the range having a lower limit of any of 2.0, 2.2, 2.5, 2.7, 2.9, 3.0, and 3.2 GPa and an upper limit of any of 3.0, 3.2, 3.4, 3.6, 3.8, and 4.0 GPa, any lower limit may be used in combination with any upper limit.

[0116] In one or more embodiments, the cured crosslinkable benzoxazine resin may have a tensile strength in the range of about 15 to 100 MPa according to ASTM D 1708. For example, the cured crosslinkable benzoxazine resin may have a tensile strength in the range having a lower limit of any of 15, 30, 40, 50, 60, 70, and 80 MPa and an upper limit of any of 40, 50, 60, 70, 80, 90, and 100 MPa according to ASTM D 1708, any lower limit may be used in combination with any upper limit.

[0117] In one or more embodiments, the cured crosslinkable benzoxazine resin may have an elongation at break in the range of about 1-10% according to ASTM D 1708. For example, the cured crosslinkable benzoxazine resin may have an elongation at break in a range having a lower limit of any of 1, 1.5, 2.0, 2.5, 3.0, and 4.0% and an upper limit of any of 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 5.0%, and 10%, any lower limit may be used in combination with any upper limit.

[0118] In forming a coating or adhesive layer, application of the formulated coating can be by conventional methods such as spraying, roller coating, dip coating, and the coated system can then be cured by baking or radiation such as, but not limited to, microwave, UV, or IR.

[0119] [Example]

[0120] The following examples are merely illustrative and should not be construed as limiting the scope of the disclosure.

[0121] 〔material〕

[0122] Pd-type benzoxazine monomer (product name: Pd) was obtained from Shikoku Chemical Industry Co., Ltd. 2-Methylresorcinol (MR), 4,4'-oxydianiline, 3,3'-dimethylbisphenol A (BBPA), methacrylic anhydride, 2,2-dimethoxy-2-phenylacetophenone (DMPA), vinylpyrrolidone (VP), tetrahydrofuran (THF), epichlorohydrin, sodium hydroxide, 1,1,1-tris(4-hydroxyphenyl)ethane (THPE) and 4,4'-oxydianiline (ODA) were purchased from Sigma Aldrich. 2-Methoxyethanol, methanol and acetic anhydride were also purchased from Sigma Aldrich and VWR Chemicals. 2,2'-Diallylbisphenol A (product name: DABPA) was obtained from Daiwa Kasei Kogyo Co., Ltd.

[0123] 〔method〕

[0124] Differential scanning calorimetry (DSC) measurements were performed using a Q2000 (TA Instruments) at 20 °C / min in a N2 flow of 50 mL / min. g was measured from the onset of the baseline shift (the intersection of the two tangents before and after the inflection point).

[0125] Dynamic mechanical analysis (DMA) measurements were performed using a Q800 (TA Instruments) at 5°C / min, a frequency of 1.0 Hz, and a strain of 0.3% in air flow. g was measured from the beginning of the storage modulus curve (the intersection of the two tangents before and after the inflection point).

[0126] The melt viscosity was measured using a rheometer (DHR-2, TA instruments) at a heating rate of 5°C / min, an angular frequency of 6.283 rad / s (1.0 Hz), and a strain of 0.1%. Parallel plates with a diameter of 25 mm were used. The measurements were performed in air.

[0127] Gel permeation chromatography (GPC) measurements were performed using a GPC system (PROMINENCE, manufactured by Shimadzu Corporation). For molecular weight measurements, four GPC columns (PHENOGEL 5 μm 10E4 Å, PHENOGEL 5 μm 10E3 Å, PHENOGEL 5 μm 100 Å, and PHENOGEL 5 μm 100 Å, manufactured by Phenomenex) were used. The column was eluted with N-methylpyrrolidone at a flow rate of 0.6 mL / min using a 50 Å 5 μm column. Relative molecular weights were calibrated using polystyrene standards from Tosoh Corporation.

[0128] Thermogravimetric analysis (TGA) was performed using a TA Instruments Q50 TGA at 5° C. / min in a N2 flow of 40 ml / min. d5 was measured at the temperature at which a 5% weight loss was observed.

[0129] Resins with solid content of 20-60 wt% were dissolved in DMF to prepare solution-cast thin films. The DMF solution was cast onto a surface-treated glass substrate and then coated with a doctor blade. The films were then dried in a conventional oven at 80°C for 1 h, and then cured at 160°C for 1 h, 185°C for 3 h, and 218°C for 1 h. After curing, the cured films were peeled off from the glass substrate.

