toner

By controlling the compatibility between crystalline polyester and styrene resins through solubility parameters and glass transition temperatures, the toner maintains low-temperature fixability and fluidity, addressing issues of toner drop and carrier spend.

JP7580256B2Active Publication Date: 2024-11-11SHARP KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020191860
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-18
Publication Date
2024-11-11
Estimated Expiration
2040-11-18

AI Technical Summary

Technical Problem

Toner containing crystalline polyester resin and styrene resin faces issues with low-temperature fixability due to poor affinity with paper and deteriorated fluidity, which affects the amount of toner falling from cartridges and carrier spend.

Method used

The compatibility between crystalline polyester resin and styrene resin is controlled by adjusting their solubility parameters (SPa-SPb) and glass transition temperatures (T1, T2) within specific ranges, ensuring appropriate dispersion and maintaining low-temperature fixability and fluidity.

Benefits of technology

The toner achieves both low-temperature fixability and improved fluidity by optimizing the compatibility between the resins, reducing toner drop from cartridges and carrier spend.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580256000005
    Figure 0007580256000005
  • Figure 0007580256000001
    Figure 0007580256000001
  • Figure 0007580256000002
    Figure 0007580256000002
Patent Text Reader

Abstract

To provide a toner including a crystalline polyester resin and a styrene based resin and capable of achieving both low-temperature fixability and fluidity.SOLUTION: A toner includes toner particles including a binder resin, a crystalline polyester resin and a styrene based resin. The binder resin includes an amorphous polyester resin; when setting the SP value of the crystalline polyester resin to SPa and the SP value of the styrene based resin to SPb, 0.5≤SPa-SPb≤1.5 is satisfied; when setting the melting point of the crystalline polyester resin to T1 and the glass transition temperature of the styrene based resin to T2, 10<T2-T1<5 is satisfied.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner. [Background technology]

[0002] In recent years, there has been a demand for toners (electrophotographic toners) used in image forming devices using electrophotography, such as copying machines, multifunction machines, printers, and facsimile machines, to have even lower fixing temperatures in line with the trend toward energy saving in image forming devices.

[0003] Although the addition of a crystalline polyester resin to the toner particles improves low-temperature fixability, in order to achieve even lower temperature fixability, it is necessary to make the combination of the crystalline polyester resin and the main resin more compatible or to increase the amount of the crystalline polyester resin added.

[0004] However, when the compatibility between the crystalline polyester resin and the main resin is promoted or the amount of the crystalline polyester resin added is increased, the low-temperature fixing property of the toner is improved, but the fluidity of the toner is significantly deteriorated. When the fluidity of the toner is deteriorated, problems such as the amount of toner falling from the toner cartridge being reduced and carrier spent (the phenomenon in which toner particles stick to the carrier) being accelerated are caused.

[0005] Therefore, by further adding a styrene-based resin to toner particles containing a crystalline polyester resin, the styrene-based resin is more likely to be present on the toner particle surface (grinding interface), and the exposure of the crystalline polyester resin to the toner particle surface is reduced, thereby improving the fluidity of the toner.

[0006] As a toner containing a crystalline polyester resin and a styrene resin, for example, Patent Document 1 discloses a toner containing a crystalline resin produced by a suspension polymerization method, a polar resin such as a styrene acrylic resin, and a colorant. Patent Document 2 discloses a toner containing a crystalline polyester resin, a styrene acrylic resin, and a polymer having a specific structure.

Prior Art Documents

Patent Documents

[0007]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0008] However, in the toner containing a styrene resin as described above, the styrene resin, which has a poorer affinity with paper compared to the polyester resin, has been inhibiting the low-temperature fixability.

[0009] The present invention has been made based on the above circumstances, and an object thereof is to provide a toner that achieves both low-temperature fixability and fluidity in a toner containing a crystalline polyester resin and a styrene resin.

Means for Solving the Problems

[0010] As a result of intensive studies to solve the above problems, the present inventor has found that the low-temperature fixability and fluidity of the toner vary greatly depending on the compatibility between the crystalline polyester resin and the styrene resin, and has completed the present invention.

[0011] That is, the toner according to the present invention has toner particles containing a binder resin, a crystalline polyester resin, and a styrene resin. And, when the binder resin contains an amorphous polyester resin, the SP value (solubility parameter) of the crystalline polyester resin is SPa and the SP value of the styrene resin is SPb, 0.5 ≦ SPa - SPb ≦ 1.5 is satisfied, and when the melting point of the crystalline polyester resin is T1 and the glass transition temperature of the styrene resin is T2, -10 < T2 - T1 < 5 is satisfied.

[0012] According to the present invention described above, SPa, SPb, T1, and T2 satisfy the above-mentioned relationships, and thus the compatibility between the crystalline polyester resin and the styrene-based resin is appropriately controlled, so that the low-temperature fixability is not hindered by the styrene-based resin, and a toner having excellent fluidity can be realized while maintaining the low-temperature fixability of the toner.

[0013] In the above toner, it is preferable that the styrene resin has a weight average molecular weight of 10,000 or less.

[0014] As the weight average molecular weight of the styrene resin increases, the low temperature fixability of the toner tends to be impaired. By setting the weight average molecular weight of the styrene resin to the above upper limit or less, the low temperature fixability is less likely to be impaired, and a toner with excellent low temperature fixability can be realized.

[0015] In the above toner, the glass transition temperature T2 of the styrene resin is preferably 50° C. or higher and 75° C. or lower.

[0016] When the glass transition temperature of the styrene resin is within the above range, the toner has excellent low-temperature fixing property, flowability, and heat-resistant storage stability.

[0017] In the above toner, it is preferable that the content of the styrene-based resin in the toner particles is 1% by weight or more and 10% by weight or less.

[0018] When the content of the styrene-based resin is within the above range, it becomes easier to achieve both low-temperature fixability and fluidity of the toner.

