A method for growing thick oxide films with high thermal oxidation quality at low temperatures

The high-pressure silicon oxidation method using an amine additive at controlled temperatures and pressures forms high-quality, conformal silicon oxide films on semiconductor substrates, addressing the limitations of high-temperature processes and enhancing film quality and deposition capabilities.

JP7580386B2Active Publication Date: 2024-11-11APPLIED MATERIALS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021555610
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-20
Filing Date
2020-02-23
Publication Date
2024-11-11
Estimated Expiration
2040-02-23

AI Technical Summary

Technical Problem

Current silicon oxidation techniques for forming low-k dielectric films on semiconductor substrates are limited by high temperatures above 800°C, which can damage materials and result in poor film quality and limited thickness, especially for films thicker than 100 angstroms.

Method used

A method involving high-pressure silicon oxidation using an oxidizing medium with an amine additive at pressures above 1 bar and temperatures between 100°C and 550°C, allowing for the formation of conformal silicon oxide films with uniform thickness between 100 and 400 angstroms, using a high-pressure vessel with controlled gas flow and heating.

Benefits of technology

The method enables high-quality silicon oxide films to be deposited at lower temperatures, achieving conformality and uniform thickness comparable to high-temperature processes, expanding the process window and improving film quality and oxidation rates by up to three times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580386000001
    Figure 0007580386000001
  • Figure 0007580386000002
    Figure 0007580386000002
  • Figure 0007580386000003
    Figure 0007580386000003
Patent Text Reader

Abstract

The embodiments described herein generally relate to methods for forming low-k dielectric materials on semiconductor substrates. More specifically, the implementations described herein relate to methods for forming silicon oxide films at high pressure and low temperature. The method for forming a silicon oxide film includes loading a substrate having a silicon-containing film formed thereon into a processing region of a high-pressure vessel. The method further includes forming a silicon oxide film on the silicon-containing film. Forming the silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium containing an amine additive at a pressure greater than about 1 bar and maintaining the high-pressure vessel at a temperature between about 100°C and about 550°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE Embodiments described herein generally relate to methods for forming low dielectric materials on semiconductor substrates. More specifically, embodiments described herein relate to methods for forming silicon oxide films at high pressure and low temperature using an oxidizing medium that includes an additive. [Background technology]

[0002] The formation of semiconductor devices, such as memory devices, logic devices, microprocessors, etc., involves the deposition of low-k dielectric films on semiconductor substrates. The low-k dielectric films are used to create circuits for the fabrication of the devices. Current dry or wet silicon oxidation techniques are often performed at temperatures above 800°C. However, materials deposited on semiconductor substrates may not be able to withstand temperatures above 800°C. As a result, low-k dielectric films cannot be deposited at temperatures above the thermal budget of 800°C and often suffer from poor quality of films deposited within the thermal budget. In addition, current dry or wet silicon oxidation techniques cannot deposit high quality low-k dielectric films with thicknesses greater than 100 angstroms.

[0003] Therefore, what is needed is a method for depositing high quality low k dielectric films at temperatures that meet thermal budget targets. Summary of the Invention

[0004] The embodiments described herein generally relate to a method for forming a low-k dielectric material on a semiconductor substrate. More specifically, the embodiments described herein relate to a method for forming a silicon oxide film at high pressure and low temperature. The method for forming a silicon oxide film includes loading a substrate having a silicon-containing film formed thereon into a processing region of a high pressure vessel. The method further includes forming a silicon oxide film on the silicon-containing film. Forming the silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium containing an amine additive at a pressure greater than about 1 bar and maintaining the high pressure vessel at a temperature between about 100° C. and about 550° C.

[0005] A method of forming a silicon oxide film includes loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel and forming a silicon oxide film on the silicon-containing film. Forming the silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium having an amine additive at a pressure greater than about 1 bar and maintaining the high pressure vessel at a temperature between about 100° C. and about 550° C.

[0006] The method of forming a conformal silicon oxide film includes depositing a silicon-containing film on a substrate including a plurality of vias. A silicon-containing film is deposited on each exposed surface of the substrate and on the plurality of vias. The method further includes loading the substrate having the silicon-containing film deposited thereon into a processing region of a high pressure vessel, and forming a conformal silicon oxide film on the silicon-containing film. Forming the conformal silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium including an amine additive, the oxidizing medium including about 1,000 ppm to about 20,000 ppm of the amine additive, and maintaining the high pressure vessel at a temperature between about 100° C. and about 550° C. and a pressure between about 1 bar and about 65 bar.

