SUBSTRATE PROCESSING METHOD, SEMICONDUCTOR DEVICE MANUFACTURING METHOD, SUBSTRATE PROCESSING APPARATUS, AND PROGRAM
By cyclically supplying specific materials to form films on substrates, the method addresses the challenge of controlling composition ratios, achieving improved film quality and nitrogen concentration control in semiconductor manufacturing.
Patent Information
- Application Number
- JP2023501985
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing methods struggle with controlling the composition ratio of films containing predetermined elements, oxygen, and nitrogen formed on substrates during semiconductor device manufacturing.
A method involving a cycle of supplying a first raw material, a second raw material with a different molecular structure, an oxidizing agent, and a nitriding agent to form a film on the substrate, with specific steps performed in a predetermined order to improve composition ratio control.
Enhances the controllability of the composition ratio of films containing predetermined elements, oxygen, and nitrogen, resulting in improved film quality and reduced impurities, with the ability to adjust nitrogen concentration as desired.
Smart Images

Figure 0007579959000001 
Figure 0007579959000002 
Figure 0007579959000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to Substrate processing method, The present invention relates to a method for manufacturing a semiconductor device, a substrate processing apparatus, and a program. [Background technology]
[0002] 2. Description of the Related Art As one step in the manufacturing process of a semiconductor device, a substrate processing step may be performed in which raw materials, an oxidizing agent, and a nitriding agent are supplied to a substrate to form a film containing predetermined elements, oxygen, and nitrogen on the substrate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-61218 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to improve the controllability of the composition ratio of a film containing a predetermined element, oxygen, and nitrogen formed on a substrate. [Means for solving the problem]
[0005] According to one aspect of the present disclosure, (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a predetermined number of cycles, thereby forming a film containing the predetermined element, oxygen, and nitrogen on the substrate. Effect of the Invention
[0006] According to the present disclosure, it is possible to provide a technique capable of improving the controllability of the composition ratio of a film containing a predetermined element, oxygen, and nitrogen formed on a substrate. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in vertical cross section. [Diagram 2] FIG. 2 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in a cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 3 is a schematic configuration diagram of a controller 121 of a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller 121. [Figure 4] FIG. 4 is a flow diagram showing a gas supply sequence according to one embodiment of the present disclosure. [Figure 5A] FIG. 2 is a diagram showing a schematic view of a surface state of a substrate before a film formation process is started; [Figure 5B] 4 is a diagram showing a schematic view of the surface state of the substrate when step B is performed. FIG. [Figure 5C] 4 is a diagram showing a schematic view of the surface state of the substrate when step A is carried out after step B is completed. FIG. [Figure 5D] 10 is a diagram showing a schematic view of the surface state of the substrate when step C is carried out after steps B and A are completed. FIG. [Figure 5E] FIG. 13 is a diagram showing a schematic view of the surface state of the substrate when step D is carried out after steps B, A, and C are completed. [Figure 6] 1A to 1C are diagrams illustrating various measurement results of a film formed on a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described mainly with reference to Figures 1 to 4 and Figures 5A to 5E. Note that all of the drawings used in the following description are schematic, and the dimensional relationships and ratios of each element on the drawings do not necessarily match those in reality. Furthermore, the dimensional relationships and ratios of each element between multiple drawings do not necessarily match.
[0009] (1) Configuration of the substrate processing device 1, the process furnace 202 has a heater 207 as a temperature regulator (heating unit). The heater 207 is cylindrical and is installed vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) gas by heat.
[0010] A reaction tube 203 is disposed concentrically with the heater 207 inside the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A manifold 209 is disposed concentrically with the reaction tube 203 below the reaction tube 203. The manifold 209 is made of a metal material such as stainless steel (SUS) and is formed in a cylindrical shape with an open upper end and a closed lower end. The upper end of the manifold 209 engages with the lower end of the reaction tube 203 and is configured to support the reaction tube 203. An O-ring 220a is provided between the manifold 209 and the reaction tube 203 as a seal member. The reaction tube 203 is installed vertically like the heater 207. The reaction tube 203 and the manifold 209 mainly constitute a processing vessel (reaction vessel). A processing chamber 201 is formed in a cylindrical hollow portion of the processing vessel. The processing chamber 201 is configured to be capable of accommodating a wafer 200 as a substrate. In the processing chamber 201, processing of the wafer 200 is performed.
[0011] Nozzles 249a to 249c serving as first to third supply units are provided in the processing chamber 201 so as to penetrate the sidewall of the manifold 209, respectively. The nozzles 249a to 249c are also referred to as first to third nozzles, respectively. The nozzles 249a to 249c are made of a heat-resistant material such as quartz or SiC. Gas supply pipes 232a to 232c are connected to the nozzles 249a to 249c, respectively. The nozzles 249a to 249c are different nozzles, and the nozzles 249b and 249c are provided adjacent to the nozzle 249a.
[0012] Gas supply pipes 232a-232c are provided with mass flow controllers (MFCs) 241a-241c, which are flow rate controllers (flow rate control parts), and valves 243a-243c, which are on-off valves, in order from the upstream side of the gas flow. Gas supply pipes 232d and 232e are connected to the gas supply pipe 232a downstream of the valve 243a. Gas supply pipes 232f and 232g are connected to the gas supply pipes 232b and 232c downstream of the valves 243b and 243c. Gas supply pipes 232e-232g are provided with MFCs 241e-241g and valves 243e-243g in order from the upstream side of the gas flow. Gas supply pipes 232a-232g are made of a metal material, such as SUS.
[0013] As shown in FIG. 2, the nozzles 249a to 249c are provided in a circular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, from the lower part to the upper part of the inner wall of the reaction tube 203, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a to 249c are provided in a region horizontally surrounding the wafer arrangement region on the side of the wafer arrangement region in which the wafers 200 are arranged, so as to extend along the wafer arrangement region. In a plan view, the nozzle 249a is arranged to face an exhaust port 231a (described later) on a straight line across the center of the wafer 200 loaded into the processing chamber 201. The nozzles 249b and 249c are arranged to sandwich a straight line L passing through the nozzle 249a and the center of the exhaust port 231a from both sides along the inner wall of the reaction tube 203 (the outer periphery of the wafer 200). The straight line L is also a straight line passing through the nozzle 249a and the center of the wafer 200. In other words, the nozzle 249c is provided on the opposite side of the nozzle 249b across the line L. The nozzles 249b and 249c are arranged in line symmetry with the line L as the axis of symmetry. Gas supply holes 250a to 250c for supplying gas are provided on the side surfaces of the nozzles 249a to 249c, respectively. The gas supply holes 250a to 250c are each opened to face (face) the exhaust port 231a in a plan view, and are capable of supplying gas toward the wafer 200. A plurality of gas supply holes 250a to 250c are provided from the lower part to the upper part of the reaction tube 203.
[0014] A first raw material (first raw material gas) containing a predetermined element is supplied from the gas supply pipe 232a into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a.
[0015] An oxidant (oxidizing gas) is supplied from the gas supply pipe 232b into the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b.
[0016] A nitriding agent (nitriding gas) is supplied from the gas supply pipe 232c into the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b.
[0017] A second raw material (second raw material gas) having a molecular structure different from that of the first raw material described above and containing a specified element and oxygen (O) is supplied from gas supply pipe 232d into the processing chamber 201 via MFC 241d, valve 243d, gas supply pipe 232a, and nozzle 249a.
[0018] Inert gas is supplied from the gas supply pipes 232e, 232f, and 232g through the MFCs 241e, 241f, and 241g, the valves 243e, 243f, and 243g, the gas supply pipes 232a, 232b, and 232c, and the nozzles 249a, 249b, and 249c into the processing chamber 201. The inert gas acts as a purge gas, a carrier gas, a dilution gas, etc.
