Substrate processing method
The substrate processing method forms a precoat film on chamber parts using controlled plasma conditions to suppress sputtering, addressing particle generation and ensuring chamber cleanliness for semiconductor manufacturing.
Patent Information
- Application Number
- JP2020211353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-12-21
AI Technical Summary
Existing substrate processing methods face challenges in suppressing particle generation during chamber precoating due to ion sputtering of chamber parts, which can lead to contamination and shape abnormalities in semiconductor devices.
A substrate processing method that forms a precoat film on chamber parts using a first plasma under conditions to suppress sputtering, followed by a second plasma to apply a second film, ensuring the chamber is precoated while minimizing particle generation.
The method effectively precoats the chamber interior, reducing particle generation and preventing contamination, thereby enhancing the quality of semiconductor device manufacturing.
Smart Images

Figure 0007580264000001 
Figure 0007580264000002 
Figure 0007580264000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for processing a substrate. [Background technology]
[0002] Patent Document 1 discloses a method for reducing particles by coating the inner wall of a chamber with a silicon-containing film before substrate processing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] U.S. Patent No. 7,204,913 Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique for pre-coating the inside of a chamber while suppressing particle generation. [Means for solving the problem]
[0005] A substrate processing method according to an embodiment of the present disclosure includes (a) forming a precoat film on a chamber part disposed in a chamber, and (b) processing one or more substrates after (a), in which (a1) forming a first film on the chamber part without using plasma or using a first plasma generated from a reactive gas under conditions capable of suppressing sputtering of the chamber part, and (a2) forming a second film on a surface of the first film using a second plasma. Effect of the Invention
[0006] According to the present disclosure, the inside of a chamber can be pre-coated while suppressing generation of particles. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a substrate processing apparatus according to an embodiment. [Diagram 2] FIG. 2 is a flowchart showing an example of a substrate processing method according to the embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing the state inside the chamber during conventional precoating. [Figure 4] FIG. 4 is a flow chart showing an example of a pre-coating step in the substrate processing method according to the embodiment. [Diagram 5] FIG. 5 is a diagram showing an example of an etching rate according to the embodiment. [Figure 6] FIG. 6 is a diagram showing a schematic view of the state inside the chamber in the pre-coating step according to the embodiment. [Figure 7] FIG. 7 is a diagram showing an example of a change in film thickness in a conventional precoat. [Figure 8] FIG. 8 is a diagram showing an example of a change in film thickness in the precoat according to the embodiment. [Figure 9] FIG. 9 is a diagram showing another example of the change in film thickness in the pre-coating step according to the embodiment. [Figure 10] FIG. 10 is a diagram showing an example in which high frequency power for plasma generation is increased in the pre-coating step according to the embodiment. [Figure 11] FIG. 11 is a diagram showing another example in which the high frequency power for generating plasma is increased in the pre-coating step according to the embodiment. [Figure 12] FIG. 12 is a diagram showing an example of the relationship between the thickness of the precoat film and the ion energy of ions penetrating the precoat film. [Figure 13] FIG. 13 is a diagram showing an example of the relationship between the thickness of the precoat film and the ion energy of ions penetrating the precoat film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the disclosed substrate processing method will be described in detail with reference to the drawings. Note that the disclosed substrate processing method is not limited to this embodiment.
[0009] In the manufacture of semiconductor devices, a substrate such as a semiconductor wafer is placed in a chamber and a substrate process such as plasma etching is performed. The chamber has an inner wall covered with a metal compound such as Al (aluminum) or Y (yttrium). When a substrate process is performed in the chamber, the metal compound covering the inner wall of the chamber may peel off, and the peeled metal compound particles may cause shape abnormalities in the semiconductor device. Therefore, before performing the substrate process, the inside of the chamber is pre-coated to suppress contamination by the metal compound. The pre-coating is performed by generating plasma from a film forming material supplied into the chamber. At this time, ions may be incident on the parts in the chamber before the pre-coat film is formed, generating particles.
[0010] Therefore, a new technology is desired that can pre-coat the inside of the chamber while suppressing particle generation.
[0011] [Embodiment] [Configuration of deposition equipment] An embodiment will be described. In the following, a case where a plasma process such as plasma etching is performed as a substrate process will be mainly described as an example. FIG. 1 is a diagram showing a schematic configuration of a substrate processing apparatus 10 according to an embodiment. The substrate processing apparatus 10 is an example of a substrate processing apparatus according to an embodiment. The substrate processing apparatus 10 shown in FIG. 1 can be used to realize a substrate processing method according to an embodiment. The substrate processing apparatus 10 shown in FIG. 1 is a so-called inductively-coupled plasma (ICP) apparatus, and has a plasma source for generating inductively-coupled plasma. However, the substrate processing apparatus according to the embodiment may use plasma generated by other methods. For example, the substrate processing apparatus according to the embodiment may be an apparatus that uses capacitively-coupled plasma (CCP), ECR plasma (electron-cyclotron-resonance plasma), helicon wave excited plasma (HWP), surface wave plasma (SWP), or the like.
[0012] The substrate processing apparatus 10 includes a chamber 12. The chamber 12 is made of a metal containing Al (aluminum) or Y (yttrium). For example, the chamber 12 is made of Al. 2 O 3 Or, Y 2 O 3 The chamber 12 has, for example, a substantially cylindrical shape. A space 12c in which processing is performed is provided within the chamber 12.
[0013] A substrate support 14 is disposed below the space 12c. The substrate support 14 is configured to hold a substrate W placed thereon. The substrate W is, for example, a semiconductor wafer.
[0014] The substrate support 14 can be supported by a support mechanism 13. The support mechanism 13 extends upward from the bottom of the chamber 12 within the space 12c. The support mechanism 13 can be substantially cylindrical. The support mechanism 13 can be made of an insulating material such as quartz.