[0130] A hydraulic hot press was used to mold the thin film under the influence of heat and pressure. A 150 micron thick fiberglass / Teflon film was used as a release film to mold the thin film. First, a base layer of fiberglass / Teflon film measuring 6×12 inches was placed on a steel plate. On a separate release film with the same dimensions as the base layer, three strips measuring 250 mm×5 mm were cut into the film at a distance of 25 mm apart, and the release film served as a frame or spacer for molding and was placed on top of the base layer. Powdered resin was measured and poured evenly along the length of each of the three strips. The steel plate was then placed on the bottom platen of a heat press preheated to 135° C. After the resin melted (as confirmed by visual observation), a third top layer of release film was placed on the frame and a pressure of 2 MPa was first applied through a series of 20 bumps. A portion was then run at a constant pressure of 2 MPa for the remainder of the molding cycle as follows: 1) ramp 5°C / min to 160°C and hold for 60 minutes, 2) ramp 5°C / min to 185°C and hold for 180 minutes, 3) ramp 5°C / min to 218°C and hold for 60 minutes, 4) cool to room temperature at 5°C / min. After cooling, the thin film strips were carefully separated from the release film and then cut to the appropriate lengths required for tensile testing and DMA measurements.

[0131] Solubility in THF was tested by adding about 25 mg of test material to about 5 mL of THF, and the mixture was then sonicated for about 5 minutes.

[0132] UV curing was performed using either a handheld lamp or a UV curing device. The handheld UV curing lamp was obtained from VWR and has a wavelength of 365 nm, a current of 0.16 Amp, and a voltage of 110 V. The UV curing device was a Heraeus LC6B Lighthammer with a wavelength of 200-400 nm and an output of 467 watts / inch.

[0133] Synthesis and Purification of Ring-Opening Crosslinkable Thermoplastic Made from Pd Benzoxazine and Resorcinol in 2-Methoxyethanol (Example 1)

[0134] Selected amounts of Pd and MR were mixed in 2-methoxyethanol in a molar ratio of 1.5:1. After mixing, the mixture was heated to 70° C. for 95 hours. No solid precipitated from the solution after the reaction was cooled to room temperature. According to the GPC results shown in FIG. 8, the Mw obtained from this reaction was 4359 Da (calibrated) and Mn was 1552 Da (calibrated), indicating that 2-methoxyethanol is an effective solvent for synthesizing ring-opened crosslinkable benzoxazine resins.

[0135] Precipitation was then performed by dropping the solution directly into methanol to precipitate the high molecular weight components. GPC results of the purified product shown in Figure 9 showed a Mw of 7081 Da (calibrated) and Mn of 2802 Da (calibrated), indicating effective removal of unreacted monomer and most of the oligomers.

[0136] The rheological data shown in FIG. 10 showed that the minimum melt viscosity of the unrefined sample was 30,000 Pa.s, while the minimum melt viscosity of the refined sample was 70 Pa.s.

[0137] Synthesis and Purification of Ring-Opening Crosslinkable Thermoplastic Made from Pd Benzoxazine and Resorcinol in Ethyl Acetate (Example 2)

[0138] Selected amounts of Pd and MR were mixed in ethyl acetate in a molar ratio of 1.5:1. After mixing, the mixture was heated to 70° C. for 95 hours. No solid precipitated from the solution after the reaction was cooled to room temperature. According to the GPC results shown in FIG. 11, the Mw obtained from this reaction was 5376 Da (calibrated) and Mn was 1782 Da (calibrated), indicating that ethyl acetate is an effective solvent for synthesizing ring-opened crosslinkable benzoxazine resins.

[0139] Acetylation of Purified Ring-Opening Crosslinkable Thermoplastic Resin Made from Pd Benzoxazine and Resorcinol (Example 3)

[0140] The purified resin according to Example 1 (10 g) was combined with 31.5 g of sodium bicarbonate and 5 g of acetic anhydride in 100 mL of THF. The mixture was reacted for 24 hours, and the reaction product was precipitated in water and subsequently washed with methanol.

[0141] As shown in FIG. 12, the acetylated resin showed different viscosity behavior compared to the resin before acetylation. The GPC results shown in FIG. 13 indicate that acetylation may also result in some ring opening of the terminal BZ groups, as evidenced by the increase in molecular weight of the acetylated product. As shown in FIG. 14, the acetylated product was verified by NMR testing and showed a very weak proton signal around 10 ppm, which corresponds to phenol. In addition, the typical signals from the methylene of the terminal benzoxazine functional group at 4.5 ppm and 5.4 ppm also became weaker, indicating that at least some of the benzoxazine functional groups were ring opened.

