Polarizing plate and optical display device including the same

A polarizing plate with a protective coating layer using a thermosetting composition addresses the need for thinning and UV protection, ensuring structural integrity and minimizing damage to display panels.

JP7579978B2Active Publication Date: 2024-11-08ホアードサン ヘンシン(ウーシー) マテリアルズ カンパニーリミテッド
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023530915
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-23
Filing Date
2021-11-05
Publication Date
2024-11-08
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

The challenge is to create a polarizing plate that achieves thinning while providing effective UV protection and preventing bending and cracking, especially for display panels exposed to external ultraviolet light.

Method used

A polarizing plate design with a protective coating layer formed from a thermosetting composition containing an adhesive resin, isocyanate curing agent, and UV absorber, which includes a modulus of 10 MPa or more, ensuring UV protection and structural integrity.

Benefits of technology

The solution provides a thinner polarizing plate with enhanced UV protection, minimizing damage to display panels and suppressing bending and cracking due to thermal shock.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579978000008
    Figure 0007579978000008
  • Figure 0007579978000001
    Figure 0007579978000001
  • Figure 0007579978000002
    Figure 0007579978000002
Patent Text Reader

Abstract

The present application provides a polarizer, which includes: a protective coating layer formed on an upper surface of the polarizer; and a protective layer and an adhesive layer formed in this order on a lower surface of the polarizer, wherein the protective coating layer is formed of a thermosetting composition, and the polarizer has a modulus of about 10 MPa or more as measured by a microindenter on the surface of the protective coating layer. The polarizer also provides an optical display device including the polarizer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate and an optical display device including the same. [Background technology]

[0002] An optical display device includes a polarizing plate for the purpose of improving light efficiency, screen quality, etc. The polarizing plate includes a polarizer and a protective film formed on at least one surface of the polarizer. The polarizing plate may be laminated on an adherend after coating one surface of the protective film with a pressure-sensitive adhesive composition or laminating a pressure-sensitive adhesive film formed from the pressure-sensitive adhesive composition.

[0003] Recently, as the trend for optical display devices to be thinner continues, there is a trend for polarizing plates to be thinner as well. There are many methods for thinning polarizing plates, and recently, a method of using a protective coating layer as a protective layer for a polarizer instead of a protective film has been considered. Meanwhile, polarizing plates, especially polarizing plates on the viewing side, can be easily exposed to external ultraviolet light, and the ultraviolet light entering the polarizing plate can damage the polarizing plate's adherend, for example, a liquid crystal panel or an OLED panel. Therefore, a thinning effect and a UV blocking effect should be obtained at the same time.

[0004] The protective coating layer can provide a thin polarizing plate. However, the difference in thickness and physical properties between the protective layers laminated on the upper and lower surfaces of the polarizer can cause the polarizing plate to bend. In addition, since the protective coating layer is formed directly on the polarizer, it must prevent the polarizer from cracking under reliability conditions such as thermal shock.

[0005] The background art of the present invention is disclosed in JP 2013-072951 A and the like. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a polarizing plate having a thinning effect.

[0007] Another object of the present invention is to provide a polarizing plate that can contain a relatively excessive amount of UV absorber in a protective coating layer, thereby minimizing UV damage to a polarizer and a substrate to which the polarizing plate is attached, such as a display panel.

[0008] It is yet another object of the present invention to provide a polarizing plate which provides a barrier effect to a polarizer and suppresses bending of the polarizing plate. [Means for solving the problem]

[0009] One aspect of the present invention relates to a polarizing plate.

[0010] 1. A polarizing plate includes a polarizer; a protective coating layer formed on an upper surface of the polarizer; and a protective layer and an adhesive layer formed in sequence on a lower surface of the polarizer, the protective coating layer being formed of a thermosetting composition, and the polarizing plate has a modulus of about 10 MPa or more as measured by a microindenter on the protective coating layer surface.

[0011] In 2.1, the protective coating layer can be formed directly on the top surface of the polarizer.

[0012] In 3.1 to 2, only the protective coating layer may be laminated on the upper surface of the polarizer as a protective layer for the polarizer.

[0013] In 4.1 to 3, the thermosetting composition may include an adhesive resin, an isocyanate-based curing agent, and a UV absorber.

[0014] In 5.4, the UV absorbent may be included in an amount of about 0.1 parts by weight to about 10 parts by weight based on 100 parts by weight of the adhesive resin.

[0015] In 6.4, the UV absorber may have a maximum absorption wavelength of 390 nm or more.

[0016] In 7.4, the UV absorber may include one or more of an indole type and a triazine type.

[0017] In 8.1 to 7, the adhesive resin may be a monomer mixture including a (meth)acrylic monomer having an alkyl group and a (meth)acrylic monomer having a hydroxyl group, and at least one of the monomers included in the monomer mixture may include a (meth)acrylic copolymer of the monomer mixture including a monomer having a homopolymer glass transition temperature of about 50° C. or higher.

[0018] In 9.8, the monomer having a homopolymer glass transition temperature of about 50° C. or higher may be contained in an amount of about 1% by weight to about 60% by weight in the monomer mixture.

[0019] In 10.8 to 9, the monomer having a homopolymer glass transition temperature of about 50° C. or higher may include one or more of methyl methacrylate, t-butyl methacrylate, iso-propyl methacrylate, sec-butyl methacrylate, and isobornyl methacrylate.

[0020] In 11.8 to 10, the monomer mixture may contain about 85% by weight to about 99.9% by weight of the (meth)acrylic monomer having an alkyl group, and about 0.1% by weight to about 15% by weight of the (meth)acrylic monomer having a hydroxyl group.