[0019] In the toner, the content of the crystalline polyester resin in the toner particles is preferably 1% by weight or more and 10% by weight or less.

[0020] When the content of the crystalline polyester resin is within the above range, it becomes easier to achieve both low-temperature fixability and fluidity of the toner.

[0021] In the toner, it is preferable that the average dispersion diameter of the styrene resin is 1 μm or less.

[0022] When the average dispersion diameter of the styrene-based resin is within the above range, the styrene-based resin is not exposed too much on the toner surface, and it becomes easier to achieve both low-temperature fixability and fluidity of the toner.

[0023] In the above toner, when the SP value of the amorphous polyester resin is defined as SPc, it is preferable that SPc-SPa is 2.1 or less.

[0024] When SPa and SPc satisfy the above relationship, the crystalline polyester resin is less likely to cause poor dispersion, and the toner can more easily achieve both low-temperature fixability and fluidity. Effect of the Invention

[0025] According to the present invention, it is possible to provide a toner that has both low-temperature fixability and fluidity. [Brief description of the drawings]

[0026] [Figure 1] 1 is a conceptual diagram showing a cross-sectional structure of a conventional toner containing a crystalline polyester resin and a styrene-based resin, and a cross-sectional structure of a toner according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] [Toner, toner particles] The toner of the present invention has toner particles containing a binder resin, a crystalline polyester resin, and a styrene-based resin. If necessary, any optional components may be contained within a range that does not impair the effects of the present invention. The volume average particle size of the primary particles of the toner particles is not particularly limited, but examples thereof include toner particles having a volume average particle size of 4 μm or more and 8 μm or less. Each component will be described below.

[0028] In the present invention, crystalline resins and amorphous resins are distinguished by their crystallinity index, with a resin having a crystallinity index in the range of 0.6 to 1.5 being crystalline resins, and a resin having a crystallinity index less than 0.6 or more than 1.5 being amorphous resins. Resins having a crystallinity index greater than 1.5 are amorphous, and resins having a crystallinity index less than 0.6 have low crystallinity and many amorphous portions.

[0029] The crystallinity index is a physical property that is an index of the degree of crystallization of a resin, and is defined by the ratio of the softening temperature to the highest endothermic peak temperature (softening temperature / highest endothermic peak temperature). Here, the highest endothermic peak temperature refers to the temperature of the highest endothermic peak among the observed endothermic peaks. In the case of a crystalline polyester resin, the highest peak temperature is the melting point, and in the case of an amorphous polyester resin, the highest endothermic peak is the glass transition point.

[0030] The degree of crystallization can be controlled by adjusting the types and ratio of raw material monomers, as well as production conditions (for example, reaction temperature, reaction time, cooling rate), and the like.

[0031] <Binding resin> The toner particles according to the present invention contain an amorphous polyester resin as a binder resin. The binder resin may contain components other than the amorphous polyester resin as long as the effects of the present invention are not impaired.

[0032] (Amorphous polyester resin) The amorphous polyester resin used in the toner of the present invention is an amorphous polyester resin obtained by polycondensation of a dicarboxylic acid monomer containing terephthalic acid or isophthalic acid as a main component and a diol monomer containing ethylene glycol as a main component.

[0033] The dicarboxylic acid monomer used in the synthesis of the amorphous polyester resin contains terephthalic acid or isophthalic acid as a main component, and the molar content of terephthalic acid or isophthalic acid in the dicarboxylic acid monomer is preferably 70% or more and 100% or less, and more preferably 80% or more and 100% or less.

[0034] The dicarboxylic acid monomer may include aromatic dicarboxylic acids other than terephthalic acid and isophthalic acid, and aliphatic dicarboxylic acids. Examples of aromatic dicarboxylic acids other than terephthalic acid and isophthalic acid include fumaric acid, and examples of aliphatic dicarboxylic acids include adipic acid, sebacic acid, and succinic acid. The dicarboxylic acid monomer may also include an ester-forming derivative of terephthalic acid or isophthalic acid, an ester-forming derivative of an aromatic dicarboxylic acid other than terephthalic acid and isophthalic acid, and an ester-forming derivative of an aliphatic dicarboxylic acid. In the present invention, the ester-forming derivative includes an acid anhydride or an alkyl ester of a carboxylic acid. When a dicarboxylic acid monomer other than terephthalic acid and isophthalic acid is used, the dicarboxylic acid monomer may be used alone or in combination of two or more.

[0035] In the synthesis of the amorphous polyester resin, a polycarboxylic acid monomer having three or more valences may be used together with the dicarboxylic acid monomer. As the polycarboxylic acid monomer having three or more valences, a polycarboxylic acid having three or more valences, such as trimellitic acid and pyromellitic acid, or an ester-forming derivative thereof may be used. When a polycarboxylic acid monomer having three or more valences is used, the polycarboxylic acid monomer may be used alone or in combination of two or more kinds.

[0036] The diol monomer used in the synthesis of the amorphous polyester resin contains ethylene glycol as a main component, and the molar content of ethylene glycol in the diol monomer is preferably 70% or more and 100% or less, and more preferably 80% or more and 100% or less.

[0037] The diol monomer may include 1,3-propylene glycol, 1,4-butanediol, etc. When a diol monomer other than ethylene glycol is used, the diol monomer may be used alone or in combination of two or more kinds.

[0038] The amorphous polyester resin used in the toner of the present invention can be produced in the same manner as in the ordinary polyester production method. For example, the amorphous polyester resin can be synthesized by carrying out a polycondensation reaction at a temperature of 190 to 240° C. in a nitrogen gas atmosphere using a dicarboxylic acid monomer, a diol monomer, and optionally a trivalent or higher polycarboxylic acid monomer.