[0142] The TGA results (Figure 15) show that the acetylated product has a higher T value compared to the parent resin, from 147°C to 263°C after acetylation. d5 It was shown that the increase in

[0143] Due to the improved processability, the acetylated products were processed into thin films by coating methods for DMA and tensile testing. To prepare the cured film sample solutions, the resin (25 wt%) in DMF solution was coated onto the substrate. The films were dried and cured according to the following conditions: 80°C for 2 h, 120°C for 1 h, 150°C for 30 min, 200°C for 30 min, 240°C for 1 h, and 260°C for 15 min. According to the DMA results, the T of the cured films was g The T of the cured film was 198°C. d5 The cured film properties made from the acetylated resin are summarized in Table 1 below and compared to the properties of the original resin (in powder form) used as the feedstock for acetylation. [Table 1]

[0144] Synthesis of ring-opening crosslinkable thermoplastics made from Pd benzoxazine and 4,4'-oxydianiline in 2-methoxyethanol (Example 4)

[0145] Selected amounts of Pd and 4,4'-oxydianiline were mixed in 2-methoxyethanol in a molar ratio of 1.5:1. After mixing, the mixture was heated to 50°C for 92 hours. After the reaction was cooled to room temperature, no solids precipitated from the solution. The GPC results after 72 and 92 hours are shown in Figure 16.

[0146] [Synthesis of PBB (Example 5)]

[0147] A general illustration of the synthesis method of one or more embodiments is provided by FIG. 17A. The synthesis of Example 1 is specifically illustrated in FIG. 17B and involves melt polymerization of bis-BZ(Pd) and 3,3'-dimethylbisphenol A (BBPA). A given amount of Pd and BBPA powders were mixed in THF and the mixture was stirred for 2 hours. After stirring, the THF solvent was removed by rotary evaporation, followed by drying overnight in a vacuum oven. For the purposes of these experiments, Pd / BBPA was defined as Group A with a molar ratio of 1.2-1 and Group B with a molar ratio of 1-1. The Pd / BBPA powder mixture was placed in a disposable Al pan and the pan was placed in a convection oven for polymerization. The reaction conditions were controlled by three parameters: heating rate, isothermal temperature, and time. The molecular weight was adjusted by varying the isothermal temperature and time. The oligomer was generated under isothermal conditions at 120°C for 30 minutes (PBB(120-2-30)A). When isothermal at 150°C for 5 min, the polymer had a medium MW (PBB(150-2-5)A). At 150°C for 10 min isothermal conditions, a higher MW was achieved (PBB(150-2-10)A). Further extension of the isothermal time to 25 min produced a partially crosslinked polymer (PBB(150-2-25)A). PBB resin is a mixture of monomers, oligomers, and polymers.

[0148] [Synthesis of PPBB (Example 6)]

[0149] The GPC results show that PBB resin is a mixture of monomers, oligomers, and polymers. Further purification was applied to remove these monomers and oligomers to obtain the pure thermoplastic polymer PPBB. This purification was carried out by dissolving PBB in THF, followed by adding methanol to obtain the polymer as a precipitate. The polymer was collected by centrifugation and then dried in a vacuum oven for 24 hours.

[0150] [Synthesis of acetylated PPBB (A-PPBB) (Example 7)]

[0151] PPBB powder (1 g, 5.8 mmol-OH) was dissolved in 50 mL of THF. To the above mixture was added AcO2 (29 mol) and NaHCO3 (11.6 mol). The THF solution was stirred at room temperature for 3 days. After completion of the reaction, the mixture was filtered and the filtrate was concentrated. To the residue was added dichloromethane (50 mL) and water (15 mL) and the phases were separated. The organic phase was dried (Na2SO4) and concentrated. The final powder was dried in a vacuum oven at 60° C. overnight.

[0152] Synthesis of PDA (Example 8)

[0153] The synthesis of Example 8 by melt polymerization of Pd and diallyl bisphenol A (DABPA) is shown in Figure 18. Pd and DABPA were mixed directly in a molten state at 75°C. The PDA polymer was synthesized using the same method as PBB. By adjusting the reaction conditions, PDA resins with different molecular weights were obtained.

[0154] Synthesis of PPDA (Example 9)

[0155] PPDA was obtained by purification of PDA using the same method as for PPBB (Example 7).