[0007] A method for forming a silicon oxide film includes loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel and forming a silicon oxide film on the silicon-containing film. Forming the silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium comprising ammonia, the oxidizing medium being selected from the group of steam, oxygen, and peroxide, and maintaining the high pressure vessel at a temperature between about 400° C. and about 505° C. and a pressure greater than about 10 bar. The silicon oxide film has a uniform thickness between about 100 Angstroms and about 400 Angstroms.

[0008] So that the above-mentioned features of the present disclosure may be understood in detail, a more particular description of the present disclosure briefly summarized above can be made by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings depict only exemplary embodiments and therefore should not be considered as limiting the scope thereof, which may admit of other equally effective embodiments. [Brief description of the drawings]

[0009] [Figure 1] 1 shows a simplified cross-sectional front view of one example of a high pressure vessel that may be used to implement one or more implementations described herein. [Figure 2A] 1 illustrates a semiconductor device having a silicon-containing film deposited thereon, according to embodiments disclosed herein. [Figure 2B] 1 shows an illustration of a semiconductor device having a conformal and uniform silicon oxide film formed thereon according to embodiments disclosed herein. [Figure 2C] 1 shows an illustration of a semiconductor device having a conformal and uniform silicon oxide film formed thereon according to embodiments disclosed herein. [Figure 2D] 1 shows an illustration of a semiconductor device having a conformal and uniform silicon oxide film formed thereon according to embodiments disclosed herein. [Diagram 3] 1 is a flow chart illustrating a method of forming a conformal silicon oxide film, according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] For ease of understanding, wherever possible, the same reference numerals have been used to designate identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0011] The embodiments described herein generally relate to a method for forming a low-k dielectric material on a semiconductor substrate. More specifically, the embodiments described herein relate to a method for forming a silicon oxide film at high pressure and low temperature. The method for forming a silicon oxide film includes loading a substrate having a silicon-containing film formed thereon into a processing region of a high-pressure vessel. The method further includes forming a silicon oxide film on the silicon-containing film. Forming the silicon oxide film on the silicon-containing film includes exposing the silicon-containing film to an oxidizing medium containing an amine additive at a pressure greater than about 1 bar and maintaining the high-pressure vessel at a temperature between about 100° C. and about 550° C.

[0012] The implementations described herein will be described below with reference to high pressure oxidation processes that can be carried out using a high pressure oxidation system. The illustration of the apparatus described herein in Figure 1 is exemplary and should not be understood or construed as limiting the scope of the embodiments described herein.

[0013] FIG. 1 is a simplified cross-sectional front view of a high pressure vessel 100 for a high pressure annealing process. The high pressure vessel 100 has a body 110 including an outer surface 112 and an inner surface 113 surrounding a processing region 115. In some implementations, such as in FIG. 1, the body 110 has an annular cross section, but in other embodiments, the cross section of the body 110 may be rectangular or any closed shape. The outer surface 112 of the body 110 may be made of a corrosion resistant steel (CRS), such as, for example, but not limited to, stainless steel. In one implementation, the inner surface 113 of the body 110 is made of a nickel-based alloy steel that is highly resistant to corrosion, such as, for example, but not limited to, Hastelloy®.

[0014] The high pressure vessel 100 has a door 120 configured to enclose a processing region 115 within the body 110, such that when the door 120 is open, the processing region 115 can be accessed. A high pressure seal 122 is utilized to seal the door 120 to the body 110, thus sealing the processing region 115 for processing. The high pressure seal 122 may be made from a polymer, such as, for example, but not limited to, perfluoroelastomer. A cooling channel 124 is disposed on the door 120 adjacent the high pressure seal 122, such that the high pressure seal 122 is maintained at a temperature below the maximum safe operating temperature of the high pressure seal 122 during processing. A coolant (such as, for example, but not limited to, an inert, dielectric, and / or high performance heat transfer fluid) may be circulated through the cooling channel 124 to maintain the high pressure seal 122 at a temperature between about 150° C. and about 250° C. The flow of coolant through the cooling channels 124 is controlled by the controller 180 via feedback received from the temperature sensor 116 or a flow sensor (not shown).

[0015] The high pressure vessel 100 has a port 117 extending through the body 110. The port 117 has a pipe 118 passing therethrough that is connected to a heater 119. One end of the pipe 118 is connected to the process region 115. The other end of the pipe 118 branches into an inlet conduit 157 and an outlet conduit 161. The inlet conduit 157 is fluidly connected to the gas panel 150 via a shutoff valve 155. The inlet conduit 157 is connected to a heater 158. The outlet conduit 161 is fluidly connected to a condenser 160 via a shutoff valve 165. The outlet conduit 161 is connected to a heater 162. The heaters 119, 158, and 162 are configured to maintain a process gas, e.g., an oxidizing medium, passing through the pipe 118, the inlet conduit 157, and the outlet conduit 161, respectively, at a temperature between the condensation point of the process gas and about 250°C. Heaters 119 , 158 , and 162 are powered by power supply 145 .