[0021] In 12.8 to 11, the monomer mixture may further include a monomer having a carboxylic acid group.

[0022] In 13.8 to 12, the monomer mixture may contain about 70% by weight to about 98% by weight of the (meth)acrylic monomer having an alkyl group, about 0.1% by weight to about 15% by weight of the (meth)acrylic monomer having a hydroxyl group, and about 0.1% by weight to about 15% by weight of the monomer having a carboxylic acid group.

[0023] In 14.1 to 13, the isocyanate-based curing agent may include a polyisocyanate-based curing agent containing a urethane bond and a plurality of alkylene group-containing units having two or more carbon atoms.

[0024] In 15.1 to 14, the isocyanate-based curing agent may include a polyisocyanate curing agent having a plurality of units of the following chemical formula 1:

[0025] [ka]

[0026] (In the above Chemical Formula 1, * is a linking site, R 1 , R 2 are the same or different and are divalent aliphatic hydrocarbon groups having 2 to 20 carbon atoms. In 16.1 to 15, the adhesive resin may contain 100 parts by weight, about 10 to about 40 parts by weight of the isocyanate-based curing agent, and about 0.1 to about 10 parts by weight of the UV absorber.

[0027] In either 17.1 or 16, the polarizing plate may have a light transmittance of about 3% or less at a wavelength of 380 nm or 405 nm, respectively.

[0028] Another aspect of the invention relates to an optical display device.

[0029] 18. An optical display device comprises the polarizing plate of the present invention.

[0030] In 19.18, the optical display device may include the polarizer, a transparent adhesive film laminated on an upper surface of the polarizer, and an OLED panel formed on a lower surface of the polarizer.

[0031] In 20.19, a cover glass may be further laminated on the upper surface of the transparent adhesive film. Effect of the Invention

[0032] The present invention provides a polarizing plate having a thinning effect.

[0033] The present invention provides a polarizing plate that minimizes UV damage to a polarizer and a substrate to which the polarizing plate is attached, such as a display panel, by allowing a relatively large amount of UV absorber to be included in the protective coating layer.

[0034] The present invention provides a polarizing plate that provides a barrier effect to the polarizer and suppresses bending of the polarizing plate. [Brief description of the drawings]

[0035] [Figure 1] FIG. 1 is a cross-sectional view of a polarizing plate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] [First Mode for Carrying Out the Invention] Hereinafter, the present application will be described in more detail with reference to the accompanying drawings. However, the technology disclosed in the present application is not limited to the embodiments described herein and may be embodied in other forms. However, the embodiments described herein are provided so that the disclosed content will be thorough and complete, and so that the concept of the present application will be fully conveyed to those skilled in the art.

[0037] In the drawings, the dimensions of the width, thickness, etc. of each device are somewhat exaggerated in order to clearly show the components of the device, and the dimensions of the width, thickness, etc. of the components of the present invention are not limited by the scope of the present invention. The same reference numerals in multiple drawings refer to substantially the same components.

[0038] In this specification, "upper" and "lower" are defined with reference to the drawing, and "upper" may be changed to "lower" and "lower" to "upper" depending on the viewing angle, and "on" may include not only directly on but also cases where other structures are interposed. Meanwhile, "directly on", "directly on", or "directly formed on" indicates that no other structures such as intermediates are interposed.

[0039] In this specification, "modulus" measured from the plane of the protective coating layer relative to the polarizing plate means elastic modulus.

[0040] In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0041] In this specification, the "weight average molecular weight" may be a value determined by gel permeation chromatography in terms of polystyrene.

[0042] In this specification, "substituted" in "substituted or unsubstituted" means that one or more hydrogen atoms of the functional group are substituted with an ester group having an alkyl group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a hydroxyl group, or the like.

[0043] In this specification, when describing a numerical range, "X to Y" means X or more and Y or less (X≦and≦Y).

[0044] The polarizing plate of the present invention provides a thin polarizing plate by forming a protective coating layer instead of a protective layer on one side of the polarizer. The polarizing plate of the present invention provides a thin polarizing plate by forming the protective coating layer from a heat-curable composition on the outermost side of the polarizer where external light is incident, and can contain a relatively large amount of UV absorbent compared to a photo-curable composition, thereby minimizing damage caused by UV to the polarizer and the substrate of the polarizing plate, for example, a display panel. The polarizing plate of the present invention provides a barrier effect for the polarizer and also provides an effect of suppressing bending of the polarizing plate by having a modulus of about 10 MPa or more on the surface of the protective coating layer measured by a microindenter.

[0045] The polarizing plate of the present invention includes a polarizer; a protective coating layer formed on an upper surface of the polarizer; and a protective layer and an adhesive layer formed in this order on a lower surface of the polarizer, the protective coating layer being formed of a thermosetting composition, and the polarizing plate has a modulus of 10 MPa or more as measured by a microindenter on the surface of the protective coating layer.

[0046] Hereinafter, a polarizing plate according to an embodiment of the present invention will be described with reference to FIG.

[0047] Referring to FIG. 1, the polarizing plate includes a polarizer 100, a protective coating layer 200 formed on an upper surface of the polarizer 100, a protective layer 300 formed on a lower surface of the polarizer 100, and an adhesive layer 400.

[0048] The polarizing plate has a modulus of about 10 MPa or more as measured by a microindenter on the surface of the protective coating layer. In this range, a barrier effect is provided for the polarizer, and cracks in the polarizer caused by thermal shock can be suppressed, and bending can be suppressed. The present invention controls the modulus of the protective coating layer measured by a microindenter on the surface of the protective coating layer to about 10 MPa or more by directly forming the protective coating layer on the polarizer, thereby suppressing cracks in the polarizer caused by thermal shock, reducing the possibility of decolorization of heterochromatic dyes including iodine in the polarizer, and suppressing bending of the polarizing plate caused by the difference in thickness between the protective coating layer formed on the upper surface of the polarizer and the protective layer and adhesive layer formed on the lower surface of the polarizer.