[0015] The substrate support 14 includes an electrostatic chuck 16 and a lower electrode 18. The lower electrode 18 includes a first plate 18a and a second plate 18b. The first plate 18a and the second plate 18b are made of a metal such as aluminum. The first plate 18a and the second plate 18b are, for example, substantially cylindrical. The second plate 18b is disposed on the first plate 18a. The second plate 18b is electrically connected to the first plate 18a.
[0016] The electrostatic chuck 16 is disposed on the second plate 18b. The electrostatic chuck 16 includes an insulating layer and a thin-film electrode disposed in the insulating layer. A DC power supply 22 is electrically connected to the thin-film electrode of the electrostatic chuck 16 via a switch 23. The electrostatic chuck 16 generates an electrostatic force from a DC voltage of the DC power supply 22. The electrostatic chuck 16 attracts and holds the substrate W by the generated electrostatic force.
[0017] In the substrate processing apparatus 10, an edge ring ER is disposed on the second plate 18b and around the second plate 18b so as to surround the outer periphery of the substrate W and the electrostatic chuck 16. The edge ring ER has a role of improving the uniformity of the process. The edge ring ER is made of, for example, silicon.
[0018] A flow path 24 is formed in the second plate 18b. A heat exchange medium such as a refrigerant is supplied to the flow path 24 from a temperature adjustment unit (e.g., a chiller unit) disposed outside the chamber 12 for temperature control. The temperature adjustment unit adjusts the temperature of the heat exchange medium. The heat exchange medium is supplied from the temperature adjustment unit to the flow path 24 through a pipe 26a. The heat exchange medium supplied from the temperature adjustment unit to the flow path 24 through the pipe 26a is returned to the temperature adjustment unit through a pipe 26b. After the temperature adjustment by the temperature adjustment unit, the heat exchange medium is returned to the flow path 24 in the substrate support 14. In this manner, the temperature of the substrate support 14, i.e., the temperature of the substrate W, can be adjusted.
[0019] The substrate processing apparatus 10 further includes a gas supply line 28 that extends through the substrate support 14 to the upper surface of the electrostatic chuck 16. A heat exchange gas, such as helium (He) gas, is supplied from a heat exchange gas supply mechanism through the gas supply line 28 to a space between the upper surface of the electrostatic chuck 16 and the lower surface of the substrate W. The heat exchange gas promotes heat exchange between the substrate support 14 and the substrate W.
[0020] Alternatively, a heater HT may be disposed in the substrate support 14. The heater HT is a heating device. The heater HT is embedded in, for example, the second plate 18b or the electrostatic chuck 16. The heater HT is connected to a heater power supply HP. The heater power supply HP supplies power to the heater HT, thereby adjusting the temperature of the substrate support 14 and, in turn, the temperature of the substrate W.
[0021] A radio frequency (RF) power supply 30 is connected to the lower electrode 18 of the substrate support 14 via a matching box 32. The radio frequency power supply 30 is an example of a radio frequency power supply for bias. The radio frequency power supply 30 supplies radio frequency power for bias to the lower electrode 18, and attracts ions to the substrate W placed on the substrate support 14. The frequency of the radio frequency power generated by the radio frequency power supply 30 is within a range of, for example, 400 kHz to 40.68 MHz. In one example, the frequency of the radio frequency power is 13.56 MHz.
[0022] The matching circuit 32 includes a circuit that performs matching between the output impedance from the high frequency power supply 30 and the impedance on the load side, that is, the lower electrode 18 side.
[0023] The substrate processing apparatus 10 further includes a shield 34 detachably attached to the inner wall of the chamber 12. The shield 34 is also disposed so as to surround the outer periphery of the support mechanism 13. The shield 34 prevents by-products generated by the processing from adhering to the chamber 12. The shield 34 is a Y 2 O 3 Alternatively, the ceramic member may be an aluminum member coated with a ceramic such as aluminum alloy.
[0024] An exhaust path is formed between the substrate support 14 and the side wall of the chamber 12. The exhaust path is connected to an exhaust port 12e formed in the bottom of the chamber 12. The exhaust port 12e is connected to an exhaust device 38 via a pipe 36. The exhaust device 38 includes a pressure adjustment unit and a vacuum pump such as a turbo molecular pump (TMP). A baffle plate 40 is disposed in the exhaust path, i.e., between the substrate support 14 and the side wall of the chamber 12. The baffle plate 40 has a plurality of through holes penetrating the baffle plate 40 in the thickness direction. The baffle plate 40 has a Y 2 O 3 Alternatively, the aluminum member may be one having a surface coated with a ceramic such as aluminum alloy.
[0025] An opening is formed in the upper side of the chamber 12. The opening is closed by a dielectric window 42. The dielectric window 42 is made of quartz or the like. The dielectric window 42 is, for example, a flat plate.
[0026] A gas supply port 12i is formed in the side wall of the chamber 12. The gas supply port 12i is connected to a gas supply unit 44 via a gas supply pipe 46. The gas supply unit 44 supplies various gases used in processing to the space 12c. The gas supply unit 44 includes a plurality of gas sources 44a, a plurality of flow rate controllers 44b, and a plurality of valves 44c. Although not shown in FIG. 1, a different gas supply port may be provided for each gas to be supplied to prevent the gases from being mixed together.
[0027] The multiple gas sources 44a include gas sources for various gases, which will be described later. One gas source may supply one or more gases. The multiple flow rate controllers 44b may be mass flow controllers (MFCs). The flow rate controllers 44b realize flow rate control by pressure control. Each gas source included in the multiple gas sources 44a is connected to a gas supply port 12i via a corresponding one of the multiple flow rate controllers 44b and a corresponding one of the multiple valves 44c. The position of the gas supply port 12i is not particularly limited. For example, the gas supply port 12i may be formed in the dielectric window 42 instead of the sidewall of the chamber 12.