[0039] In the polycondensation reaction, the reaction ratio of the diol monomer and the carboxylic acid monomer (including the dicarboxylic acid monomer and, in some cases, the trivalent or higher polycarboxylic acid monomer) is preferably 1.3:1 to 1:1.2 in terms of the equivalent ratio [OH]:[COOH] of the hydroxyl group to the carboxyl group. In the polycondensation reaction, the molar content of the dicarboxylic acid monomer in the carboxylic acid monomer is preferably 80 to 100%. Furthermore, in the polycondensation reaction, an esterification catalyst such as dibutyltin oxide or titanium alkoxide (e.g., tetrabutoxytitanate) can be used as necessary.

[0040] The SP value (solubility parameter) of the amorphous polyester resin is preferably 10 or more and 12.5 or less. In the toner of the present invention, the content of the amorphous polyester resin is not particularly limited, but is preferably from 60% by weight to 85% by weight in the toner particles.

[0041] <Crystalline polyester resin> In the toner of the present invention, the crystalline polyester resin is dispersed in the amorphous polyester resin. The crystalline polyester resin is a crystalline polyester resin composed of linear saturated aliphatic polyester units obtained by polycondensation of a dicarboxylic acid monomer containing an aliphatic dicarboxylic acid having 9 to 22 carbon atoms as a main component and a diol monomer containing an aliphatic diol having 2 to 10 carbon atoms as a main component. By being composed of linear saturated aliphatic polyester units, the crystalline polyester resin and the amorphous polyester resin are less likely to be compatible with each other.

[0042] The dicarboxylic acid monomer used in the synthesis of the crystalline polyester resin contains, as a main component, an aliphatic dicarboxylic acid having 9 to 22 carbon atoms. Here, the molar content of the aliphatic dicarboxylic acid having 9 to 22 carbon atoms in the dicarboxylic acid monomer is preferably 80% or more and 100% or less.

[0043] Examples of the aliphatic dicarboxylic acid having 9 to 22 carbon atoms include azelaic acid, zebacinic acid, 1,10-decanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. The dicarboxylic acid monomer may also include an ester-forming derivative of these aliphatic dicarboxylic acids. These dicarboxylic acid monomers may be used alone or in combination of two or more.

[0044] In the synthesis of the crystalline polyester resin, a polycarboxylic acid monomer having three or more valences may be used together with the dicarboxylic acid monomer. As the polycarboxylic acid monomer having three or more valences, a polycarboxylic acid having three or more valences, such as trimellitic acid and pyromellitic acid, or an ester-forming derivative thereof may be used. When a polycarboxylic acid monomer having three or more valences is used, the polycarboxylic acid monomer may be used alone or in combination of two or more kinds.

[0045] The diol monomer used in the synthesis of the crystalline polyester resin contains, as a main component, an aliphatic diol having 2 to 10 carbon atoms. Here, the molar content of the aliphatic diol having 2 to 10 carbon atoms in the diol monomer is preferably 80% or more and 100% or less.

[0046] Examples of the aliphatic diol having 2 to 10 carbon atoms include ethylene glycol, 1,4-butanediol, 1,6-hexanediol, etc. These diol monomers may be used alone or in combination of two or more.

[0047] In the synthesis of the crystalline polyester resin, a polyol monomer having three or more valences may be used together with the diol monomer. As the polyol monomer having three or more valences, glycerin, trimethylolpropane, etc. can be used. When a polyol monomer having three or more valences is used, the polyol monomer may be used alone or in combination of two or more kinds.

[0048] The crystalline polyester resin used in the toner of the present invention can be produced in the same manner as in the ordinary polyester production method. For example, the crystalline polyester resin can be synthesized by carrying out a polycondensation reaction at a temperature of 190 to 240° C. in a nitrogen gas atmosphere using a dicarboxylic acid monomer, a diol monomer, and optionally a trivalent or higher polycarboxylic acid monomer or a trivalent or higher polyol monomer.

[0049] In the polycondensation reaction, the equivalent ratio (OH group / COOH group) of the hydroxyl group of the polyol monomer (including a diol monomer and, in some cases, a polyol monomer having a valence of three or more) to the carboxyl group of the carboxylic acid monomer (including a dicarboxylic acid monomer and, in some cases, a polycarboxylic acid monomer having a valence of three or more) is preferably 0.83 to 1.3 from the viewpoint of storage stability. In addition, in the polycondensation reaction, the molar content of the dicarboxylic acid monomer in the carboxylic acid monomer is preferably 90 to 100%. The smaller the molar content of the dicarboxylic acid monomer, the lower the crystallization rate and speed, and the toner aggregation resistance becomes insufficient. In addition, in the polycondensation reaction, the molar content of the diol monomer in the polyol monomer is preferably 80 to 100%. In the polycondensation reaction, an esterification catalyst such as dibutyltin oxide or titanium alkoxide (e.g., tetrabutoxytitanate) can be used as necessary.

[0050] The melting point of the crystalline polyester resin is preferably 50° C. or higher, and more preferably 60 to 90° C. from the viewpoints of fixability, storage stability, durability, etc. If the melting point is lower than 50° C., the durability may be insufficient. If the melting point is higher than 90° C., the fixability may be insufficient.

[0051] The SP value of the crystalline polyester resin is preferably 9.5 or more and 10.5 or less.

[0052] In the toner of the present invention, when the SP value of the crystalline polyester resin is SPa and the SP value of the amorphous polyester resin is SPc, SPc-SPa is preferably 2.1 or less, more preferably 1.0 or more and 1.8 or less. When SPc-SPa exceeds the upper limit, the dispersion diameter of the crystalline polyester resin becomes large, and the low-temperature fixability, heat-resistant storage stability and fluidity of the toner may be deteriorated. On the other hand, when SPc-SPa is less than the lower limit, the low-temperature fixability is excellent, but the heat-resistant storage stability may be deteriorated.