[0049] Specifically, the modulus may be, for example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40 MPa, about 10 MPa to about 40 MPa, and more specifically, about 10 MPa to about 30 MPa.

[0050] Protective Coating Layer The protective coating layer 200 may be located at a portion of the polarizing plate where external light is first incident. That is, only the protective coating layer 200 may be laminated as a protective layer on the upper surface of the polarizer 100. As described below in detail, the protective coating layer may contain a UV absorber to effectively block UV rays from external light and prevent UV damage to the polarizer and the polarizing plate to which it is attached.

[0051] The protective coating layer 200 may be formed directly on the upper surface of the polarizer 100. The term "directly formed" means that there is no adhesive or bonding layer between the protective coating layer and the polarizer.

[0052] The protective coating layer 200 may have a thickness of about 15 μm or less, specifically, more than about 0 μm to about 15 μm or less, in which case the effect of making the polarizing plate thinner can be obtained.

[0053] The protective coating layer 200 may be optically transparent and have a total light transmittance of about 90% or more, specifically about 90% to about 100%, in the visible light region, for example, at a wavelength of 550 nm, in which case the protective coating layer 200 may be used in the polarizing plate without affecting the light emitted from the polarizing plate.

[0054] The protective coating layer 200 may be formed of a thermosetting composition including an adhesive resin, an isocyanate-based curing agent, and a UV absorber. Since the protective coating layer is formed of a thermosetting composition, a relatively large amount of UV absorber can be included in the protective coating layer, so that UV damage to the polarizer and the substrate of the polarizing plate, for example, a display panel, can be minimized.

[0055] The tackifying resin can increase the modulus measured by a microindenter at the surface of the protective coating layer against the polarizing plate, and can improve adhesion to the polarizer.

[0056] The adhesive resin is a monomer mixture containing a (meth)acrylic monomer having an alkyl group and a (meth)acrylic monomer having a hydroxyl group, and at least one of the monomers contained in the monomer mixture is a monomer having a homopolymer glass transition temperature of 50°C or higher, which is more preferable as a (meth)acrylic copolymer.

[0057] The modulus of the present invention measured by a microindenter on the surface of the protective coating layer of the polarizing plate can be achieved by including at least one of the monomers included in the monomer mixture having a homopolymer glass transition temperature of about 50° C. or more. Specifically, the monomer mixture may include a monomer having a homopolymer glass transition temperature of, for example, about 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150, 155, 160, 165, 170, 175, 180, 185, 190, 195, 200° C., about 50° C. to about 200° C., more specifically, about 80° C. to about 150° C.

[0058] The monomer having a homopolymer glass transition temperature of about 50° C. or higher is about 1% by weight to about 60% by weight of the monomer mixture, for example, It may be included in an amount of 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60% by weight, specifically about 10% to about 60% by weight, about 20% to about 60% by weight, about 30% to about 60% by weight, more specifically about 40% to about 50% by weight. This range may help the polarizing plate to reach a modulus measured by a microindenter on the surface of the protective coating layer.

[0059] The (meth)acrylic monomer having an alkyl group may include one or more of (meth)acrylic acid esters having a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms. For example, the (meth)acrylic monomer having an alkyl group may include one or more of methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, iso-butyl (meth)acrylate, sec-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, iso-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and isobornyl (meth)acrylate, but is not limited thereto.

[0060] Among (meth)acrylic monomers having an alkyl group, monomers having a homopolymer glass transition temperature of about 50° C. or higher can be selected and used by referring to a product catalog, etc. For example, among (meth)acrylic monomers having an alkyl group, monomers having a homopolymer glass transition temperature of about 50° C. or higher can include one or more of methyl methacrylate, t-butyl methacrylate, iso-propyl methacrylate, sec-butyl methacrylate, and isobornyl methacrylate, but are not limited thereto.

[0061] The (meth)acrylic monomer having a hydroxyl group can include one or more of a (meth)acrylic monomer having a hydroxyl group and a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, a (meth)acrylic monomer having a hydroxyl group and a substituted or unsubstituted alicyclic group having 3 to 20 carbon atoms, and a (meth)acrylic monomer having a hydroxyl group and a substituted or unsubstituted aromatic group having 6 to 20 carbon atoms. For example, the (meth)acrylic monomer having a hydroxyl group can include one or more of 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 1-chloro-2-hydroxypropyl (meth)acrylate, diethylene glycol mono(meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, 4-hydroxycyclopentyl (meth)acrylate, and 4-hydroxycyclohexyl (meth)acrylate.

[0062] For example, the monomer having a hydroxyl group may include, but is not limited to, one or more monomers having a homopolymer glass transition temperature of about 20° C. or higher. For example, the monomer having a hydroxyl group may include, but is not limited to, one or more monomers having a homopolymer glass transition temperature of about 20° C. or higher, for example, about 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80° C., specifically, about 20° C. to about 80° C. The monomer having a hydroxyl group may include, but is not limited to, 2-hydroxyethyl methacrylate, etc.

[0063] The monomer mixture may further include a monomer having a carboxylic acid group. The monomer having a carboxylic acid group may include, but is not limited to, (meth)acrylic acid, fumaric acid, itaconic acid, etc.

