Sputtering target for producing a layer containing molybdenum oxide
A sputtering target with molybdenum and doping elements like tantalum or niobium stabilizes the process and ensures uniform layer deposition, addressing process instability and non-uniformity in molybdenum oxide layer production.
Patent Information
- Application Number
- JP2021557471
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-03
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-03-03
AI Technical Summary
Existing sputtering processes for producing molybdenum oxide-containing layers face challenges such as unstable process control, high etch rates, and layer non-uniformity due to hysteresis effects and target poisoning, making it difficult to produce high-quality layers on an industrial scale.
A sputtering target composed of molybdenum with doping elements like tantalum, niobium, or vanadium, forming a mixed oxide (Mo1-xMx)5O14, where the oxygen content matches the desired layer, ensuring stable process control and uniform layer deposition by minimizing the need for additional oxygen supply.
The solution provides a stable, high-quality molybdenum oxide layer with controlled etch rates and uniform composition, reducing arcing and particle formation, suitable for industrial-scale production.
Smart Images

Figure 0007580390000001 
Figure 0007580390000002 
Figure 0007580390000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a sputtering target for producing a molybdenum oxide containing layer and to the use of such a sputtering target for depositing a molybdenum oxide containing layer. [Background technology]
[0002] Molybdenum oxide-containing layers (especially based on molybdenum oxide) are used in particular in layer structures for optical or optoelectronic applications, such as for example electronic displays, due to their interesting optical properties. They are often used in combination with or directly adjacent to metal layers, for example from aluminum (Al), copper (Cu), titanium (Ti) or (metallic) molybdenum (Mo), which act for example as electrical conducting paths. An example of the use of molybdenum oxide layers can be found in JP 2013020347, where metal conducting paths in displays (touch screens) of capacitive touch sensors are coated with MoO 2 in order to suppress undesired reflections of the metal conducting paths. x The optical fiber is covered with a light-absorbing layer from
[0003] Important properties such as light absorption, light reflectance, light transmittance, etching rate, thermal stability, and stability against further chemicals (e.g. photoresist developer or photoresist remover) used in the manufacturing process depend on the exact stoichiometric composition of the deposited molybdenum oxide-containing layer and the added doping elements (e.g. Ta, Nb, etc.). Here, the etching rate is important in the subsequent structuring of the deposited layer by photolithography associated wet chemical etching processes. Thus, for example, in many applications such as the above-mentioned capacitive touch sensor, a molybdenum oxide-containing layer is required in which the oxide (molybdenum oxide and / or molybdenum-containing mixed oxide) is present in a substoichiometric composition, i.e. the oxide has unoccupied oxygen valences and oxygen vacancies are present in the deposited molybdenum oxide-containing layer. In such substoichiometric molybdenum oxide-containing layers (especially based on molybdenum oxide), interesting electro-optical properties can be achieved, such as, for example, high optical absorption (and correspondingly low optical reflectance) in the visible wavelength range, especially at a reference wavelength of 550 nm, and at the same time sufficient electrical conductivity (especially sheet resistances of <20 kΩ / square or <20 kΩ / square). Although pure molybdenum oxide layers have attractive electro-optical properties, they usually exhibit too high etching rates in common wet etching media (e.g. PAN etching based on phosphoric acid, nitric acid and acetic acid for structuring aluminum metallizations, etching based on H2O2 for structuring Cu), which leads to unstable etching results. By adding doping elements, such as, for example, Ta and / or Nb, to the substoichiometric molybdenum oxide-containing layers (and correspondingly to the target material of the sputtering target), the etching rate can be reduced to acceptable levels without significantly changing the electro-optical properties.
[0004] Such molybdenum oxide-containing layers (especially based on molybdenum oxide) are produced industrially in coating processes by cathodic atomization ("sputtering"). In principle, it is possible to produce such molybdenum oxide-containing layers by reactive sputtering of a metal target material, which is reactively sputtered, for example, in appropriately adjusted argon and oxygen process gas atmospheres. Here, the metal atoms of the target material react mostly with oxygen from the process gas only during the coating process, so that process control is made difficult by hysteresis effects (discontinuous changes in the layer deposition rate, discharge current and / or target voltage due to changes in the oxygen partial pressure) and poisoning of the target surface (target poisoning). In contrast thereto, deposition of sputtering targets with oxide target materials is advantageous under industrial conditions, since the coating process can be carried out with pure noble gas process gas (usually argon) or with noble gas (usually argon) as the main component with the addition of small amounts of other gases, such as, for example, oxygen. In particular, when using oxide target materials, process control is simplified while higher coating speeds and higher process stability are possible. Furthermore, many of the coating equipment already installed are designed only for depositing metal layers of metal sputtering targets, and therefore cannot supply oxygen to the sputtering gas. The versatility of such available sputtering equipment can be increased by using oxide target materials.
[0005] In German Patent Application Publication No. 102012112739, oxygen deficiency is 5-y , TiO 2-y , MoO 3-y , WO 3-y , V2O 5-yUS 2001 / 0020586 describes a substoichiometric target material that is prepared solely by a reduced oxide phase of a substoichiometric and thereby conductive oxide or oxynitride based on (Y>0) or mixtures thereof, or by this reduced oxide phase together with a metal mixture. y where M is at least one metal from the group consisting of Ti, Nb, Ta, Mo, W, Zr and Hf.
[0006] Apart from the above problems and configurations regarding molybdenum oxide-containing layers and corresponding target materials, academic publications have described the production of powdered molybdenum-containing mixed oxide compounds on a laboratory scale (i.e., several grams of product amount) with holding times at high temperatures of one week or more. For example, Ekstroem and Nygren (Thommy Ekstroem and Mats Nygren, Acta Chemica Scandinavica 26 (1972) 1836-1842) reported the production of (MoO) in the homogeneity range of 0.06≦x≦0.08 by mixing Ta2O5 powder with MoO3 and MoO2, filling the powder mixture into a quartz ampoule, degassing the quartz ampoule, and heating it to 640-750 °C for a period of one week to several weeks. 1-x Ta x )5O 14 The publication describes the synthesis of (Mo 1-x Nb x )5O 14 The synthesis of Nb2O5, MoO3 and MoO2 is also described. The starting powders are Nb2O5, MoO3 and MoO2, and the synthesis conditions are (Mo 1-x Ta x )5O 14The mixed oxides were obtained in the temperature range 600-750 °C, but in a further publication (Thommy Ekstroem and Mats Nygren, Acta Chemica Scandinavica 26 (1972) 1827-1835), similar to the mixed oxides already described, were prepared from powder mixtures of V2O5 with MoO3 and MoO2 (Mo 1-x V x )5O 14 also describes the synthesis of (Mo) with a homogeneity range of 0.03≦x≦0.05, where a wide homogeneity range of 0.02≦x≦0.11 was observed when heated to 640°C or 0.05≦x≦0.11 when heated to 750°C. 1-x Ti x )5O 14 The synthesis of was also already described by Ekstroem (Thommy Ekstroem, Acta Chemica Scandinavica 26 (1972) 1843-1846), where its preparation from a powder mixture of TiO2, MoO2 and MoO3 was carried out similarly to the mixed oxides already described, but by heating to temperatures of 600-750 °C. In all syntheses, the products were obtained only in small quantities (gram scale) in loose powder form, and not as consolidated macroscopic solids. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent No. 2013020347 [Patent Document 2] DE 102012112739 [Patent Document 3] US Patent Application Publication No. 2001 / 0020586 [Non-patent literature]
[0008] [Non-Patent Document 1] Thommy Ekstroem and Mats Nygren, Acta Chemica Scandinavica 26 (1972) 1836-1842 [Non-Patent Document 2] Thommy Ekstroem and Mats Nygren, Acta Chemica Scandinavica 26 (1972) 1827-1835 [Non-Patent Document 3] Thommy Ekstroem, Acta Chemica Scandinavica 26 (1972) 1843-1846 Summary of the Invention [Problem to be solved by the invention]
[0009] It is therefore an object of the present invention to provide a doped molybdenum oxide-containing sputtering target, which allows for a stable sputtering process for producing high-quality layers, and which should be producible cheaply and process-reliably on an industrial scale.