[0019] A first raw material supply system is mainly composed of the gas supply pipe 232a, the MFC 241a, and the valve 243a. An oxidizing agent supply system is mainly composed of the gas supply pipe 232b, the MFC 241b, and the valve 243b. A nitriding agent supply system is mainly composed of the gas supply pipe 232c, the MFC 241c, and the valve 243c. A second raw material supply system is mainly composed of the gas supply pipe 232d, the MFC 241d, and the valve 243d. An inert gas supply system is mainly composed of the gas supply pipes 232e to 232g, the MFCs 241e to 241g, and the valves 243e to 243g.
[0020] At least one of the first raw material gas, the second raw material gas, the oxidizing gas, and the nitriding gas is also referred to as a film formation gas, and at least one of the first raw material supply system, the second raw material supply system, the oxidizing agent supply system, and the nitriding agent supply system is also referred to as a film formation gas supply system.
[0021] Any or all of the various gas supply systems described above may be configured as an integrated gas supply system 248 in which the valves 243a to 243g and the MFCs 241a to 241g are integrated. The integrated gas supply system 248 is connected to the gas supply pipes 232a to 232g, and the supply operation of various gases into the gas supply pipes 232a to 232g, i.e., the opening and closing operation of the valves 243a to 243g and the flow rate adjustment operation by the MFCs 241a to 241g, are controlled by a controller 121, which will be described later. The integrated gas supply system 248 is configured as an integrated or separate type integrated unit, and can be attached and detached to and from the gas supply pipes 232a to 232g, etc., in units of integrated units, and is configured so that maintenance, replacement, expansion, etc. of the integrated gas supply system 248 can be performed in units of integrated units.
[0022] An exhaust port 231a for exhausting the atmosphere in the processing chamber 201 is provided at the lower side of the side wall of the reaction tube 203. As shown in FIG. 2, the exhaust port 231a is provided at a position facing the nozzles 249a to 249c (gas supply holes 250a to 250c) across the wafer 200 in a plan view. The exhaust port 231a may be provided along the side wall of the reaction tube 203 from the lower part to the upper part, that is, along the wafer arrangement area. An exhaust pipe 231 is connected to the exhaust port 231a. The exhaust pipe 231 is made of a metal material such as SUS. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 can evacuate and stop the evacuation of the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is operating, and further, can adjust the pressure inside the processing chamber 201 by adjusting the valve opening based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is operating. An exhaust system is mainly configured by the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.
[0023] Below the manifold 209, a seal cap 219 is provided as a furnace port cover body capable of airtightly closing the lower end opening of the manifold 209. The seal cap 219 is made of a metal material such as SUS, and is formed in a disk shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a seal member that abuts against the lower end of the manifold 209. Below the seal cap 219, a rotation mechanism 267 is provided for rotating the boat 217, which will be described later. A rotation shaft 255 of the rotation mechanism 267 is made of a metal material such as SUS, and is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be vertically raised and lowered by a boat elevator 115 as a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transfer device (transfer mechanism) that transfers the wafers 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219.
[0024] A shutter 219s is provided below the manifold 209 as a furnace port cover that can airtightly close the lower end opening of the manifold 209 when the seal cap 219 is lowered and the boat 217 is carried out of the processing chamber 201. The shutter 219s is made of a metal material such as SUS and is formed in a disk shape. An O-ring 220c is provided on the upper surface of the shutter 219s as a seal member that comes into contact with the lower end of the manifold 209. The opening and closing operation (lifting and lowering operation, rotating operation, etc.) of the shutter 219s is controlled by a shutter opening and closing mechanism 115s.
[0025] The boat 217 as a substrate support is configured to support a plurality of wafers 200, for example 25 to 200, in multiple stages in a horizontal position and aligned vertically with their centers aligned, i.e., arranged at intervals. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, heat insulating plates 218 made of a heat-resistant material such as quartz or SiC are supported in multiple stages.
[0026] A temperature sensor 263 serving as a temperature detector is installed in the reaction tube 203. By adjusting the power supply to the heater 207 based on temperature information detected by the temperature sensor 263, the temperature distribution in the process chamber 201 becomes a desired one. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.
[0027] 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122 configured as, for example, a touch panel, is connected to the controller 121.
[0028] The storage device 121c is composed of, for example, a flash memory, a hard disk drive (HDD), a solid state drive (SSD), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe in which procedures and conditions of the substrate processing described later are described, etc. are readably stored in the storage device 121c. The process recipe is a combination of procedures in the substrate processing described later that are executed by the controller 121 to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. In addition, the process recipe is also simply referred to as a recipe. In this specification, when the word program is used, it may include only a recipe, only a control program, or both. The RAM 121b is configured as a memory area (work area) in which the programs, data, etc. read by the CPU 121a are temporarily stored.
[0029] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241g, valves 243a to 243g, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, boat elevator 115, shutter opening / closing mechanism 115s, and the like.
[0030] The CPU 121a is configured to be able to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to an input of an operation command from the input / output device 122, etc. The CPU 121a is configured to be able to control the flow rate adjustment operation of various gases by the MFCs 241a to 241g, the opening and closing operations of the valves 243a to 243g, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotation mechanism 267, the lifting and lowering operation of the boat 217 by the boat elevator 115, the opening and closing operation of the shutter 219s by the shutter opening and closing mechanism 115s, etc., in accordance with the contents of the read recipe.
[0031] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 in a computer. The external storage device 123 includes, for example, a magnetic disk such as an HDD, an optical disk such as a CD, a magneto-optical disk such as an MO, and a semiconductor memory such as a USB memory or an SSD. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. When the term recording media is used in this specification, it may include only the storage device 121c alone, only the external storage device 123 alone, or both of them. The program may be provided to the computer using a communication means such as the Internet or a dedicated line without using the external storage device 123.
[0032] (2) Substrate processing An example of a sequence for processing a wafer 200 as a substrate as one step in a manufacturing process of a semiconductor device using the above-mentioned substrate processing apparatus, i.e., an example of a film formation sequence for forming a film on the wafer 200, will be described mainly with reference to Fig. 4. In the following description, the operation of each part constituting the substrate processing apparatus is controlled by a controller 121.
[0033] In the film formation sequence of this embodiment, Step A of supplying a first source material containing a predetermined element to the wafer 200; A step B of supplying a second source material having a molecular structure different from that of the first source material and containing a predetermined element and oxygen to the wafer 200; A step C of supplying an oxidizing agent to the wafer 200; Step D of supplying a nitriding agent to the wafer 200; A film containing a predetermined element, oxygen, and nitrogen is formed on the wafer 200 by performing a cycle including the above a predetermined number of times (n times, n is an integer of 1 or more).
[0034] In the gas supply sequence shown in FIG. This shows the case where steps A and B are followed by steps C and D in each cycle, specifically, the case where steps A, B, C, and D are performed non-simultaneously, or more specifically, the case where steps B, A, C, and D are performed in this order.
[0035] In this specification, the above-mentioned film formation sequence may be expressed as follows for convenience. Similar notations will be used in the following descriptions of modified examples and other aspects.
[0036] (2nd raw material → 1st raw material → oxidizing agent → nitriding agent) × n
[0037] In this specification, the term "wafer" may refer to the wafer itself or a laminate of the wafer and a predetermined layer or film formed on its surface. In this specification, the term "surface of the wafer" may refer to the surface of the wafer itself or the surface of a predetermined layer or the like formed on the wafer. In this specification, the phrase "forming a predetermined layer on a wafer" may refer to forming a predetermined layer directly on the surface of the wafer itself or forming a predetermined layer on a layer or the like formed on the wafer. In this specification, the term "substrate" is synonymous with the term "wafer".
[0038] (Wafer charge and boat load) After a plurality of wafers 200 are loaded into the boat 217 (wafer charge), the shutter 219s is moved by the shutter opening / closing mechanism 115s to open the lower end opening of the manifold 209 (shutter open). Then, as shown in Fig. 1, the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115 and carried into the processing chamber 201 (boat load). In this state, the seal cap 219 seals the lower end of the manifold 209 via the O-ring 220b.