[0016] The gas panel 150 is configured to supply a process fluid, such as an oxidizing medium, under pressure into the inlet conduit 157 for transfer into the processing region 115 through the pipe 118. The oxidizing medium includes an amine additive. The pressure of the process gas introduced into the processing region 115 is monitored by a pressure sensor 114 coupled to the body 110. The condenser 160 is fluidly connected to the cooling fluid and configured to condense the gaseous product that flows through the outlet conduit 161 after being removed from the processing region 115 through the pipe 118. The condenser 160 changes the gaseous product from a gas phase to a liquid phase. A pump 170 is fluidly connected to the condenser 160 and discharges the liquefied product from the condenser 160. The operation of the gas panel 150, the condenser 160, and the pump 170 are controlled by a controller 180.

[0017] Shutoff valves 155 and 165 are configured to allow only one fluid at a time to enter processing region 115 through pipe 118. When shutoff valve 155 is open, shutoff valve 165 is closed, allowing process fluid through inlet conduit 157 into processing region 115 and preventing process gas flow from entering condenser 160. Meanwhile, when shutoff valve 165 is open, shutoff valve 155 is closed, allowing gas product to be removed from processing region 115 and flow through outlet conduit 161 and preventing gas product flow from entering gas panel 150.

[0018] One or more heaters 140a, 140b (collectively 140) are mounted on the body 110 and configured to heat a processing region 115 within the high pressure vessel 100. In some implementations, the heaters 140 are mounted on an exterior surface 112 of the body 110, as shown in FIG. 1, while in other embodiments, the heaters 140 may be mounted on an interior surface 113 of the body 110. Each heater 140 may be a resistive coil, a lamp, a ceramic heater, a graphite-based carbon fiber composite (CFC) heater, a stainless steel heater, or an aluminum heater. The heaters 140 are powered by a power supply 145. Power to the heaters 140 is controlled by a controller 180 via feedback received from a temperature sensor 116. A temperature sensor 116 is coupled to the body 110 to monitor the temperature of the processing region 115.

[0019] A cassette 130 coupled to an actuator (not shown) is moved into and out of the processing region 115. The cassette 130 has a top surface 132, a bottom surface 134, and a wall 136. The wall 136 of the cassette 130 has a plurality of substrate storage slots 138. Each substrate storage slot 138 is evenly spaced along the wall 136 of the cassette 130. Each substrate storage slot 138 is configured to hold a substrate 135 therein. The cassette 130 may have as many as 50 storage slots 138 for holding substrates 135. The cassette 130 provides an efficient transport means for transferring multiple substrates 135 into and out of the high pressure vessel 100, as well as for processing multiple substrates 135 within the processing region 115.

[0020] A controller 180 controls the operation of the high pressure vessel 100. The controller 180 controls the operation of the gas panel 150, the condenser 160, the pump 170, the shutoff valves 155 and 165, and the power supply 145. The controller 180 is also communicatively connected to the temperature sensor 116, the pressure sensor 114, and the cooling channel 124. The controller 180 includes a central processing unit (CPU) 182, a memory 184, and auxiliary circuits 186. The CPU 182 may be any form of general purpose computer processor that may be used in an industrial setting. The memory 184 may be random access memory, read only memory, a floppy or hard disk drive, or other form of digital storage. The auxiliary circuits 186 are conventionally connected to the CPU 182 and may include cache, clock circuits, input / output systems, power supplies, etc.

[0021] The high pressure vessel 100 provides a convenient chamber for carrying out a method of forming silicon oxide films on a plurality of substrates 135 at temperatures up to 550° C. The heater 140 is powered to preheat the high pressure vessel 100 and maintain the processing region 115 at a temperature up to about 550° C. At the same time, heaters 119, 158, and 162 are powered to preheat the pipe 118, the inlet conduit 157, and the outlet conduit 161, respectively.

[0022] A number of substrates 135 are loaded into a cassette 130. The door 120 of the high pressure vessel 100 is opened to move the cassette 130 into the processing region 115. The door 120 is then sealed, turning the high pressure vessel 100 into a high pressure vessel. Once the door 120 is closed, a high pressure seal 122 ensures that there is no pressure leakage from the processing region 115.

