Biodegradable short fiber nonwoven fabric
A biodegradable short fiber nonwoven fabric combining cellulose and poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) fibers addresses the issues of strength and biodegradability, offering improved mechanical properties and environmental friendliness.
Patent Information
- Application Number
- JP2021010368
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-26
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-01-26
AI Technical Summary
Existing biodegradable short fiber nonwoven fabrics lack sufficient tensile strength and texture, and biodegradability is compromised when using polyethylene terephthalate fibers.
A biodegradable short fiber nonwoven fabric composed of cellulose short fibers and poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) fibers, which enhances mechanical strength, flexibility, and biodegradability.
The fabric achieves high tensile strength, flexibility, and complete biodegradability, suitable for industrial and daily life applications, particularly in wet-laid nonwoven fabrics.
Smart Images

Figure 0007580283000001 
Figure 0007580283000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a biodegradable staple fiber nonwoven fabric which has good biodegradability, as well as excellent mechanical strength and texture. [Background technology]
[0002] Plastics are widely used in industrial materials such as packaging materials and containers. However, plastic waste is a cause of a large burden on the global environment, such as impacts on ecosystems, generation of harmful gases during combustion, and global warming due to the large amount of heat generated by combustion. As one solution to such problems, the use of biodegradable plastics has been carried out. For example, Patent Document 1 proposes a biodegradable short fiber nonwoven fabric made by three-dimensionally entangling short fibers made of a biodegradable thermoplastic polymer and short cellulose fibers. In addition, Patent Document 2 proposes a microbially degradable nonwoven fabric made of fibers made of poly-ε-caprolactone and / or poly-β-propiolactone and natural fibers or cellulose fibers.
[0003] On the other hand, wetlaid nonwoven fabrics using cellulosic short fibers such as natural pulp are reinforced with binder fibers to increase their strength. For example, Patent Document 3 describes the production of high-strength paper using polyethylene terephthalate fibers. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-200457 [Patent Document 2] Japanese Patent Application Publication No. 5-214648 [Patent Document 3] JP 2013-174028 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is a demand for further improvement in tensile strength and texture of the short fiber nonwoven fabrics described in Patent Documents 1 and 2. In addition, when the polyethylene terephthalate fiber described in Patent Document 3 is used, there is a problem that the biodegradability of the nonwoven fabric is poor.
[0006] In order to solve the above-mentioned problems in the conventional art, the present invention provides a biodegradable staple fiber nonwoven fabric which has good biodegradability, as well as excellent mechanical strength and texture. [Means for solving the problem]
[0007] In one or more embodiments, the present invention relates to a biodegradable staple fiber nonwoven fabric comprising cellulosic staple fiber A and staple fiber B containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate). Effect of the Invention
[0008] The present invention can provide a biodegradable staple fiber nonwoven fabric which has good biodegradability, as well as excellent mechanical strength and texture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present inventors have conducted extensive research to solve the above problems, and as a result have found that by using cellulosic staple fiber A and staple fiber B containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) in combination, a biodegradable staple fiber nonwoven fabric having high biodegradability and mechanical strength and a soft feel can be obtained, and in particular, even in the case of a wet-laid nonwoven fabric, the fabric has high biodegradability and mechanical strength and is excellent in feel.
[0010] (Short Cellulosic Fiber A) The cellulose-based short fiber A is not particularly limited, and may be either a natural cellulose fiber or a regenerated cellulose fiber.
[0011] The natural cellulose fiber may be of plant origin or animal origin. For example, plant-derived pulp can be used. For example, plant-derived pulp can be pulped from a plant raw material by chemical, mechanical or a combination of both. For example, plant raw materials can be pulped from wood, cotton, bamboo, hemp, shoots, kenaf, etc.
[0012] The natural cellulose fibers are not particularly limited, but from the viewpoint of excellent water dispersibility and miscibility with the short fiber B and suitable use in wetlaid nonwoven fabrics, the average fiber length is preferably 1 to 10 mm, more preferably 2 to 8 mm, and even more preferably 3 to 7 mm. In one or more embodiments of the present invention, the average fiber length of the natural cellulose fibers can be measured, for example, by the method of JIS P 8226-2.
[0013] The natural cellulose fibers are not particularly limited, but from the viewpoint of, for example, excellent water dispersibility and miscibility with short fiber B and suitable use in wetlaid nonwoven fabrics, the average fiber diameter is preferably 5 to 100 μm, more preferably 10 to 60 μm, and even more preferably 20 to 40 μm. In one or more embodiments of the present invention, the average fiber diameter of the natural cellulose fibers can be calculated by measuring the diameters of a certain number of fibers (e.g., 20 fibers) using a microscope and taking the arithmetic average.
[0014] Examples of regenerated cellulose fibers include rayon, polynosic, cupra, and lyocell.