[0039] (Pressure and temperature regulation) After the boat loading is completed, the inside of the processing chamber 201, i.e., the space in which the wafers 200 are present, is evacuated (reduced pressure exhaust) by the vacuum pump 246 so that the inside of the processing chamber 201 is at a desired pressure (vacuum level). At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information (pressure adjustment). Also, the wafers 200 in the processing chamber 201 are heated by the heater 207 so that the temperature is a desired processing temperature. At this time, the power supply to the heater 207 is feedback-controlled based on temperature information detected by the temperature sensor 263 so that the inside of the processing chamber 201 has a desired temperature distribution (temperature adjustment). Also, the rotation mechanism 267 starts rotating the wafers 200. The evacuation inside the processing chamber 201 and the heating and rotation of the wafers 200 are all continued at least until the processing of the wafers 200 is completed.
[0040] 5A, the surface of the wafer 200 is terminated with hydroxyl groups (-OH) (OH termination). The OH terminations present on the surface of the wafer 200 function as adsorption sites for molecules and atoms.
[0041] (Film formation process) Then, the following steps B, A, C, and D are executed in sequence.
[0042] [Step B] In this step, the second source material is supplied to the wafer 200 in the processing chamber 201 .
[0043] Specifically, the valve 243d is opened to allow the second source material to flow into the gas supply pipe 232d. The flow rate of the second source material is adjusted by the MFC 241d, and the second source material is supplied into the processing chamber 201 via the gas supply pipe 232a and the nozzle 249a, and exhausted from the exhaust port 231a. At this time, the second source material is supplied to the wafer 200 (second source material supply). At this time, the valves 243e to 243g are opened to supply an inert gas into the processing chamber 201 via each of the nozzles 249a to 249c. Note that in some of the methods described below, the supply of the inert gas into the processing chamber 201 may not be performed.
[0044] The second raw material may be a gas having a molecular structure containing an alkoxy group bonded to silicon (Si) as a predetermined element. For example, the second raw material may be a gas having an amino group bonded to one bond of Si as a predetermined element constituting the central atom X, and alkoxy groups bonded to the remaining three bonds.
[0045] An amino group has a structure in which hydrogen (H) has been removed from either ammonia (NH3), a primary amine, or a secondary amine, and is a monovalent functional group represented by one of the structural formulas -NH2, -NHR, or -NRR'. R and R' shown in the structural formula are alkyl groups including methyl, ethyl, propyl, and butyl groups. R and R' may be not only linear alkyl groups but also branched alkyl groups such as isopropyl, isobutyl, secondary butyl, and tertiary butyl. R and R' may be the same alkyl group or different alkyl groups.
[0046] An alkoxy group is a monovalent functional group having a structure in which an alkyl group (R) is bonded to an oxygen (O) atom and is represented by the structural formula -OR. Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, and the like. The alkoxy group may be not only these linear alkoxy groups but also branched alkoxy groups such as an isopropoxy group, an isobutoxy group, a secondary butoxy group, and a tertiary butoxy group. The above-mentioned alkyl group includes a methyl group, an ethyl group, a propyl group, and a butyl group. The alkyl group may be not only these linear alkyl groups but also branched alkyl groups such as an isopropyl group, an isobutyl group, a secondary butyl group, and a tertiary butyl group.
[0047] As the second raw material, for example, a dialkylaminotrialkoxysilane gas such as trimethoxydimethylaminosilane ((CH3)2NSi(OCH3)3, abbreviated as TMDMAS) gas, trimethoxydiethylaminosilane ((C2H5)2NSi(OCH3)3) gas, triethoxydimethylaminosilane ((CH3)2NSi(OC2H5)3) gas, or triethoxydiethylaminosilane ((C2H5)2NSi(OC2H5)3) gas can be used. The Si contained in these gases has four bonds, and of the four bonds of Si, three bonds are bonded to alkoxy groups, and the remaining bond of the four bonds of Si is bonded to an amino group. The ratio of the number of amino groups to the number of alkoxy groups contained in the gas molecule is 1:3. The bond energy E between the alkoxy group and Si is O is the bond energy E between the amino group and Si A That is, the amino group has an active property that makes it easier to be eliminated from silicon compared to the alkoxy group.
[0048] As the inert gas, for example, nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, or other rare gases can be used. As the inert gas, one or more of these can be used. This also applies to each step described later.
[0049] When, for example, TMDMAS gas is used as the second raw material, by performing this step under the processing conditions described below, it is possible to remove dimethylamino groups (-NMe2) from Si contained in the TMDMAS gas without removing methoxy groups (-OMe). In addition, it is possible to adsorb (chemisorb) Si in a state in which the dimethylamino groups are removed and the bond with the methoxy groups is maintained on the surface of the wafer 200. That is, it is possible to adsorb Si to a part of the adsorption sites on the surface of the wafer 200 in a state in which alkoxy groups are bonded to three of the four bonds of Si. In this way, it is possible to form a first layer containing a component in which an alkoxy group is bonded to Si on the outermost surface of the wafer 200. The reaction product generated when forming this layer constitutes, for example, a gaseous substance containing amino groups, and is discharged from the processing chamber 201.
[0050] Moreover, by performing this step under processing conditions described later, it becomes possible to prevent the amino group desorbed from Si contained in the second source material from being adsorbed on the surface of the wafer 200. As a result, it becomes possible to prevent the amino group desorbed from Si contained in the second source material from being contained in the first layer formed on the wafer 200.
[0051] In this step, the methoxy groups bonded to the Si adsorbed on the surface of the wafer 200, that is, the three bonds of the Si adsorbed on the surface of the wafer 200 are filled with the methoxy groups, so that it is possible to inhibit the adsorption of atoms or molecules to the Si adsorbed on the surface of the wafer 200. Also, in this step, the methoxy groups bonded to the Si adsorbed on the surface of the wafer 200 act as steric hindrances, so that it is possible to inhibit the adsorption of atoms or molecules to the adsorption sites (OH termination) on the surface of the wafer 200 around the Si adsorbed on the surface of the wafer 200. As a result, in this step, it is also possible to retain at least a part of the adsorption sites (OH termination) on the surface of the wafer 200 around the Si adsorbed on the surface of the wafer 200. In other words, it is also possible to suppress the reduction (consumption) in other steps of at least a part of the adsorption sites (OH termination) on the surface of the wafer 200 around the Si adsorbed on the surface of the wafer 200.
[0052] In this step, the supply of the second source material is continued until the adsorption reaction (chemical adsorption reaction) of Si to the surface of the wafer 200 is saturated. Even if the supply of the second source material is continued in this manner, the methoxy group bonded to Si acts as a steric hindrance, so that Si can be adsorbed discontinuously on the surface of the wafer 200. Specifically, Si can be adsorbed on the surface of the wafer 200 to a thickness of less than one atomic layer.
[0053] When the adsorption reaction of Si onto the surface of the wafer 200 is saturated, the surface of the wafer 200 is covered with methoxy groups bonded to Si as shown in Fig. 5B, and a part of the surface of the wafer 200 is maintained without consuming the adsorption sites (OH terminations). When the adsorption reaction of Si onto the surface of the wafer 200 is saturated, the layer formed by Si adsorbed onto the surface of the wafer 200 becomes a discontinuous layer with a thickness of less than one atomic layer.
[0054] After the first layer is formed, the valve 243d is closed to stop the supply of the second source material into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove (purge) gas remaining in the processing chamber 201 from the processing chamber 201. At this time, the valves 243e to 243g are opened to supply an inert gas into the processing chamber 201. The inert gas acts as a purge gas.
[0055] [Step A] After step B is completed, a first source material is supplied to the wafer 200 in the processing chamber 201, that is, to the first layer formed on the wafer 200.