[0010] This problem is solved by a sputtering target according to claim 1 and by the use of a sputtering target according to claim 15. Advantageous developments of the invention are set forth in the dependent claims. [Means for solving the problem]
[0011] In accordance with the present invention, there is provided a sputtering target having a conductive oxide target material, wherein the target material comprises: - Molybdenum (Mo) as the main metallic component, and at least one doping element M from the group consisting of tantalum (Ta), niobium (Nb), vanadium (V) and titanium (Ti); The metal oxide of the present invention is at least one of the metal oxides.
[0012] The target material is a mixed oxide (Mo) with a range of 0.01≦x≦0.13 (measured on its ground cross section by Raman microscopy (Raman spectroscopy)). 1-x M x )5O 14 wherein M is one or more elements from the group consisting of tantalum (Ta), niobium (Nb), vanadium (V) and titanium (Ti).
[0013] Here, the invention is based on the recognition that, with regard to the process stability of the sputtering process, it is advantageous if the oxygen content of the target material is identical or substantially identical to the oxygen content of the layer to be produced. Preferably, the oxygen content (wt%) of the target material and the oxygen content (wt%) of the layer to be produced differ from each other by a maximum of ±2 wt%. Thus, no or only a small supply of oxygen via the process gas is required, which suppresses hysteresis effects and simplifies the process control.
[0014] Furthermore, it should be considered that in principle a large number of phase compositions of the doped molybdenum oxide-containing target material are possible. On the one hand, molybdenum can exist in different oxidation states, in particular in the form of MoO2, MoO3, as well as in several substoichiometric oxides, MoO y , e.g., MoO 11 (y=2.75), Mo 17 O 47 (y=2.76), MoO 14 (y=2.8), MoO 23 (y=2.875), Mo9O 26 (y=2.89) and Mo 18 O 52 (y=2.89), where Mo9O 26 is a high temperature transformation, and Mo 18 O 52is a low temperature transformation. According to the invention, it is intended that at least one doping element M is contained in the target material. This adds an additional degree of freedom with respect to the possible phase compositions of the target material, since at least the doping element M can essentially be present in the target in elemental form (i.e. as metallic form, for example Ta, Nb, V, Ti), as an oxide (for example Ta2O5, V2O5, Nb2O5, TiO2), as a substoichiometric oxide and even form mixed oxides with one or more of the above-mentioned molybdenum oxides and / or with one or more oxides of at least one further doping element M. With regard to the large number of possible phase compositions, the invention is based on the recognition that different phases of the target material, especially if they are partially insulating or dielectric, can lead to particle formation due to the formation of arcs during sputtering. This can result in layer defects or damage to the sputtering target. Furthermore, the strength of oxide targets is rather low, especially when the microstructure has multiple different, unevenly distributed, rough and / or porous phases. In terms of strength, this is particularly critical when the phases have different densities or CTEs (CTE: coefficient of thermal expansion) and / or when adjacent phases are not sufficiently strongly connected to each other, for example due to diffusion holes, different lattice types, etc. Different phases may also have partially different sputtering rates, which may lead to poor layer uniformity and layer stoichiometry of the produced layer, especially in the case of multiple unevenly distributed rough and porous phases of the target material. Some phases (e.g. MoO3) are slightly water-soluble, so that during the production process (e.g. machining, cleaning), changes in the stoichiometry of the surface region and / or inclusion of residual moisture may occur, which may have a negative effect on the sputtering process and the produced layer (e.g. vacuum inhibition, inclusion of H2O in the layer).
[0015] In contrast, the (Mo) of 0.01≦x≦0.13 contemplated by the present invention in the target material 1-x M x )5O 14The mixed oxide phase has been found to be particularly advantageous, since it is electrically conductive, insoluble in water, and stable under ambient conditions. Moreover, the doping element M is thereby also (at least partially) bound in this matrix phase, and thus in the electrically conductive phase, and is evenly distributed throughout the target material. By forming the matrix phase with this mixed oxide phase according to the invention, in which an optionally present second phase (preferably finely distributed) may be included, this mixed oxide phase occupies a significant proportion of the target material throughout the sputtering target, and thus the entire target material takes on these advantageous properties. Thereby, for example, the entire target material is electrically conductive, and contact with water is relatively unimportant, since the matrix is not attacked by it. As explained above, these properties are advantageous with respect to uniform sputtering rates, avoidance of arcing and particle formation, uniform layer composition and uniform layer thickness, stable process control during the sputtering process, and easy manufacture, storage and handling of the sputtering target. It is further advantageous that the sputtering targets according to the invention can be produced on an industrial scale as dense components (e.g., at least 1 kg of dense target material per target segment) having high relative density and high phase purity within short process times (e.g., typically <12 hour holding times), as described in more detail below.
[0016] "Sputtering", also called cathodic atomization, is a physical process in which atoms or molecules are released from a solid (target material) into the gas phase by the impact of energetic ions (e.g. noble gas ions of the process gas). To produce thinner layers, the atomized target material is deposited on a substrate, where it forms a solid layer. This coating process, sometimes called sputtering deposition, is one of the PVD methods (PVD: physical vapor deposition), hereinafter also called "sputtering". The target material is the sputtering target material present as a solid material that is intended to be atomized and layered during the sputtering process (optionally together with further material from the process gas and / or of the further sputtering target). The sputtering target may be formed only by the target material, or may further have further components connected directly or indirectly (i.e. via at least one further component) with the target material, such as backplate(s), support tube(s), connector(s), insert(s), etc. Here, the sputtering target (and correspondingly the target material) can be provided in various shapes, in particular as planar sputtering targets having various basic shapes, such as square, rectangular, circular, etc., or also as tubular sputtering targets. In particular, the target material forms a macroscopic solid extending along at least one spatial direction of at least 0.03 m (meters).