[0156] [Results and Discussion of Examples 5 to 9]

[0157] The melt polymerization products obtained from the reaction of Pd / BBPA mixtures with various molar ratios: 2.6-1.0, 1.5-1.0, 1.2-1.0, 1.0-1.0, and 0.6-1.0 under the conditions of heating rate of 1°C / min from 20°C to 150°C and heating isothermally at 150°C for 10 min were characterized using GPC. All the products obtained under the heating conditions successfully produced oligomers and polymers, but unreacted monomers were also present. With increasing amount of Pd monomer, the intensity of the unreacted Pd peak also increased. Pd / BBPA mixtures with molar ratios of 1.2-1.0 and 1.0-1.0 produced PBB with the highest molecular weight. It was also found that with increasing isothermal time, the polymer molecular weight became higher. This indicates that the molecular weight of the polymer can be tuned by controlling the isothermal time. Figure 19 shows examples of GPC results of PBB obtained under different conditions.

[0158] The GPC results show that the product after polymerization has unreacted monomers and oligomers. Further purification was applied to remove these monomers and oligomers to obtain a pure thermoplastic polymer. The purification process was carried out by dissolving the product in THF and then adding methanol to precipitate the polymer. The polymer was recovered by centrifugation. After drying in an oven, the purified polymer PPBB became insoluble in THF. The insolubility of PPBB is theorized to be due to strong intermolecular hydrogen bonds. PBB and PPBB also exhibited different viscosity behaviors as shown in Figure 20. The viscosity of PBB was as low as 48 Pa.s, while the viscosity of PPBB was as low as 28264 Pa.s at 153 °C. The significant decrease in viscosity comes from small amounts of monomers and oligomers.

[0159] PPBB has abundant hydroxyl groups on the backbone. Further modification of these hydroxyl groups with acetyl groups can block the intermolecular hydrogen bonds that would otherwise occur, improving the solubility of PPBB. The acetylation reaction was carried out using NaHCO3 as a catalyst and acetic anhydride as an acetylation reagent. After the acetylation reaction, a new peak at 1.9 ppm appeared in the NMR data, which could be attributed to the methylene protons of acetic acid, indicating that the acetylation occurred successfully in PPBB and A-PPBB was produced as a result of the reaction. The A-PPBB powder was completely dissolved in THF when the solid content was about 25 wt%. The GPC results show that A-PPBB has a higher molecular weight than PPBB due to the addition of acetyl groups. Compared with PPBB, A-PPBB has a much lower viscosity of 200 Pa.s at 153°C, and its lowest viscosity occurs at 220°C, with a value of 2 Pa.s.

[0160] PPBB is a crosslinkable thermoplastic. The end terminal BZ ring can further react with another BZ ring or phenol group on the backbone to form a crosslinked structure. Cured PPBB thin films were prepared by solution casting. A DMF solution with 25 wt% PPBB(150-1-5)B was cast onto a surface-treated glass substrate. The film was dried at 80°C for 1 h and 160°C for 1 h, and then post-cured at 185°C for 3 h and 218°C for 1 h. The DMA results (Figure 21) showed that the T of the cured PPBB was g The results show that the tensile strength is 163°C. The tensile properties of the cured PPBB are shown in Table 1, including a tensile modulus of 3.31 GPa and a tensile strength of 31.64 MPa. The film is very brittle and its tensile strength has a large standard deviation. The elongation at break is only 1.2%. Thermoset Pd has a modulus of 3.12 GPa, a tensile strength of 82.08 MPa and an elongation at break of 3.23%. Compared to Pd, the tensile strength and elongation at break of the cured PPBB have a significant decrease.

[0161] [Table 2]

[0162] The tensile properties of the cured PBB are listed in Table 2. The cured PBB(150-1-5)B has a similar modulus to the cured PPBB, but has higher tensile strength (75% improvement) and elongation at break (56% improvement). The possible reasons for this improvement in tensile strength and elongation at break are that the unreacted BBPA acts as a chain extender to improve the molecular weight, and Pd acts as a crosslinker to further crosslink the polymer (Figure 22). Importantly, the omission of the purification process did not impair the mechanical properties of the cured resin. Meanwhile, the omission of the purification process made the application of the composite more practical.