[0015] The regenerated cellulose fibers are not particularly limited, but from the viewpoint of excellent water dispersibility and miscibility with the short fiber B and suitable use in wetlaid nonwoven fabrics, the average fiber length is preferably 1 to 10 mm, more preferably 2 to 8 mm, and even more preferably 3 to 7 mm. In one or more embodiments of the present invention, the average fiber length of the regenerated cellulose fibers can be measured in accordance with JIS L 1015.
[0016] The regenerated cellulose fiber is not particularly limited, but from the viewpoint of excellent water dispersibility and miscibility with the short fiber B and suitable use in wetlaid nonwoven fabrics, the single fiber fineness is preferably 0.5 to 20 dtex, more preferably 1 to 10 dtex, and even more preferably 1 to 5 dtex. In one or more embodiments of the present invention, the single fiber fineness of the regenerated cellulose fiber is measured in accordance with JIS L 1015.
[0017] (Short Fiber B) In one or more embodiments of the present invention, "containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate)" means containing 80% by weight or more of poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate), preferably 85% by weight or more, more preferably 90% by weight or more. Short fiber B may be composed of 100% by weight of poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0018] Poly(3-hydroxyalkanoates) containing 3-hydroxyalkanoates such as 3-hydroxybutyrate are widely used as biodegradable thermoplastic polymers. The present inventors have found that, when used in combination with cellulosic staple fibers, short fiber B containing poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), which is a copolymer of 3-hydroxybutyrate and 3-hydroxyhexanoate, maintains high biodegradability while exhibiting excellent reinforcing properties as a binder fiber, can improve the mechanical strength of nonwoven fabrics, particularly wet-laid nonwoven fabrics, and can impart a soft texture to nonwoven fabrics, particularly wet-laid nonwoven fabrics.
[0019] Poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter simply referred to as "P3HB3HH") has a composition ratio of repeating units (monomer structural units) that is not particularly limited. However, from the perspective of the balance between flexibility and strength, the molar ratio of 3-hydroxybutyrate / 3-hydroxyhexanoate is preferably from 99 / 1 to 80 / 20, and more preferably from 97 / 3 to 85 / 15. P3HB3HH may be used alone or as a mixture of two or more with different composition percentages of 3HB. In one or more embodiments of the present invention, the composition ratio of the monomers in P3HB3HH can be measured as follows.
[0020] <Composition ratio of monomers in P3HB3HH> Add 2 mL of a sulfuric acid-methanol mixture (15:85) and 2 mL of chloroform to about 20 mg of the sample, seal it, and heat at 100 °C for 140 minutes to obtain methyl esters of the polyester degradation products. After cooling, add 1.5 g of sodium hydrogen carbonate little by little to neutralize it, and leave it standing until the generation of carbon dioxide gas stops. Add 4 mL of diisopropyl ether, mix well, then centrifuge, and analyze the composition of the methyl hydroxyalkanoate of the polyester degradation products in the supernatant by capillary gas chromatography to determine the composition ratio (monomer ratio) of the monomer units of P3HB3HH.
[0021] P3HB3HH is not particularly limited and can be produced by a known method. When P3HB3HH is produced by a microorganism, Aeromonas caviae, C. necator, and the like are known as the microorganism. In addition, in order to increase the productivity of P3HB3HH, Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) or the like into which genes of a group of enzymes synthases for poly(3-hydroxyalkanoate) have been introduced may be used. In addition, as P3HB3HH, a commercially available product such as biodegradable polymer PHBH (registered trademark) manufactured by Kaneka Corporation may be used.
[0022] P3HB3HH is not particularly limited, but from the viewpoint of moldability and strength, the weight average molecular weight is preferably 50,000 to 3,000,000, and more preferably 100,000 to 1,500,000. In one or more embodiments of the present invention, the weight average molecular weight is measured from the polystyrene equivalent molecular weight distribution using gel permeation chromatography (GPC) using a chloroform eluent. As a column for the GPC, a column appropriate for measuring the molecular weight may be used.
[0023] Although there are no particular limitations on P3HB3HH, the melt flow rate (MFR) measured in accordance with JIS K 7210-1 at a temperature of 165° C. and a load of 5 kg (49 N) is preferably 0.1 to 100 g / 10 min, more preferably 1 to 50 g / 10 min, and even more preferably 10 to 40 g / 10 min. If the melt flow rate is too low, the fluidity of the molten resin is insufficient, and if it is too high, the fluidity is too high, and in either case, spinning of fibers tends to be difficult.
[0024] The short fibers B may be composed of a resin composition containing P3HB3HH. The resin composition is not particularly limited, but preferably contains 80% by weight or more of P3HB3HH, more preferably 85% by weight or more, and even more preferably 90% by weight or more. On the other hand, the upper limit may be 100% by weight, but may be, for example, 98% by weight or less or 95% by weight or less. By making the content of P3HB3HH 80% by weight or more, the biodegradability of the obtained nonwoven fabric tends to be further improved.