[0023] A process gas (i.e., an oxidizing medium with an amine additive) is provided by gas panel 150 into processing region 115 inside high pressure vessel 100. Shut-off valve 155 is opened by controller 180 to allow process gas to flow into processing region 115 via inlet conduit 157 and pipe 118. Process gas is introduced at a flow rate of, for example, about 500 sccm to about 2000 sccm. At this point, shut-off valve 165 remains closed. In some implementations, the pressure in high pressure vessel 100 is gradually increased. High pressure is effective to drive oxygen into the silicon-containing film for more complete oxidation, especially in the deeper portions of the trench.

[0024] In some implementations described herein, the process gas is steam with an amine additive under a pressure between about 1 bar and about 65 bar (e.g., between about 35 bar and about 65 bar, or between about 40 bar and 60 bar). However, in other implementations, other oxidizing media (e.g., but not limited to, ozone, oxygen, peroxides, or hydroxide-containing compounds) may be used in conjunction with or in place of the steam. The amine additive added to the oxidizing media may be ammonium or ammonia. When sufficient steam has been released by the gas panel 150, the shutoff valve 155 is closed by the controller 180.

[0025] During processing of the substrate 135, the processing region 115 and the inlet conduit 157, the outlet conduit 161, and the pipe 118 are maintained at a temperature and pressure such that the processing gas remains in the gas phase. The temperature of the processing region 115 and the inlet conduit 157, the outlet conduit 161, and the pipe 118 is also maintained at a temperature above the condensation point of the processing gas (e.g., 100° C.) at the applied pressure, but below 550° C. The processing region 115 and the inlet conduit 157, the outlet conduit 161, and the pipe 118 are also maintained at a pressure below the condensation pressure of the processing gas at the applied temperature. The processing gas is selected accordingly. In the implementation described herein, when the high pressure vessel is maintained at a temperature between about 100° C. and about 550° C., steam under a pressure between about 1 bar and about 65 bar is an effective processing gas. This ensures that the steam does not condense into water, which would be detrimental to the silicon film deposited on the substrate 135.

[0026] Once the film is confirmed to have the target density, verified by testing the film's wet etch rate and leakage and breakdown characteristics, the process is complete. Then, the shutoff valve 165 is opened to allow the process gas to flow from the process area 115 through the pipe 118 and the outlet conduit 161 into the condenser 160. The process gas is condensed to liquid phase in the condenser 160. The liquefied process gas is then removed by the pump 170. When the liquefied process gas is completely removed, the shutoff valve 165 is closed. Then, the heaters 140, 119, 158, and 162 are turned off. Then, the door 120 of the high pressure vessel 100 is opened to remove the cassette 130 from the process area 115.

[0027] FIG. 2A illustrates a semiconductor device 200 including a substrate 202 and a silicon-containing film 208 deposited on the substrate 202 according to one or more implementations described herein. The substrate 202 may be used in place of each of the substrates 135 when loaded into the cassette 130 as illustrated in FIG. 1. One or more openings or vias 204 may be formed in the substrate 202. Although only one via 204 is illustrated in the semiconductor device 200, multiple vias 204 may be included. In such an embodiment, each via 204 of the multiple vias may have the same dimensions, such as having a depth of about 10 μm. Additionally, the side surface 214 and bottom surface 216 of the via 204 may be patterned and may not be flat as illustrated. A silicon-containing film 208 may be deposited on each exposed surface of the substrate 202 (i.e., the top surface 212, the side surface 214, and the bottom surface 216) and the via 204. The silicon-containing film 208 may be deposited using atomic layer deposition (ALD). The silicon-containing film 208 may be composed of silicon or silicon nitride.

[0028] The substrate 202 may include one or more materials used in the formation of semiconductor devices, such as metal contacts, trench isolations, gates, bitlines, or any other interconnect features. The substrate 202 may include one or more metal layers, one or more dielectric materials, semiconductor materials, and combinations thereof utilized to fabricate semiconductor devices. For example, the substrate 202 may include oxide materials, nitride materials, polysilicon materials, etc., depending on the application. In one implementation targeted for memory applications, the substrate 202 may include silicon substrate materials, oxide materials, and nitride materials (with or without polysilicon present therebetween).

[0029] In other implementations, the substrate 202 may include multiple alternating oxide and nitride materials deposited on a surface of the substrate (i.e., oxide-nitride-oxide (ONO)) (not shown). In various implementations, the substrate 202 may include multiple alternating oxide and nitride materials, one or more oxide or nitride materials, polysilicon or amorphous silicon materials, oxide alternating with amorphous carbon, oxide alternating with polysilicon, undoped silicon alternating with doped silicon, undoped polysilicon alternating with doped polysilicon, or undoped amorphous silicon alternating with doped amorphous silicon. The substrate 202 may be any substrate or material surface on which film processing is performed. For example, the substrate 202 can be a material such as crystalline silicon, silicon oxide, silicon oxynitride, silicon nitride, strained silicon, silicon germanium, tungsten, titanium nitride, doped or undoped polysilicon, doped or undoped silicon wafers and patterned or unpatterned wafers, silicon on insulator (SOI), carbon doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, low-k dielectrics, and combinations thereof.