[0163] Another formulation based on DABPA and Pd was made by non-solvent blending method. The advantages of using DABPA instead of BBPA as the paired monomer include: 1) non-solvent blending with Pd, 2) the ability to further crosslink with BMI by the introduction of allyl groups in the final polymer, and 3) the ability to blend with acrylate monomers via allyl groups extends the curing method from thermal to UV curing. DABPA is liquid at room temperature and was directly mixed with Pd powder at 75°C. As seen from the DSC results, the polymerization mechanism between Pd / DABPA is similar to Pd / BBPA. Therefore, similar melt polymerization conditions were applied for Pd / DABPA. Several heating rates were tested for Pd / DABPA: 1°C / min, 2°C / min, and 5°C / min. The obtained products were characterized by GPC and solubility tests in THF. At 2°C / min, the polymer had the maximum molecular weight and was found to be completely soluble in THF. At 1°C / min, the monomers took longer to diffuse and react, and the polymer formed longer molecular chains, resulting in insolubility in THF. At 5°C / min, the increased heating rate meant that there was not enough time for the monomers to diffuse and react. Polymers with short chains were formed. The isothermal time and temperature were also adjusted to obtain the best reaction conditions. Under a heating rate of 2°C / min, an isothermal at 150°C for 10 minutes was found to produce the highest MW of 1 MDa.

[0164] For PBB, it has been demonstrated that the molecular weight of the thermoplastic can be tuned by changing the polymerization conditions. For PDA crosslinkable thermoplastics, different molecular weights were also obtained by varying the isothermal temperature and time. As shown in Figure 23, under isothermal conditions of 120°C for 30 min, only oligomers were formed (PDA(120-2-30)A). For isothermal conditions of 150°C for 5 min, the polymer had a moderate MW (PDA(150-2-5)A). The highest MW was achieved under isothermal conditions of 150°C for 10 min (PDA(150-2-10)A). Further extension of the isothermal time to 25 min resulted in the formation of crosslinked structures and the polymer was only partially soluble in NMP (PDA(150-2-25)A).

[0165] The rheological behavior of PDAs with different MW was characterized by a rheometer. As shown in Figure 24, the viscosity of PDA increases with increasing MW of PDA. PDA(120-2-30)A has the lowest viscosity of 2 Pa.s at 140°C. PDA(150-2-5)A has the lowest viscosity of 22 Pa.s at 150°C, while the viscosity of PDA(150-2-10)A increases to 2500 Pa.s at 150°C. PDA(150-2-25)A has the highest viscosity among all four samples due to its partially crosslinked structure. These rheological data indicate that all PDA resins except PDA(150-2-25)A have melt viscosities low enough to be molded (remolded) into films using a hot press or oven. Films of crosslinkable thermoplastic PDA (150-2-10) with free-standing properties were also prepared by coating its DMF solution on glass substrates and drying in an oven at temperatures below 150 °C. DSC results showed that PDA (150-2-10) had a T of 91 °C. g , and an exothermic peak resulting from curing the benzoxazine groups in the thermoplastic PDA (150-2-10) film at temperatures above 180°C.

[0166] The three types of PDA resin powders were molded (remolded) into thin films by hot pressing, and then cured under the conditions of 160°C for 1 hour, 185°C for 3 hours, and 218°C for 1 hour. The DMA curves and corresponding data of these cured PDA films are shown in Figures 25A-B and Table 3. These cured PDA resin films showed similar storage modulus at 50°C. With increasing test temperature, these films showed a sharp decrease in storage modulus around 120°C, indicating a transformation of the film morphology from a glassy state to a rubbery state. The cured PDA (150-2-10) A film showed the highest T g and T g It showed the highest storage modulus at higher temperatures. The high modulus in the rubbery plateau suggests a highly crosslinked network. All three cured PDA resins showed a tensile modulus of about 3.1-3.2 GPa, a tensile strength of about 62-64 MPa, and an elongation at break of about 2.4%.

[0167] [Table 3]

[0168] The cured PPDA resin film was also prepared by hot pressing under the same molding conditions as the PDA resin. g The thermal and tensile properties are shown in Table 3. Compared to the cured PDA film, the cured PPDA film has a higher T at 145 °C. g However, the tensile properties were approximately 10-20% inferior in comparison.