[0025] The resin composition is not particularly limited, but preferably further contains a crystal nucleating agent from the viewpoint of productivity. The crystal nucleating agent is not particularly limited as long as it is a compound that has the effect of promoting the crystallization of P3HB3HH. For example, from the viewpoint of improving the crystallization rate and being contained in the fiber, pentaerythritol, sugar alcohol compounds, polyvinyl alcohol, chitin, chitosan, etc. are preferable, and pentaerythritol is more preferable. These may be used alone or in combination of two or more.
[0026] The content of the crystal nucleating agent in the resin composition is not particularly limited, but is preferably 0.05 to 12 parts by weight, more preferably 0.1 to 10 parts by weight, even more preferably 0.5 to 8 parts by weight, and particularly preferably 1 to 5 parts by weight, relative to 100 parts by weight of P3HB3HH. By making the content of the crystal nucleating agent 0.05 parts by weight or more, the crystallization promotion effect is improved, and the productivity of the fiber tends to be improved. In addition, by making the content of the crystal nucleating agent 12 parts by weight or less, it is easy to suppress the decrease in viscosity during processing and the decrease in fiber properties, while maintaining a sufficient crystallization rate promotion effect.
[0027] The resin composition is not particularly limited, but preferably further contains a lubricant from the viewpoint of productivity. The lubricant is not particularly limited as long as it is a compound that has the effect of imparting lubricity to P3HB3HH. Examples of the lubricant include fatty acid amide, alkylene fatty acid amide, glycerin mono fatty acid ester, organic acid monoglyceride, sorbitan fatty acid ester, polyglycerin fatty acid ester, and higher alcohol fatty acid ester.
[0028] Among the above lubricants, compounds having an effect of imparting external lubricity, specifically fatty acid amides and glycerin fatty acid esters, are particularly preferred. Examples of fatty acid amides include fatty acid monoamides and bisamides. The fatty acid (fatty acid moiety) constituting the fatty acid amide preferably has 12 to 30 carbon atoms, more preferably 18 to 22 carbon atoms, from the viewpoint of making the melting point of the resin composition moderately high and suppressing a decrease in processability during melt processing. Specific examples of fatty acid amides include behenic acid amide, erucic acid amide, palmitic acid amide, oleic acid amide, stearic acid amide, methylene bis stearic acid amide, ethylene bis stearic acid amide, ethylene bis oleic acid amide, and ethylene bis erucic acid amide. Examples of glycerin fatty acid esters include glycerin monoesters, glycerin diesters, and glycerin triesters (e.g., glycerin diacetomonoesters such as glycerin diacetomonolaurate, glycerin diacetomonooleate, glycerin diacetomonostearate, glycerin diacetomonocaprylate, and glycerin diacetomonodecanoate). These may be used alone or in combination of two or more.
[0029] The content of the lubricant in the resin composition is not particularly limited, but is preferably 0.05 to 12 parts by weight, more preferably 0.1 to 10 parts by weight, even more preferably 0.5 to 8 parts by weight, and particularly preferably 1 to 5 parts by weight, relative to 100 parts by weight of P3HB3HH. By making the content of the lubricant 0.05 parts by weight or more, friction between the resin composition and the metal surface in the extruder or spinning machine is suppressed, decomposition of P3HB3HH due to shear heat is suppressed, and adhesion of the fibers extruded from the nozzle to each other is also easily prevented. In addition, by making the content of the lubricant 12 parts by weight or less, P3HB3HH is melted more efficiently in the extruder, and as a result, the fibers do not become too hard and yarn breakage is suppressed, and productivity is easily improved.
[0030] The resin composition may contain other components such as plasticizers, inorganic fillers, organic fillers (such as cellulose), antioxidants, ultraviolet absorbers, colorants such as dyes and pigments, and antistatic agents, as necessary, within the range that does not impair the effects of the present invention. The amount of other components added may be 5 parts by weight or less, or 1 part by weight or less, per 100 parts by weight of P3HB3HH.
[0031] The resin composition may contain resin components other than P3HB3HH (other resin components) within a range that does not impair the effects of the present invention. Examples of the other resin components include biodegradable resins, such as petroleum-derived resins such as polylactic acid, polybutylene adipate terephthalate, polybutylene succinate adipate, and polybutylene succinate, and natural polymers such as starch and cellulose. The content of the other resin components is preferably 20% by weight or less, more preferably 10% by weight or less, and even more preferably 5% by weight or less, based on the total amount (100% by weight) of the resin components. The other resin components may be used alone or in combination of two or more types.
[0032] The short fibers B can be produced, for example, by melt-spinning the above-mentioned resin composition to obtain a multifilament, and then cutting the multifilament to a predetermined fiber length.