[0056] Specifically, the valve 243a is opened to allow the first source material to flow into the gas supply pipe 232a. The flow rate of the first source material is adjusted by the MFC 241a, and the first source material is supplied into the processing chamber 201 through the nozzle 249a and exhausted from the exhaust port 231a. At this time, the first source material is supplied to the wafer 200 (first source material supply). At this time, the valves 243e to 243g are opened to supply an inert gas into the processing chamber 201 through each of the nozzles 249a to 249c. Note that in some methods described below, the supply of the inert gas into the processing chamber 201 may not be performed.
[0057] As the first raw material, for example, a gas having a molecular structure containing a halogen element bonded to silicon (Si) as a predetermined element, i.e., a halosilane gas, can be used. Halogen elements include chlorine (Cl), fluorine (F), bromine (Br), iodine (I), etc. As the halosilane gas, for example, a chlorosilane gas containing Si and Cl can be used.
[0058] As the first raw material, for example, chlorosilane gas such as hexachlorodisilane (Si2Cl6, abbreviated as HCDS) gas, monochlorosilane (SiH3Cl, abbreviated as MCS) gas, dichlorosilane (SiH2Cl2, abbreviated as DCS) gas, trichlorosilane (SiHCl3, abbreviated as TCS) gas, tetrachlorosilane (SiCl4, abbreviated as STC) gas, and octachlorotrisilane (Si3Cl8, abbreviated as OCTS) gas can be used. These gases do not contain oxygen. As the first raw material, one or more of these can be used.
[0059] As the first raw material, in addition to chlorosilane gas, for example, fluorosilane gas such as tetrafluorosilane (SiF4) gas or difluorosilane (SiH2F2) gas, bromosilane gas such as tetrabromosilane (SiBr4) gas or dibromosilane (SiH2Br2) gas, or iodosilane gas such as tetraiodosilane (SiI4) gas or diiodosilane (SiH2I2) gas can be used. These gases do not contain oxygen. One or more of these can be used as the first raw material.
[0060] As the first source material, in addition to the above, for example, a gas containing Si and an amino group, that is, an aminosilane gas, can also be used.
[0061] As the first raw material, for example, aminosilane gas such as tetrakis(dimethylamino)silane (Si[N(CH3)2]4, abbreviated as 4DMAS) gas, tris(dimethylamino)silane (Si[N(CH3)2]3H, abbreviated as 3DMAS) gas, bis(diethylamino)silane (Si[N(C2H5)2]2H2, abbreviated as BDEAS) gas, bis(tertiarybutylamino)silane (SiH2[NH(C4H9)]2, abbreviated as BTBAS) gas, and (diisopropylamino)silane (SiH3[N(C3H7)2], abbreviated as DIPAS) gas can be used. These gases do not contain oxygen. As the first raw material, one or more of these can be used.
[0062] When, for example, HCDS gas is used as the first source material, by performing this step under the processing conditions described below, it is possible to decompose a part of the methoxy groups contained in the first layer formed on the wafer 200 and to detach methyl groups from a part of O bonded to Si. In addition, it is possible to bond Si contained in the first source material to O having dangling bonds due to the detachment of the methyl groups. This makes it possible to form a silicon (Si)-containing layer containing a halogen element such as chlorine (Cl) of a predetermined thickness as a second layer on the top surface of the wafer 200 as a base, that is, on the first layer containing a component in which an alkoxy group is bonded to Si. The Si-containing layer containing a halogen element is formed by physical adsorption or chemical adsorption of molecules of the first source material, physical adsorption or chemical adsorption of molecules of a substance obtained by decomposing a part of the first source material, deposition of Si by thermal decomposition of the first source material, or the like. The Si-containing layer containing a halogen element may be an adsorption layer (physical adsorption layer or chemical adsorption layer) of molecules of the first source material or molecules of a substance obtained by decomposing a part of the first source material, or may be a deposition layer of Si containing a halogen element. When the above-mentioned chemical adsorption layer or the above-mentioned deposition layer is formed on the outermost surface of the wafer 200, Si contained in the first source material is adsorbed to the outermost surface of the wafer 200.
[0063] When this step is performed, at least a part of the alkoxy groups contained in the first layer is retained (maintained) as it is without being detached from Si or decomposed (alkyl groups are not detached from O constituting the alkoxy groups). As shown in FIG. 5C, the layer formed on the wafer 200 by performing this step (a layer formed by stacking the second layer on the first layer) is a layer containing Si-O-Si bonds, and containing alkoxy groups (e.g., methoxy groups) bonded to Si and halogen groups (e.g., chloro groups) bonded to Si. The reaction products generated when forming this layer constitute gaseous substances containing, for example, halosilane and amino groups, and are discharged from the processing chamber 201.
[0064] After the second layer is formed on the first layer, the valve 243a is closed to stop the supply of the first source material into the processing chamber 201. Then, gases remaining in the processing chamber 201 are removed (purged) from the processing chamber 201 by a processing procedure similar to that of the purging in step B.
[0065] [Step C] After step A is completed, an oxidizing agent is supplied to the wafer 200 in the processing chamber 201, that is, to the first layer and the second layer formed on the wafer 200.
[0066] Specifically, the valve 243b is opened to allow the oxidizing agent to flow into the gas supply pipe 232b. The flow rate of the oxidizing agent is adjusted by the MFC 241b, and the oxidizing agent is supplied into the processing chamber 201 through the nozzle 249b and exhausted from the exhaust port 231a. At this time, the oxidizing agent is supplied to the wafer 200 (oxidizing agent supply). At this time, the valves 243e to 243g are opened to supply an inert gas into the processing chamber 201 through each of the nozzles 249a to 249c. Note that in some of the methods described below, the supply of the inert gas into the processing chamber 201 may not be performed.
[0067] Examples of oxidizing agents include oxygen (O2) gas and plasma-excited O2 gas (O2 * ), ozone (O3) gas, O2 gas + hydrogen (H2) gas, water vapor (H2O gas), nitric oxide (NO) gas, nitrous oxide (N2O) gas, and other oxygen (O)-containing gases can be used. As the oxidizing agent, one or more of these can be used.
[0068] When an O-containing gas is used as an oxidizing agent, this step can be performed under processing conditions described below to oxidize (modify) at least a part of the first layer and the second layer formed on the wafer 200. For example, it is possible to remove an amino group or an alkoxy group from the first layer and bond a hydroxyl group to Si contained in the first layer. Also, for example, it is possible to remove hydrogen from Si contained in the second layer and bond a hydroxyl group to the dangling bond of Si generated thereby. As a result, a layer obtained by oxidizing the first and second layers, that is, a silicon oxide layer (SiO layer) containing Si and O, is formed as a third layer on the top surface of the wafer 200 as a base.
[0069] In addition, when this step is performed, at least a part of the halogen group contained in the second layer is retained (maintained) as it is without being detached from Si. As shown in FIG. 5D, by performing this step, the layer (third layer) formed on the wafer 200 is a layer containing Si-O-Si bonds and containing hydroxyl groups (-OH) bonded to Si and halogen groups such as chloro groups bonded to Si. These halogen groups function as reaction sites with the nitriding agent supplied to the wafer 200 in step D described later, that is, reaction sites necessary for nitriding the third layer. In addition, the reaction products generated when forming this layer constitute gaseous substances containing, for example, alkoxy groups and amino groups, and are discharged from the processing chamber 201.
[0070] After the SiO layer is formed as the third layer, the valve 243b is closed to stop the supply of the oxidizing agent into the processing chamber 201. Then, gases remaining in the processing chamber 201 are removed (purged) from the processing chamber 201 by a processing procedure similar to that of the purging in step B.
[0071] [Step D] After step C is completed, a nitriding agent is supplied to the wafer 200 in the processing chamber 201, that is, to the third layer formed on the wafer 200.