[0017] By "oxide" target material, it is understood that the metals contained in the target material are present substantially completely as oxides. In particular, the proportion of metal phases in the target material is <1% by volume with respect to its ground cross section. In particular, the proportion of metal phases in the target material is below the detection limit by Raman measurements, which are used here and will be explained in more detail below. A target material is called "conductive" if it has a conductivity of at least 80 S / m, measured by a resistance measuring stand (Ulvac ZEM3) in the four-point measurement method. By "phase" of a target material is understood that spatial region, within which there is a uniform chemical composition and a uniform crystal structure, the orientation of the individual crystal grains in the phase may vary. By "mixed oxide" is understood an oxide whose crystal lattice has a crystal structure composed of oxygen ions and cations of several elements, here in particular Mo and at least one doping element M. By "matrix phase" it is understood that this matrix phase extends throughout the target material in a continuous, permeable network, in which an optionally present further phase ("second phase") is embedded as island regions (observation of ground cross sections by Raman spectroscopy using a Raman microscope).
[0018] The different phases and their volume fractions, as well as the density of the target material, are determined on the basis of a representative cross-section of the sample, where an isotropic structure can be assumed, and the volume data are derived from the area fractions measured at the cut surface (i.e. the volume fractions correspond to the measured area fractions). For this purpose, metallographic grindings of the sample are produced by dry preparation, whereby Raman spectroscopy with a Raman microscope is applied to determine the spatial resolution of the different metal oxide phases. As described in more detail below, in Raman spectroscopy, the sample surface of the target material to be analyzed is scanned point-wise with a laser beam, and a complete Raman spectrum is created for each measurement point ("Raman mapping"). By comparing the Raman spectrum obtained for each measurement point with the corresponding reference spectra of the different metal oxides, the corresponding phases are assigned to each measurement point, whereby a two-dimensional representation of the phase composition of the sample is created, from which the area fractions (or volume fractions) of the different phases are calculated. (Mo 1-x M x )5O 14 The matrix phase can be clearly identified by Raman spectroscopy. (Mo 0.93 Ta 0.07 )5O 14 The reference Raman spectrum of the phases is shown in FIG. 1. Powder diffractogram data can be obtained from the International Centre for Diffraction Data (ICDD) under PDF number 01-070-0952. The volume data (or the equivalent area data) of the different metal oxide phases are normalized and are relative to the total volume (or total area) occupied by the material particles of the target material. The volume (or the equivalent area) occupied by the pores of the target material is excluded from this total volume (or this total area). The volume data (or the equivalent area data) of the individual metal oxide phases therefore add up to 100% without including the pore volume.
[0019] According to the invention, the target material can be formed from one metal oxide or even from several metal oxides of different chemical composition (which then form different phases). Here, each metal oxide can be a stoichiometric or substoichiometric metal oxide of exactly one metal or alternatively several metals (i.e. in the latter case mixed oxides). According to the invention, Mo is the major constituent based on the metals contained (present as cations), i.e. the Mo ratio (Mo; atomic %) to the sum (Me: atomic %) of all metals contained including the Mo ratio (Mo; atomic %), i.e. Mo / (Me+Mo), is at least 50%. In particular, this is at least 80%, even more preferably at least 84%. Basically, in addition to Mo and at least one doping element M, further metals may also be contained in the target material. However, preferably, the further metals contained in the target material in addition to Mo (excluding any impurities present) are formed only from at least one doping element M. Basically, two or more doping elements M from the group Ta, Nb, V and Ti may be contained in the target material. In particular, however, exactly one doping element M from this group is contained in the target material. Preferably, this exactly one doping element M is Ta or alternatively Nb. By adding Ta and / or Nb as doping elements, the wet etching rate of a common aluminum etchant (a mixture of phosphoric acid, nitric acid, acetic acid and water) can be reduced to an acceptable level. The wet etching rate of a copper etchant based on hydrogen peroxide can also be influenced by adding Ta or Nb. Ta or Ta oxide powder is a starting product available in large quantities, but with a large price fluctuation. Nb or Nb oxide powder is usually available at a relatively low price.
[0020] As previously mentioned, the target material may contain manufacturing-related "impurities" (both metallic and non-metallic), such as tungsten (W), sodium (Na), potassium (K), antimony (Sb), vanadium (V), chromium (Cr), iron (Fe), carbon (C) and nitrogen (N). The total content of such impurities is typically <1,000 μg / g.
[0021] Basically, according to the invention, a mixed oxide (Mo 1-x M x )5O 14 may contain two or more doping elements M from the group Ta, Nb, V and Ti. In particular, however, exactly one doping element M from this group is contained in the mixed oxide (Mo 1-x M x )5O 14 Furthermore, according to the present invention, a plurality of different mixed oxides (Mo 1-x M x )5O 14 can be contained in the target material, in which case exactly one of these mixed oxides forms the matrix phase. However, in particular such mixed oxides (Mo 1-x M x )5O 14 In particular, the mixed oxide of the matrix phase (Mo 1-x M x )5O 14 The range of x in is 0.02≦x≦0.12.
[0022] According to one development, the target material is - Molybdenum (Mo) as the main metallic component, and at least one doping element M from the group consisting of tantalum (Ta), niobium (Nb), vanadium (V) and titanium (Ti); It is therefore possible to say that no further metals are contained, apart from possible impurities (see above for the definition of "impurities"), and that all metals are oxidatively bound (e.g. not present as nitrides, borides, etc.). In this way, the advantageous properties of the molybdenum oxide(s) are achieved in combination with the effect of at least one doping element M (e.g. influence on the wet etching rate), without the occurrence of possible further disadvantageous interactions.
[0023] According to one development, the mixed oxide (Mo 1-x M x )5O 14 The matrix phase from has a proportion in the target material of ≧60% by volume (measured with a Raman microscope (Raman spectroscopy)) with respect to the ground cross section of the target material, i.e. this proportion is in the range of 60-100% by volume. In particular, this proportion is ≧75% by volume, i.e. this proportion is in the range of 75-100% by volume, and even more preferably this proportion is ≧90% by volume, i.e. this proportion is in the range of 90-100% by volume. The higher the proportion of the mixed oxide phase, the more the target material takes on the advantageous properties explained above of this matrix phase. A very high proportion means that the composition of the target material is dominated by mixed oxides (Mo 1-x M x )5O 14 In one development, this ratio is 100% by volume (i.e. no second phases can be detected). To achieve 100% by volume, the composition of the target material must approximately correspond to the ratio of the elements in the mixed oxide. For the determination of the ratio in volume %, see the general description above and the detailed description below of sample preparation and Raman spectroscopy.