[0033] First, the pellet-shaped resin composition obtained by melt-kneading the resin composition is melted using a melt extruder, and is continuously extruded from a spinneret (also called a spinning die) to form fibers, thereby producing spun filaments. The melt spinning temperature is, for example, preferably 145 to 190°C, more preferably 150 to 190°C, and even more preferably 150 to 180°C. By setting the melt spinning temperature at 145°C or higher, the resin composition can be sufficiently dissolved, so that spinning is easily stabilized. In addition, by setting the spinning temperature at 190°C or lower, the thermal decomposition of P3HB3HH is suppressed, spinning is easily stabilized, and the physical properties of the obtained fiber tend to be further improved. The melt spinning temperature refers to the highest temperature range of temperatures applied during the fiberization of the resin composition.
[0034] The resin composition is not particularly limited, but from the viewpoints of moldability and strength, the weight average molecular weight is preferably 50,000 to 3,000,000, and more preferably 100,000 to 1,500,000.
[0035] The resin composition is not particularly limited, but for example, the melt flow rate (MFR) measured according to JIS K 7210-1 at a temperature of 165° C. and a load of 5 kg (49 N) is preferably 0.1 to 100 g / 10 min, more preferably 1 to 50 g / 10 min, and even more preferably 10 to 40 g / 10 min. If the melt flow rate is too low, the fluidity of the molten resin composition is insufficient, and if it is too high, the fluidity is too high, and in either case, spinning of fibers tends to be difficult.
[0036] The temperature of the atmosphere extruded from the spinneret is not particularly limited, and can be appropriately adjusted within the range of, for example, 5 to 40°C. It is preferable to apply rectified air to the fiber (spun filament) extruded from the spinneret. The rectified air is also called quench air, and has the function of stabilizing the flow of the yarn. It is also possible to cool the spun filament by using a cooled gas as the quench air. The temperature of the quench air is preferably 5 to 40°C, more preferably 10 to 30°C. If it is lower than 5°C, residual stress may occur in the fiber, and the fiber may shrink. If it is higher than 40°C, the resin may not be solidified sufficiently, and the fiber may stick. The wind speed of the quench air is preferably 0.1 to 3.0 m / sec. If it is lower than 0.1 m / sec, the effect of rectification is likely to be low, and if it is higher than 3.0 m / sec, the quench air is too strong, which may cause the yarn to become turbulent, and may cause the fibers to stick to each other or break.
[0037] Next, the spun filament is drawn and thinned to obtain a drawn filament (multifilament) of the desired fineness. The spinning speed by air drawing is preferably 200 to 7000 m / min, more preferably 500 to 7000 m / min, further preferably 700 to 5000 m / min, and particularly preferably 700 to 3000 m / min. Before drawing, an oil may be applied as necessary.
[0038] The staple fibers B are not particularly limited, but from the viewpoint of excellent water dispersibility and miscibility with the cellulose staple fibers A and suitable use in wetlaid nonwoven fabrics, the staple fibers B preferably have a single fiber fineness of 0.1 to 50 dtex, more preferably 0.5 to 25 dtex, and even more preferably 1.0 to 10 dtex. In one or more embodiments of the present invention, the single fiber fineness of the staple fibers B is measured in accordance with JIS L 1015.
[0039] The staple fibers B are not particularly limited, but from the viewpoint of excellent water dispersibility and miscibility with the cellulose staple fibers A and suitable use in wetlaid nonwoven fabrics, the average fiber length of the staple fibers B is preferably 1 to 10 mm, more preferably 2 to 8 mm, and even more preferably 3 to 7 mm. In one or more embodiments of the present invention, the average fiber length of the staple fibers B can be measured in accordance with JIS L 1015.
[0040] The short fiber B is not particularly limited, but for example, the melting point is preferably 110 to 165°C, more preferably 120 to 155°C, and further preferably 130 to 150°C. When the melting point of the short fiber B is 110°C or higher, the mechanical strength of the biodegradable short-fiber nonwoven fabric is improved. When the melting point of the short fiber B is 165°C or lower, it is easy to function as a binder and it is easy to obtain a biodegradable short-fiber nonwoven fabric having a soft texture. In one or more embodiments of the present invention, the melting point of the short fiber B is measured by differential scanning calorimetry (DSC). Note that, in one or more embodiments of the present invention, the melting point of the short fiber B may be confirmed by measuring the melting point of the multifilament.
[0041] The short fiber B is not particularly limited, but for example, the tensile strength is preferably 1.0 to 6.0 cN / dtex, more preferably 1.5 to 6.0 cN / dtex, and even more preferably 2.0 to 6.0 cN / dtex. When the tensile strength of the short fiber B is within the above-mentioned range, the mechanical strength and flexibility of the biodegradable short fiber nonwoven fabric are improved. In one or more embodiments of the present invention, the tensile strength of the short fiber B is measured in accordance with JIS L 1015.