[0072] Specifically, the valve 243c is opened to allow the nitriding agent to flow into the gas supply pipe 232c. The nitriding agent is adjusted in flow rate by the MFC 241c, supplied into the processing chamber 201 via the nozzle 249c, and exhausted from the exhaust port 231a. At this time, the nitriding agent is supplied to the wafer 200 (nitriding agent supply). At this time, the valves 243e to 243g are opened to supply an inert gas into the processing chamber 201 via each of the nozzles 249a to 249c. Note that in some of the methods described below, the supply of the inert gas into the processing chamber 201 may not be performed.
[0073] As the nitriding agent, for example, ammonia (NH3) gas, diazane (N2H2) gas, hydrazine (N2H4) gas, N3H8 gas, or other hydrogen nitride gas, i.e., a gas containing nitrogen (N) and hydrogen (H), can be used. As the nitriding agent, one or more of these can be used.
[0074] As the nitriding agent, for example, a nitrogen (N), carbon (C) and hydrogen (H) containing gas can be used. As the N, C and H containing gas, for example, an amine-based gas or an organic hydrazine-based gas can be used. The N, C and H containing gas can be an N containing gas, a C containing gas, an H containing gas, or an N and C containing gas.
[0075] As the nitriding agent, for example, ethylamine-based gases such as monoethylamine (C2H5NH2, abbreviated as MEA) gas, diethylamine ((C2H5)2NH, abbreviated as DEA) gas, and triethylamine ((C2H5)3N, abbreviated as TEA) gas, methylamine-based gases such as monomethylamine (CH3NH2, abbreviated as MMA) gas, dimethylamine ((CH3)2NH, abbreviated as DMA) gas, and trimethylamine ((CH3)3N, abbreviated as TMA) gas, and organic hydrazine-based gases such as monomethylhydrazine ((CH3)HN2H2, abbreviated as MMH) gas, dimethylhydrazine ((CH3)2N2H2, abbreviated as DMH) gas, and trimethylhydrazine ((CH3)2N2(CH3)H, abbreviated as TMH) gas can be used. As the nitriding agent, one or more of these can be used.
[0076] When an N- and H-containing gas is used as a nitriding agent, this step is performed under the processing conditions described below, thereby making it possible to nitride (modify) at least a part of the third layer formed on the wafer 200. For example, a halogen group such as a chloro group contained in the third layer is reacted with an N- and H-containing gas to remove the halogen group from the third layer, and the N- and H-containing gas is decomposed to bond with the Si having a dangling bond due to the removal of the halogen group, thereby making it possible to bond a group containing N such as an amino group (-NH2) formed by the decomposition of the N- and H-containing gas. As a result, a layer obtained by nitriding the third layer, that is, a silicon oxynitride layer (SiON layer) containing Si, O, and N, is formed as a fourth layer on the top surface of the wafer 200 as a base.
[0077] In addition, when this step is performed, at least a part of the hydroxyl groups contained in the third layer is retained (maintained) as it is without being detached from Si. In other words, the nitridation reaction of the third layer in this step can proceed due to the presence of halogen groups on the surface of the third layer. If the entire surface of the third layer is OH-terminated and no halogen groups are present on the surface of the third layer, it can be said that it is difficult to nitride the third layer even if this step is performed. As shown in FIG. 5E, the layer (fourth layer) formed on the wafer 200 by performing this step is a layer that contains Si-O-Si bonds and contains hydroxyl groups (-OH) bonded to Si and groups containing N, such as amino groups (-NH2) bonded to Si. In addition, the reaction products generated when forming this layer constitute gaseous substances containing hydrogen halides such as HCl, and are discharged from the processing chamber 201.
[0078] After the SiON layer is formed as the fourth layer, the valve 243b is closed to stop the supply of the nitriding agent into the processing chamber 201. Then, gases remaining in the processing chamber 201 are removed (purged) from the processing chamber 201 by a processing procedure similar to that of the purging in step A.
[0079] [Perform the specified number of times] By performing the above-mentioned steps B, A, C, and D asynchronously, that is, in this order, a cycle is performed a predetermined number of times (n times, n is an integer of 1 or more), so that a film, for example, a silicon oxynitride film (SiON film) can be formed on the surface of the wafer 200. It is preferable to repeat the above-mentioned cycle multiple times. That is, it is preferable to make the thickness of the SiON layer formed per cycle thinner than the desired film thickness, and to repeat the above-mentioned cycle multiple times until the thickness of the SiON film formed by stacking the SiON layers reaches the desired thickness. In addition, when a gas containing N, C, and H is used as the nitriding agent, it is also possible to form, for example, a silicon oxycarbonitride layer (SiOCN layer) as the fourth layer, and by performing the above-mentioned cycle a predetermined number of times, it is also possible to form, for example, a silicon oxycarbonitride film (SiOCN film) as a film on the surface of the wafer 200.
[0080] The processing conditions for each step described above are exemplified below. In this specification, a numerical range such as "1 to 2666 Pa" means that the lower limit and the upper limit are included in the range. Therefore, for example, "1 to 2666 Pa" means "1 Pa or more and 2666 Pa or less". The same applies to other numerical ranges. In this specification, the processing temperature means the temperature of the wafer 200, and the processing pressure means the pressure inside the processing chamber 201, which is the space in which the wafer 200 exists. In addition, a gas supply flow rate of 0 slm means that the gas is not supplied. These are the same in the following explanations.
[0081] The processing conditions in step B are as follows: Second raw material supply flow rate: 0.01 to 2 slm, preferably 0.1 to 1 slm Second raw material supply time: 1 to 120 seconds, preferably 1 to 60 seconds Inert gas supply flow rate: 0 to 30 slm Treatment temperature: 550 to 700°C, preferably 600 to 650°C Treatment pressure: 1 to 2666 Pa, preferably 67 to 1333 Pa Examples are given below.
[0082] The processing conditions in step A are as follows: First raw material supply flow rate: 0.01 to 2 slm, preferably 0.1 to 1 slm First raw material supply time: 1 to 120 seconds, preferably 1 to 60 seconds Other processing conditions may be the same as those in step B.
[0083] The processing conditions in step C are as follows: Oxidizer supply flow rate: 0.1 to 10 slm Oxidizing agent supply time: 1 to 120 seconds, preferably 1 to 60 seconds Treatment pressure: 1 to 4000 Pa, preferably 1 to 3000 Pa Other processing conditions may be the same as those in step B.
[0084] The processing conditions in step D are as follows: Nitriding agent supply flow rate: 0.1 to 10 slm Nitriding agent supply time: 1 to 120 seconds, preferably 1 to 60 seconds Treatment pressure: 1 to 4000 Pa, preferably 1 to 3000 Pa Other processing conditions may be the same as those in step B.
[0085] In addition, by adjusting the ratio of the supply time of the second source material in step B to the supply time of the first source material in step A, it is possible to adjust the concentration of nitrogen contained in the SiON film formed on the wafer 200 to a desired value.
[0086] For example, by increasing the ratio of the supply time of the second source in step B to the supply time of the first source in step A, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0087] Furthermore, for example, by making the supply time of the first source material in step A shorter than the supply time of the second source material in step B, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0088] Moreover, by adjusting the ratio of the processing pressure in step B to the processing pressure in step A, the concentration of nitrogen contained in the SiON film formed on the wafer 200 can be adjusted to a desired value.
[0089] For example, by increasing the ratio of the processing pressure in step B to the processing pressure in step A, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0090] Furthermore, for example, by making the process pressure in step A lower than the process pressure in step B, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0091] In addition, by adjusting the ratio of the supply flow rate of the second source in step B to the supply flow rate of the first source in step A, it is possible to adjust the concentration of nitrogen contained in the SiON film formed on the wafer 200 to a desired value.