[0024] According to one development, in the target material a. MoO2 and / or Mo4O 11 , and b. Optionally, one or more compounds from the following group: - MoO3, - Mo 17 O 47 , Mo5O 14 , Mo8O 23 , Mo9O 26 and further sub-stoichiometric molybdenum oxides from the group of Mo 18 O 52 , - Stoichiometric (e.g., Ta2O5) and / or sub-stoichiometric (e.g., Ta2O 5-l ; 0 < l < 1) Ta oxides (plural), - Stoichiometric (e.g., Nb2O5) and / or sub-stoichiometric (e.g., Nb2O 5-m ; 0 < m < 1) Nb oxides (plural), - Stoichiometric (e.g., V2O5) and / or sub-stoichiometric (e.g., V2O 5-n ; 0 < n < 1) V oxides (plural), and - Stoichiometric (e.g., TiO2) and / or sub-stoichiometric (e.g., TiO 2-o ; 0 < o < 1) titanium oxides (plural) are contained as one or more second phases distributed as islands in the matrix phase, and these second phases, with respect to the ground section of the target material, (measured using a Raman microscope (by Raman spectroscopy)) total ≤ 40% by volume, i.e., this ratio is in the range of 0.1 - 40% by volume. In particular, when the composition of the target material deviates from the ratio of elements in the mixed oxide (Mo 1-x M x )5O 14 , a second phase is strongly formed. For example, when the ratio of the doping element M is relatively low, thereby restricting the formation of the mixed oxide (Mo 1-x M x )5O 14 , a molybdenum oxide phase is formed. Here, among the second phases mentioned, the previously mentioned phases MoO2 and Mo4O 11 have a high (nearly metallic) conductivity (MoO2: 1.25×10 6 S / m; monoclinic Mo4O 11 : 1.25×106 S / m) and has a relatively low vapor pressure, which is favorable for the stability of the coating process. 17 O 47 , Mo5O 14 , Mo8O 23 , Mo9O 26 and Mo 18 O 52 This also applies to the optionally present phases from a. to b., which typically do not occur or occur only in small proportions in the course of the production considered here. Preferably, the proportion of the second phases mentioned under a. and b. is ≦25% by volume (i.e. this proportion is in the range from 0.1 to 25% by volume), even more preferably ≦10% by volume (i.e. this proportion is in the range from 0.1 to 10% by volume), the remaining volume proportions being in each case made up of particularly advantageous mixed oxides (Mo 1-x M x )5O 14 It is composed of:
[0025] According to one development, the proportion of the second phase MoO3 in the target material, with respect to its ground cross section (measured with a Raman microscope (Raman spectroscopy)), is in the range of 0-2 vol.%, i.e. this proportion is ≦2 vol.%. MoO3 is electrically insulating (electrical conductivity <1×10 -5 The proportion of the second phase MoO3 must be kept as low as possible, since the MoO3 content is 0.05 S / m, which can lead to the formation of particles during the coating process. Furthermore, MoO3 is water-soluble, which is disadvantageous in terms of mechanical processing and storage of the target. Preferably, the second phase MoO3 in the target material is not detectable at all by Raman spectroscopy (i.e. the measured proportion is 0% by volume) or, if it cannot be completely avoided, is kept to a proportion in the range of 0.1-1.0% by volume.
[0026] According to one development, the oxygen content in weight percent in the target material is in the range of 26-32 weight percent. Since the oxygen content in the deposition layer affects the light reflection, preferably an approximately corresponding oxygen content, typically in the above-mentioned range, is adjusted in the target material. Furthermore, within this range, sufficient electrical conductivity is achieved, so that a DC (direct current) sputtering process is possible (while electrically insulating targets have to be sputtered in an RF (RF: radio frequency, i.e. radio frequency) sputtering process (i.e. alternating current), which is associated with increased costs (especially with regard to the design of the sputtering installation). Here, the oxygen content can be adjusted in the production process by weighing the corresponding oxide-containing powder, as will be explained in further more detail below, whereby the weighed oxygen ratio (relative to the weighed metal ratio) corresponds to the desired oxygen content of the target material. At the same time, the oxygen content mentioned is adjusted in the production process by weighing the mixed oxide (Mo 1-x M x )5O 14 This is favorable for the sintering behavior and formation of. Since the exact occupancy of the various lattice sites in the metal oxide phase can also be varied in a temperature-dependent manner if necessary, it is reasonable to consider only the total oxygen content in the target material. Here, the total oxygen content in the target material is determined by carrier gas thermal extraction (detection of oxygen as CO or CO2 by an infrared measuring cell, for example with LECO RO300 or LECO 836 devices).
[0027] According to one further development, the ratio of the (at least one) doping element M in atomic % to the total content of Mo and the doping element M in atomic %, i.e. M / (Mo+M), in the target material is in the range of 0.02 to 0.15. 1-x M x )5O 14 A minimum content of (at least one) doping element M is required so that the matrix phase (Mo 1-x M x )5O 14There are certain tolerances here, since the ratio x of the doping element M in the matrix phase can vary to some extent and therefore may even decrease slightly. Moreover, a minimum content of the doping element M is necessary in order for the desired properties of the layer to be produced (especially with regard to the wet etching behavior). Conversely, a too high content of the doping element M is disadvantageous, since the doping element M can no longer be absorbed in the matrix phase, which results in an increase in the proportion of oxides of the doping element (for example, Ta2O5, Nb2O5, VO5, TiO2) in the form of a second phase. Moreover, the reflectivity of the layer to be produced increases again to a certain extent with an increasing content of the doping element M (for example, in the case of Ta), and the etching rate also no longer corresponds to the desired range. Against this background, a range of 0.05 to 0.12 is particularly preferred for the ratio M / (Mo+M). The desired ratio M / (Mo+M) is practically unchanged in the manufacturing route described below, and can therefore be adjusted in the manufacturing process by weighing the corresponding powder. For the target material itself, the proportions of the metals contained and the ratio M / (Mo+M) can be determined by chemical analysis, in particular ICP-MS (Inductively Coupled Plasma Mass Spectrometry; Mass Spectrometry with Inductively Coupled Plasma) or by ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometry; Optical Emission Spectrometry with Inductively Coupled Plasma).
[0028] According to one development, in the target material, the doping element M is formed by Ta and the matrix phase from the mixed oxide is (Mo 1-x Ta x )5O 14 Typically, the matrix phase (Mo 1-x Ta x )5O 14The Ta ratio in the matrix phase (Mo) has a value of 0.07. Depending on the availability of Ta for forming the matrix phase in the production (i.e., depending in particular on the composition and amount ratio of the starting powder), x is usually in the range of 0.06≦x≦0.08, and the matrix phase is stably formed in this range. As mentioned above, Ta is particularly preferred from the viewpoint of influencing the wet etching rate and availability. 1-x Ta x )5O 14 has also proven to be particularly advantageous in practice.
[0029] Preferably, the highest possible proportion of the added doping element M (here Ta) is present in the form of a mixed oxide (Mo 1-x M x )5O 14 In the matrix phase from the target material, preferably the doping element M (here Ta) is present as a metal oxide (for example, mixed oxide, Ta2O5) and not as a metallic element if it is not fully incorporated. Ta as a metallic phase would result in significantly different properties. The proportion of Ta2O5 is also preferably relatively low, since Ta2O5 is dielectric and therefore can be a source of particles and layer defects during sputtering. Furthermore, Ta2O5 can be optically transparent as a thin partial layer in the produced layer, which can deteriorate the optical properties of the layer. Thus, according to one development, Ta (preferably as the only contained doping element M) is present in the target material completely as a metal oxide (for example, mixed oxide, Ta2O5) (i.e. not present as a metallic element), and the proportion of the phase Ta2O5 is in the target material, with respect to its ground cross section (measured with a Raman microscope (Raman spectroscopy)) ≦3% by volume (i.e. a proportion of 0-3% by volume), preferably ≦1% by volume (i.e. a proportion of 0-1% by volume). This is especially true when the ratio of the doping element Ta in atomic % to the total content of Mo and Ta in atomic %, ie M / (Mo+M), is in the range 0.02 to 0.15, preferably in the range 0.05 to 0.12.