[0042] The short fiber B is not particularly limited, but for example, the weight average molecular weight is preferably 50,000 to 3,000,000, more preferably 100,000 to 3,000,000, and further preferably 100,000 to 1,500,000. When the weight average molecular weight of the short fiber B is within the above range, the mechanical strength of the biodegradable short fiber nonwoven fabric is improved. The weight average molecular weight of the short fiber B may be confirmed by measuring the average molecular weight of the resin composition constituting the short fiber B.
[0043] (Biodegradable short fiber nonwoven fabric) The biodegradable staple fiber nonwoven fabric contains cellulosic staple fiber A and staple fiber B. In the biodegradable staple fiber nonwoven fabric, from the viewpoints of mechanical strength, texture, and flexibility, the mixing ratio of cellulosic staple fiber A to staple fiber B, cellulosic staple fiber A / staple fiber B, is preferably 50 / 50 to 90 / 10 by weight, and more preferably 50 / 50 to 85 / 15. The biodegradable staple fiber nonwoven fabric may contain other biodegradable fibers in addition to the cellulosic staple fiber A and staple fiber B, within a range that does not impair the effects of the present invention.
[0044] In one or more embodiments of the present invention, the biodegradable staple fiber nonwoven fabric may be a wet-laid nonwoven fabric, for example, from the viewpoint of cost and productivity, but is not particularly limited thereto.
[0045] The tensile strength of biodegradable short fiber nonwoven fabrics can be determined appropriately depending on the application and purpose. In the case of wet nonwoven fabrics, from the viewpoint of increasing the mechanical strength, the tensile strength measured according to the nonwoven fabric core test method of JIS L 1085 is set to 50g / 5cm / g / m 2 It is preferable that the thickness is 55g / 5cm / g / m or more. 2 More preferably, it is 60g / 5cm / g / m or more. 2 More preferably, it is 65 g / 5 cm / g / m or more. 2 More preferably, it is equal to or greater than this.
[0046] The compression characteristics of biodegradable short fiber nonwoven fabrics can be determined according to the application and purpose. In the case of wet nonwoven fabrics, the basis weight is set at 40±2 g / m2 from the viewpoint of soft texture when compressed. 2 The sample is used and measured with a compression tester KES-FB3 (manufactured by Kato Tech Co., Ltd.) under the condition of a sensor compression speed of 50 mm / sec. The measurement item of compression characteristics RC (elasticity against compression (%)) is preferably 35% or more.
[0047] The bending properties of biodegradable short fiber nonwoven fabrics can be determined according to the application and purpose. In the case of wet nonwoven fabrics, the basis weight is set to 40±2 g / m2 from the viewpoint of softness when bent. 2 A sample with a curvature of K = ±2.5 cm was used in a compression tester KES-FB3 (manufactured by Kato Tech Co., Ltd.). One end of the sample (effective length 20 cm, width 1 cm) was fixed and the other end was moved. -1 Within the range of constant speed (deformation speed 0.5 cm -1 The bending stiffness B measured by a pure bending test under the condition of 0.06 gf cm 2 / cm or less, and the bending hysteresis 2HB is preferably 0.30 g·cm / cm or less.
[0048] In one or more embodiments of the present invention, the biodegradable staple fiber nonwoven fabric has good biodegradability. For example, when 10 g of the biodegradable staple fiber nonwoven fabric is buried in microbially activated soil at 25 to 30° C. for 5 months and then weighed or observed, it is preferred that the biodegradable staple fiber nonwoven fabric is completely decomposed.
[0049] The basis weight of the biodegradable short fiber nonwoven fabric can be determined according to the application and purpose. In the case of wet-laid nonwoven fabric, the basis weight is set to 5 to 500 g / m from the viewpoints of mechanical strength, texture, and flexibility. 2 It is preferable that the thickness is 10 to 300 g / m 2 More preferably, the thickness is 20 to 200 g / m 2 It is even more preferable that:
[0050] The thickness of the biodegradable short fiber nonwoven fabric may be determined depending on the application, purpose, etc., but in the case of a wetlaid nonwoven fabric, from the viewpoints of mechanical strength, texture, and flexibility, the thickness is preferably 0.05 to 3 mm, more preferably 0.1 to 2 mm, and even more preferably 0.2 to 1 mm.
[0051] The air permeability of the biodegradable short fiber nonwoven fabric can be determined depending on the application or purpose. In the case of wet-laid nonwoven fabric, the air permeability measured according to the Frangill method described in JIS L 1096 is set to 30 to 800 cm from the viewpoint of flexibility and air permeability. 3 / cm 2 / sec, preferably 50 to 500 cm 3 / cm 2 / sec is more preferable.
[0052] In one or more embodiments of the present invention, the biodegradable short fiber nonwoven fabric has excellent mechanical strength and good flexibility when compressed and bent, and therefore can be suitably used for various materials such as industrial materials, daily living materials, agricultural materials, etc. In particular, in the case of wet-laid nonwoven fabrics, they can be widely used in the paper field. Specifically, they can be suitably used for envelopes, agricultural bags (grape bags, loquat bags, peach bags, etc.), paper cartons for beverages, food packaging materials, food packs for sweets, bread and cakes, paper cups, paper ice cream containers, masks, etc.