[0169] Synthesis of PDODA (Example 10)

[0170] PDODA was synthesized using the same method as described in Example 4. The PDODA synthesis scheme is shown in structure (XII). [ka]

[0171] Synthesis of PDODA-MA (Example 11)

[0172] PDODA and methacrylic anhydride were added to a flask with a molar ratio of reactive phenol to methacrylic anhydride of 1:5. To the mixture, 2 equivalents of sodium bicarbonate and an appropriate amount of THF were further added. The reaction was carried out at room temperature for 24 hours. The PDODA-MA synthesis scheme is shown in structure (XIII). [ka]

[0173] Example 12: UV curing of PDODA-MA, VP, and DMPA

[0174] PDODA-MA was blended with VP and DMPA in a weight ratio of 20:65:15, and the mixture was sonicated for 5 minutes. The resulting mixture was liquid at room temperature. UV radiation at 365 nm was applied to the liquid via a handheld UV lamp for 60 minutes. As shown in FIG. 26A, the resulting product was solid at room temperature and had a rough surface.

[0175] The solubility of the resin was tested to determine the extent of crosslinking that occurred from the UV treatment: the solid did not dissolve in THF, indicating effective crosslinking from UV exposure.

[0176] Comparative Example 12: UV curing of VP and DMPA

[0177] For comparison, VP (2 g) and DMPA (350 mg) were blended in a ratio of 85:15 to form a liquid. The mixture was then cured according to the method of Example 12 to yield a solid with a relatively smooth surface at room temperature, as shown in Figure 26B. The resin was readily soluble in THF, indicating that no significant crosslinking had occurred.

[0178] Example 13: UV curing of PDODA-MA and DMPA

[0179] The UV curability of PDODA-MA without additional monomer was tested by blending PDODA-MA with DMPA in a weight ratio of 95:5. THF was added to the mixture (approximately 0.5 mL of THF per gram of powder), and then the THF was evaporated in a rotary evaporator under vacuum at room temperature to obtain a paste. UV irradiation was applied to the paste for 10 seconds using a UV curing machine. After UV curing, the sample was a solid powder. The solid powder did not dissolve in THF, indicating that effective crosslinking occurred during the UV curing process.

[0180] DSC was performed on the PDODA-MA samples before and after UV curing and the data is summarized in Table 4. [Table 4]

[0181] As shown in Table 4, the curing temperature of the UV-treated resin was higher than that of the non-UV-treated resin. In addition, the glass transition temperature of the UV-treated resin was 33°C higher than that of the non-UV-treated resin. These results indicate the effective crosslinking of the resin by UV treatment.

[0182] [Synthesis of PDODA-EP (Example 14)]

[0183] 2 g of PDODA, 25 ml of epichlorohydrin, 378 mg of NaOH, and 4.68 ml of water were added to the flask. The reaction was carried out at 50° C. for 24 hours. The product was obtained by extraction with dichloromethane followed by evaporation of the solvent on a rotary evaporator. The structure of PDODA-EP is shown in structure (XIV), where "BZ" represents the benzoxazine moiety. [ka]

[0184] Example 15: Microwave curing of PDODA-EP

[0185] The PDODA-EP resin was cured in a 900W microwave for 5, 10, and 15 minutes. The comparative sample did not undergo microwave curing, meaning that it was thermally cured during heating by DSC experiments. The samples were tested by DSC and the results can be found in Table 5 below.

[0186] Comparative Example 15: Microwave curing of PDODA

[0187] As comparative examples, PDODA and PD (benzoxazine), which do not have microwave curable epoxide functionality, were cured in a microwave at 900 W for 5, 10, and 15 minutes. Samples of each resin were heat cured and did not undergo microwave curing. The samples were tested by DSC and the results can be found in Table 5 below. [Table 5]

[0188] As shown in Table 5, all three materials are microwave curable to some degree. The PDODA and PD samples require more than 10-15 minutes to fully cure, while the PDODA-EP sample containing microwave curable groups takes 5-10 minutes to fully cure. This indicates a higher microwave curing efficiency in the samples containing microwave curable groups. Also, the sample containing microwave curable groups in the polymer chain (PDODA-EP) has a dramatic T from below 150 °C for PDODA to over 200 °C for PDODA-EP. g The T of microwave-treated PDODA-EP is improved. g It was also found that microwave treatment had an improved effect compared to samples that had undergone only thermal curing, as evidenced by the fact that the thermal curing rate was 10°C higher than that of PDODA-EP when cured only by thermal treatment.