[0030] According to one further development, in the target material, the doping element M is formed by Nb and the matrix phase from the mixed oxide is (Mo 1-x Nb x )5O 14 Depending on the availability of Nb to form the matrix phase in the production (i.e., depending on the composition and amount ratio of the starting powder in particular), x is usually in the range of 0.07≦x≦0.12, and the matrix phase is stably formed in this range. As mentioned above, Nb is advantageous in terms of its effect on the wet etching rate and its cheap availability, since the matrix phase is stably formed over a wider range of 0.07≦x≦0.12.
[0031] Similarly, as explained above for Ta, preferably the highest possible proportion of the added doping element M (here Nb) is present in the form of a mixed oxide (Mo 1-x M x )5O 14 Preferably, the doping element M (here Nb) is present in the target material completely as a metal oxide (e.g. mixed oxide, Nb2O5) and not as a metallic element, if it is not completely incorporated. Thus, according to one development, Nb is present in the target material completely as a metal oxide (e.g. mixed oxide, Nb2O5) (i.e. not present as a metallic element), and the proportion of the phase Nb2O5 in the target material, with respect to its ground cross section (measured with a Raman microscope (Raman spectroscopy)) is ≦3% by volume (i.e. a proportion of 0-3% by volume), preferably ≦1% by volume (i.e. a proportion of 0-1% by volume). This applies in particular when the ratio of the doping element Nb in atomic % to the total content of Mo and Nb in atomic %, i.e. M / (Mo+M), is in the range of 0.02-0.15, preferably in the range of 0.05-0.12.
[0032] According to one development, the target material has a relative density of ≧95% (i.e. in the range of 95-99.9%), in particular ≧97% (i.e. in the range of 97-99.9%), preferably ≧98% (i.e. in the range of 98-99.9%). Dense target materials with high relative density are important for the quality of the deposited layer, since less dense target materials can cause flash discharges ("arcs") and particle formation during sputtering. The relative density is determined by digital image analysis based on optical microscope images of metallographic grindings of the target material, in which the relative area ratio of pores "FA" (FA: area ratio of pores to the total area to be examined) is evaluated. The relative density corresponds to this value (1-FA), whereby the relative density is calculated as the arithmetic mean of three such porosity measurements. This procedure is described in detail below.
[0033] According to one development, the target material has a conductivity of ≧100 S / m at 25° C. This allows DC sputtering and also results in a sufficient conductivity in the produced layers, where the conductivity is measured by a resistance measuring stand (e.g. Ulvac ZEM3) in the four-point measurement method.
[0034] According to one development, the target material is present as a (macroscopic) solid produced by powder metallurgy. The powder metallurgical production route allows the target material to be produced inexpensively on an industrial scale as a dense component (e.g. at least 1 kg of dense target material per target segment) with high relative density and high phase purity within a short process time (e.g. typically <12 hours holding time). Powder metallurgical production is understood here as corresponding starting powders (in the case of several powders, appropriately mixed beforehand) being compressed by application of pressure and / or temperature. Here, powder metallurgical production results in a characteristic microstructure of the target material, in particular a multiphase and fine-grained structure. Powder metallurgical production is easily recognizable from the target material by the skilled person on the basis of ground cross sections, by optical microscope, by scanning electron microscope (SEM) or by Raman microscope.
[0035] The starting powder may optionally contain a small proportion of substoichiometric molybdenum oxide, in particular MoO 11 It is preferred to form a powder mixture of MoO2, MoO3 and one or more oxides of the doping element M (Ta2O5, V2O5, Nb2O5, TiO2), containing, for example, MoO3, MoO4, MoO5, MoO6, MoO7, MoO8, MoO9, MoO10, MoO11, MoO12, MoO13, MoO14, MoO15, MoO16, MoO17, MoO18, MoO19, MoO20, MoO31, MoO32, MoO33, MoO21, MoO32, MoO33, MoO22, MoO33, MoO31, MoO32, MoO33, MoO2 ...
[0036] During the subsequent compression step, the mixed oxide (Mo 1-x M x )5O 14 It should be noted that, on the one hand, in order to achieve the desired high proportion of the desired matrix phase from, the corresponding ratio of amounts of powders weighed out is close to the mixed oxide. Moreover, it is also essential that the powders used are very fine (typically d50 values of <10 μm) and very well mixed before the compaction step. As will be explained on the basis of the manufacturing examples, in the case of MoO2 powder and powder from oxides of doping element M (and also, if necessary, in the case of substoichiometric molybdenum oxides), the coarse fraction >63 μm is respectively sieved by a suitable sieving step (for example, a sieve with a mesh size of 63 μm). In the case of MoO3 powder, too, a particularly fine powder is used (for example, a d50 value of 3 μm and particle size measurement is performed by laser diffraction, for example, with a device from Malvern). It should be noted that the mixing of the powders is preferably carried out in an intensive mixer or with a plowshare mixer (Pflugscharmischer), in which case the powders are very well mixed.
[0037] Compaction can be carried out in particular by hot pressing, hot isostatic pressing, spark plasma sintering (SPS) or press sintering. Here, compaction is carried out in particular at temperatures of 600-800 ° C and pressing pressures of 15-110 MPa. Preferably, compaction is carried out in a vacuum or protective gas atmosphere (for example argon), especially when high temperatures are set. In the case of SPS, compaction is carried out by applying pressure and temperature, whereby heat is generated internally by an electric current passing through the powder mixture. In the case of hot pressing, compaction is likewise carried out by applying pressure and temperature, whereby heat is supplied from the outside via a heated mold. In the case of hot isostatic pressing, the starting powder is in a closed capsule and compaction is carried out by applying pressure and temperature to the capsule. In the case of compaction by press sintering, the starting powder is pressed into a green body, which is subsequently sintered by heat treatment below the melting temperature.
[0038] During the compaction process, the starting powder is converted into the target material in a solid-state reaction or, depending on the chemical composition and the process conditions, in a liquid-phase reaction or even in a multiphase reaction (e.g. solid-liquid). The reaction taking place here is similar to a comproportionierung: MoO3 is optionally converted into various substoichiometric oxides (e.g. Mo 18 O 52 , MoO 11 , ...), whereas MoO2 is at least partially oxidized to various substoichiometric oxides as required. Furthermore, at least one oxide of the doping element M (Ta2O5, V2O5, Nb2O5, TiO2) is mostly mixed oxides (Mo 1-x M x )5O 14 and form the matrix phase. After compaction, mechanical post-processing may be performed, for example by cutting tools, to obtain the desired final shape or for surface post-treatment (adjustment of the desired surface roughness). If necessary, further components such as, for example, backplate(s), support tube(s), connector(s), insert(s) must be further attached to complete the sputtering target.
[0039] According to one development of the invention, one or more second phases are formed in the target material as fine and evenly distributed small islands in the matrix phase (measured with a Raman microscope (Raman spectroscopy)) on its ground cross section. In particular, at least 95% of the islands of the second phase(s) have a circle equivalent diameter of ≦60 μm each (calculated from the corresponding area of the islands shown in the form of a circle with the same area and "circle equivalent diameter" respectively). Here, the number of "small islands each having a circle equivalent diameter of ≦60 μm" is taken into account relative to the total number of islands in a representatively selected analysis area of 1,000 μm × 1,000 μm. This fine island structure of the second phase(s) can be visualized by Raman images of the ground cross section and can be appropriately evaluated by qualitative image evaluation in terms of the area and size of the islands.