[0028] An opening 12p is formed in the sidewall of the chamber 12. The opening 12p serves as a path for loading and unloading the substrate W. The substrate W is loaded from the outside into the space 12c of the chamber 12 through the opening 12p, and is unloaded from the space 12c to the outside of the chamber 12. A gate valve 48 is provided on the sidewall of the chamber 12, and is capable of opening and closing the opening 12p.
[0029] An antenna 50 and a shield 60 are disposed on the chamber 12 and the dielectric window 42. The antenna 50 and the shield 60 are disposed outside the chamber 12. In one embodiment, the antenna 50 includes an inner antenna element 52A and an outer antenna element 52B. The inner antenna element 52A is a spiral coil disposed in the center of the dielectric window 42. The outer antenna element 52B is a spiral coil disposed on the dielectric window 42 and on the outer periphery side of the inner antenna element 52A. The inner antenna element 52A and the outer antenna element 52B are each made of a conductive material such as copper, aluminum, stainless steel, or the like.
[0030] The inner antenna element 52A and the outer antenna element 52B are gripped and held together by a plurality of clamps 54. Each of the clamps 54 is rod-shaped. The clamps 54 extend radially from approximately the center of the inner antenna element 52A to the outer periphery of the outer antenna element 52B.
[0031] The antenna 50 is covered with a shield 60. The shield 60 includes an inner shield wall 62A and an outer shield wall 62B. The inner shield wall 62A has a cylindrical shape. The inner shield wall 62A is disposed between the inner antenna element 52A and the outer antenna element 52B and surrounds the inner antenna element 52A. The outer shield wall 62B has a cylindrical shape. The outer shield wall 62B is disposed outside the outer antenna element 52B and surrounds the outer antenna element 52B.
[0032] A disk-shaped inner shield plate 64A is disposed on the inner antenna element 52A. The inner shield plate 64A covers the opening of the inner shield wall 62A. A flat ring-shaped outer shield plate 64B is disposed on the outer antenna element 52B. The outer shield plate 64B covers the opening between the inner shield wall 62A and the outer shield wall 62B.
[0033] The shapes of the shield wall and shield plate included in the shield 60 are not limited to those described above. For example, the shield wall of the shield 60 may be a prism having a rectangular cross section.
[0034] The inner antenna element 52A and the outer antenna element 52B are connected to the high frequency power supply 70A and the high frequency power supply 70B, respectively. The high frequency power supply 70A and the high frequency power supply 70B are an example of a high frequency power supply for generating plasma. The inner antenna element 52A and the outer antenna element 52B are supplied with power of the same or different frequencies from the high frequency power supply 70A and the high frequency power supply 70B, respectively. When high frequency power is supplied from the high frequency power supply 70A to the inner antenna element 52A, an induction magnetic field is generated in the space 12c, which excites the gas in the space 12c to generate plasma above the center of the substrate W. On the other hand, when high frequency power is supplied from the high frequency power supply 70B to the outer antenna element 52B, an induction magnetic field is generated in the space 12c, which excites the gas in the space 12c to generate plasma in a ring shape above the outer periphery of the substrate W.
[0035] The electrical length of each of inner antenna element 52A and outer antenna element 52B is adjusted according to the frequency output from high frequency power supply 70A and high frequency power supply 70B. Therefore, the positions of inner shield plate 64A and outer shield plate 64B in the z-axis direction are adjusted independently by actuators 68A and 68B.
[0036] The substrate processing apparatus 10 further includes a controller 80. The controller 80 is, for example, a computer including a processor, a storage unit such as a memory, an input unit, a display, and the like. The controller 80 operates based on a control program and recipe data stored in the storage unit, and controls each unit of the substrate processing apparatus 10. For example, the controller 80 controls a plurality of flow rate controllers 44b, a plurality of valves 44c, an exhaust device 38, high frequency power supplies 70A and 70B, a high frequency power supply 30, a matching box 32, a heater power supply HP, and the like. The controller 80 reads out the program and data from the storage unit and controls each unit of the substrate processing apparatus 10, thereby performing substrate processing according to a substrate processing method according to an embodiment, which will be described later.
[0037] [An example of a process flow for a substrate processing method] The substrate processing apparatus 10 performs substrate processing by a substrate processing method described below. The substrate processing apparatus 10 also pre-coats the inside of a chamber 12 in which a substrate W is placed before performing substrate processing by a substrate processing method described below. The following description will be given taking as an example a case in which the substrate processing apparatus 10 performs plasma processing such as plasma etching as substrate processing.
[0038] 2 is a flow chart showing an example of a substrate processing method according to an embodiment of the present invention. The substrate processing apparatus 10 according to the embodiment performs plasma processing on a substrate W such as a semiconductor substrate by the substrate processing method.
[0039] In step S1, seasoning is performed so that the inside of the chamber 12 is in a state suitable for substrate processing. In the seasoning, for example, before starting plasma processing on the first substrate W, a dummy wafer is placed on the substrate support 14, and then plasma is generated to increase the inner surface temperature of the chamber 12.
[0040] In step S2, the inside of the chamber 12 is pre-coated. The details of this pre-coating process will be described later.
[0041] In step S3, the substrate W is carried into the chamber 12 through the opening 12p, and the substrate W is placed on the substrate support 14. In step S4, a plasma process is performed on the substrate W. For example, in step S4, plasma etching is performed on the substrate W. In step S5, the plasma-processed substrate W is carried out from the chamber 12 through the opening 12p. In step S6, the pre-coated film is removed from the chamber 12.