[0189] Although only a few exemplary embodiments have been described in detail above, those skilled in the art will readily appreciate that many variations in the exemplary embodiments are possible without substantially departing from the present invention. Accordingly, all such variations are intended to be included within the scope of the present disclosure as defined in the following claims. In the claims, any means-plus-function clauses are intended to cover structures described herein as performing the described function and equivalents of those structures. Similarly, any step-plus-function clauses in the claims are intended to cover acts described herein as performing the described function and equivalents of those acts. Applicant's express intent is not to implement 35 USC § 112(f) to any limitation of any claim herein, except where the claim expressly uses the words "means for" or "steps for" with the relevant function. [Brief description of the drawings]

[0190] [Figure 1] FIG. 1 is a schematic diagram of the synthesis of a crosslinkable thermoplastic resin according to one or more embodiments. [Diagram 2] FIG. 1 is a schematic diagram of the curing of a crosslinkable thermoplastic resin of one or more embodiments. [Diagram 3] FIG. 1 is a schematic diagram of the purification of a crosslinkable thermoplastic resin according to one or more embodiments. [Figure 4] FIG. 1 is a schematic diagram of a polymer modification strategy according to one or more embodiments of the present disclosure. [Diagram 5] FIG. 1 is a schematic diagram of a polymer synthesis strategy according to one or more embodiments of the present disclosure. [Figure 6A] FIG. 1 is a schematic diagram of a polymer including a curable functional group according to one or more embodiments of the present disclosure. [Figure 6B] FIG. 1 is a schematic diagram of a cured resin according to one or more embodiments of the present disclosure. [Figure 7A]FIG. 1 is a schematic diagram of a polymer composition including a hardenable component according to one or more embodiments of the present disclosure. [Figure 7B] FIG. 1 is a schematic diagram of a cured resin according to one or more embodiments of the present disclosure. [Figure 8] 1 provides gel permeation chromatography (GPC) data for exemplary thermoplastic compositions of one or more embodiments. [Figure 9] 1 provides gel permeation chromatography (GPC) data for exemplary thermoplastic compositions of one or more embodiments. [Figure 10] 1 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments. [Figure 11] 1 provides GPC data for an exemplary thermoplastic composition of one or more embodiments. [Figure 12] 1 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments. [Figure 13] 1 provides GPC data for an exemplary thermoplastic composition of one or more embodiments. [Figure 14] 1 shows 1H NMR data for an exemplary thermoplastic resin composition of one or more embodiments. [Figure 15] 1 shows TGA results for an exemplary thermoplastic composition of one or more embodiments. [Figure 16] 1 provides GPC data for an exemplary thermoplastic composition of one or more embodiments. [Figure 17A] FIG. 1 is a schematic diagram of the synthesis of an exemplary crosslinkable thermoplastic resin of one or more embodiments. [Figure 17B] FIG. 1 is a schematic diagram of the synthesis of an exemplary crosslinkable thermoplastic resin of one or more embodiments. [Figure 18] FIG. 1 is a schematic diagram of the synthesis of an exemplary crosslinkable thermoplastic resin of one or more embodiments. [Figure 19]FIG. 1 shows gel permeation chromatography (GPC) data for exemplary thermoplastic resin compositions of one or more embodiments: (a) PBB(120-2-30)A, (b) PBB(150-2-5)A, (c) PBB(150-2-10)A, and (d) PBB(150-2-25)A. [Figure 20] 1 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments. [Figure 21] 1 is a graphical representation of DMA results of an exemplary cured thermoplastic composition of one or more embodiments. [Figure 22] FIG. 2 is a schematic diagram of the reaction between a monomer and a polymer during curing of a thermoplastic resin of one or more embodiments. [Diagram 23] FIG. 1 is a graphical representation of GPC results of thermoplastics (powder partially dissolved in NMP) for exemplary thermoplastic compositions of one or more embodiments: (A) PDA(120-2-30)A, (b) PDA(150-2-5)A, (c) PDA(150-2-10)A, and (d) PDA(150-2-25)A. [Figure 24] 1 illustrates the rheological behavior of an exemplary thermoplastic composition of one or more embodiments. [Figure 25A] 1 shows a dynamic mechanical analysis of the storage modulus of an exemplary cured thermoplastic composition of one or more embodiments. [Figure 25B] 1 shows a dynamic mechanical analysis of the loss tangent (tan delta) of an exemplary cured thermoplastic composition of one or more embodiments. [Figure 26A] 1 is a photograph of a cured polymer composition according to one or more embodiments of the present disclosure. [Figure 26B] 1 is a photograph of a cured polymer composition according to one or more embodiments of the present disclosure.