[0064] In one embodiment, the monomer mixture may contain about 85% by weight to about 99.9% by weight, for example, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 99.9% by weight, specifically, about 90% by weight to about 95% by weight, and about 0.1% by weight to about 15% by weight, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15% by weight, specifically, about 1% by weight to about 10% by weight, of a (meth)acrylic monomer having an alkyl group. The modulus and degree of cure of the barrier properties can be adjusted within the above ranges.

[0065] In another specific example, the monomer mixture contains about 70% by weight to about 98% by weight, for example, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98% by weight, specifically, about 85% by weight to about 90% by weight of a (meth)acrylic monomer having an alkyl group, and about The monomer may be about 0.1% by weight to about 15% by weight, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15% by weight, specifically about 1% by weight to about 10% by weight, and a monomer having a carboxylic acid group may be about 0.1% by weight to about 15% by weight, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15% by weight, specifically about 1% by weight to about 10% by weight. In the above range, additional hardening properties may be imparted to improve modulus properties.

[0066] The monomer mixture may further include at least one of (meth)acrylamide, acrylonitrile, benzyl methacrylate, cyclohexyl methacrylate, N,N-dimethylacrylamide, styrene, and dihydrodicyclopentadienyl acrylate (DCPA) as a monomer having a homopolymer glass transition temperature of about 50° C. or higher, but is not limited thereto.

[0067] The (meth)acrylic copolymer can be produced by polymerizing the monomer mixture by a conventional polymerization method. The polymerization method can include conventional methods known to those skilled in the art. For example, the (meth)acrylic copolymer can be produced by adding an initiator to the monomer mixture, followed by conventional polymerization, such as suspension polymerization, emulsion polymerization, solution polymerization, etc. The polymerization temperature can be 60°C to 70°C, and the polymerization time can be 6 hours to 8 hours. The initiator can be a conventional one including an iso-based polymerization initiator and / or a peroxide such as benzoyl peroxide or acetyl peroxide.

[0068] The adhesive resin, specifically, the (meth)acrylic copolymer, may have a weight average molecular weight of about 200,000 or more, for example, 200,000, 250,000, 300,000, 350,000, 400,000, 450,000, 500,000, 550,000, 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, or 1,000,000, specifically, 200,000 to 1,000,000, and more specifically, 100,000 to 300,000. Within the above range, the effects of the present invention can be easily achieved.

[0069] The isocyanate-based hardener can harden the adhesive resin to improve the crosslinking degree of the protective coating layer and increase the adhesion to the polarizer. The isocyanate-based hardener can heat-cure the adhesive resin to form the protective coating layer as a thermal hardener. As such, the protective coating layer of the present invention is formed of a thermosetting composition, and even if it contains an excessive amount of a UV absorber described below, the protective coating layer can be realized without problems with the crosslinking degree of the protective coating layer.

[0070] The isocyanate-based curing agent may be included in an amount of about 10 parts by weight to about 40 parts by weight, for example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40 parts by weight, specifically, about 15 parts by weight to about 30 parts by weight, based on 100 parts by weight of the adhesive resin. Within this range, the crosslinking degree and adhesion of the protective coating layer may be improved, and flexibility may be improved.

[0071] The isocyanate-based curing agent may include a polyisocyanate-based curing agent containing a urethane bond and a plurality of alkylene group-containing units having 2 or more carbon atoms. The polyisocyanate-based curing agent may be useful for curing the adhesive resin to reach the modulus. The "alkylene group" may be a linear alkylene group having 6 to 20 carbon atoms, such as, but not limited to, a hexamethylene group, a dodecamethylene group, or a trimethylhexamethylene group.

[0072] In one specific example, the isocyanate-based curing agent may include an adduct of a polyisocyanate-based curing agent having a plurality of urethane-modified linear alkylene group-containing units having 2 or more carbon atoms. For example, the polyisocyanate-based curing agent may be an aliphatic polyisocyanate containing urethane. In this case, the aliphatic polyisocyanate curing agent may be a C4 to C20 diisocyanate, such as tetramethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, trimethylhexamethylene diisocyanate including 2,2,4-trimethylhexamethylene diisocyanate, etc. The urethane-modified polyisocyanate-based curing agent may be used in commercially available products.

[0073] In one embodiment, the isocyanate-based curing agent may include a polyisocyanate curing agent having a unit of the following formula 1. The curing agent preferably has a plurality of structural units of the following formula 1:

[0074] [ka]

[0075] (In the above Chemical Formula 1, * is a linking site, R 1 , R 2 are the same or different and are divalent aliphatic hydrocarbon groups having 2 to 20 carbon atoms. The curing agent may be synthesized by methods known to those skilled in the art or may be a commercially available product, such as AE 700-100 (Asahi Kasei Corporation).

[0076] The UV absorbent is contained in the protective coating layer and reduces the amount of ultraviolet light incident on the polarizing plate from external light, thereby preventing damage caused by UV rays to the polarizer and the substrate (e.g., display panel) to which the polarizing plate is attached.

[0077] The UV absorbent may have a maximum absorption wavelength of about 390 nm or more, specifically, about 390 nm or more and about 400 nm or less, more specifically, more than about 390 nm and less than about 400 nm. In this range, outside light with a wavelength of 420 nm or less, 400 nm to 420 nm, or 405 nm or less is sufficiently absorbed to reduce UV transmittance, thereby preventing damage to the polarizer and the adherend of the polarizing plate.

[0078] The "maximum absorption wavelength" refers to the wavelength showing the maximum absorption peak, i.e., the wavelength showing the maximum absorbance in the wavelength-dependent absorbance curve. The "absorbance" can be measured by a conventional method known to those skilled in the art.