[0053] The content of the crystalline polyester resin in the toner particles according to the present invention is preferably 1% by weight or more and 10% by weight or less, and more preferably 5% by weight or more and 8% by weight or less. When the content of the crystalline polyester resin is within the above range, it becomes easier to balance the low-temperature fixability and fluidity of the toner. If the content is less than the above lower limit, the low-temperature fixability of the toner may be insufficient. On the other hand, if the content exceeds the above upper limit, the fluidity of the toner may deteriorate.

[0054] <Styrene resin> Examples of the styrene resin include homopolymers of styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, ethylstyrene, isopropylstyrene, and dimethylstyrene, and copolymers thereof, and copolymers of styrene-based monomers and vinyl monomers copolymerizable with styrene-based monomers. Examples of the vinyl monomer include monofunctional monomers such as alkyl (meth) acrylates such as methyl (meth) acrylate, ethyl (meth) acrylate, and butyl (meth) acrylate, and (meth) acrylonitrile, and bifunctional monomers such as divinylbenzene and alkylene glycol dimethacrylate. Here, "(meth) acrylate" means acrylate and methacrylate. Among these styrene resins, a copolymer of styrene or α-methylstyrene and (meth) acrylate (styrene acrylic copolymer) is preferred.

[0055] In the toner of the present invention, when the SP value of the crystalline polyester resin is SPa and the SP value of the styrene resin is SPb, 0.5 ≦ SPa - SPb ≦ 1.5 is satisfied, and when the melting point of the crystalline polyester resin is T1 and the glass transition temperature of the styrene resin is T2, -10 < T2 - T1 < 5 is satisfied. A more preferable range of SPa - SPb is 0.6 ≦ SPa - SPb ≦ 1.0. A more preferable range of T2 - T1 is -5 ≦ T2 - T1 ≦ 3.

[0056] By satisfying the above relationship between SPa, SPb, T1, and T2, the compatibility between the crystalline polyester resin and the styrene resin is appropriately controlled, so that the low-temperature fixability is not hindered by the styrene resin. Therefore, the toner of the present invention can achieve both low-temperature fixability and fluidity. FIG. 1 shows a conceptual diagram of the cross-sectional structure of a conventional toner containing a crystalline polyester resin and a styrene resin, and the cross-sectional structure of the toner according to the embodiment of the present invention. In this way, the styrene resin and the crystalline polyester resin are appropriately compatible with each other, so that the styrene resin and the crystalline polyester resin can exhibit their respective characteristics (fluidity and low-temperature fixability), and the drop amount from the toner cartridge can be reduced and carrier spent can be suppressed.

[0057] If SPa-SPb is less than the lower limit, the crystalline polyester resin and the styrene-based resin are too compatible with each other, which may impair low-temperature fixability and may also deteriorate the heat-resistant storage stability and flowability.If SPa-SPb is more than the upper limit, the crystalline polyester resin and the styrene-based resin are incompatible with each other, which may also impair the low-temperature fixability and heat-resistant storage stability.

[0058] If T2-T1 is outside the above range, the compatibility between the crystalline polyester resin and the styrene-based resin may deteriorate.

[0059] The glass transition temperature T2 of the styrene resin is preferably 50° C. or more and 75° C. or less, more preferably 60° C. or more and 70° C. or less. If the glass transition temperature T2 is less than the lower limit, the heat-resistant storage stability may deteriorate. If the glass transition temperature T2 is more than the upper limit, the low-temperature fixability may be impaired.

[0060] The weight average molecular weight of the styrene resin is preferably not more than 10000, and more preferably from 3000 to 6000. If the weight average molecular weight exceeds the above upper limit, the low temperature fixability may deteriorate.

[0061] The content of the styrene resin in the toner particles according to the present invention is preferably 1% by weight or more and 10% by weight or less, more preferably 5% by weight or more and 8% by weight or less. If the content of the styrene resin exceeds the upper limit, the low-temperature fixing property may be impaired by the styrene resin. If the content of the styrene resin is less than the lower limit, the effect of improving the flowability of the toner by the styrene resin may be insufficient.

[0062] The average dispersion diameter of the styrene resin is preferably 1 μm or less, and more preferably 0.3 μm or more and 0.8 μm or less. By having the average dispersion diameter of the styrene resin within the above range, the exposure of the styrene resin to the toner surface is not too much, and it is easier to balance the low-temperature fixability and fluidity of the toner. If the average dispersion diameter of the styrene resin exceeds the above upper limit, the styrene resin is likely to be exposed to the toner surface, which may impair the low-temperature fixability. If the average dispersion diameter of the styrene resin is less than the above lower limit, the effect of improving the fluidity of the toner by the styrene resin may be insufficient.

[0063] <Other internal additives> The toner particles according to the present invention may contain internal additives other than those described above, if necessary. Examples of the internal additives other than those described above include colorants and charge control agents. The colorants and charge control agents are dispersed in the binder resin.

[0064] The colorant is not particularly limited, and organic dyes, organic pigments, inorganic dyes, inorganic pigments, and the like used in the field of electrophotography can be used.

[0065] As black colorants, for example, carbon black, copper oxide, manganese dioxide, aniline black, activated carbon, non-magnetic ferrite, magnetic ferrite, and magnetite can be used.

[0066] As the yellow colorant, for example, CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 15, CI Pigment Yellow 17, CI Pigment Yellow 74, CI Pigment Yellow 93, CI Pigment Yellow 94, CI Pigment Yellow 138, CI Pigment Yellow 180, and CI Pigment Yellow 185 can be used.

[0067] As magenta colorants, for example, CI Pigment Red 48:1, CI Pigment Red 53:1, CI Pigment Red 57:1, CI Pigment Red 122, CI Pigment Red 123, CI Pigment Red 139, CI Pigment Red 144, CI Pigment Red 149, CI Pigment Red 166, CI Pigment Red 177, CI Pigment Red 178, and CI Pigment Red 222 can be used.

[0068] Examples of cyan colorants include CI Pigment Blue 15, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 16, CI Pigment Blue 60, and the like.