[0030] 2B illustrates a semiconductor device 200 with a conformal silicon oxide film 206 formed in a via 204 according to one or more implementations described herein. The silicon oxide film 206 is formed on the substrate 202 and the silicon-containing film 208 at a temperature up to 550° C., for example, at a temperature between 350° C. and 505° C. The silicon oxide film 206 is formed using high pressure annealing in an oxidizing medium containing an amine additive at a pressure greater than 1 bar, for example, at a pressure between about 35 bar and about 65 bar.

[0031] The oxidizing medium may include steam, oxygen, peroxide, etc., and the amine additive may include ammonium (NH4) or ammonia (NH3). The oxidizing medium may include about 1,000 ppm to about 20,000 ppm of the amine additive, for example about 7,000 ppm of the amine additive. In one embodiment, steam is used as the oxidizing medium with about 7,000 ppm of NH3 as the amine additive. When reacting a film containing silicon nitride, a hydrogen-based additive may be added to the oxidizing medium. The hydrogen-based additive may be added in addition to or instead of the amine additive when reacting a film containing silicon nitride. The hydrogen-based additive may include pure hydrogen (H2), or a trace amount of hydrogen as a component of an inert gas. The amine additive and / or hydrogen-based additive added to the oxidizing medium may increase the oxidation rate by about 2 to 3 times compared to high temperature rapid thermal oxidation films. In one embodiment, the annealing process used to form the silicon oxide film 206 is performed at a pressure between about 40 bar and about 60 bar for about 1 hour.

[0032] The silicon-containing film 208 is disposed between the substrate 202 and the silicon oxide film 206, although the silicon-containing film 208 may be of a thinner thickness after the formation of the silicon oxide film 206. In one embodiment, the silicon-containing film 208 is fully oxidized, such that the silicon-containing film 208 is no longer disposed between the silicon oxide film 206 and the substrate 202 (i.e., the silicon oxide film 206 may be in contact with the substrate 202). Although not shown, the silicon oxide film 206 and / or the silicon-containing film 208 may be disposed on the surface 212 of the substrate 202.

[0033] FIG 2C shows an enlarged cross-sectional view taken through the top of the semiconductor device 200 at line 2C-2C, which may be approximately 500 nm below the surface 212 of the semiconductor device 200. FIG 2D shows an enlarged cross-sectional view taken through the bottom of the semiconductor device 200 at line 2D-2D, which may be approximately 500 nm above the bottom 216 of the semiconductor device 200. The silicon oxide film 206 at the top of FIG 2C has a thickness 210A, and the silicon oxide film 206 at the bottom of FIG 2D has a thickness 210B (collectively 210).

[0034] 2C and 2D, the thickness 210A of the top of the silicon oxide film 206 is approximately the same as the thickness 210B of the bottom of the silicon oxide film 206. The silicon oxide film 206 has a substantially uniform thickness 210 at both the top and bottom of the via 204, exhibiting a conformality of approximately 100% (i.e., the ratio of the top thickness 210A to the bottom thickness 210B) of the silicon oxide layer 206. A silicon oxide film 206 formed using an oxidation medium with an amine additive at a temperature less than about 550° C. and a pressure greater than 1 bar may have a substantially uniform conformality at the sidewalls 214 and bottom 216 of the via 204, with a conformality greater than about 90%. The silicon oxide film 206 has a uniform thickness 210 between about 20 Angstroms and about 400 Angstroms, for example between about 150 Angstroms and about 400 Angstroms.

[0035] 3 illustrates a process flow diagram of a method 300 for forming a silicon oxide film on a substrate in accordance with one or more implementations described herein. The substrate may be substrate 135 as described in FIG. 1 or substrate 202 as shown in FIG. 2A-2D. For clarity, method 300 will be described with reference to components of semiconductor device 200 of FIG. 2A-2D.

[0036] The method 300 begins in operation 310 by loading a substrate 202 having a silicon-containing film 208 deposited thereon (as shown in FIG. 2A) into a high pressure vessel. The high pressure vessel may be the high pressure vessel 100 shown in FIG. 1. The substrate 202 may be placed in a cassette, such as the cassette 130 shown in FIG. 1. Prior to loading the substrate 202 into the high pressure vessel, a silicon-containing film 208 is deposited on each exposed side or surface 212, 214, 216 of the substrate 202 and on the vias 204. The silicon-containing film 208 may be deposited using ALD. The silicon-containing film 208 may be comprised of silicon or silicon nitride. The substrate 202 may be comprised of any of the materials previously described in FIGS. 2A-2D.