[0053] Biodegradable short-fiber nonwoven fabrics and various materials using the same will biodegrade if left in an environment where microorganisms exist after use, so they do not require special disposal treatment and are environmentally friendly. EXAMPLES
[0054] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0055] The measurement and evaluation methods used in the examples and comparative examples are as follows. (1) Tensile strength of nonwoven fabric According to the nonwoven fabric test method of JIS L 1085, a sample piece of 5 cm wide and 20 cm long was used, and the load value (g) at break was measured at a gripping distance of 10 cm and a pulling speed of 30 cm / min. The weight per unit area (g / m 2 ) to calculate the average value in the longitudinal and transverse directions, which was used as the tensile strength. (2) Compression characteristics The compression characteristics of the nonwoven fabric were measured using a compression tester KES-FB3 (manufactured by Kato Tech Co., Ltd.) The compression speed of the sensor was set to 50 mm / sec. When the measurement item of compression property RC (elasticity against compression (%)) was 35% or more, the nonwoven fabric was evaluated as having a soft feel. (3) Bending properties The bending properties of the nonwoven fabric were evaluated using a compression tester KES-FB3 (manufactured by Kato Tech Co., Ltd.). One end of the sample (effective length 20 cm, width 1 cm) was fixed and the other end was moved to obtain a curvature K = ±2.5 cm. -1 Within the range of constant speed (deformation speed 0.5 cm -1 / sec) pure bending test and bending stiffness B (gf cm 2 / cm) and bending hysteresis 2HB (g·cm / cm) were calculated. Bending stiffness B is 0.06 gf cm 2 / cm or less and bending hysteresis 2HB of 0.30 g·cm / cm or less, the flexibility of the nonwoven fabric was evaluated as good. (4) Biodegradability test After storing 10 g of nonwoven fabric in the microbially activated soil for 5 months, the weight was measured or the appearance was observed, and the biodegradability was evaluated according to the following criteria. The evaluation temperature was 25°C to 30°C. Good: Completely decomposed. Normal: Only partially decomposed, not completely decomposed. Bad: Almost no decomposition. (5) Melting point A differential scanning calorimeter DSC [Seiko Instruments Inc., DSC6200] was used. Specifically, 5 to 6 mg of a sample was melted by heating from 40°C to 220°C at a heating rate of 10°C / min, then crystallized by cooling from 220°C to 40°C at a heating rate of 10°C / min, and then further heated from 40°C to 220°C at a heating rate of 10°C / min. The melting peak temperature in the DSC curve during the second heating was taken as the melting point. (6) Weight average molecular weight (Mw) 10 mg of sample was dissolved in 10 mL of chloroform, and insoluble matter was removed by filtration. The resulting solution (filtrate) was subjected to molecular weight measurement using a Shimadzu GPC system equipped with "Shodex K805L (300x8mm, 2 connected)" (Showa Denko) and chloroform as the mobile phase. Commercially available standard polystyrene was used as the molecular weight standard sample. (7) Composition ratio of poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) To approximately 20 mg of the sample, 2 mL of a sulfuric acid-methanol mixture (15:85) and 2 mL of chloroform were added, sealed, and heated at 100°C for 140 minutes to obtain methyl esters of polyester decomposition products. After cooling, 1.5 g of sodium bicarbonate was gradually added to neutralize the mixture, and the mixture was left to stand until the generation of carbon dioxide gas stopped. 4 mL of diisopropyl ether was added and mixed well, and then the mixture was centrifuged. The composition of the hydroxyalkanoic acid methyl esters of the polyester decomposition products in the supernatant was analyzed by capillary gas chromatography to determine the composition ratio (monomer ratio) of the monomer units of P3HB3HH. The gas chromatograph used was a GC-17A manufactured by Shimadzu Corporation, and the capillary column used was a NEUTRA BOND-1 manufactured by GL Sciences (column length 25 m, column inner diameter 0.25 mm, liquid film thickness 0.4 μm). The temperature conditions were as follows: the initial temperature was raised from 100°C to 200°C at a rate of 8°C / min, and then the temperature was raised further from 200°C to 290°C at a rate of 30°C / min. (8) Melt flow rate (MFR) Measurements were performed in accordance with JIS K 7210-1 at a temperature of 165°C and a load of 5 kg (49 N). (9) Single fiber fineness and tensile strength of fibers Measurement was performed in accordance with JIS L 1015.