[0040] The present invention further relates to the use of a sputtering target according to the invention, which can be further formed by one or more of the above-mentioned developments and variants, for depositing a molybdenum oxide-containing layer, in which the sputtering process is carried out as a DC or pulsed DC sputtering process in a noble gas atmosphere without oxygen or alternatively with up to 20% by volume of oxygen supplied as reactive gas. In direct current or DC sputtering, a direct voltage is applied between the sputtering target connected as a cathode and the anode (usually a shielding steel plate in the housing and / or vacuum chamber of the coating installation). Here, the DC or pulsed DC sputtering process is carried out non-reactively in a noble gas atmosphere, in particular an argon gas atmosphere, preferably without additional oxygen supply. The layer deposited here may have a slightly lower oxygen content than the target material used due to slight oxygen deficiency during the coating process (removal of formed oxygen by the drawn-in process gas), which may vary slightly depending on the coating installation and the operating method. To produce a molybdenum oxide-containing layer having a higher oxygen content than that of the target material, the target material can also be subjected to reactive sputtering under a supply of oxygen of up to 20% by volume, preferably <10% by volume, even more preferably <5% by volume (based on the composition of the reactive gas), whereby the amount of oxygen supplied can be kept relatively low by using an oxide target material, and thus the disadvantages of reactive sputtering (hysteresis effects, potential non-uniformity of the deposited layer) do not affect as strongly.
[0041] Further advantages and usefulness of the present invention will become apparent on the basis of the following description of examples with reference to the accompanying figures, in which: -1 ) versus the Raman shift in (number or counts), respectively. [Brief description of the drawings]
[0042] [Figure 1]Raman reference spectrum of the mixed oxide (Mo0.93Ta0.07)5O14. [Diagram 2] Raman reference spectrum of Ta2O5. [Diagram 3] Raman reference spectrum of Mo18O52. [Figure 4] Raman reference spectrum of MoO2. [Diagram 5] Raman reference spectrum of MoO3. [Figure 6] Raman reference spectrum of Mo4O11. [Figure 7] The microstructure of the example according to the present invention created by Raman mapping. [Figure 8] The microstructure of the comparative example created by Raman mapping. [Figure 9] Graph in which the deposition rates (nm / min), i.e., nanometers per minute, are plotted for two sputtering targets (Example 1, Example 2) and a comparative example (reference) according to the present invention (each abbreviated as MoOz (2 < z < 3) and each having Ta2O5 in a corresponding molar ratio to the starting powder). [Figure 10] Graph in which the reflectance (%) is plotted against the wavelength (nm) (nanometers) for the layer systems deposited using two sputtering targets (Example 1, Example 2) and a comparative example (reference) according to the present invention shown in FIG. 8.
Mode for Carrying Out the Invention
[0043] Example 1: MoO2 powder (Plansee SE; d50 value of about 6 μm) is sieved through a sieve with a mesh size of 63 μm, and the coarse fraction >63 μm is not used any further. The 40 Mol% MoO2 powder thus obtained is mixed with 57 Mol% MoO3 powder (Molymet, here d50 value of about 3 μm) and 3 Mol% tantalum pentoxide powder (HC Starck, d50 value of about 2 μm; sieved to <63 μm; Ta2O5) in a ploughshare mixer (Loedige) for 20 min, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ250 mm (i.e. diameter 250 mm) and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 30 MPa, at a temperature of 800 °C and a holding time of 480 min. The relative density of the densified component is 97.5%. The bulk of the obtained target material is made up of mixed oxide (Mo) with a ratio of 79.4% by volume. 0.93 Ta 0.07 )5O 14 Furthermore, the target material consists of a matrix phase of 8.5% by volume of MoO2 phase and 12.1% by volume of Mo4O 11 It has a phase.
[0044] Example 2: MoO2 powder (Plansee SE; d50 value of about 6 μm) is sieved through a sieve with a mesh size of 63 μm, and the coarse fraction >63 μm is not used any further. The 40 Mol% MoO2 powder thus obtained is mixed with 57 Mol% MoO3 powder (Molymet, here with a d50 value of about 3 μm) and 3 Mol% tantalum pentoxide powder (HC Starck, d50 value of about 2 μm; sieved to <63 μm; Ta2O5) in an intensive mixer (Eirich) for 10 min, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ250 mm (i.e., diameter 250 mm) and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 30 MPa, a temperature of 800 °C and a holding time of 360 min. The relative density of the densified components is 99.5%. The bulk of the obtained target material is made up of mixed oxide (Mo) with a ratio of 94.3% by volume. 0.93 Ta 0.07 )5O 14 In addition, the target material contains a matrix phase of 2.6% by volume of MoO2 phase, 3.0% by volume of Mo4O 11 phase, and a Ta2O5 phase with a volume ratio of 0.1%.
[0045] FIG. 7 shows the microstructure of the target material produced in this way as determined by Raman mapping. In this microstructure, there are two regions, one with MoO2 phase, one with Mo4O phase, and one with MoO phase, corresponding to the above phase ratio. 11 It is possible to discern regions with Ta2O5 phase and regions with Ta2O5 phase. These different phases are 0.93 Ta 0.07 )5O 14 The crystalline structure is embedded in a matrix formed by the phases.
[0046] In contrast, FIG. 8 shows a comparative example of a mixed oxide (Mo 0.93 Ta 0.07 )5O 14 Raman mapping of the target material without the matrix phase from (Mo 0.93 Ta 0.07 )5O14 The phase is present in a proportion of 24.0% by volume. Mo4O 11 The Mo phase accounts for 50.3% by volume, the MoO2 phase accounts for 12.5% by volume, and the Mo 18 O 52 %。 As can be seen from Figure 8, the phases in the comparative target material are significantly coarser and more unevenly distributed than the target material according to the invention of Figure 7.
[0047] Example 3: MoO2 powder (Plansee SE; d50 value of about 6 μm) is sieved through a sieve with a mesh size of 63 μm, and the coarse fraction >63 μm is not used any further. The 52 Mol% MoO2 powder thus obtained is mixed with 42 Mol% MoO3 powder (Molymet, here d50 value of about 3 μm) and 6 Mol% tantalum pentoxide powder (HC Starck, d50 value of about 2 μm; sieved to <63 μm; Ta2O5) in a ploughshare mixer (Loedige) for 20 min, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ250 mm (i.e. diameter 250 mm) and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 30 MPa, a temperature of 800 °C and a holding time of 480 min. The relative density of the densified component is 97.5%. The bulk of the obtained target material is a mixed oxide (Mo) with a ratio of 80.3% by volume. 0.93 Ta 0.07 )5O 14 The resulting target material consists of a matrix phase of 18.9 vol.% MoO2 phase, 0.2 vol.% Mo4O 11 phase, and a Ta2O5 phase with a volume ratio of 0.6%.