[0092] For example, by increasing the ratio of the supply flow rate of the second source in step B to the supply flow rate of the first source in step A, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0093] Furthermore, for example, by making the supply flow rate of the first source material in step A smaller than the supply flow rate of the second source material in step B, it is possible to lower the concentration of nitrogen contained in the SiON film formed on the wafer 200.
[0094] (After purging and atmospheric pressure recovery) After the formation of a film of a desired thickness on the wafer 200 is completed, an inert gas as a purge gas is supplied into the processing chamber 201 from each of the nozzles 249a to 249c, and exhausted from the exhaust port 231a. This purges the processing chamber 201, and gases and reaction by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (after-purge). Thereafter, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).
[0095] (Boat unloading and wafer discharging) Thereafter, the seal cap 219 is lowered by the boat elevator 115, and the lower end of the manifold 209 is opened. Then, the processed wafers 200 are carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 while being supported by the boat 217 (boat unloading). After the boat unloading, the shutter 219s is moved, and the lower end opening of the manifold 209 is sealed by the shutter 219s via the O-ring 220c (shutter close). After being carried out to the outside of the reaction tube 203, the processed wafers 200 are taken out of the boat 217 (wafer discharge).
[0096] (3) Effects of this mode According to this aspect, one or more of the following effects can be obtained.
[0097] (a) By performing a cycle of performing the above-mentioned steps B, A, C, and D in this order a predetermined number of times, it is possible to control the nitrogen concentration (composition ratio) in the SiON film formed on the wafer 200 to a desired value, for example, to reduce the nitrogen concentration to a desired value.
[0098] In addition, when step A is not performed and the above steps B, C, and D are cycled in this order a predetermined number of times, the nitriding reaction does not proceed easily, making it difficult to include N in the film formed on the wafer 200, and a silicon oxide film (SiO film) containing almost no N is formed on the wafer 200. This is considered to be because N contained in the nitriding agent N and H-containing gas is difficult to bond to the bond of Si contained in the Si-containing layer formed on the wafer 200 by performing step B. As in this embodiment, by performing step A after step B, it is possible to make halogen groups that can react with N and H-containing gas exist on the surface of the Si-containing layer formed on the wafer 200 even after the oxidizing agent is supplied, and as a result, it is possible to include N in the layer formed on the wafer 200 and form a SiON film on the wafer 200 to which N is added at a desired concentration.
[0099] In addition, if step B is not performed and the above-mentioned steps A, C, and D are performed in this order for a predetermined number of cycles, N is excessively incorporated into the film formed on the wafer 200, making it difficult to reduce the nitrogen concentration in the SiON film formed on the wafer 200 to a desired value. This is considered to be because the reactivity of the Si-containing layer formed by performing step A with the N- and H-containing gas is high, and it is difficult to suppress the addition of N to the Si-containing layer formed on the wafer 200 even if the processing conditions in steps C and D are changed widely. As in this embodiment, by performing step B before step A, it is possible to appropriately suppress the addition of N to the Si-containing layer formed on the wafer 200 and reduce the nitrogen concentration in the SiON film formed on the wafer 200 to a desired value.
[0100] (b) In step B, by continuing to supply the second raw material until the adsorption reaction (chemical adsorption reaction) of Si of the second raw material onto the surface of the wafer 200 becomes saturated, the ratio of Si and oxygen contained in the first layer can be maximized, and the nitrogen concentration in the SiON film formed on the wafer 200 can be reduced.
[0101] (c) In step B, the amino group is eliminated from the Si contained in the second source material without eliminating the alkoxy group, and the Si in a state in which the amino group is eliminated and the bond with the alkoxy group is maintained is adsorbed on the surface of the wafer 200, so that the action of the alkoxy group bonded to the Si makes it possible to inhibit the adsorption of atoms or molecules to the adsorption sites on the surface of the wafer 200, including the Si adsorbed on the surface of the wafer 200 and its surroundings, due to the action of the alkoxy group bonded to the Si. This makes it possible to make the layer composed of the Si adsorbed on the surface of the wafer 200 a discontinuous layer with a thickness of less than one atomic layer. This makes it possible to improve the in-plane thickness uniformity and step coverage of the SiON film formed on the wafer 200, and makes it possible to make this film a conformal film. Note that, when a gas in which an amino group is bonded to the central atom Si and no alkoxy group is bonded, such as 3DMAS gas, is used as the source gas, the action of the alkoxy group (methoxy group) in this embodiment cannot be obtained, and the in-plane thickness uniformity and step coverage of the SiON film formed on the wafer 200 may be reduced.
[0102] (d) In step B, by preventing the amino groups released from Si contained in the second source material from being adsorbed onto the surface of the wafer 200, the Si-containing layer formed on the wafer 200 can be a layer with less impurities such as C. This allows the SiON film formed on the wafer 200 to be a film with excellent processing resistance.
[0103] (e) In steps C and D, the amino group, methoxy group, and halogen group are eliminated from the layer to be modified, so that the modified layer has less impurities such as C and halogen elements. This makes it possible to form the SiON film formed on the wafer 200 into a film with excellent processing resistance.
[0104] (f) In steps C and D, by supplying an oxidizing agent or a nitriding agent in a non-plasma atmosphere, it is possible to avoid plasma damage to the film formed on the wafer 200, its underlying film, components inside the processing chamber 201, etc.
[0105] (g) The above-mentioned effects can be obtained similarly when the various raw materials, the various oxidizing agents, the various nitriding agents, and the various inert gases described above are used.
[0106] (4) Variations The substrate processing sequence in this embodiment can be modified as shown in the following modified examples. These modified examples can be combined as desired. Unless otherwise specified, the process procedure and process conditions in each step of each modified example can be the same as the process procedure and process conditions in each step of the above embodiment.
[0107] (Variation 1) As shown in the gas supply sequence below, steps A, B, C, and D may be performed in this order in each cycle.
[0108] (First raw material → Second raw material → Oxidizing agent → Nitriding agent) × n
[0109] The present modification also provides the same effect as the above-mentioned embodiment. In the present modification, the first layer having halogen termination is formed on the wafer 200 by supplying the first source material in advance. Since the first layer having halogen termination is unlikely to undergo a substitution reaction with the amino group contained in the second source material, the ratio of the first layer having halogen termination, which is likely to react with the N- and H-containing gas as the nitriding agent, becomes relatively larger than the ratio of the second layer formed by the second source material, and it becomes easier to increase the nitrogen concentration in the SiON film formed on the wafer 200 than in the above-mentioned embodiment.
[0110] (Variation 2) As shown in the gas supply sequence below, steps A, B, D, and C may be performed in this order in each cycle.
[0111] (First raw material → Second raw material → Nitriding agent → Oxidizing agent) × n
[0112] This modification also provides the same effect as the above-mentioned embodiment. In addition, in this modification, the reaction between the N- and H-containing gas and the first and second layers in step D occurs more easily than in the above-mentioned embodiment, so it is easier to adjust the nitrogen concentration in the SiON film formed on the wafer 200 to be relatively high compared to the above-mentioned embodiment in which the oxidizing agent is supplied in step C prior to step D. In other words, in order to adjust the nitrogen concentration in the SiON film formed on the wafer 200 to be lower, the above-mentioned embodiment and modification 1 are more suitable for supplying the oxidizing agent to the wafer 200 in step C prior to step D. In addition, in this modification, it is possible to increase the formation rate of the SiON film formed on the wafer 200 compared to the above-mentioned embodiment and modification 1.
[0113] (Variation 3) As shown in the gas supply sequence below, steps B, A, D, and C may be performed in this order in each cycle.
[0114] (2nd raw material → 1st raw material → nitriding agent → oxidizing agent) × n
[0115] This modification also provides the same effects as the above-mentioned embodiment. Also, in this modification, as in modification 2, it is easier to adjust the nitrogen concentration in the SiON film formed on the wafer 200 to be relatively high compared to the above-mentioned embodiment and modification 1. Also, in this modification, as in modification 2, it is possible to increase the formation rate of the SiON film formed on the wafer 200 compared to the above-mentioned embodiment and modification 1.