[0042] In step S7, it is determined whether or not to end the substrate processing sequence. For example, if there is an unprocessed substrate W in the lot, it is determined not to end the sequence (step S7: No), and the process proceeds to step S2, where the unprocessed substrate W is loaded and subjected to plasma processing. On the other hand, if the plasma processing has been performed on all substrates W in the lot, it is determined to end the sequence (step S7: Yes), and the process is terminated.
[0043] It is not necessary to perform the process of removing the precoat film in step S6. Also, the process of removing the precoat film in step S6 may be performed only once when the sequence is terminated. Also, if the precoat film can withstand multiple substrate processings, the precoat process in step S2 may not be performed for each substrate W, but may be performed for each substrate processing that the precoated film can withstand.
[0044] [First example of precoating] In conventional precoating, a precoat film is formed in the chamber 12 by plasma generated from a gas containing a film-forming material. However, after the start of precoating, if ions in the plasma are incident on the parts in the chamber 12 before the precoat film is formed, particles are generated.
[0045] FIG. 3 is a diagram showing a schematic diagram of the state inside the chamber 12 during conventional precoating. FIG. 3 shows a simplified view of the inside of the chamber 12. The chamber 12 has a substrate support 14 disposed therein. When plasma is generated inside the chamber 12, ions are incident on the parts disposed inside the chamber, such as the inner wall of the chamber 12, the substrate support 14, and the dielectric window 42 (hereinafter referred to as "parts inside the chamber"), and particles are generated inside the chamber 12. For example, an ion flux Γ that sputters the parts inside the chamber I is the plasma density N e and the electron temperature Te are related as shown in the following equation (1).
[0046] Gamma i ∝ N e ×(Te) 1 / 2 (1)
[0047] Therefore, the plasma density N e When the ion flux Γ increases, i increases, which results in an increase in the amount of particles generated.
[0048] Therefore, in the substrate processing method according to the embodiment, a pre-coating step is performed as follows: Fig. 4 is a flow chart showing an example of the pre-coating step in the substrate processing method according to the embodiment.
[0049] In step S11, the exhaust device 38 is controlled to adjust the pressure of the parts in the chamber 12 to a predetermined pressure suitable for pre-coating. The pressure in the chamber 12 is set to, for example, 100 mTorr or more.
[0050] In step S12, a first film of the precoat film is formed on the parts in the chamber by supplying a reactive gas containing a component of the first film from the gas supply unit 44 into the chamber 12. In step S12, the first film of the precoat film is formed on the parts in the chamber by, for example, CVD (Chemical Vapor Deposition). Specifically, the first film may be formed by supplying high frequency power for plasma generation from the high frequency power sources 70A and 70B and generating a first plasma from the reactive gas. At this time, the first plasma is generated under conditions that can suppress sputtering of the parts in the chamber. For example, in step S12, sputtering of the parts in the chamber by the first plasma may be suppressed by controlling at least one of the high frequency power for plasma generation, the high frequency power for bias, the pressure in the chamber, and the temperature in the chamber. In addition, when the reactive gas contains a halogen-containing gas, sputtering of the parts in the chamber by the first plasma may be suppressed by the concentration of the halogen-containing gas. In one example, sputtering of parts inside the chamber can be suppressed by controlling the high-frequency power for generating plasma and adjusting the potential difference between the parts inside the chamber and the plasma to 100 V or less or 50 V or less.
[0051] In step S12, the first film may be formed by ALD (Atomic Layer Deposition). In the case of ALD, a first reactive gas is supplied into the chamber 12, and the first reactive gas is adsorbed to the parts in the chamber. At this time, the excess first reactive gas that is not adsorbed to the parts in the chamber may be purged from the chamber 12. Thereafter, a second reactive gas is supplied into the chamber 12, and the first reactive gas adsorbed to the parts in the chamber is reacted with plasma (first plasma) generated from the second reactive gas, thereby forming the first film. ALD has a lower plasma density N e This allows the first film to be formed evenly on the parts inside the chamber.
[0052] Step S12 is performed until the thickness of the first film reaches a predetermined thickness that can protect parts inside the chamber from sputtering by plasma in the next step S12.
[0053] In step S13, a reactive gas containing the components of the second film is supplied from the gas supply unit 44 into the chamber 12, and a second film is formed on the surface of the first film using a second plasma generated from the reactive gas. The first film and the second film may be the same type of film or different types of films. The second film can be formed, for example, by CVD. Specifically, a reactive gas containing the components of the second film is supplied into the chamber 12, and a plasma (second plasma) is generated from the reactive gas, thereby forming the second film. At this time, the first film formed in step S12 protects the parts in the chamber from sputtering by the second plasma. Therefore, in step S13, the generation of particles during pre-coating can be suppressed.
[0054] The pre-coating conditions in step S13 are not particularly limited as long as the first film protects the parts inside the chamber from sputtering by the second plasma. For example, when the first film is formed by CVD in step S12, the conditions can be selected according to the pre-coating conditions in step S12 so as to satisfy at least one of the following (1) to (4): (1) The high frequency power for plasma generation supplied in step S13 is greater than the high frequency power for plasma generation supplied in step S12. (2) The bias high frequency power supplied in step S13 is greater than the bias high frequency power supplied in step S12. (3) The temperature in the chamber in step S13 is higher than the temperature in the chamber in step S12. (4) When the reactive gas contains a halogen-containing gas, the concentration of the halogen-containing gas in step S13 is higher than the concentration of the halogen-containing gas in step S12.
[0055] Step S13 is performed until the thickness of the precoat film made of the first film and the second film becomes thick enough to protect the parts inside the chamber from the plasma processing, and then the process proceeds to step S3 in FIG.