[0079] Through this, the polarizing plate may have a light transmittance of about 3% or less at a wavelength of 380 nm, specifically about 0% to about 3%, or a light transmittance of about 3% or less at a wavelength of 405 nm, specifically about 0% to about 3%. In particular, the polarizing plate of the present invention can block even UV damage to the polarizer by making the light transmittance at a wavelength of 380 nm about 3% or less.

[0080] In one specific example, the UV absorbent may include an absorbent having a melting point of about 100° C. or higher, specifically, about 140° C. to about 220° C., and being in a solid phase at room temperature.

[0081] The UV absorber may include at least one of an indole absorber and a triazine absorber having the maximum absorption wavelength. In one embodiment, the indole absorber may include a compound represented by the following formula 2:

[0082] [ka]

[0083] (In the above Chemical Formula 2, R 1 is hydrogen or a substituted or unsubstituted C1 to C10 alkyl group; R 2 is hydrogen or a substituted or unsubstituted C6 to C20 aryl group; R 3is hydrogen or a substituted or unsubstituted C1 to C10 alkyl group; R 4 represents hydrogen, a cyano group (CN) or a substituted or unsubstituted C1-C10 alkyl group; R 5 is a cyano group or -(C=O)OR 6 (At this time, R 6 represents a substituted or unsubstituted C1 to C10 alkyl group or a substituted or unsubstituted C6 to C20 aryl group).

[0084] Specifically, R 1 is a C1 to C5 alkyl group, specifically, a methyl group, R 2 is a C6 to C10 aryl group, specifically a phenyl group, R 3 is hydrogen or an alkyl group having 1 to 5 carbon atoms, specifically, hydrogen, R 4 is a cyano group, R 5 is a cyano group or -(C=O)OR 6 (At this time, R 6 is a substituted or unsubstituted C1 to C5 alkyl group). More specifically, the compound of Chemical Formula 2 can include a compound of the following Chemical Formula 2-1 or 2-2:

[0085] [ka]

[0086] In one embodiment, the triazine-based absorber may include a compound of Formula 3:

[0087] [ka]

[0088] (In the above Chemical Formula 3, R 1 , R 2 , R 3 are each independently a substituted or unsubstituted hydroxyphenyl group.

[0089] The UV absorbent may be included in an amount of about 0.1 to about 10 parts by weight, for example, 0.1, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, or 10 parts by weight, specifically, about 1 to about 5 parts by weight, based on 100 parts by weight of the adhesive resin. Within this range, there are no problems such as UV blocking effect and elution of the UV absorbent from the protective coating layer.

[0090] The composition may further contain a conventional heat curing agent known to those skilled in the art in addition to the isocyanate-based curing agent.

[0091] For example, the thermal curing agent may further include one or more of a carbodiimide-based curing agent, a metal chelate-based curing agent, an aziridine-based curing agent, and an epoxy-based curing agent. The curing agent may be included in an amount of about 0.001 to about 5 parts by weight, for example, about 0.01 to about 1 part by weight, based on 100 parts by weight of the adhesive resin. This range may be useful for forming a protective coating layer.

[0092] The composition may further comprise a silane coupling agent.

[0093] The silane coupling agent can increase the adhesion of the protective coating layer to the polarizer. The silane coupling agent can include a typical silane coupling agent known to those skilled in the art. For example, the silane coupling agent can include, but is not limited to, an epoxy group-containing silane coupling agent such as glycidoxypropyltrimethoxysilane, glycidoxypromethyldimethoxysilane, etc.

[0094] The silane coupling agent may be contained in an amount of about 0.01 to about 5 parts by weight, for example, about 0.1 to about 2.5 parts by weight, based on 100 parts by weight of the adhesive resin. In this range, the adhesive strength to the polarizer may be increased.

[0095] The composition may further include a crosslinking catalyst. The crosslinking catalyst may increase the degree of crosslinking of the protective coating layer produced from the composition. The crosslinking catalyst may include one or more of a metal or a metal-containing compound. Specifically, the crosslinking catalyst may include one or more of a tin-containing compound, a zinc-containing compound, a titanium compound, and a bismuth compound. More specifically, the crosslinking catalyst may include one or more of dibutyltin dilaurate and tin dimaleate.

[0096] The crosslinking catalyst may be included in an amount of 0.01 to 1.5 parts by weight based on 100 parts by weight of the adhesive resin. Within this range, the degree of crosslinking may be increased and moisture penetration may be suppressed.

[0097] The composition may further include an additive. The additive may provide additional functions to the protective coating layer. Specifically, the additive may include at least one of a reaction inhibitor, an adhesion improver, a thixotropic agent, a conductivity imparting agent, a pigment adjuster, a stabilizer, an antioxidant, and a leveling agent, but is not limited thereto.

[0098] The composition may further contain a common solvent to improve coatability, for example, a ketone solvent such as methyl ethyl ketone or isobutyl ketone, but is not limited thereto.

[0099] The protective coating layer 200 can be formed by coating the composition on a polarizer or a release film to a predetermined thickness, and then heat curing the composition at 90° C. to 100° C. for 1 to 3 minutes.

[0100] Polarizer The polarizer 100 may include a polarizer made of a polyvinyl alcohol-based resin film. Specifically, the polarizer may be a polyvinyl alcohol-based polarizer in which one or more of iodine and heterochromatic dyes are adsorbed on a polyvinyl alcohol-based resin film, or a polyene-based polarizer manufactured by dehydrating a polyvinyl alcohol-based resin film.