[0048] Example 4: MoO2 powder (Plansee SE; d50 value of about 6 μm) is sieved through a sieve with a mesh size of 63 μm, and the coarse fraction >63 μm is not used any further. The 45 Mol% MoO2 powder thus obtained is mixed with 51 Mol% MoO3 powder (Molymet, here d50 value of about 3 μm) and 4 Mol% niobium pentoxide powder (HC Starck, d50 value of about 2 μm; sieved to <63 μm; Nb2O5) in a ploughshare mixer (Loedige) for 20 min, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ250 mm (i.e. diameter 250 mm) and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 30 MPa, at a temperature of 800 °C and a holding time of 360 min. The majority of the obtained target material was a mixed oxide (Mo 0.91 Nb 0.09 )5O 14 The matrix phase consists of the MoO2 phase with a volume fraction of 18.7%, the Mo4O phase with a volume fraction of 2.6%. The relative density of the densified component is 98.2%. The target material obtained consists of the MoO2 phase with a volume fraction of 18.7%, the Mo4O 11 phase, and a Nb2O5 phase with a volume ratio of 0.1%.
[0049] Example 5: MoO2 powder (Plansee SE; d50 value of about 6 μm) is sieved through a sieve with a mesh size of 63 μm, and the coarse fraction >63 μm is not used further. The 39 Mol% MoO2 powder thus obtained is ground in a ball mill for 10 min with 52 Mol% MoO3 powder (Molymet, here with a d50 value of about 3 μm) and 8 Mol% titanium dioxide powder (rutile; d50 value of <1 μm; TiO2) and subsequently mixed in an intensive mixer (Eirich) for 10 min to ensure a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ100 mm and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 30 MPa, a temperature of 800 °C and a holding time of 120 min. The relative density of the densified component is 91.2%. The resulting target material was a mixed oxide (Mo0.97 Ti 0.03 )5O 14 The matrix phase is made of
[0050] Sputtering Test: In the course of a series of tests, the molybdenum-tantalum oxide target materials produced according to Examples 1 and 2 were subjected to non-reactive sputtering under defined process conditions in comparison with a molybdenum-tantalum oxide target material not according to the invention (reference) in order to identify the properties of the layer. The molybdenum-tantalum oxide target material used as the reference had the same composition as in Examples 1 and 2, but contained a mixed oxide (Mo 0.93 Ta 0.07 )5O 14 No matrix phase was present from the ZnO phase. Here, the sputtering power was 100 W and the ZnO phase was 5.0 × 10 -3 A process pressure of argon at 1000 nm and 1000 nm argon at 1000 nm argon (22 sccm; sccm: standard cubic centimeters per minute) was used. The deposition rates of the sputtering targets used are shown in Figure 9, where the left column of Figure 9 corresponds to the target material of Example 1, the center column to the target material of Example 2, and the right column to the reference target material.
[0051] The reflectance of the prepared layer was used as the evaluation criterion. To determine the reflectance, a glass substrate (Corning Eagle XG, 50 × 50 × 0.7 mm 3) was coated with molybdenum-tantalum oxide and a cover layer of 200 nm Al (aluminum). In this case, the above molybdenum-tantalum oxide target material produced according to Example 1 and Example 2 was subjected to non-reactive sputtering under given process conditions, in comparison with the above molybdenum-tantalum oxide target material (reference) not according to the invention. The reflection was measured through the glass substrate over the specified wavelength range using a Perkin Elmer Lambda 950 spectrophotometer. In order to obtain the lowest possible reflectance, the layer thickness of the molybdenum-tantalum oxide was varied in the range of 40-60 nm. The results of this series of tests for a layer thickness of molybdenum-tantalum oxide of 50 nm are shown in FIG. 10, where the reflectance in (%) against the wavelength in (nm; nanometers), respectively, is plotted. Here, the reflectance curves of Example 1 (dotted curve) and Example 2 (dashed curve) are almost overlapping, except that the reflectance curve of Example 1 is slightly higher in the relatively high wavelength range. These curves are clearly below the reference reflectance curve not according to the invention, which is drawn with a solid line.
[0052] As can be seen from a comparison of Figures 9 and 10, in the case of the target materials according to examples 1 and 2, a relatively low reflectivity is achieved over the observed wavelength range (see Figure 10), and this is achieved at comparable deposition rates (see Figure 9). Furthermore, the target materials according to the invention have the further advantages explained above. In particular, due to their electrical conductivity and advantageous phase composition (matrix phase; finely distributed second phase), these target materials have a favorable sputtering behavior (uniform sputtering rate while avoiding arcs and particle formation), which has a favorable effect on the layer quality (uniform layer composition; uniform layer thickness).
[0053] Sample preparation: To determine the volume fraction of the phases contained in the target material and the density of the target material, a sample of approximately 10-15 x 10-15 mm 2Metallographic grindings from representative sample parts were produced by dry preparation, by cutting samples with an area of 100 nm in a dry cutting process (diamond wire saw, band saw, etc.), cleaning with compressed air, followed by embedding in warm and conductive (C-doped) phenolic resin, grinding and polishing. Dry preparation is important, since at least the MoO3 phase fraction is water soluble. The grindings so obtained were then analyzed by optical microscopy.
[0054] Determination of phase ratio by Raman spectroscopy: To determine the spatial resolution of the phases contained in the target material, a confocal optical microscope (Olympus BX41) combined with a Raman spectrometer (Horiba LabRAM HR800) was used, where the surface to be analyzed was imaged on a 1 × 1 mm2 area using a focused laser beam (He-Ne laser, wavelength λ = 632.81 nm, total power 15 mW). 2 An area of 201 × 201 was scanned point by point with a step size of 5 μm (the sample surface to be examined was fixed on a motorized XYZ table, which was moved). For each individual measurement point of the 201 × 201 measurement points, a complete Raman spectrum was generated ("Raman mapping"). The Raman spectrum was generated by scanning the sample with an optical grating (300 lines / mm, spectral resolution: 2.6 cm -1 ) and is obtained from the backscattered radiation recorded using a CCD detector (1024 × 256 pixel multichannel CCD, spectral range: 200-1050 nm). A microscope objective with a magnification of 100x and a numerical aperture of NA0.9, which serves to focus the laser beam from the Raman spectrometer, provides a 0.7 μm 2 The theoretical measurement spot size of 1000 nm was achieved. 2) is chosen to be sufficiently low to avoid phase transformations in the sample. The penetration depth of the excitation radiation is limited to a few micrometers for molybdenum oxide (for pure MoO3 it is, for example, about 4 μm). For each measurement point, the Raman signal was averaged in time over an acquisition time of 1 s, whereby a sufficiently good signal-to-noise ratio was obtained. By automatic evaluation of these Raman spectra (evaluation software Horiba LabSpec 6), a two-dimensional representation of the surface composition of the sample is produced, from which the area sizes, area proportions, etc. of the various phases are quantitatively determined. To accurately identify the molybdenum oxide phase, a reference spectrum of a previously synthesized reference sample or a reference spectrum of a relatively large homogeneous sample area is recorded, where it should be noted that the reference spectrum corresponds to exactly one metal oxide phase. Figures 1-6 show the Raman spectra of (Mo 0.93 Ta 0.07 )5O 14 (Fig. 1), Ta2O5 (Fig. 2), Mo 18 O 52 (Fig. 3), MoO2 (Fig. 4), MoO3 (Fig. 5), Mo4O 11 The reference spectra used in (Figure 6) are shown (in the individual spectra, the Raman shift (cm -1 ) versus the scattered light intensity (number). Here, the analysis and assignment of the Raman spectra is carried out by the "multivariate analysis module" of the evaluation software mentioned above using the CLS method (Classical Least Squares). For this purpose, the sample spectrum S is multiplied by the individual normalized reference spectra R i is expressed as a linear combination of i are the respective weighting coefficients, Δ is the offset value, and S = Σc i R i Then, a color corresponding to the metal oxide phase is assigned to each measurement point, with the color assignment being weighted by the largest weighting factor c i Only phases with weighting coefficient c i The magnitude (amount) of determines the brightness of the measurement point. This approach is justified because the spectrum of a measurement point can usually be unambiguously assigned to a single metal oxide phase.