[0056] (Production Example 1) As P3HB3HH, 100 parts by weight of copolymer resin (manufactured by Kaneka Corporation, "X131A") having a molar composition ratio of 3HB unit / 3HH unit of 95 / 5, Mw of 320,000, and MFR (165°C, 5kg) of 3g / 10min, 1 part by weight of pentaerythritol (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., "Neurizer P") as a crystal nucleating agent, 0.5 parts by weight of erucic acid amide and 0.5 parts by weight of behenic acid amide as lubricants were dry blended, melt-kneaded at 150°C using an extruder, and pelletized to obtain a pellet-shaped resin composition. The obtained pellet-shaped resin composition had Mw of 300,000 and MFR (165°C, 5kg) of 16.7g / 10min. The obtained resin composition (pellets) was melted in a single-screw extruder with a screw diameter of 25 mm, the flow rate was adjusted with a gear pump, and the melt spinning temperature was 170 ° C., and the extrusion was performed from a spinning nozzle (hole diameter 0.3 mm, shape of discharge hole: circular) into a space (quenching farm) where air (quench air) of 14 ° C. and 1.0 m / s was blown at 14 ° C., an oil agent was applied, and the spinning speed was taken up at 540 m / min with a roll heated to 60 ° C., and the roll was continuously heated to 70 ° C. and stretched 1.8 times, and 5% relaxation was performed at room temperature (about 23 ° C.) to obtain a multifilament. This multifilament had a single fiber fineness of 2.0 dtex, a tensile strength of 2.0 cN / dtex, and a melting point of 150 ° C. The multifilament obtained above was cut to a fiber length of 5 mm to obtain P3HB3HH staple fiber 1 (single fiber fineness 2.0 dtex).
[0057] (Production Example 2) A pellet-shaped resin composition was obtained in the same manner as in Production Example 1, except that a copolymer resin (manufactured by Kaneka Corporation, "X151A") having a molar composition ratio of 3HB units / 3HH units of 89 / 11, Mw of 800,000, and MFR (165°C, 5 kg) of 3 g / 10 min was used as P3HB3HH. The pellet-shaped resin composition obtained had an Mw of 300,000 and an MFR (165°C, 5 kg) of 8.1 g / 10 min. The obtained resin composition (pellets) was used to produce a multifilament by fiberization in the same manner as in Production Example 1, except that the melt spinning temperature was set to 145° C. The multifilament had a single fiber fineness of 2.0 dtex, a tensile strength of 1.9 cN / dtex, and a melting point of 128° C. The multifilament obtained above was cut to a fiber length of 5 mm to obtain P3HB3HH staple fiber 2 (single fiber fineness 2.0 dtex).
[0058] (Production Example 3) Polylactic acid (hereinafter referred to as PLA) resin (Nature Works, "3251D", MFR (165 ° C, 5 kg) 29 g / 10 min, melting point 170 ° C) was melted in a single screw extruder with a screw diameter of 25 mm, the flow rate was adjusted with a gear pump, and the melt spinning temperature was 190 ° C., and the resin was extruded from a spinning nozzle (hole diameter 0.4 mm, shape of discharge hole: circular) into a space (quenching farm) where air (quench air) of 20 ° C. and 1.0 m / s was blown, and an oil agent was added, and the resin was taken up at a spinning speed of 700 m / min at room temperature, and continuously stretched 2.5 times with a roll heated to 70 ° C., and relaxed by 5% at 120 ° C. to obtain a multifilament. The obtained multifilament was cut to a fiber length of 5 mm to obtain a PLA short fiber. The PLA short fibers had a single fiber fineness of 2.0 dtex, a tensile strength of 2.5 cN / dtex, and a melting point of 172°C.
[0059] Example 1 A nonwoven fabric was produced by a wet papermaking method. Cellulosic short fiber A was pulp (average fiber length 4 mm, average fiber diameter 28 μm) at 80% by weight, and biodegradable short fiber B was P3HB3HH short fiber 1 at 20% by weight. The mixed fibers were dispersed in water to a fiber concentration of 0.03% by weight, and paper was made using a papermaking machine (Kumagaya Riki Kogyo Co., Ltd., agitator-type square sheet machine). The nonwoven fabric was then dried at 100°C, and the fibers were thermally bonded by passing through a heated roll at 120°C to a basis weight of 40 g / m. 2 As a result, a short fiber nonwoven fabric was obtained.
[0060] Example 2 A fabric having a basis weight of 40 g / m was prepared in the same manner as in Example 1, except that P3HB3HH-based staple fiber 2 was used as the biodegradable staple fiber B. 2 As a result, a short fiber nonwoven fabric was obtained.
[0061] Example 3 The same procedure as in Example 2 was repeated to obtain a fabric having a basis weight of 42 g / m, except that the mixing ratio was changed to 50% by weight of pulp / 50% by weight of P3HB3HH-based short fiber 2. 2 As a result, a short fiber nonwoven fabric was obtained.
[0062] Comparative Example 1 A fabric having a basis weight of 40 g / m was prepared in the same manner as in Example 1, except that biodegradable short fiber B was not used and pulp was used at 100% by weight. 2 As a result, a short fiber nonwoven fabric was obtained.