[0101] The polarizer 100 may have a thickness of about 5 μm to about 30 μm, specifically, about 5 μm to about 20 μm. When the thickness is in this range, the polarizer 100 can be used in a polarizing plate, and the effect of making the polarizing plate thinner can be realized.

[0102] protective layer The protective layer 300 may be formed on the lower surface of the polarizer 100 to protect the polarizer. The protective layer may include an optically transparent polymer film or a liquid crystal layer.

[0103] In one embodiment, the protective layer 300 is an optically transparent resin film, and may include one or more of cellulose ester-based resins including triacetyl cellulose (TAC), cyclic polyolefin-based resins including amorphous cyclic olefin polymer (COP), (meth)acrylic-based resins, poly(meth)acrylate-based resins, polycarbonate (PC)-based resins, polyester-based resins including polyethylene terephthalate (PET), polyestersulfone-based resins, polysulfone-based resins, polyamide-based resins, polyimide-based resins, acyclic polyolefin-based resins, polyarylate-based resins, polyvinyl alcohol-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, and acrylic-based resins.

[0104] The protective layer 300 may have a retardation in a predetermined range in consideration of the function of the polarizing plate. For example, the protective layer 300 may have an in-plane retardation (Re) of about 100 nm to about 350 nm at a wavelength of 550 nm. The protective layer 300 may be a laminate of two or more protective layers having the above-mentioned in-plane retardation. In this specification, the "in-plane retardation (Re)" may be calculated by Re=(nx-ny)×d (nx and ny are the refractive indexes of the protective layer in the slow axis direction and the fast axis direction, respectively, and d is the thickness of the protective layer (unit: nm)).

[0105] The protective layer 300 may be thinner or thicker than the protective coating layer. Specifically, the protective layer may have a thickness of about 0.1 μm to about 200 μm, specifically about 10 μm to about 150 μm, and more specifically about 20 μm to about 100 μm. A thickness in the above range may be used in a polarizing plate.

[0106] Although not shown in Fig. 1, the protective layer 300 may be attached to the polarizer by an adhesive layer. For example, the adhesive layer may be formed of one or more of a water-based adhesive and a photocurable adhesive. The adhesive layer may have a thickness of about 30 μm or less, for example, more than about 0 μm and about 30 μm or less.

[0107] adhesive layer The adhesive layer 400 may be formed on the lower surface of the protective layer 300 to adhere the polarizing plate to an adherend.

[0108] The adhesive layer 400 may be formed of a composition for an adhesive layer including an adhesive resin such as a (meth)acrylic adhesive resin, a silicone adhesive resin, a urethane adhesive resin, or an epoxy adhesive resin. Preferably, the adhesive layer 400 may be formed of a (meth)acrylic adhesive resin in consideration of ease of manufacture of the adhesive layer. The (meth)acrylic adhesive resin may include an adhesive resin applied in a conventional composition known to those skilled in the art.

[0109] The adhesive layer 400 may have a thickness of about 5 μm to about 200 μm, specifically about 10 μm to about 150 μm, and more specifically about 20 μm to about 100 μm. Within this range, the adhesive layer 400 can be used in a polarizing plate.

[0110] An optical display device according to an embodiment of the present invention will now be described.

[0111] The optical display device includes the polarizer of the present invention. The optical display device may be, but is not limited to, a liquid crystal display device, an organic light emitting display device, a flexible organic light emitting display device, and the like.

[0112] In one embodiment, an optical display device may include the polarizing plate of the present invention, a transparent adhesive film (e.g., OCA) laminated on an upper surface of the polarizing plate, and a panel for an optical display device, specifically, an OLED panel, formed on a lower surface of the polarizing plate.

[0113] In another embodiment, an optical display device may include the polarizing plate of the present invention, a transparent adhesive film (e.g., OCA) laminated on the upper surface of the polarizing plate, a cover glass laminated on the upper surface of the transparent adhesive film, and a panel for an optical display device formed on the lower surface of the polarizing plate.

[0114] <Mode for carrying out the invention> The present invention will be described in more detail with reference to the following examples, which are provided for the purpose of aiding understanding of the present invention and are not intended to limit the scope of the present invention.

[0115] <Production Example 1> In a 1L reactor equipped with a cooling device to allow nitrogen gas to be refluxed and to easily control the temperature, 100 parts by weight of a monomer mixture containing 40 parts by weight of n-butyl acrylate, 5 parts by weight of 2-hydroxyethyl methacrylate, 50 parts by weight of methyl methacrylate, and 5 parts by weight of acrylic acid were added, and 100 parts by weight of ethyl acetate was added as a solvent. Then, in order to remove oxygen, nitrogen gas was added for 1 hour to replace the inside of the reactor with nitrogen gas, and the temperature of the reactor was maintained at 62°C. After the monomer mixture was uniformly stirred, 0.03 parts by weight of azobisisobutyronitrile (AIBN) was added as a reaction initiator, and the mixture was reacted for 8 hours to produce a (meth)acrylic copolymer with a weight average molecular weight of 200,000.

[0116] <Production Example 2> 100 parts by weight of a monomer mixture containing 90 parts by weight of n-butyl acrylate, 5 parts by weight of 4-hydroxybutyl acrylate, and 5 parts by weight of acrylic acid was added to a 1L reactor equipped with a cooling device to allow nitrogen gas to be refluxed and to facilitate temperature control, and 100 parts by weight of ethyl acetate was added as a solvent. Then, in order to remove oxygen, nitrogen gas was added for 1 hour to replace the reactor with nitrogen gas, and the temperature of the reactor was maintained at 62°C. After the monomer mixture was uniformly stirred, 0.03 parts by weight of azobisisobutyronitrile (AIBN) was added as a reaction initiator and reacted for 8 hours to produce a (meth)acrylic copolymer with a weight average molecular weight of 200,000.