[0116] (Variation 4) As in the gas supply sequence shown below, a nitriding agent may be supplied (preflow) to the wafer 200 before the cycle is performed a predetermined number of times.
[0117] Nitriding agent → (second raw material → first raw material → oxidizing agent → nitriding agent) × n Nitriding agent → (first raw material → second raw material → oxidizing agent → nitriding agent) × n Nitriding agent → (second raw material → first raw material → nitriding agent → oxidizing agent) × n Nitriding agent → (first raw material → second raw material → nitriding agent → oxidizing agent) × n
[0118] In this modification, the same effect as that of the above-mentioned embodiment can be obtained. In addition, in this modification, by preflowing N and H-containing gas as a nitriding agent, H termination (NH termination) that becomes an adsorption site is formed on the surface of the wafer 200 before the cycle is performed, and it becomes possible to make the surface of the wafer 200 and the first source material or the second source material easily react with each other in step A or step B. This promotes the formation of a Si-containing layer on the wafer 200 after the cycle starts, and makes it possible to shorten the incubation time when forming a SiON film on the wafer 200.
[0119] The supply conditions of the nitriding agent in the preflow and the supply conditions of the nitriding agent in step D may be different. Furthermore, the nitriding agent in the preflow and the nitriding agent in step D may use the same type of gas or different types of gas.
[0120] (Variation 5) In each cycle, the period during which the first raw material is supplied in step A and the period during which the second raw material is supplied in step B may be at least partially overlapped. In this modification, the same effects as those of the above-mentioned embodiment can be obtained. In addition, in this modification, it is possible to shorten the cycle time and improve the throughput of the film forming process.
[0121] (Variation 6) In step B, the supply of the second source material may be stopped before the adsorption reaction of the second source material on the surface of the wafer 200 becomes saturated. By adjusting the supply time of the second source material in a state in which the adsorption reaction of the second source material is not saturated (unsaturated state), it becomes possible to adjust the ratio of Si and oxygen contained in the Si-containing layer formed in step B and control the nitrogen concentration in the SiON film formed on the wafer 200. For example, in a state where the adsorption reaction of the second source is not saturated, the supply time of the second source in step B can be shortened, thereby making it possible to adjust the nitrogen concentration in the SiON film formed on the wafer 200 in a direction to increase it.
[0122] <Other Aspects of the Disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.
[0123] The oxidizing agent or the nitriding agent may be supplied after being excited into plasma. In these cases, the processing procedures and processing conditions may be the same as those in steps C and D of the above-mentioned embodiment. Even in these cases, the same effects as those of the above-mentioned embodiment can be obtained.
[0124] The predetermined element constituting the central atom X contained in the raw material may be, for example, a metal element such as aluminum (Al), titanium (Ti), zirconium (Zr), hafnium (Hf), or lanthanum (La). The predetermined element may be, for example, a Group 14 element like Si, or a Group 4 element. When the predetermined element is a Group 14 element or a Group 4 element, the second raw material preferably has a molecular structure in which an amino group is bonded to one bond of the atom of the predetermined element, and alkoxy groups are bonded to the remaining three bonds. When a raw material containing these metal elements is used as the predetermined element, it is possible to form a metal oxynitride film such as an aluminum oxynitride film (AlON) film, a titanium oxynitride film (TiON film), a zirconium oxynitride film (ZrON film), a hafnium oxynitride film (HfON film), or a lanthanum oxynitride film (LaON film) on the wafer 200. The process procedure and process conditions in these cases may be the same as those in the above-mentioned embodiment. In these cases, the same effects as those in the above-mentioned embodiment can be obtained.
[0125] It is preferable that the recipes used for each process are prepared individually according to the process contents and stored in the storage device 121c via an electric communication line or an external storage device 123. Then, when starting each process, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the process contents from among the multiple recipes stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using a single substrate processing device. It is also possible to reduce the burden on the operator and quickly start each process while avoiding operational errors.
[0126] The above-mentioned recipes may not only be newly created, but may also be prepared by modifying an existing recipe that has already been installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe has been recorded. In addition, an existing recipe that has already been installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus.
[0127] In the above-mentioned embodiment, an example of forming a film using a batch-type substrate processing apparatus that processes multiple substrates at a time has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a single-wafer type substrate processing apparatus that processes one or several substrates at a time. Also, in the above-mentioned embodiment, an example of forming a film using a substrate processing apparatus having a hot-wall type processing furnace has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a substrate processing apparatus having a cold-wall type processing furnace.
[0128] When using these substrate processing apparatuses, each process can be performed using the same processing procedures and processing conditions as those in the above-mentioned aspects and modifications, and the same effects as those in the above-mentioned aspects and modifications can be obtained.
[0129] The above-mentioned aspects and modifications may be used in appropriate combination. The processing procedures and processing conditions in such a case may be the same as those in the above-mentioned aspects and modifications. EXAMPLES
[0130] As Sample 1, the above-mentioned substrate processing apparatus was used to supply TMDMAS gas as the second source, HCDS gas as the first source, O2 gas as the oxidizing agent, and NH3 gas as the nitriding agent in this order to the wafer, and the cycle was repeated a predetermined number of times to form a SiON film on the wafer. The processing conditions in each step were set to predetermined conditions within the processing condition range described in the above-mentioned embodiment.
[0131] For sample 2, the above-mentioned substrate processing apparatus was used to perform a cycle of supplying the first source material, the second source material, the oxidizing agent, and the nitriding agent to the wafer in this order a predetermined number of times to form a SiON film on the wafer. The processing conditions in each step and the number of cycles performed were the same as those used for producing sample 1.
[0132] For sample 3, the above-mentioned substrate processing apparatus was used to perform a cycle of supplying the first source material, the oxidizing agent, and the nitriding agent to the wafer in this order a predetermined number of times to form a SiON film on the wafer. The processing conditions in each step and the number of times the cycle was performed were the same as those used for producing sample 1.
[0133] Then, the wafer-wide average thickness (Thickness), refractive index (RI), and nitrogen concentration (N concentration) of the SiON film of each sample were measured. The refractive index was used as an index of the Si concentration in the SiON film, and the higher the refractive index, the higher the Si concentration. As a result, it was confirmed that the SiON films of samples 1 and 2, which were fabricated using both the first and second raw materials, had a lower N concentration than the SiON film of sample 3, which was fabricated using only the first raw material without using the second raw material as a raw material. It was also confirmed that the SiON film of sample 1, which was fabricated by supplying the second raw material, the first raw material, the oxidizing agent, and the nitriding agent in this order, had a lower N concentration than the SiON film of sample 2, which was fabricated by supplying the first raw material, the second raw material, the oxidizing agent, and the nitriding agent in this order. [Explanation of symbols]
[0134] 200 wafers (substrates)
Claims
1. (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a)(b)(c)(d), (b)(a)(c)(d), or (a)(b)(d)(c) a predetermined number of times in any one of the following orders, thereby forming a film on the substrate, the film containing the predetermined element, oxygen, and nitrogen.
2. (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a step of forming a film containing the predetermined element, oxygen, and nitrogen on the substrate by performing a cycle including the steps of: supplying the nitriding agent to the substrate before performing the cycle the predetermined number of times; A substrate processing method comprising the steps of:
3. 2. The substrate processing method according to claim 1, wherein the second source material has a molecular structure including an alkoxy group bonded to an atom of the predetermined element.
4. (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source containing the predetermined element and oxygen, the second source having a molecular structure different from that of the first source and a molecular structure in which an amino group is bonded to at least one bond of an atom of the predetermined element and an alkoxy group is bonded to the remaining bond; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a predetermined number of cycles to form a film containing the predetermined element, oxygen and nitrogen on the substrate.