[0055] With the objective lens used, sample spectra were obtained from all 201 × 201 measurement points, even when measuring in the pores. In this case, the signal originated from the deeper regions below the pores. If a Raman spectrum is not available for an individual measurement point, for example because of pores, this Raman spectrum may be excluded from the determination of the area ratio, i.e. the volume occupied by the pores of the target material is excluded from the total volume. The volume data of the individual molybdenum oxide phases therefore sum to 100% without including the pore volume.
[0056] The analytical methods described herein are very well suited for determining the relative phase proportions of the phases of interest here.
[0057] Determination of relative density: The relative density of the target material is determined by digital image analysis of optical microscope images of metallographic grindings, in which the relative area fraction of pores, “FA”, is identified. For this purpose, after sample preparation, 1 × 1 mm 2 Three bright field images of the size of the sample were taken at 100x magnification, avoiding as much as possible zones of obvious chipping or other damage patterns such as scratches due to dry preparation. The images obtained were evaluated with the aid of a digital image processing software implemented in the IMAGIC image database. For that purpose, the pore areas (dark areas) were marked on the image based on a histogram as a function of the greyscale. The lower limit of the interval was set to 0 (= black). In contrast to that, the upper limit has to be subjectively evaluated based on the greyscale intensity histogram (255 = white). The image area to be measured was set (ROI) to exclude the scale bar. As a result, an image is obtained that is coloured according to the relative area proportion "FA" of the pores (in percentage) and the selected greyscale interval (colouring means that this pixel was included in the measurement and therefore counted as a pore). The value for relative density (1-FA) was determined as the arithmetic mean of three such porosity measurements.
Claims
1. 1. A sputtering target having a conductive oxide target material, the target material comprising: Molybdenum (Mo) as the main metallic constituent element, and in a sputtering target containing at least one metal oxide of at least one doping element M from the group tantalum (Ta), niobium (Nb) and titanium (Ti), The target material was found to be a mixed oxide (Mo) based on its cut cross section measured using a Raman microscope. 1-x M x ) 5 O 14 wherein 0.01≦x≦0.13, and M in the mixed oxide is one or more elements from the group consisting of tantalum (Ta), niobium (Nb) and titanium (Ti).
2. The target material is Molybdenum (Mo) as the main metallic constituent element, and 2. The sputtering target according to claim 1, characterized in that it is formed by at least one metal oxide of at least one doping element M from the group: tantalum (Ta), niobium (Nb) and titanium (Ti).
3. 3. The sputtering target according to claim 1 or 2, characterized in that in the target material, the matrix phase from the mixed oxide has a proportion of ≧60% by volume based on a cut cross-section of the target material measured by Raman microscopy.
4. In the target material, a. MoO 2 and / or Mo 4 O 11 , and b. Optionally: - MO 3 、 -Mo 17 O 47 , Mo 5 O 14 , Mo 8 O 23 , Mo 9 O 26 and Mo 18 O 52 Further substoichiometric molybdenum oxides from the group - stoichiometric and / or substoichiometric Ta oxide(s), - Stoichiometric and / or substoichiometric Nb oxide(s) and - stoichiometric and / or substoichiometric Ti oxide(s) One or more compounds from the group is contained as one or more second phases distributed as islands in the matrix phase, and these second phases have a total volume fraction of ≦40% based on a ground cross section of the target material measured using a Raman microscope.
5. The second phase is MoO 3 The MoO 3 The sputtering target according to claim 4, characterized in that the proportion of in the target material is in the range of 0 to 2 volume % based on its ground cross section measured using a Raman microscope.
6. 6. The sputtering target according to claim 1, wherein the oxygen content in the target material is in the range of 26 to 32% by weight.
7. The sputtering target according to any one of claims 1 to 6, characterized in that in the target material, the ratio of the doping element M in atomic % to the total content of Mo and the doping element M in atomic % is in the range of 0.02 to 0.
15.
8. In the target material, the doping element M is formed by Ta, The matrix phase is a mixed oxide of (Mo 1-x T x ) 5 O 14 The sputtering target according to any one of claims 1 to 7, characterized in that it is formed from (wherein 0.06≦x≦0.08).
9. In the target material, Ta as the doping element is completely in the form of metal oxide Ta. 2 O 5 It exists as In the target material, the Ta 2 O 5 9. The sputtering target according to claim 8, characterized in that the proportion of the phase consisting of is ≦3 vol. %, based on a ground cross-section of the target material measured using a Raman microscope.
10. In the target material, the doping element M is formed by Nb, The matrix phase is a mixed oxide of (Mo 1-x Nb x ) 5 O 14 The sputtering target according to any one of claims 1 to 7, characterized in that it is formed from (wherein 0.07≦x≦0.12).
11. In the target material, Nb as the doping element is completely in the form of metal oxide Nb 2 O 5 It exists as In the target material, the Nb 2 O 5 11. The sputtering target according to claim 10, characterized in that the proportion of the phase consisting of is ≦3 vol. %, based on a ground cross-section of the target material measured using a Raman microscope.
12. 12. The sputtering target of claim 1, wherein the target material has a relative density of ≧95% at 25° C. and an electrical conductivity of ≧100 S / m.
13. The sputtering target according to any one of claims 1 to 12, characterized in that in the target material, one or more second phases are formed in the matrix phase as small islands that are finely and evenly distributed based on a ground cross-section of the target material measured using a Raman microscope.
14. A method for producing a sputtering target according to any one of claims 1 to 13, comprising producing the target material as a solid by powder metallurgy.
15. A method for producing a molybdenum oxide-containing layer, comprising using the sputtering target according to any one of claims 1 to 13, and forming a molybdenum oxide-containing layer by either a DC sputtering method or a pulsed DC sputtering method in a rare gas atmosphere without oxygen or in which 20 volume % or less of oxygen is supplied as a reactive gas.
Citation Information
Patent Citations
Light-absorbing layer system and its fabrication, as well as a suitable sputtering target
DE102012112739A1
Touch panel and touch panel manufacturing method
JP2013020347A
Superabsorbent layer system, method for producing this layer system and sputter targets suitable therefor
JP2016504484A
Double layer system with partially absorbing layer and method for producing said layer and sputtering target for producing said layer
JP2017525852A
Target and process for its production, and method for forming a film having a high refractive index
US20010020586A1