[0063] Comparative Example 2 A fiber having a basis weight of 41 g / m was prepared in the same manner as in Example 1, except that the PLA short fibers obtained in Production Example 3 were used instead of the P3HB3HH short fibers 1. 2 As a result, a short fiber nonwoven fabric was obtained.
[0064] Example 4 A fabric having a basis weight of 41 g / m was prepared in the same manner as in Example 1, except that rayon fiber (single fiber fineness 2 dtex, average fiber length 5 mm) was used instead of pulp. 2 As a result, a short fiber nonwoven fabric was obtained.
[0065] Comparative Example 3 A fabric having a basis weight of 41 g / m was prepared in the same manner as in Example 4, except that biodegradable short fiber B was not used and 100% by weight of rayon fiber was used. 2 As a result, a short fiber nonwoven fabric was obtained.
[0066] Comparative Example 4 A fabric having a basis weight of 40 g / m was fabricated in the same manner as in Example 4, except that a low melting point polyester staple fiber (manufactured by Kuraray Co., Ltd., "N701Y", fineness 5.6 dtex, fiber length 5 mm, melting point 130°C) was used instead of the P3HB3HH staple fiber 1. 2 As a result, a short fiber nonwoven fabric was obtained.
[0067] In the examples and comparative examples, the tensile strength, compression properties, bending properties and biodegradability of the short fiber nonwoven fabrics were measured and evaluated as described above, and the results are shown in the following Tables 1 and 2. In the bending properties columns in the following Tables 1 and 2, B is bending rigidity and 2HB is bending hysteresis.
[0068] [Table 1]
[0069] [Table 2]
[0070] As can be seen from the data in Tables 1 and 2, the nonwoven fabrics of Examples 1 to 4 containing cellulose-based short fibers and P3HB3HH-based short fibers have good biodegradability, high tensile strength, and a soft feel as indicated by the compression properties and bending properties.
[0071] On the other hand, the nonwoven fabrics of Comparative Examples 1 and 3, which contained cellulosic staple fibers but not P3HB3HH staple fibers, had good biodegradability but low tensile strength. The nonwoven fabric of Comparative Example 2, which contained cellulosic staple fibers and PLA staple fibers, was inferior to the nonwoven fabrics of the Examples in terms of biodegradability, tensile strength, and texture. The nonwoven fabric of Comparative Example 4, which contained cellulosic staple fibers and low-melting-point polyester staple fibers, was significantly inferior in biodegradability and had a poor texture as measured by compression properties.
Claims
1. A biodegradable staple fiber nonwoven fabric comprising cellulosic staple fiber A and staple fiber B containing poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate), The mixing ratio of the cellulose-based short fiber A to the short fiber B is, in weight ratio, cellulose-based short fiber A / biodegradable short fiber B=50 / 50 to 90 / 10; The biodegradable staple fiber nonwoven fabric is a wet-laid nonwoven fabric, and the wet-laid nonwoven fabric has a basis weight of 10 to 300 g / m 2 .
2. 2. The biodegradable staple fiber nonwoven fabric according to claim 1, wherein the staple fiber B has a single fiber fineness of 0.1 to 50 dtex.
3. The biodegradable staple fiber nonwoven fabric according to claim 1 or 2, wherein the average fiber length of the staple fibers B is 1 to 10 mm.
4. The biodegradable staple nonwoven fabric according to any one of claims 1 to 3, wherein the monomer ratio of the poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate) is, in molar ratio, 3-hydroxybutyrate / 3-hydroxyhexanoate = 99 / 1 to 80 / 20.
5. The biodegradable staple fiber nonwoven fabric according to any one of claims 1 to 4, wherein the staple fiber B contains 0.05 to 12 parts by weight of a crystal nucleating agent and 0.05 to 12 parts by weight of a lubricant per 100 parts by weight of poly-(3-hydroxybutyrate-co-3-hydroxyhexanoate).
6. The biodegradable staple fiber nonwoven fabric according to any one of claims 1 to 5, wherein the staple fiber B has a melting point of 110 to 165°C.
7. The biodegradable staple fiber nonwoven fabric according to any one of claims 1 to 6, wherein the staple fiber B has a tensile strength of 1.0 to 6.0 cN / dtex.
8. The biodegradable staple fiber nonwoven fabric according to any one of claims 1 to 7, wherein the staple fibers B have a weight average molecular weight of 50,000 to 3,000,000.
Citation Information
Patent Citations
Microbially degradable nonwoven fabric and its production
JP1993214648A
Biodegradable short fiber non-woven fabric
JP1994200457A
Biodegradable short fiber non-woven fabric
JP1994200458A
Production of biodegradable composite paper and sheet
JP1994346399A
Undrawn polyester binder fiber for papermaking
JP2013174028A