5. 5. The substrate processing method according to claim 4, wherein the predetermined element is silicon.
6. (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source having a molecular structure different from that of the first source and including an alkoxy group bonded to an atom of the predetermined element, the second source including the predetermined element and oxygen; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a step of forming a film containing the predetermined element, oxygen and nitrogen on the substrate by performing a cycle including the steps of: In (b), a substrate processing method is provided in which the second source material is supplied to the substrate under conditions in which the alkoxy group is not detached from the atom of the specified element, and at least one other group bonded to the atom of the specified element is detached, and the atom of the specified element in a state in which the at least one group is detached and the bond with the alkoxy group is maintained is adsorbed onto the surface of the substrate.
7. 2. The substrate processing method according to claim 1, wherein the first source material has a molecular structure containing a halogen element bonded to an atom of the predetermined element.
8. (a) supplying a first source material containing a predetermined element to a substrate; (b) supplying to the substrate a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen; (c) supplying an oxidizing agent to the substrate; (d) supplying a nitriding agent to the substrate; a step of forming a film containing the predetermined element, oxygen and nitrogen on the substrate by performing a cycle including the steps of: A substrate processing method, comprising: setting at least one of a ratio of a supply time of the second source in (b) to a supply time of the first source in (a) to a pressure of the space in which the substrate is present in (b) to a pressure of the space in which the substrate is present in (a) to a pressure of the space in which the substrate is present in (b) to a supply flow rate of the second source in (b) to a supply flow rate of the first source in (a) so that a concentration of nitrogen to be contained in the film is a predetermined value.
9. 2. The substrate processing method according to claim 1, wherein in (a), the supply of the second source is continued until an adsorption reaction of the second source onto the surface of the substrate is saturated.
10. 2. The substrate processing method according to claim 1, wherein in (a), the supply of the second source is stopped before an adsorption reaction of the second source onto the surface of the substrate becomes saturated.
11. A method for manufacturing a semiconductor device, comprising a substrate processing method step according to any one of claims 1 to 10.
12. A method for manufacturing a semiconductor device comprising: a first source supply system for supplying a first source containing a predetermined element to a substrate; a second source supply system that supplies a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen to the substrate; an oxidant supply system for supplying an oxidant to the substrate; a nitriding agent supply system for supplying a nitriding agent to the substrate; a control unit configured to be capable of controlling the first source supply system, the second source supply system, the oxidizing agent supply system, and the nitriding agent supply system so as to perform a process of forming a film containing the predetermined element, oxygen, and nitrogen on the substrate by performing a cycle including: (a) a process of supplying the first source to the substrate; (b) a process of supplying the second source to the substrate; (c) a process of supplying the oxidizing agent to the substrate; and (d) a process of supplying the nitriding agent to the substrate a predetermined number of times in any one of the orders of (a)(b)(c)(d), (b)(a)(c)(d), and (a)(b)(d)(c); A substrate processing apparatus comprising:
13. A method for manufacturing a semiconductor device comprising: a first source supply system for supplying a first source containing a predetermined element to a substrate; a second source supply system that supplies a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen to the substrate; an oxidant supply system for supplying an oxidant to the substrate; a nitriding agent supply system for supplying a nitriding agent to the substrate; a control unit configured to be capable of controlling the first raw material supply system, the second raw material supply system, the oxidizing agent supply system, and the nitriding agent supply system so as to perform a process of forming a film containing the predetermined element, oxygen, and nitrogen on the substrate by performing a cycle including: (a) a process of supplying the first raw material to the substrate; (b) a process of supplying the second raw material to the substrate; (c) a process of supplying the oxidizing agent to the substrate; and (d) a process of supplying the nitriding agent to the substrate a predetermined number of times, and a process of supplying the nitriding agent to the substrate before performing the cycle the predetermined number of times; A substrate processing apparatus comprising:
14. A method for manufacturing a semiconductor device comprising: a first source supply system for supplying a first source containing a predetermined element to a substrate; a second source supply system for supplying to the substrate a second source having a molecular structure different from that of the first source, and having a molecular structure in which an amino group is bonded to at least one bond of an atom of the predetermined element and an alkoxy group is bonded to the remaining bond, the second source containing the predetermined element and oxygen; an oxidant supply system for supplying an oxidant to the substrate; a nitriding agent supply system for supplying a nitriding agent to the substrate; a control unit configured to be capable of controlling the first source supply system, the second source supply system, the oxidizing agent supply system, and the nitriding agent supply system so as to perform a process of forming a film containing the predetermined element, oxygen, and nitrogen on the substrate by performing a cycle including: (a) a process of supplying the first source to the substrate; (b) a process of supplying the second source to the substrate; (c) a process of supplying the oxidizing agent to the substrate; and (d) a process of supplying the nitriding agent to the substrate a predetermined number of times; A substrate processing apparatus comprising:
15. a first source supply system that supplies a first source containing a predetermined element to the substrate; a second source supply system that supplies to the substrate a second source having a molecular structure different from that of the first source and including an alkoxy group bonded to an atom of the predetermined element, the second source including the predetermined element and oxygen; an oxidant supply system for supplying an oxidant to the substrate; a nitriding agent supply system for supplying a nitriding agent to the substrate; a control unit configured to be capable of controlling the first source supply system, the second source supply system, the oxidizing agent supply system, and the nitriding agent supply system so that a process of forming a film containing the predetermined element, oxygen, and nitrogen is performed on the substrate by performing a cycle including: (a) a process of supplying the first source to the substrate; (b) a process of supplying the second source to the substrate; (c) a process of supplying the oxidizing agent to the substrate; and (d) a process of supplying the nitriding agent to the substrate a predetermined number of times, and in (b), the second source is supplied to the substrate under a condition in which the alkoxy group is not detached from the atom of the predetermined element, and at least one other group bonded to the atom of the predetermined element is detached, and the atom of the predetermined element in a state in which the at least one group is detached and the bond with the alkoxy group is maintained is adsorbed to a surface of the substrate; A substrate processing apparatus comprising:
16. A method for manufacturing a semiconductor device comprising: a first source supply system for supplying a first source containing a predetermined element to a substrate; a second source supply system that supplies a second source having a molecular structure different from that of the first source and containing the predetermined element and oxygen to the substrate; an oxidant supply system for supplying an oxidant to the substrate; a nitriding agent supply system for supplying a nitriding agent to the substrate; a control unit configured to be capable of controlling the first source supply system, the second source supply system, the oxidizing agent supply system, and the nitriding agent supply system so as to perform a process of forming a film containing the predetermined element, oxygen, and nitrogen on the substrate by performing a cycle including: (a) a process of supplying the first source to the substrate; (b) a process of supplying the second source to the substrate; (c) a process of supplying the oxidizing agent to the substrate; and (d) a process of supplying the nitriding agent to the substrate a predetermined number of times; having A substrate processing apparatus in which at least any one of a ratio of a supply time of the second source in (b) to a supply time of the first source in (a) to a pressure of the space in which the substrate is present in (b) to a pressure of the space in which the substrate is present in (a) to a pressure of the space in which the substrate is present in (b) to a supply flow rate of the first source in (a) is set so that a concentration of nitrogen to be contained in the film is a predetermined value.
17. A procedure for carrying out the steps of the substrate processing method according to any one of claims 1 to 10, A program that is executed by a computer in a substrate processing apparatus.
Citation Information
Patent Citations
Method of manufacturing semiconductor device and substrate processing apparatus
JP2011061218A
Substrate processing apparatus, method of manufacturing semiconductor device and semiconductor device
JP2012104720A
Method of manufacturing semiconductor device, substrate processing device, and program
JP2017005095A
Semiconductor device manufacturing method, substrate processing apparatus and program
JP2018137356A
Material layer, semiconductor device including the same, and methods of fabricating the material layer and the semiconductor device
US20170117140A1