Claims

1. A crosslinkable thermoplastic resin composition comprising a crosslinkable thermoplastic resin comprising the following polymer: the polymer is formed from the reaction between a bis-benzoxazine monomer and a difunctional comonomer having a phenolic, amine, and / or thiol functional group and includes at least one crosslinkable group; Where: the crosslinkable thermoplastic resin has a weight average molecular weight in the range of 1 to 1,000 kilodaltons; the crosslinkable thermoplastic resin composition has a polymer content in the range of 30 to 90 wt %, based on the total weight of the crosslinkable thermoplastic resin composition; The crosslinkable thermoplastic resin composition has a melt viscosity of 10,000 Pa s or less at a temperature of 140° C. Crosslinkable thermoplastic resin composition.

2. The crosslinkable thermoplastic composition of claim 1 , wherein said at least one crosslinkable group is an endcap on said polymer.

3. The crosslinkable thermoplastic resin composition of claim 1 , wherein said at least one crosslinkable group is on the backbone of said polymer.

4. 10. The crosslinkable thermoplastic resin composition of claim 1 further comprising UV or microwave curable functional groups.

5. The crosslinkable thermoplastic resin composition of claim 1 , wherein said at least one crosslinkable group is a UV or microwave curable functional group.

6. The crosslinkable thermoplastic composition of claim 4 , wherein said UV or microwave curable functional group reacts with said at least one crosslinkable group.

7. 2. The crosslinkable thermoplastic resin composition according to claim 1, comprising unreacted monomer in an amount of 25% by weight or less.

8. 1. A method for forming a crosslinkable thermoplastic composition comprising reacting a bis-benzoxazine monomer with a difunctional comonomer to form a crosslinkable thermoplastic comprising a polymer that includes at least one crosslinkable group, the crosslinkable thermoplastic resin has a weight average molecular weight in the range of 1 to 1,000 kilodaltons; the crosslinkable thermoplastic resin composition has a polymer content in the range of 30 to 90 wt %, based on the total weight of the crosslinkable thermoplastic resin composition; The crosslinkable thermoplastic resin composition has a melt viscosity of 10,000 Pa s or less at a temperature of 140° C. A method for forming a crosslinkable thermoplastic composition.

9. 9. The method of claim 8, wherein the reacting step comprises solution polymerization in a solvent having a boiling point greater than 75° C. at 1 atmosphere to form a benzoxazine resin in solution.

10. 10. The method of claim 9, wherein the solvent is selected from the group consisting of ethyl acetate, 2-methoxyethanol, dimethylformamide (DMF), N-methylpyrrolidone (NMP), butyl acetate, a mixture of 2-methoxyethanol / tetrahydrofuran (THF), and combinations thereof.

11. 10. The method of claim 9, further comprising purifying the benzoxazine resin from the solution.

12. The method of claim 9, wherein the molar ratio between the bis-benzoxazine monomer and the difunctional comonomer is from 1:1 to 2:

1.

13. The method of claim 8, wherein the reacting step comprises melt polymerization of the bis-benzoxazine monomer and a bisphenol comonomer.

14. The method of claim 13, wherein the molar ratio between the bis-benzoxazine monomer and the bisphenol comonomer is from 1:10 to 10:

1.

15. 9. The method of claim 8, further comprising modifying the crosslinkable thermoplastic composition to include UV or microwave curable functional groups.

16. 1. A method for forming a cured crosslinkable thermoplastic resin, comprising: Providing a crosslinkable thermoplastic composition comprising a crosslinkable thermoplastic resin comprising a polymer comprising: the polymer is formed from the reaction between a bis-benzoxazine monomer and a difunctional comonomer having a phenolic, amine, and / or thiol functional group and includes at least one crosslinkable group; the crosslinkable thermoplastic resin has a weight average molecular weight in the range of 1 to 1,000 kilodaltons, and the crosslinkable thermoplastic resin composition has a polymer content in the range of 30 to 90 weight percent based on the total weight of the crosslinkable thermoplastic resin composition; The process and curing the crosslinkable thermoplastic resin composition by applying an external stimulus to form the cured crosslinkable thermoplastic resin; A method comprising:

17. 17. The method of claim 16, wherein the external stimulus is selected from the group consisting of heat, ultraviolet radiation, microwave radiation, and moisture.

18. 17. The method of claim 16, wherein the crosslinkable thermoplastic composition further comprises UV or microwave curable functional groups and the external stimulus comprises ultraviolet radiation or microwave radiation.

Citation Information

Patent Citations

  • thermosetting components

    JP2010518207A

  • thermosetting components

    JP2010532392A

  • Amine / epoxy curing of benzoxazine

    JP2015502416A

  • Curable benzoxazine compositions with improved thermal stability

    JP2017538836A

  • Benzoxazine-thiol adducts

    US20100307680A1