[0037] In one implementation, the surface 212 of the substrate 202 includes patterned structures, such as a surface having trenches, holes, or vias 204 formed therein, as shown in FIGS. 2A-2D. In such an embodiment, the silicon-containing film 208 is disposed on the sides 214 and bottoms 216 of the vias 204. Alternatively, the surface 212 of the substrate 202 can be substantially flat. The substrate 202 can also have a substantially flat surface 212 having a targeted stepped structure formed therein. The surface 212 of the substrate 202 can include trenches, holes, vias, or steps, and the patterns of the surface 212 are referred to throughout as vias, although the term "vias" is not intended to be limiting.

[0038] In operation 320, the substrate 202 is exposed to an oxidizing medium containing an amine additive at a target temperature between the condensation point of the oxidizing medium (e.g., about 100° C.) and about 550° C., and at a pressure greater than 1 bar. In one implementation, the target temperature is between about 100° C. and about 550° C. (e.g., between about 350° C. and about 520° C., or between about 400° C. and about 505° C.). The temperature can be increased to the target temperature using the heaters 140a, 140b. In addition to increasing the temperature, the pressure can be increased to the target pressure. In one implementation, the pressure is between about 1 bar and about 65 bar (e.g., between about 30 bar and about 65 bar, or between about 40 bar and about 60 bar).

[0039] In one implementation, the oxidizing medium is selected from the group consisting of steam, ozone, oxygen, water vapor, heavy water, peroxides, compounds containing hydroxide, oxygen isotopes (14, 15, 15, 17, 18, etc.), and hydrogen isotopes (1, 2, 3), and combinations thereof. The peroxide can be hydrogen peroxide in gas phase. In some implementations, the oxidizing medium contains hydroxide ions, including, but not limited to, water vapor, or heavy water in steam form. The amine additive can be comprised of ammonium or ammonia. The oxidizing medium can contain about 1,000 ppm to about 20,000 ppm of the amine additive, such as about 7,000 ppm of the amine additive. In one embodiment, steam is used as the oxidizing medium containing about 7,000 ppm of NH3 as the amine additive. When reacting a film containing silicon nitride, a hydrogen-based additive can be added to the oxidizing medium. Hydrogen-based additives can be added in addition to or instead of amine additives when reacting films containing silicon nitride. Hydrogen-based additives can include pure hydrogen (H2) or trace amounts of hydrogen as a component of an inert gas. Amine additives and / or hydrogen-based additives added to the oxidation medium can increase the oxidation rate by about 2-3 times compared to high temperature rapid thermal oxidation films.

[0040] In some implementations, the substrate 202, or substrates, are exposed to the vapor at a pressure between about 5 bar and about 60 bar, where the pressure can be gradually increased from about 5 bar to about 60 bar. In some implementations, the vapor containing the amine additive is introduced into the high pressure vessel at a flow rate of, for example, between about 500 sccm and about 5,000 sccm (e.g., between about 500 sccm and about 5,000 sccm, or between about 500 sccm and about 2,000 sccm). In one implementation, water vapor containing the amine additive is injected into the high pressure vessel, and the water vapor forms the vapor containing the amine additive as it is heated in the high pressure vessel. In another implementation, water or water vapor containing the amine additive is present in the high pressure vessel prior to heating to the target temperature. The water or water vapor present in the high pressure vessel forms the vapor containing the amine additive as the high pressure vessel is heated to the target temperature.

[0041] At block 330, a silicon oxide film 206 is formed on the substrate 202. The silicon oxide film 206 is formed as a conformal or uniform layer. The silicon oxide film 206 is formed uniformly on the side 214 and bottom 216 of the via 204, as well as on the surface 212 of the substrate 202. The silicon oxide film 206 may be deposited to have a conformality of greater than about 90% on the side 214 and bottom 216 of the via 204, as shown in FIGS. 2A-2D. The silicon oxide film 206 may have a thickness 210 of about 20 angstroms to about 400 angstroms, such as about 150 angstroms to about 400 angstroms.