[0117] The specific specifications of the components used in the following examples and comparative examples are as follows:

[0118] (A) Adhesive resin: (A1) (Meth)acrylic copolymer of Production Example 1 (A2) (Meth)acrylic copolymer of Production Example 2 (B) Isocyanate-based hardener: (B1) AE 700-100 Asahi Kasei, isocyanate-based hardener) (B2) Coronate L (Japan Polyurethane, trimethylolpropane adduct of toluene diisocyanate) (C)UV absorber: (C1) UV 3912 (Orient Chemical, indole type) as a UV absorber (C2) Tinuvin 477 (BASF, triazine type) as a UV absorber (D) Silane coupling agent: KBM-403 (Shin-Etsu, 3-glycidoxypropyltrimethoxysilane) <Example 1> A polyvinyl alcohol-based film (Kuraray, saponification degree: 99.5 mol%, polymerization degree: 2000, thickness: 80 μm) washed with water was swollen in a swelling tank of 30°C water. The polyvinyl alcohol-based film that passed through the swelling tank was treated for 30 to 200 seconds in a dyeing tank at 30°C containing an aqueous solution containing 3% by weight of potassium iodide. The polyvinyl alcohol-based film that passed through the dyeing tank was passed through a wet crosslinking tank containing an aqueous solution at 30°C to 60°C containing 3% by weight of boric acid. The polyvinyl alcohol-based film that passed through the crosslinking tank was stretched in an aqueous solution at 50°C to 60°C containing 3% by weight of boric acid, and stretched so that the total stretch ratio was 6 times to produce a polarizer (thickness: 20 μm).

[0119] Based on the solid content, 100 parts by weight of the (meth)acrylic copolymer of Preparation Example 1, 30 parts by weight of the isocyanate-based curing agent (B1), 1.5 parts by weight of the UV absorber (C1), 0.1 parts by weight of the silane coupling agent (D), and 20 parts by weight of the solvent methyl ethyl ketone were mixed and stirred at 25° C. for 5 minutes to prepare a composition for a protective coating layer.

[0120] The prepared protective coating layer composition was applied to a predetermined thickness on the upper surface of the polarizer, treated at 90° C. for 3 minutes to remove the solvent, and aged at 25° C. for 72 hours to form a protective coating layer (thickness: 7 μm) on the upper surface of the polarizer.

[0121] A triacetyl cellulose film (Fuji, n-TAC, thickness: 80 μm) was attached to the bottom surface of the polarizer as a protective film using a water-based adhesive (containing a polyvinyl alcohol-based resin), and then an adhesive layer (thickness: 20 μm, (meth)acrylic adhesive layer) was formed on the other surface of the triacetyl cellulose film to manufacture a polarizing plate laminated in the order of protective coating layer-polarizer-adhesive layer-triacetyl cellulose film-adhesive layer. The adhesive layer was formed from a composition containing a (meth)acrylic adhesive resin and an isocyanate-based curing agent.

[0122] <Examples 2 to 5> A polarizing plate was manufactured in the same manner as in Example 1, except that the components and / or the contents of the protective coating layer composition were changed as shown in the following Table 1 (unit: parts by weight). In the following Table 1, "-" means that the corresponding component is not included.

[0123] <Comparative Example 1 and Comparative Example 2> A pressure-sensitive adhesive composition for a polarizing plate was prepared in the same manner as in Example 1, except that the components and / or the content thereof of the composition were changed as shown in Table 1 below.

[0124] The polarizing plates of the examples and comparative examples were evaluated for the following physical properties, and the results are shown in Table 1 below.

[0125] (1) Modulus (unit: MPa): The modulus was measured on the surface of the protective coating layer for the polarizing plates of the examples and comparative examples. A polarizing plate was cut into length x width (10 cm x 10 cm) to prepare a test specimen. The adhesive layer of the test specimen was attached to a glass plate to fix the test specimen to the glass plate, and a micro indenter (Hysitron TI750 Ubi) was applied to the protective coating layer surface of the test specimen at 25°C with a constant force of 200 mN for 5 seconds, maintained for 2 seconds, and relaxed for 5 seconds, followed by calculation.

[0126] (2) Cracks in polarizer: The polarizing plates of the examples and comparative examples (without cracks in the polarizer) were cut into length x width (10 cm x 10 cm), and the adhesive layer of the polarizing plate was laminated to a glass plate and autoclaved at 50°C and 1 atmosphere to produce a test specimen in which the polarizing plate was fixed to the glass plate. The test specimen was left in a thermal shock chamber for 30 minutes at -30°C and 30 minutes at 80°C, and was subjected to 200 cycles. After 200 cycles, the maximum length of the cracks generated from the polarizer was measured. The cracks were formed in the MD of the polarizer. If the crack length was 4 mm or less, it was evaluated as "OK", and if the crack length was more than 4 mm, it was evaluated as "NG".

[0127] (3) Light transmittance of polarizing plate (unit: %): The polarizing plates of the examples and comparative examples were attached to a glass plate via the adhesive layer of the polarizing plate and measured using a light transmittance measuring device V-7100 (JASCO Co., Ltd.) The light transmittance was measured at wavelengths of 380 nm and 405 nm.

[0128] (4) Tackiness (unit: gf): A probe (a curved surface in the shape of a cone with a radius of 2.5 mm, made of SUS) was placed in contact with the surface of the protective coating layer of the polarizing plates of the examples and comparative examples at 25°C for 10 seconds, and the force applied to the probe when the probe was removed from the surface of the protective coating layer was measured using a tackiness measuring device UTM (TA-Analyzer). The tackiness measured is preferably 10gf or less, for example, 0gf to 10gf.