[0069] In the toner of the present invention, the content of the colorant is not particularly limited, but is preferably 4% by weight or more and 10% by weight or less in the toner particles. The colorant may be used alone or in combination of two or more kinds. The colorant may be used in the form of a master batch in order to disperse it uniformly in the binder resin.

[0070] The charge control agent is added to the toner in order to impart a desired chargeability to the toner. There are no particular limitations on the charge control agent, and charge control agents for positive charge control and negative charge control used in the electrophotographic field can be used.

[0071] As the charge control agent for controlling positive charges, for example, quaternary ammonium salts, pyrimidine compounds, triphenylmethane derivatives, guanidine salts, and amidine salts can be used.

[0072] Examples of charge control agents that can be used for negative charge control include metal-containing azo compounds, azo complex dyes, metal complexes and metal salts of salicylic acid and its derivatives (metals include chromium, zinc, zirconium, etc.), organic bentonite compounds, and boron compounds.

[0073] In the toner of the present invention, the content of the charge control agent is not particularly limited, but is preferably 0.5% by weight or more and 5% by weight or less in the toner particles. The charge control agent may be used alone or in combination of two or more kinds.

[0074] <External additives> The toner according to the present invention may contain an external additive, if necessary. The external additive is attached to the surface of the toner particles. In the following description, the toner according to the present invention having toner particles with an external additive attached to the surface thereof is referred to as an external additive toner.

[0075] The external additive is not particularly limited, and external additives used in the field of electrophotography can be used. In the toner according to the present invention, the content of the external additive is not particularly limited, but is preferably 0.5 parts by weight or more and 3 parts by weight or less with respect to 100 parts by weight of the toner particles. The external additive may be used alone or in combination of two or more kinds.

[0076] <Toner manufacturing method> The toner of the present invention can be produced by a pulverization method. The method for producing the toner of the present invention by a pulverization method includes a mixing step, a kneading step, a cooling step, a pulverization step, a classification step, and an external addition step.

[0077] In the mixing step, the binder resin, the crystalline polyester resin, the styrene-based resin, and other internal additives as necessary are mixed to obtain a mixture. In the kneading step, the mixture obtained in the mixing step is kneaded while being melted in a twin-screw kneader to further uniformly disperse the crystalline polyester resin, the styrene-based resin, and other internal additives in the binder resin to obtain a kneaded product. In the cooling step, the kneaded product obtained in the kneading step is cooled and solidified to obtain a solidified product.

[0078] In the pulverization step, the solidified material obtained in the cooling step is pulverized by a pulverizer to obtain a pulverized material. Examples of the pulverizer include a jet pulverizer that uses a supersonic jet stream to pulverize the solidified material, and an impact pulverizer that introduces the solidified material into a space formed between a rotor and a stator (liner) that rotate at high speed to pulverize the solidified material. In the pulverization step, the average circularity of the toner particles can be adjusted by appropriately changing the pulverization conditions. One example of changing the pulverization conditions is changing the rotation speed of the rotor of the impact pulverizer within the range of 1000 rpm to 10000 rpm.

[0079] In the classification process, the particle size of the pulverized material obtained in the pulverization process is adjusted. This results in toner particles. As a classifier, a known classifier capable of removing over-pulverized toner particles by centrifugal force classification and wind force classification can be used. For example, a rotary wind classifier (rotary wind classifier) ​​can be used. In the external addition process, the toner particles and the external additive are mixed in a powder mixer such as a Henschel mixer, so that the external additive is attached to the toner particles. In the external addition process, the adhesion strength of the external additive to the toner particles can be adjusted by appropriately changing the mixing conditions. One example of changing the mixing conditions is changing the rotation speed of the stirring blade of the powder mixer within the range of 1000 rpm to 1500 rpm. EXAMPLES

[0080] The present invention will be described below based on examples and comparative examples, but the present invention is not limited to these examples.

[0081] <Production Example of Amorphous Polyester Resin> (Amorphous polyester resin A) In a reaction vessel, 440g (2.7 mol) of terephthalic acid, 235g (1.4 mol) of isophthalic acid, 7g (0.05 mol) of adipic acid, 554g (8.9 mol) of ethylene glycol, and 0.5g of tetrabutoxy titanate as a polymerization catalyst were placed, and reacted for 5 hours while distilling off the water and ethylene glycol produced under a nitrogen stream at 210°C, and then reacted for 1 hour under a reduced pressure of 666.7 Pa (5 mmHg) to 2666.4 Pa (20 mmHg). Next, 103g (0.54 mol) of trimellitic anhydride was added, and reacted for 1 hour under normal pressure, and then reacted under a reduced pressure of 2666.4 Pa (20 mmHg) to 5332.9 Pa (40 mmHg), and the resin was taken out at a predetermined softening point. The amount of ethylene glycol recovered was 219g (3.5 mol). The obtained resin was cooled to room temperature and then pulverized into particles. This was designated as amorphous polyester resin A. The SP value (SPc) of amorphous polyester resin A was 11.6.

[0082] (Amorphous polyester resins B to D) Amorphous polyester resins B to D were obtained in the same manner as the above-mentioned amorphous polyester resin A, except that the blending amounts of terephthalic acid, isophthalic acid, adipic acid, and ethylene glycol were adjusted so as to obtain the SP value (SPc) shown in Table 1 below.

[0083] [Table 1]

[0084] <Production Example of Crystalline Polyester Resin> (Crystalline polyester resin A) In a reaction vessel, 132 g (1.12 mol) of 1,6-hexanediol, 230 g (1.0 mol) of 1,10-decanedicarboxylic acid, and 3 g of tetrabutoxy titanate as a polymerization catalyst were placed, and the mixture was reacted for 5 hours at 210°C under normal pressure while distilling off the water produced. The reaction was then continued under reduced pressure of 666.7 Pa (5 mmHg) to 2666.4 Pa (20 mmHg), and the resin was taken out when the acid value became 2 mgKOH / g or less. The resin obtained was cooled to room temperature and then pulverized into particles. This was designated as crystalline polyester resin A. The SP value (SPa) of crystalline polyester resin A was 9.8.