[0042] In operation 330, the high pressure vessel is maintained at a temperature between the condensation point of the oxidizing medium and about 550° C. while the substrate 202 having the silicon-containing film 208 is exposed to an oxidizing medium including an amine additive to form the silicon oxide film 206. In one implementation where steam including an amine additive is used at a pressure between about 40 bar and about 60 bar, the temperature of the high pressure vessel is maintained between about 400° C. and about 505° C. In some implementations, forming the silicon oxide film 206 on the substrate 202 in operation 330 is performed for a time period between about 5 minutes and about 150 minutes, for example, between about 30 minutes and about 120 minutes. In at least one implementation, utilizing an oxidizing medium containing an amine additive at a temperature between about 400° C. and about 505° C. and a pressure of about 60 bar for about 120 minutes completely oxidizes the silicon-containing film 208 such that the silicon-containing film 208 is no longer disposed between the substrate 202 and the silicon oxide layer 206.

[0043] The application of an oxidizing medium containing an amine additive, such as ammonia-containing vapor, under high pressure allows a high concentration of oxidizing species from the oxidizing medium to penetrate deeper into the silicon-containing film, which allows the oxidizing species to generate more silicon oxide film material through oxidation. Without being bound by theory, it is believed that the high pressure in the high pressure vessel promotes the diffusion of the oxidizing species into deeper vias. In addition, the presence of the amine additive in the vapor allows the target pressure to be reached at a much faster rate compared to high temperature rapid thermal oxide films, which is believed to increase the oxidation rate by a factor of 2-3.

[0044] The quality of the silicon oxide film 206 can be verified by comparing the wet etch rate of the silicon oxide film 206 formed at a temperature below 550° C. and a pressure higher than 1 bar using an oxidizing medium containing an amine additive with the wet etch rate of the silicon oxide film formed at a temperature above 800° C. and a low pressure without an amine additive (i.e., a high temperature rapid thermal oxide film). When wet etching is performed on both the silicon oxide film 206 having a thickness greater than about 20 angstroms and the high temperature rapid thermal oxide film of the same thickness, the wet etch rate is approximately the same for both films. In one embodiment, both the silicon oxide film 206 and the high temperature rapid thermal oxide film have wet etch rates of about 26 angstroms / min to about 32 angstroms / min.

[0045] Additionally, the quality of the silicon oxide film 206 can be further verified by comparing the leakage and equivalent volume thickness of the silicon oxide film 206 formed with an oxidation medium containing an amine additive at a temperature below 550° C. and a pressure above 1 bar with that of a high temperature rapid thermal oxide film. When comparing the leakage of the silicon oxide film 206 having a thickness greater than about 20 Angstroms with that of the high temperature rapid thermal oxide film of the same thickness, both silicon oxide films were located along the thermal trend line or extrapolated thermal trend line of the leakage voltage vs. thickness graph. Thus, the leakage and equivalent volume thickness of the silicon oxide film 206 are approximately the same or comparable to that of the high temperature rapid thermal oxide film. In one embodiment, both the silicon oxide film 206 and the high temperature rapid thermal oxide film have leakage vs. equivalent volume thicknesses of about 0.22 V / Angstrom to about 0.25 V / Angstrom.

[0046] Thus, for a process carried out at a relatively low temperature below 550° C., the results in improving film quality are substantially similar to a process carried out at 800° C. and at a lower pressure. The process carried out at a relatively low temperature below 550° C. using an oxidizing medium containing an amine additive allows the uniform deposition of silicon oxide layers, including on substrates with difficult or non-uniform structures.

[0047] Furthermore, by forming silicon oxide films at temperatures below 550° C. and pressures above 1 bar using an oxidizing medium with an amine additive and / or a hydrogen-based additive, the silicon oxide films can be made to thicknesses that exceed the capabilities of high-temperature rapid thermal oxidation processes while still maintaining high quality. Thus, depositing silicon oxide films using an oxidizing medium with an amine additive at temperatures below 550° C. and pressures above 1 bar increases the oxidation rate and results in conformal or uniform silicon oxide films with the same quality as high-temperature rapid thermal oxide films.

[0048] Additionally, depositing silicon oxide films utilizing an oxidizing medium with an amine additive at temperatures below about 550° C. expands the process window for forming silicon oxide films since the process window is no longer limited to temperatures above about 800° C. Expanding the process window increases the capabilities of current tools used to form silicon oxide films, reducing overall resource footprint.

[0049] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, the scope of the disclosure being defined by the following claims.

Claims

1. 1. A method for forming a silicon oxide film, comprising: loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel; forming a silicon oxide film on the silicon-containing film, exposing the silicon-containing film to an oxidizing medium containing an amine additive at a pressure greater than 1 bar; and Maintaining the high pressure vessel at a temperature between 100° C. and 550° C. forming a silicon oxide film comprising: Including, The method wherein said oxidizing medium comprises from 1,000 ppm to 20,000 ppm of said amine additive.