[0056] The pre-coat film may be, for example, a silicon-containing film, an organic film, or a metal-containing film. The silicon-containing film may be, for example, a silicon oxide film or a silicon nitride film. The metal-containing film may be, for example, a film containing a metal such as titanium (Ti), tantalum (Ta), ruthenium (Ru), aluminum (Al), hafnium (Hf), or tin (Sn), or a film containing an oxide, nitride, sulfide, or halide of these metals.
[0057] Hereinafter, examples of materials for forming various precoat films will be described.
[0058] When forming a silicon-containing film by CVD, a mixed gas of a silicon-containing gas and an oxygen-containing gas or a nitrogen-containing gas can be used as a reactive gas. When forming a silicon-containing film by ALD, a silicon-containing gas can be used as a first reactive gas, and an oxygen-containing gas or a nitrogen-containing gas can be used as a second reactive gas. More specifically, when forming a silicon oxide film, aminosilane, SiCl 4 or SiF 4 The oxygen-containing gas can be O 2 In the case of forming a silicon nitride film, the silicon-containing gas may be aminosilane, SiCl 4 , dichlorosilane, hexachlorodisilane, or the like can be used, and NH 2 Gas or N 2 Gas or the like can be used.
[0059] The organic film is, for example, C 2 H 4The plasma can be formed by generating plasma from a carbon-containing gas such as epoxide, carboxylic acid, carboxylic acid halide, carboxylic acid anhydride, isocyanate, or phenol. A first reaction gas such as epoxide, carboxylic acid, carboxylic acid halide, carboxylic acid anhydride, isocyanate, or phenol is supplied into the chamber 12, and the first reaction gas is adsorbed on the parts in the chamber. Then, the first reaction gas adsorbed on the parts in the chamber is mixed with an inorganic compound gas having an NH bond, an inert gas, or N 2 and H 2 Mixture of gases, H 2 O gas, H 2 and O 2 The plasma can be formed by reacting the first reactive gas with a plasma generated from a second reactive gas such as a mixed gas of the first reactive gas and the second reactive gas.
[0060] When forming a metal-containing film by CVD, a mixed gas of a metal-containing gas and an oxidizing gas or a reducing gas can be used as a reactive gas. When forming a metal-containing film by ALD, a metal-containing gas can be used as a first reactive gas, and an oxidizing gas or a reducing gas can be used as a second reactive gas. More specifically, a gas containing a metal such as Ti, Ta, Ru, Al, Hf, or Sn, or a gas containing an oxide, nitride, sulfide, or halide of these metals can be used as the first reactive gas. H 2 Hydrogen-containing gases such as O 2 Oxygen-containing gases such as H 2 Gas and N2 gas mixture or NH 3 A hydrogen- and nitrogen-containing gas, such as a gas containing hydrogen, can be used as the second reaction gas. When a hydrogen-containing gas is used as the second reaction gas, a metal-containing film can be formed, when an oxygen-containing gas is used, a metal oxide film can be formed, and when a hydrogen- and nitrogen-containing gas is used, a metal nitride film can be formed.
[0061] Here, the conditions for forming the first film by CVD in step S12 will be described in more detail. The sputtering rate of the parts in the chamber during the formation of the first precoat film varies depending on the potential of the parts in the chamber. FIG. 5 is a diagram showing an example of an etching rate according to an embodiment. FIG. 5 shows the etching rate of a Y film formed on a silicon substrate. 2 O 3 The membrane was then washed with Cl 2 5 shows the etching rate when plasma etching is performed using a gas. The vertical axis of FIG. 5 shows the etching rate (E / R). The horizontal axis shows the RF bias voltage. The etching rate corresponds to the sputtering rate of the parts in the chamber. The RF bias voltage corresponds to the potential difference between the plasma and the parts in the chamber. The RF bias voltage increases or decreases according to the magnitude of the high-frequency power for bias supplied from the high-frequency power source 30. As shown in FIG. 5, the etching rate decreases as the RF bias voltage decreases. For example, the etching rate decreases when the RF bias voltage is 100V or less, and becomes negative when the RF bias voltage is 50V or less. From this, it is considered that when the potential of the parts in the chamber is 100V or less, sputtering of the parts in the chamber is significantly suppressed. Also, when the potential of the parts in the chamber is 50V or less, sputtering of the parts in the chamber is considered to hardly occur. Therefore, when the potential of the parts in the chamber during pre-coating is 100V or less or 50V or less, sputtering of the parts in the chamber can be generally suppressed. For example, by setting the potential difference between the parts inside the chamber and the plasma to 100 V or less or 50 V or less, sputtering of the parts inside the chamber can be suppressed.
[0062] The conditions for controlling the potential of the parts in the chamber within the above range vary depending on the structure of the chamber 12, the magnitude of the high frequency power for plasma generation, the magnitude of the high frequency power for biasing, and the plasma generation method (ICP, CCP, SWP, etc.). The potential of the parts in the chamber also varies depending on the type of gas supplied into the chamber 12 and the pressure inside the chamber 12.
[0063] Therefore, in advance, in the substrate processing apparatus 10, conditions that allow the potential of the parts in the chamber to be controlled within the above range may be obtained, and the first film may be formed under those conditions. For example, a high frequency power for plasma generation that makes the potential difference between the parts in the chamber and the plasma 100V or 50V is obtained, and the data is stored in the storage unit of the controller 80. Then, in step S12, in the substrate processing method according to the embodiment, the controller 80 controls the high frequency power supplied from the high frequency power supply 70A for plasma generation and the high frequency power supply 70B based on the data stored in the storage unit of the controller 80. For example, the controller 80 controls the high frequency power supply 70A and the high frequency power supply 70B to supply high frequency power for plasma generation that makes the potential difference between the parts in the chamber and the plasma 50V or less or 100V or less. As a result, the parts in the chamber are not sputtered, and the first film is formed, and the inside of the chamber 12 is precoated.