[0085] (Crystalline polyester resins B to G) Crystalline polyester resins B to G were obtained in the same manner as for crystalline polyester resin A, except that the amounts of 1,6-hexanediol and 1,10-decanedicarboxylic acid were adjusted so as to have the melting points and SP values ​​(SPa) shown in Table 2 below.

[0086] [Table 2]

[0087] <Production example of styrene resin> (Styrene-acrylic copolymer resin A) In a reaction vessel, 20 parts by weight of a xylene solution in which 1.5 parts by weight of di-t-butyl peroxide was uniformly dissolved in a solution consisting of 76 parts by weight of styrene, 24 parts by weight of n-butyl acrylate, and 80 parts by weight of xylene solvent was added at an internal temperature of 190°C and an internal pressure of 6 kg / cm. 2 The mixture was continuously fed at 750mL / hour into a 5L reactor held at 90°C and polymerized to obtain a styrene-acrylic resin solution. After the solvent and other substances were distilled off by flushing in a vessel at 90°C and 10mmHg, the mixture was coarsely crushed using a coarse crusher to obtain 1mm chips of styrene-acrylic resin.

[0088] (Styrene-acrylic copolymer resins B to I) Styrene-acrylic copolymer resins B to I were obtained in the same manner as for the above styrene-acrylic copolymer resin A, except that the amounts of styrene and n-butyl acrylate were adjusted so as to obtain the glass transition temperatures, weight average molecular weights, and SP values ​​(SPb) shown in Table 3 below.

[0089] [Table 3]

[0090] <Example of toner particle production> [Example 1] (Material mixing, kneading, crushing, classification process) The following components were premixed for 5 minutes using a Henschel mixer, and then melt-kneaded using a twin-screw extruder at a cylinder setting temperature of 110° C., a barrel rotation speed of 300 rpm, and a raw material supply rate of 20 kg / hour to obtain a melt-kneaded product. Binder resin: Amorphous polyester resin A 75% by weight Crystalline polyester resin A 8% by weight Colorant: Carbon black (manufactured by Cabot Corporation, product name: Regal 330) 6% by weight Release agent: ester wax (melting point 73°C, product name: WEP3, manufactured by NOF Corporation) 3% by weight Release agent dispersant: 6% by weight of styrene acrylic copolymer resin A Charge control agent: Salicylic acid compound (Orient Chemical Industry Co., Ltd., product name: Bontro E84) 2% by weight

[0091] The resulting molten and kneaded product was cooled on a cooling belt, then coarsely pulverized using a cutting mill, then finely pulverized using a jet pulverizer, and further classified using an air classifier to obtain toner particles (toner base particles) having an average particle size of 6.5 μm.

[0092] (External addition process) To 100 parts by weight of the toner particles (toner base particles) obtained in the above process, 1.0 part by weight of commercially available silica microparticles (product name: R976, manufactured by Aerosil Corporation, average primary particle diameter 7 nm) was added, and the mixture was stirred for 2 minutes using an airflow mixer (manufactured by Mitsui Mining Co., Ltd., Henschel mixer) with the tip speed of the stirring blade set to 40 m / sec, to obtain an externally added toner.

[0093] [Examples 2 to 16, 20 to 22] In Examples 2 to 16 and 20 to 22, the crystalline polyester resin and the styrene-based resin were added in the combinations and amounts shown in Table 4 below, and the amount of the amorphous polyester resin added was changed according to these amounts, but the external additive toner was obtained in the same manner as in Example 1.

[0094] [Examples 17 to 19] In Examples 17 to 19, the external additive toner was obtained in the same manner as in Example 1, except that the kneading conditions were changed so that the average dispersion diameter of the styrene-based resin became the value shown in Table 4 below.

[0095] [Comparative Example 1] In Comparative Example 1, an external additive toner was obtained in the same manner as in Example 1, except that no styrene resin was added, the amount of the amorphous polyester resin added was 82% by weight, and the amount of the crystalline polyester resin added was 7% by weight.

[0096] [Comparative Examples 2 to 4] In Comparative Examples 2 to 4, the crystalline polyester resin and the styrene-based resin were added in the combinations and amounts shown in Table 4 below, and the amount of the amorphous polyester resin added was changed to match these amounts, but the same procedure was followed as in Example 1 to obtain an external additive toner.

[0097] <Evaluation> The toners of the examples and comparative examples were subjected to various measurements according to the following methods to evaluate the low-temperature fixability, high-temperature fixability, fluidity, and heat-resistant storage stability of the toners. The evaluation results are shown in Table 4. In Table 4, T1 represents the melting point of the crystalline polyester resin, T2 represents the glass transition temperature of the styrene-based resin, SPa represents the SP value of the crystalline polyester resin, SPb represents the SP value of the styrene-based resin, and SPc represents the SP value of the amorphous polyester resin.

[0098] (Method of measuring SP value) The SP value was measured according to the method of Suh and Clarke (KW Suh, DH Clarke, "Cohesive Energy Densities of Polymers from Turbidimetric Titrations", Journal of Polymer Science, A-1, vol. 5, 1967, pp. 1671-1681) as follows.

[0099] 0.5 g of the resin to be measured was weighed into a 100 ml beaker, 10 ml of a good solvent (a mixed solution of dioxane and acetone) was added using a whole pipette, and the resin was dissolved by stirring using a magnetic stirrer. To this, a hydrophobic solvent (a mixed solution of n-hexane and ion-exchanged water) was added dropwise using a 50 ml burette, and the amount added was determined to be the point at which turbidity occurred at a measurement temperature of 20°C.