2. A method for producing a silicon-containing film comprising: loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel; forming a silicon oxide film on the silicon-containing film, exposing the silicon-containing film to an oxidizing medium containing an amine additive at a pressure greater than 1 bar; and Maintaining the high pressure vessel at a temperature between 100° C. and 550° C. forming a silicon oxide film comprising: Including, The method, wherein the silicon-containing film is a silicon nitride film and the oxidizing medium further comprises a hydrogen-based additive.

3. The method of claim 1 or 2, wherein the amine additive comprises ammonium or ammonia.

4. 3. The method of claim 1 or 2, wherein the oxidizing medium is selected from the group consisting of steam, peroxides, oxygen, ozone, water vapor, heavy water, hydroxide-containing compounds, oxygen isotopes, hydrogen isotopes, and combinations thereof.

5. 3. The method of claim 1 or 2, wherein the silicon oxide film has a uniform thickness between 20 Angstroms and 400 Angstroms and the temperature is between 400°C and 505°C.

6. 3. The method of claim 1 or 2, wherein forming the silicon oxide film on the silicon-containing film is carried out for a time period between 5 minutes and 150 minutes.

7. 1. A method for forming a conformal silicon oxide film, comprising: depositing a silicon-containing film on a substrate including a plurality of vias, the silicon-containing film being deposited on each exposed surface of the substrate and the plurality of vias; loading the substrate having the silicon-containing film deposited thereon into a processing region of a high pressure vessel; forming a conformal silicon oxide film on the silicon-containing film, exposing the silicon-containing film to an oxidizing medium comprising an amine additive, the oxidizing medium comprising 1,000 ppm to 20,000 ppm of the amine additive; and maintaining said high pressure vessel at a temperature between 100°C and 550°C and a pressure between 1 bar and 65 bar; forming a conformal silicon oxide film comprising: A method comprising:

8. 8. The method of claim 7, wherein the amine additive comprises ammonium or ammonia and the oxidizing medium comprises 7,000 ppm of the amine additive.

9. 8. The method of claim 7, wherein the oxidizing medium is selected from the group consisting of steam, peroxides, oxygen, ozone, water vapor, heavy water, hydroxide-containing compounds, oxygen isotopes, hydrogen isotopes, and combinations thereof, and the silicon-containing film comprises silicon or silicon nitride.

10. 8. The method of claim 7, wherein the oxidizing medium is steam, the amine additive is ammonia, the silicon-containing film is a silicon nitride film, and the oxidizing medium further comprises a hydrogen-based additive.

11. 8. The method of claim 7, wherein forming the silicon oxide film on the silicon-containing film is carried out at a temperature between 400° C. and 505° C. for a time period between 5 minutes and 150 minutes, and the conformal silicon oxide film has a uniform thickness between 20 Angstroms and 400 Angstroms.

12. A method for forming a silicon oxide film, comprising the steps of: loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel; forming a silicon oxide film on the silicon-containing film, exposing the silicon-containing film to an oxidizing medium comprising ammonia, the oxidizing medium being selected from the group consisting of steam, oxygen, and peroxide; and maintaining the high pressure vessel at a temperature between 400° C. and 505° C. and a pressure greater than 10 bar, wherein the silicon oxide film has a uniform thickness between 100 Angstroms and 400 Angstroms. Including, The method of claim 1, wherein the oxidizing medium comprises from 1,000 ppm to 20,000 ppm of the ammonia.

13. A method for forming a silicon oxide film, comprising the steps of: loading a substrate having a silicon-containing film deposited thereon into a processing region of a high pressure vessel; forming a silicon oxide film on the silicon-containing film, exposing the silicon-containing film to an oxidizing medium comprising ammonia, the oxidizing medium being selected from the group consisting of steam, oxygen, and peroxide; and maintaining the high pressure vessel at a temperature between 400° C. and 505° C. and a pressure greater than 10 bar, wherein the silicon oxide film has a uniform thickness between 100 Angstroms and 400 Angstroms. Including, The method, wherein the silicon-containing film comprises silicon or silicon nitride and the pressure is between 10 bar and 60 bar.

14. 14. The method of claim 12 or 13, wherein forming the silicon oxide film on the silicon-containing film is carried out for a time period between 5 minutes and 120 minutes.

Citation Information

Patent Citations

  • Manufacture of semiconductor device

    JP1981135936A

  • Formation of oxide film and production of semiconductor therewith

    JP1996031813A

  • Method of improving oxide growth rate of selective oxidation processes

    JP2012044192A

  • Metal gate electrode stack with a passivating metal nitride layer

    US20010025971A1

  • Methods for fabricating nanowire for semiconductor applications

    US20190019681A1