[0064] Fig. 6 is a diagram showing a schematic diagram of the state inside the chamber 12 in the pre-coating step according to the embodiment. Fig. 6 shows the inside of the chamber 12 in a simplified manner, similar to Fig. 3. For example, in step S12, as shown in the upper diagram, low-density plasma is generated inside the chamber 12, and the parts inside the chamber are coated with a first film C1. In step S13, as shown in the lower diagram, high-density plasma is generated inside the chamber 12. At this time, ions are incident on the parts inside the chamber, but since the parts inside the chamber are coated with the first film C1, the generation of particles is suppressed.
[0065] Here, the change in film thickness in the conventional precoat and the change in film thickness in the precoat according to the embodiment will be described. FIG. 7 is a diagram showing an example of the change in film thickness in the conventional precoat. FIG. 7 shows the relationship between the high frequency power for plasma generation, the generated ion flux Γ I The amount of ion and the thickness of the precoat film are shown in Fig. 1. In the conventional precoat, a high-density plasma is generated in the chamber 12. When a high-density plasma is generated, the ion flux Γ I There is a possibility that the concentration of ions may increase rapidly, and before the precoat film is formed or before the precoat film reaches a sufficient thickness, ions may be incident on parts in the chamber, resulting in the generation of particles.
[0066] 8 is a diagram showing an example of a change in film thickness in pre-coating according to the embodiment. In FIG. 8, the high frequency power (RF Power) for plasma generation, the amount of generated ion flux Γ i , the change over time in the film thickness D of the precoat is shown. In step S12, high frequency power HF1 for plasma generation is supplied to generate a low density plasma (first plasma) in the chamber 12. In step S12, since the plasma is low density, the amount of ion flux Γ i1 In step S13, the deposition rate is low because the amount of ion flux is small and the deposition rate is low. When the first film C1 formed in step S12 reaches a predetermined thickness D1, the process proceeds to step S13. In step S13, high-frequency power HF2 for plasma generation is supplied to generate high-density plasma (second plasma) in the chamber 12. In step S13, since the plasma is high-density, the deposition rate is high and the second film can be formed quickly. In step S13, since the plasma is high-density, the amount of ion flux Γ i2 However, the first film C1 can protect the parts inside the chamber from sputtering caused by the second plasma. In this way, the precoat according to the embodiment can quickly precoat while suppressing the generation of particles.
[0067] In addition, in FIG. 8, a case where a film is continuously formed in step S12 has been described as an example. However, this is not limited to this. A film may be intermittently formed in step S12. FIG. 9 is a diagram showing another example of a change in film thickness in the pre-coating process according to the embodiment. FIG. 9 shows a change in film thickness in accordance with a change in plasma RF power, a timing of performing ALD or CVD, an amount of ion flux generated Γ i 10 shows the change over time in the thickness D of the precoat. In step S12, the gas of the precoat material and the high frequency power HF for generating plasma are intermittently supplied to form a film.
[0068] In step S12, the high frequency power for plasma generation may be increased in accordance with an increase in the thickness of the first film. Fig. 10 is a diagram showing an example in which the high frequency power for plasma generation is increased in the pre-coating step according to the embodiment. Fig. 10 shows the relationship between the high frequency power for plasma generation (RF Power), the amount of ion flux generated Γ i 10 shows the change over time in the thickness D of the precoat. In step S12, the high frequency power for generating plasma is increased stepwise in accordance with the increase in thickness D to form a film.
[0069] In step S12, whether the ions reach the parts in the chamber and damage them, scattering particles, is determined by the relationship between the energy of the ions and the thickness of the first film C1. Therefore, in step S12, the high frequency power for generating plasma may be increased in accordance with the increase in the thickness of the first film C1, within the range in which the ions do not penetrate the first film C1.
[0070] FIG. 11 is a diagram showing another example in which the high frequency power for plasma generation is increased in the precoating step according to the embodiment. FIG. 11 shows the change over time of the high frequency power for plasma generation (RF Power) and the film thickness of the precoat film. In step S12, first, the bias RF power is adjusted so that the potential difference between the parts in the chamber and the plasma is 50V or less, and the first film C1 is formed until the film thickness reaches D1. The high frequency power for plasma generation supplied until the film thickness reaches D1 may be constant or may vary as long as the potential difference between the parts in the chamber and the plasma is 50V or less. For example, the high frequency power for plasma generation may be varied so that the potential difference between the plasma and the chamber increases at a constant rate as shown in FIG. 11(a), or the high frequency power for plasma generation may be varied so that the increase rate gradually increases or decreases as shown in FIG. 11(b) and (c). After the thickness of the first film C1 reaches D1, the first film C1 may be formed until the thickness reaches D2 at which ions no longer penetrate the first film C1 while increasing the high frequency power for plasma generation within a range in which ions do not penetrate the first film C1 as a transition period. After the thickness reaches D2, the ions do not penetrate the first film C1, so the process proceeds to step S13, in which the film formation rate is even higher.
[0071] In the transition period, the bias RF power may be increased within a range where ions do not penetrate the first film C1. Figures 12 and 13 are diagrams showing an example of the relationship between the thickness of the precoat film and the ion energy of ions penetrating the precoat film. Figure 12 shows a case where the precoat film is SiO 2FIG. 13 is an example of forming an organic film as the precoat film. FIG. 12 and FIG. 13 show the relationship between the thickness of the precoat film and the ion energy (Vmax) required for ions to penetrate the precoat film of the thickness. As shown in FIG. 12 and FIG. 13, the thicker the film, the greater the ion energy required to penetrate the precoat film. In FIG. 12 and FIG. 13, the range of film thickness that ions do not penetrate is shown by the shaded area. The film thickness D2 is the film thickness of the shaded area that does not penetrate even with the ion energy of the ions generated in step S12. In the transition period, the first film C1 is deposited to a film thickness D2 that does not penetrate even with the maximum ion energy of the ions generated in step S12. As a result, the ions do not penetrate the first film C1, so that the generation of particles can be suppressed.