[0100] From the measured values, the SP value δ of the resin was calculated by the following formula. δ=(Vl / 2δl+Vh / 2δh) / (Vl / 2+Vh / 2) In the above formula, Vl is the molar volume (ml / mol) of the solvent in the low SP solvent (hydrophobic solvent) mixed system, Vh is the molar volume (ml / mol) of the solvent in the high SP solvent (good solvent) mixed system, δl is the SP value of the solvent in the low SP solvent (hydrophobic solvent) mixed system, and δh is the SP value of the solvent in the high SP solvent (good solvent) mixed system.

[0101] (Method of measuring various peak temperatures by DSC measurement) Using a differential scanning calorimeter (product name: DSC220, manufactured by Seiko Instruments Inc.), 1 g of the sample was heated to 150° C. at a heating rate of 10° C. per minute, then held at 150° C. for 2 minutes, and cooled to 30° C. at a cooling rate of 10° C. per minute to measure a DSC curve. The endothermic peak temperature during heating and the exothermic peak temperature during cooling were determined in the obtained DSC curve, and the endothermic peak temperature during heating was taken as the melting point.

[0102] (Method of measuring glass transition temperature by DSC measurement) According to Japanese Industrial Standards (JIS) K7121-1987, a DSC curve was measured by heating 1 g of the sample at a heating rate of 10° C. per minute using a differential scanning calorimeter (product name: DSC220, manufactured by Seiko Denshi Kogyo Co., Ltd.). The glass transition temperature was determined as the temperature at the intersection of a straight line extending from the high-temperature side baseline of the endothermic peak corresponding to the glass transition of the obtained DSC curve to the low-temperature side and a tangent drawn at the point where the slope of the curve from the rising part of the peak to the apex is maximum.

[0103] (Method for measuring the average dispersion diameter of styrene resin dispersed in toner particles) The toner particles of the examples and comparative examples were embedded in a room temperature curing epoxy resin, and the cured product was subjected to surface preparation using an ultramicrotome (manufactured by Reichert, product name: Ultracut N) equipped with diamond teeth. The cross section of the obtained toner particle was observed using a scanning transmission electron microscope (manufactured by Hitachi High-Technologies Corporation, model: S-4800). A considerable number (200 to 300 pieces) of styrene resin were randomly extracted from this electron microscope photograph data, and the images were analyzed using image analysis software (product name: A-zo-kun, manufactured by Asahi Kasei Engineering Co., Ltd.). The average dispersion diameter of the styrene resin in the toner particles was obtained by averaging the dispersion diameters of a considerable number of styrene resins.

[0104] (Method of evaluating low-temperature fixability and high-temperature fixability) A fixed image was formed using a two-component developer using a commercially available copying machine (model: MX-5100FN, manufactured by Sharp Corporation) modified for evaluation. First, a sample image including a solid image (rectangle of 20 mm length and 50 mm width) was formed as an unfixed image on recording paper (model: SF-4AM3, manufactured by Sharp Corporation, PPC paper). At this time, the amount of toner adhering to the recording paper in the solid image was 1.0 mg / cm. 2 It was adjusted to be.

[0105] Next, a fixed image was produced using a belt fixing device. The fixing process speed was set to 283 mm / sec, and the temperature of the fixing belt was increased in 5°C increments from 110°C to determine the minimum and maximum temperatures at which low-temperature offset and high-temperature offset did not occur. Note that "low-temperature offset" and "high-temperature offset" are defined as the toner not being fixed to the recording paper during fixing, but remaining attached to the fixing belt and adhering to the recording paper after the fixing belt has made one revolution.

[0106] From the obtained results, the "low temperature fixability" was judged according to the following criteria. ◎: Very good (minimum temperature is less than 110℃) ○: Good (minimum temperature is 110℃ or higher and less than 120℃) △: Possible (minimum temperature is 120℃ or higher and less than 130℃) ×: Not possible (minimum temperature is 130℃ or higher)

[0107] From the obtained results, the "high temperature fixability" was judged according to the following criteria. ◎: Very good (maximum temperature is 195℃ or higher) ○: Good (maximum temperature is 185℃ or higher and less than 195℃) △: Acceptable (maximum temperature is 175℃ or higher and less than 185℃) ×: Not possible (maximum temperature is less than 175℃)

[0108] (Method for evaluating heat resistance storage stability) The heat-resistant storage stability was evaluated based on the presence or absence of aggregates after high-temperature storage. 20 g of the toner with external additives was sealed in a plastic container and left at 50°C for 72 hours, after which the toner was removed and sieved through a 230 mesh (63 μm) sieve. The weight of the toner remaining on the sieve was measured, and the remaining rate, which is the ratio of this remaining amount to the total weight of the toner, [(amount of toner remaining after 72 hours) / (total weight of toner)×100] was calculated and evaluated according to the following evaluation criteria. The lower the remaining rate, the less blocking the toner caused.

[0109] The evaluation criteria for heat resistance storage stability are as follows. ◎: Very good (no aggregation. Residual rate is less than 0.5%) ○: Good (very little aggregation. Residual rate is 0.5% or more and less than 2.0%) △: Fair (small amount of aggregation. Residual rate is 2.0% or more and less than 10.0%) ×: Unacceptable (large amount of aggregation. Residual rate is 10.0% or more)

[0110] (Method of evaluating liquidity) Using a bulk density meter (JIS bulk density meter, manufactured by Tsutsui Rikagaku Kikai Co., Ltd.), the loose apparent density was measured according to JIS K5101-12-1, and the fluidity of the two-component developer was evaluated. The larger the loose apparent density value, the better the fluidity.