[0129] (5) Curvature (unit: mm): Polarizing plates (MD of polarizer × TD of polarizer, 180 mm × 110 mm, rectangular) of the examples and comparative examples were attached to a glass plate (width × length × thickness, 190 mm × 120 mm × 0.5T, rectangular) using the adhesive layer of the polarizing plate as a medium to prepare a test specimen. The prepared test specimen was placed in an oven at 85°C and removed after 24 hours to measure the curvature of the test specimen. The test specimen was placed in a flat place, and a weight was placed on the upper corner of one side to measure the distance between the flat place and the test specimen at the diagonal corner. If the distance between the flat place and the test specimen was 0 mm or more and 2 mm or less, it was evaluated as ○, if it was more than 2 mm and 5 mm or less, it was evaluated as △, and if it was more than 5 mm, it was evaluated as ×.

[0130] [Table 1]

[0131] As shown in Table 1, the polarizing plate of the present invention provided a barrier effect to the polarizer, thereby suppressing bending of the polarizing plate.

[0132] On the other hand, the polarizing plates of the comparative examples, which are out of the modulus range of the present invention, had no barrier effect against the polarizer, had a weak curvature suppression effect, and had poor tackiness.

[0133] Simple modifications and variations of the present invention can be easily implemented by a person having ordinary skill in the art, and all such modifications and variations can be considered to be included within the scope of the present invention.

Claims

1. A polarizing plate comprising: a polarizer; a protective coating layer formed on an upper surface of the polarizer; and a protective layer and an adhesive layer sequentially formed on a lower surface of the polarizer, The protective coating layer is formed of a thermosetting composition, The thermosetting composition includes an adhesive resin, an isocyanate-based curing agent, and a UV absorber, The adhesive resin is a monomer mixture including a (meth)acrylic monomer having an alkyl group, a (meth)acrylic monomer having a hydroxyl group, and at least one monomer having a carboxylic acid group selected from the group consisting of (meth)acrylic acid, fumaric acid, and itaconic acid, at least one of the monomers included in the monomer mixture includes a (meth)acrylic copolymer of a monomer mixture including a monomer having a homopolymer glass transition temperature of 50° C. or higher, The polarizing plate has a modulus of 10 MPa or more as measured by a microindenter on the surface of the protective coating layer.

2. The polarizing plate of claim 1 , wherein the protective coating layer is formed directly on an upper surface of the polarizer.

3. The polarizing plate of claim 1 , wherein only the protective coating layer is laminated on an upper surface of the polarizer as a protective layer for the polarizer.

4. 2. The polarizing plate of claim 1, wherein the UV absorbent is included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the adhesive resin.

5. The polarizing plate according to claim 1 , wherein the UV absorbent has a maximum absorption wavelength of 390 nm or more.

6. The polarizing plate according to claim 1 , wherein the UV absorbent comprises at least one of an indole type and a triazine type.

7. 2. The polarizing plate according to claim 1, wherein the monomer having a homopolymer glass transition temperature of 50° C. or higher is included in the monomer mixture in an amount of 1% by weight to 60% by weight.

8. 2. The polarizing plate according to claim 1, wherein the monomer having a homopolymer glass transition temperature of 50° C. or higher includes at least one of methyl methacrylate, t-butyl methacrylate, iso-propyl methacrylate, sec-butyl methacrylate, and isobornyl methacrylate.

9. 2. The polarizing plate according to claim 1, wherein the monomer mixture contains 70% by weight to 98% by weight of the (meth)acrylic monomer having an alkyl group, 0.1% by weight to 15% by weight of the (meth)acrylic monomer having a hydroxyl group, and 0.1% by weight to 15% by weight of the monomer having a carboxylic acid group.

10. The polarizing plate according to claim 1 , wherein the isocyanate-based hardener comprises a polyisocyanate-based hardener having a urethane bond and a plurality of alkylene group-containing units having two or more carbon atoms.

11. The polarizing plate according to claim 10, wherein the isocyanate-based hardener comprises a polyisocyanate hardener having a plurality of units of the following Formula 1: 【Chemistry 1】 (In the above Chemical Formula 1, * is a linking site, R 1 , R 2 are the same or different and are divalent aliphatic hydrocarbon groups having 2 to 20 carbon atoms.

12. The polarizing plate described in claim 1, characterized in that the thermosetting composition contains 100 parts by weight of the adhesive resin, 10 to 40 parts by weight of the isocyanate-based curing agent, and 0.1 to 10 parts by weight of the UV absorber.

13. 2. The polarizing plate according to claim 1, wherein the polarizing plate has a light transmittance of 3% or less at a wavelength of 380 nm or 405 nm.

14. An optical display device comprising the polarizing plate according to any one of claims 1 to 13.

15. The optical display device of claim 14, comprising: the polarizing plate; a transparent adhesive film laminated on an upper surface of the polarizing plate; and an OLED panel formed on a lower surface of the polarizing plate.

16. The optical display device according to claim 15, further comprising a cover glass laminated on an upper surface of the transparent adhesive film.

Citation Information

Patent Citations

  • Organic el display device

    JP2017168430A

  • Adhesive composition for surface protective film, surface protective membrane, and surface protective film

    JP2018203823A

  • Adhesive composition for polarizing plate and polarizing plate with adhesive layer

    JP2020045379A

  • Laminate, optical film, image display device, and manufacturing method therefor

    JP2020118918A

  • Polarizing plate, composition for protective layer of the same and optical display apparatus comprising the same

    KR101802562B1