[0072] [Second example of playing court] In the first example of the precoat described above, the first film is formed using plasma, but it is also possible to form the first film without using plasma. In this case, for example, a gas containing a first organic compound and a gas containing a second organic compound can be used as the reactive gas. The second organic compound may be an organic compound different from the first organic compound.
[0073] In step S12 of the second example, a gas containing a first organic compound is supplied into the chamber 12, and the first organic compound is adsorbed onto the surface of the parts inside the chamber. At this time, the first organic compound that has not been adsorbed onto the parts inside the chamber may be purged from the chamber 12. Thereafter, a gas containing a second organic compound is supplied into the chamber 12, and the first organic compound adsorbed onto the surface of the parts inside the chamber and the second organic compound are polymerized to form the first film. In the second example, no plasma is used when forming the first film, so that the parts inside the chamber are not sputtered by the first plasma.
[0074] In the second example, for example, isocyanate, carboxylic acid, or carboxylic acid halide can be used as the first organic compound. For example, amine or a compound having a hydroxyl group can be used as the second organic compound. For example, carboxylic acid anhydride can be used as the first organic compound, and amine can be used as the second organic compound. For example, bisphenol A can be used as the first organic compound, and diphenyl carbonate or epichlorohydrin can be used as the second organic compound. Regardless of which organic compound is used, the parts in the chamber may be heated by a heater or the like to promote the polymerization reaction.
[0075] [effect] Thus, the substrate processing according to the embodiment includes a step of forming a precoat film on the chamber internal parts (e.g., the inner wall of the chamber 12, the substrate support 14, and the dielectric window 42) arranged in the chamber 12 (step S2, steps S11 to S13), and (b) a step of processing one or more substrates after step (a) (step S4). Step (a) includes a step (a1) of forming a first film on the chamber internal parts without using plasma or using a first plasma generated under conditions capable of suppressing sputtering of the chamber internal parts (step S12), and a step (a2) of forming a second film on the surface of the first film using a second plasma (step S13). As a result, the substrate processing according to the embodiment can precoat the inside of the chamber 12 while suppressing generation of particles.
[0076] In the substrate processing according to the embodiment, step (a1) forms a first film on the chamber parts using a first plasma generated from a reactive gas under conditions that can suppress sputtering of the chamber parts. This makes it possible to suppress sputtering of the chamber parts when forming the first film in the substrate processing according to the embodiment.
[0077] In the substrate processing according to the embodiment, the step (a1) is performed under at least one of the following conditions: (1) the high frequency power for plasma generation supplied in the step (a2) is higher than the high frequency power for plasma generation supplied in the step (a1), (2) the high frequency power for bias supplied in the step (a2) is higher than the high frequency power for bias supplied in the step (a1), (3) the temperature in the chamber in the step (a2) is higher than the temperature in the chamber in the step (a1), and (4) the reactive gas contains a halogen-containing gas, and the concentration of the halogen-containing gas in the step (a2) is higher than the concentration of the halogen-containing gas in the step (a1). As a result, the substrate processing according to the embodiment can suppress sputtering of parts in the chamber when forming the first film, and can pre-coat the inside of the chamber 12 while suppressing the generation of particles.
[0078] In the substrate processing according to the embodiment, in step (a1), the potential difference between the parts in the chamber and the first plasma is equal to or less than 100 V. As a result, the substrate processing according to the embodiment can form the first film while suppressing sputtering of the parts in the chamber, and can suppress generation of particles.
[0079] In the substrate processing according to the embodiment, in step (a1), the potential difference between the parts in the chamber and the first plasma is equal to or less than 50 V. As a result, the substrate processing according to the embodiment can form the first film while further suppressing sputtering of the parts in the chamber, and can further suppress generation of particles.
[0080] In the substrate processing according to the embodiment, the step (a1) is performed under the condition that the high frequency power for generating plasma is increased stepwise. This allows the substrate processing according to the embodiment to quickly form the first film while suppressing the generation of particles, and allows the inside of the chamber 12 to be quickly pre-coated in the step (a1).
[0081] In the substrate processing according to the embodiment, step (a1) is performed until the first film has a thickness sufficient to protect the parts inside the chamber from the second plasma, thereby suppressing the generation of particles when forming the second film in step (a2).
[0082] Although the embodiments have been described above, the disclosed embodiments should be considered to be illustrative and not restrictive in all respects. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the claims.
[0083] For example, in the above embodiment, the substrate processing is plasma etching, and pre-coating is performed inside the chamber 12 before the plasma etching. However, the present invention is not limited to this. The substrate processing may be any substrate processing that involves pre-coating.
[0084] In the above embodiment, the pre-coating process in step S2 is performed for each substrate W. However, this is not limited to the above. The pre-coating process in step S2 may be performed according to a predetermined substrate processing time, a predetermined number of substrates to be processed, or a predetermined number of substrate processing lots.
[0085] In addition, among the steps of forming the precoat film according to the embodiment, the step (a1) (step S12) of forming the first film using the first plasma may further include a step of acquiring information on the light emission state of the first plasma using a detector, and a step of estimating the film thickness of the first film deposited on the parts inside the chamber 12 from the acquired information. For example, a detector such as an optical sensor that detects the light emission state such as the color and light emission intensity of the plasma is provided in the chamber 12, and the light emission spectrum of each wavelength is measured based on the information on the light emission state of the plasma detected by the detector. The measured light emission spectrum of each wavelength varies depending on the film formation rate. The film formation rate may be estimated from the light emission spectrum of each wavelength to estimate the film thickness of the first film deposited on the parts inside the chamber 12, and the degree of the first film thickness deposited on the chamber parts may be estimated. Then, when the estimated film thickness of the first film reaches a predetermined thickness that can protect the parts inside the chamber from the second plasma, the step of forming the second film may be performed.