[0111] The liquidity assessment criteria are as follows: ◎: Very good (specific gravity is 0.36 g / cm 3 More than 0.41g / cm 3 less than) ○: Good (specific gravity is 0.33 g / cm 3 More than 0.36g / cm 3 less than) △: Possible (specific gravity is 0.30g / cm 3 More than 0.33g / cm 3 less than) ×: Not possible (specific gravity is 0.30 g / cm 3 less than)

[0112] <Overall evaluation method> Based on the above evaluation results (low-temperature fixability, high-temperature fixability, fluidity, and heat-resistant storage stability), a comprehensive evaluation was conducted according to the following criteria. ◎: Very good (all evaluation items are ○ or above, and there are 3 or more ◎). ○: Good (all evaluation items are ○ or above, and there are 2 or fewer ◎). △: Passable (there is no × in the evaluation items, and there is at least one △ in the evaluation items). ×: Unacceptable (there is at least one × in the evaluation items).

[0113]

Table 4

[0114] As is clear from Table 4, the toners of Examples 1 to 22 containing an amorphous polyester resin, a crystalline polyester resin, and a styrene resin, satisfying 0.5 ≦ SPa - SPb ≦ 1.5 and -10 < T2 - T1 < 5, were excellent in the evaluation of low-temperature fixability, high-temperature fixability, fluidity, and heat-resistant storage.

[0115] On the other hand, Comparative Examples 1 to 4 that did not satisfy these requirements were inferior to the Examples in the evaluation of at least one of low-temperature fixability and fluidity, and did not achieve both low-temperature fixability and fluidity.

[0116] Also, it can be seen that Example 1 is more excellent in the evaluation of fluidity and heat-resistant storage stability compared with Example 2 where SPa - SPb is the lower limit value of the above range. Also, it can be seen that Example 1 is more excellent in the evaluation of low-temperature fixability compared with Example 3 where SPa - SPb is the upper limit value of the above range.

[0117] It can be seen that Example 1 is more excellent in the evaluation of low-temperature fixability compared with Example 4 where T2 - T1 is near the lower limit value of the above range or Example 5 where T2 - T1 is near the upper limit value.

[0118] It can be seen that in Example 7, in which the weight average molecular weight of the styrene resin exceeds 10,000, the evaluation of low temperature fixability is somewhat worse than that in Example 6, in which the weight average molecular weight is 10,000 or less.

[0119] It can be seen that the evaluation of heat-resistant storage stability is slightly worse in Example 8, in which the glass transition temperature T2 of the styrene resin is less than 50° C., compared with Example 9, in which the glass transition temperature T2 of the styrene resin is 50° C. or higher. Also, it can be seen that the evaluation of low-temperature fixability is slightly worse in Example 11, in which the glass transition temperature T2 of the styrene resin is more than 75° C., compared with Example 10, in which the glass transition temperature T2 of the styrene resin is 75° C. or lower.

[0120] Compared to Examples 12 and 13, in which the styrene resin content in the toner particles is in the range of 1% by weight or more and 10% by weight or less, it can be seen that the evaluation of low temperature fixing ability is slightly worse in Example 14, in which the content exceeds 10% by weight.

[0121] It can be seen that, compared to Example 15, in which the content of crystalline polyester resin in the toner particles is in the range of 1% by weight or more and 10% by weight, Example 16, in which the content exceeds 10% by weight, has slightly worse fluidity and heat-resistant storage stability.

[0122] It can be seen that the evaluation of low temperature fixability is deteriorated in Example 19, in which the average dispersion diameter exceeds 1 μm, compared with Example 18, in which the average dispersion diameter of the styrene-based resin is 1 μm or less. Also, it can be seen that the effect of improving flowability by the styrene-based resin is somewhat weakened in Example 17, in which the average dispersion diameter is relatively small at 0.2 μm.

[0123] It can be seen that the evaluations of low-temperature fixability, fluidity, and heat-resistant storage stability are slightly worse in Example 22, where SPc-SPa exceeds 2.1, compared with Example 21, where SPc-SPa is 2.1 or less. It can be seen that the evaluations of fluidity and heat-resistant storage stability are slightly worse in Example 20, where SPc-SPa is a relatively small value of 0.5.

[0124] <Other embodiments> It should be noted that the embodiments disclosed herein are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present invention is not interpreted solely by the above-described embodiments, but is defined by the claims. The technical scope of the present invention includes all modifications within the scope and meaning equivalent to the claims. [Explanation of symbols]

[0125] T Toner particles 1. Crystalline polyester resin 2. Binder resin 3. Styrene-based resin

Claims

1. A toner having toner particles including a binder resin, a crystalline polyester resin, and a styrene-based resin, the binder resin contains an amorphous polyester resin, When the SP value of the crystalline polyester resin is SPa and the SP value of the styrene-based resin is SPb, the relationship 0.6≦SPa−SPb≦1.0 is satisfied; When the melting point of the crystalline polyester resin is T1 and the glass transition temperature of the styrene-based resin is T2, the relationship of −10<T2−T1<5 is satisfied; The toner is characterized in that the average dispersion diameter of the styrene-based resin is 0.3 μm or more and 0.8 μm or less.

2. 2. The toner according to claim 1, The toner is characterized in that the weight average molecular weight of the styrene-based resin is 10,000 or less.

3. The toner according to claim 1 or 2, The toner is characterized in that the glass transition temperature T2 of the styrene-based resin is 50° C. or higher and 75° C. or lower.

4. The toner according to any one of claims 1 to 3, The toner, wherein the content of the styrene-based resin in the toner particles is 1% by weight or more and 10% by weight or less.

5. The toner according to any one of claims 1 to 4, The toner, wherein the content of the crystalline polyester resin in the toner particles is from 1% by weight to 10% by weight.

6. The toner according to any one of claims 1 to 5, The toner is characterized in that, when the SP value of the amorphous polyester resin is SPc, SPc-SPa is 2.1 or less.

Citation Information

Patent Citations

  • Electroconductive paste

    JP1989060904A

  • Toner, manufacturing method of the toner, and process cartridge

    JP2014056143A

  • toner

    JP2015004868A