[0086] Furthermore, the step (a1) (step S12) of forming the first film using the first plasma may further include a step of obtaining information on the film formation characteristics from the acquired information and adjusting the film formation conditions. For example, a correlation between each light emission state of the plasma and the film formation characteristics such as the film formation rate is obtained in advance, and the correlation information is stored in a storage unit of the controller 80. Then, based on the correlation information stored in the storage unit, the film formation characteristics such as the film formation rate may be obtained from the light emission state of the plasma detected by the detector, and the film formation conditions may be adjusted so that the film formation characteristics are optimized.
[0087] Similarly, the process (a2) (step S13) of forming a second film using the second plasma may further include a process of acquiring information on the light emission state of the second plasma using a detector, and a process of calculating a film formation rate from the acquired information to estimate a film thickness of the second film deposited on the parts inside the chamber. The process (a2) (step S13) of forming a second film using the second plasma may further include a process of acquiring information on film formation characteristics from the acquired information and adjusting film formation conditions.
[0088] The light emission state of the plasma in the chamber 12 also changes depending on the state of the precoated film. For example, when the precoated film is reduced by processing the substrate, the light emission state of the plasma changes. Therefore, the precoating process in step S2 may be performed based on the plasma light emission state in step S4. For example, a detector for detecting the light emission state such as the color and light emission intensity of the plasma may be provided in the chamber 12, and when the light emission state detected by the detector is a light emission state in a state where the precoated film is reduced, the precoating process in step S2 may be performed.
[0089] In the above embodiment, the substrate is a semiconductor wafer, but the present invention is not limited to this. The substrate may be any substrate.
[0090] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be construed as limiting. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]
[0091] 10 Substrate processing equipment 12. Chamber 30 High frequency power supply 80 Controller W substrate C1 First membrane
Claims
1. (a) forming a precoat film on a chamber part disposed in a chamber; (b) after step (a), processing one or more substrates; Including, The step (a) (a1) forming a first film on the chamber internal part by using a first plasma generated from a reactive gas, while setting a potential difference between the chamber internal part and the first plasma to 100 V or less; (a2) forming a second film on a surface of the first film using a second plasma; A method for processing a substrate, comprising:
2. The step (a) (1) the high frequency power for plasma generation supplied in the step (a2) is greater than the high frequency power for plasma generation supplied in the step (a1); (2) the bias high frequency power supplied in the step (a2) is greater than the bias high frequency power supplied in the step (a1); (3) the temperature in the chamber in the step (a2) is higher than the temperature in the chamber in the step (a1); and (4) The reaction gas contains a halogen-containing gas, and the concentration of the halogen-containing gas in the step (a2) is higher than the concentration of the halogen-containing gas in the step (a1); The process is executed under the condition that at least one of the following conditions is satisfied: The method for processing a substrate according to claim 1 .
3. In the step (a1), a potential difference between the chamber internal parts and the first plasma is 50 V or less. The substrate processing method according to claim 1 .
4. The step (a1) is carried out under the condition that the high frequency power for generating plasma is increased stepwise. The substrate processing method according to any one of claims 1 to 3.
5. the reaction gas includes a first reaction gas and a second reaction gas; The step (a1) supplying a first reaction gas into the chamber and allowing the first reaction gas to be adsorbed by parts in the chamber; supplying a second reactive gas into the chamber and reacting the first reactive gas adsorbed on the parts in the chamber with the first plasma generated from the second reactive gas, thereby forming the first film; The method of claim 1 , comprising:
6. The step (a1) acquiring information regarding a light emission state of the first plasma using a detector; estimating a thickness of the first film deposited on the chamber internal part from the acquired information; The substrate processing method according to claim 1 , further comprising:
7. The step (a1) further includes a step of adjusting a film formation condition based on the acquired information. The substrate processing method according to claim 6 .
8. (a) forming a precoat film on a chamber part disposed in a chamber; (b) after step (a), processing one or more substrates; Including, The step (a) (a1) forming a first film on the chamber part without using plasma; (a2) forming a second film on a surface of the first film using a second plasma; Including, The step (a1) supplying a gas containing a first organic compound into the chamber and allowing the first organic compound to be adsorbed onto parts in the chamber; supplying a gas containing a second organic compound into the chamber and polymerizing the first organic compound adsorbed on the parts inside the chamber with the second organic compound to form the first film; A method for processing a substrate, comprising:
9. Step (a1) is performed until the first film has a thickness sufficient to protect the chamber parts from the second plasma. The substrate processing method according to any one of claims 1 to 8.
10. The first film and the second film are the same type of film. The substrate processing method according to any one of claims 1 to 9.
11. The step (a) is performed according to a predetermined processing time for the substrate, the number of substrates to be processed, or the number of substrate processing lots. The substrate processing method according to any one of claims 1 to 10.
12. The step (a2) acquiring information about an optical emission state of the second plasma using a detector; estimating a thickness of the second film deposited on the chamber internal part from the acquired information; Further comprising: The substrate processing method according to any one of claims 1 to 11.
13. The step (a2) further includes a step of adjusting a film formation condition based on the acquired information. The method of claim 12.
Citation Information
Patent Citations
Semiconductor device manufacturing method
JP2014187248A
Chamber undercoat preparation method for low temperature ald films
JP2015122486A
Precoat method and film deposition method
JP2019123900A
In-situ pre-coating of plasma etch chamber for improved productivity and chamber condition control
US7204913B1
Plasma doping method and plasma doping apparatus
WO2008050596A1