Sputtering target for producing a layer containing molybdenum oxide

A sputtering target with MoO2 and substoichiometric phases addresses the challenge of achieving stable, high-quality molybdenum oxide layers by enhancing thermal conductivity and electrical conductivity, thus improving layer quality and process reliability.

JP7580391B2Active Publication Date: 2024-11-11PLANSEE SE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021557474
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-13
Publication Date
2024-11-11
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Existing methods for producing molybdenum oxide-containing layers face challenges in achieving stable, high-quality layers with uniform properties, such as layer thickness and stoichiometry, while being cost-effective and process-reliable on an industrial scale, due to hysteresis effects and the need for precise oxygen control in reactive sputtering.

Method used

A sputtering target material composed of MoO2 phase and at least one substoichiometric metal oxide phase with an atomic ratio of oxygen to molybdenum ranging from 2.1 to 2.5 and a total oxygen content less than 71 at.%, combined with optional doping elements, is used to simplify process control and enhance thermal conductivity, bending strength, and electrical conductivity.

Benefits of technology

The target material allows for higher deposition rates with improved etching properties, reflectance, and conductivity, reducing the need for additional oxygen supply and minimizing hysteresis effects, resulting in higher-quality layers with reduced arcing and particle formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580391000002
    Figure 0007580391000002
  • Figure 0007580391000003
    Figure 0007580391000003
  • Figure 0007580391000004
    Figure 0007580391000004
Patent Text Reader

Abstract

The present invention relates to a sputtering target comprising a molybdenum-based conductive oxide target material, characterized in that the target material comprises a MoO phase and at least one sub-stoichiometric metal oxide phase, at least one metal of which is molybdenum, and in which the atomic ratio of oxygen to molybdenum in the target material is in the range of 2.1 to 2.5, with the proviso that the total oxygen content of the target material is less than 71 atomic %.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sputtering target for producing a molybdenum oxide containing layer, and to the use of such a sputtering target for depositing a molybdenum oxide containing layer.

[0002] Molybdenum oxide (MoO x ) are used in cathode atomization installations, such as PVD coating installations (PVD: physical vapor deposition), to deposit molybdenum oxide-containing layers from the gas phase in a vacuum process. In this coating process (sputtering process), layer-forming particles from the (sputtering) target are in the gas phase and, by condensation of these particles (optionally with the supply of oxygen as reactive gas ("reactive sputtering")), a corresponding molybdenum oxide-containing layer is formed on the substrate to be coated. [Background technology]

[0003] Molybdenum oxide-containing layers (especially based on molybdenum oxide) are used in particular in layer structures for optical or optoelectronic applications, such as for example electronic displays, due to their interesting optical properties. They are often used in combination with or directly adjacent to metal layers, for example from aluminum (Al), copper (Cu), titanium (Ti) or (metallic) molybdenum (Mo), which act for example as electrical conducting paths. An example of the use of molybdenum oxide layers can be found in JP 2013020347, where metal conducting paths in displays (touch screens) of capacitive touch sensors are coated with MoO 2 in order to suppress undesired reflections of the metal conducting paths. x The optical fiber is covered with a light-absorbing layer from

[0004] Important properties such as optical absorptivity, optical reflectivity, optical transmittance, etching rate (important for the subsequent structuring of the deposited layer by photolithography associated wet chemical etching processes), thermal stability, and stability towards further chemicals used in the manufacturing process (e.g. stability towards photoresist developers or photoresist strippers) are determined by the properties of the deposited MoO x It depends on the exact stoichiometry x of the layer or the doping elements added. For example, in many applications, such as the capacitive touch sensor mentioned above, the molybdenum oxide is present in a substoichiometric composition, i.e., the oxide has unoccupied oxygen valences and is deposited at MoO x There are oxygen vacancies in the layer, MoO x In particular, MoO 2.5 ~MoO 2.98 Substoichiometric MoO in the x range of x Layers have so far been of particular interest for such applications because of their electro-optical properties: they absorb light in the visible wavelength range and at the same time are also sufficiently conductive (<20 kΩ / square or sheet resistance of <20 kΩ / square) and typically semiconducting.

[0005] Such substoichiometric MoO x The simplest approach for producing layers is based on a metallic molybdenum target that is reactively sputtered in a suitably adjusted argon and oxygen gas atmosphere, so that in addition to molybdenum, oxygen atoms are also included in the deposited layer. In order to achieve layers with uniform properties, particularly in terms of layer thickness and stoichiometry, and especially oxygen content, reactive sputtering should provide an atmosphere with a precise, temporally and spatially uniform oxygen concentration around the substrate. This can only be achieved by very complex and expensive process techniques, which are associated with correspondingly high costs. Furthermore, during reactive sputtering, changes in the oxygen partial pressure (e.g. during start-up of the equipment) lead to hysteresis effects that are unfavorable for process stability.

[0006] In addition to metal targets, oxide ceramic target materials are known, such as MoO2 targets (US 2006 / 0165572) or target materials with substoichiometric compositions (DE 102012112739 and EP 0852266). US 2006 / 0165572 discloses a target material with at least 99% by weight of MoO2. However, this target material has too little oxygen and, without oxygen as an additional reactive gas, MoO2 with x>2 is not produced. x The layer cannot be deposited.

[0007] DE 102012112739 A1 discloses a quasi-stoichiometric MoO x Target materials are disclosed, the composition of which is close to the stoichiometry of the layer to be deposited. However, to fine-tune the stoichiometry of the layer, a relatively small supply of oxygen is still required, even in comparison with metal targets or MoO2 targets, which, as already mentioned above, can have a negative effect on the quality of the deposited layer. x More detailed data on the microstructure of the target material is not available. Furthermore, the achievable relative density of the target material is also very unfavorable. Substoichiometric oxides Nb-Mo-O x In the example embodiment, the relative density is 85%. However, coating installation operators require target materials with as high a relative density as possible, in particular >95%, in order to reduce the risk of flash discharges (arcs) during the coating process, which can lead to undesired particle formation in the deposition layer.

[0008] As already mentioned, molybdenum oxide-containing layers (especially based on molybdenum oxide) are produced industrially in coating processes by cathodic atomization ("sputtering"). In principle, it is possible to produce such molybdenum oxide-containing layers by reactive sputtering of a metal target material, which is reactively sputtered, for example, in appropriately adjusted argon and oxygen process gas atmospheres. Here, the metal atoms of the target material react mostly with oxygen from the process gas only during the coating process, so that process control is made difficult by hysteresis effects (discontinuous changes in the layer deposition rate, discharge current and / or target voltage due to changes in the oxygen partial pressure) and poisoning of the target surface (target poisoning). In contrast thereto, deposition of sputtering targets with oxide target materials is advantageous under industrial conditions, since the coating process can be carried out with pure noble gas process gas (usually argon) or with noble gas (usually argon) as the main component with the addition of small amounts of other gases, such as, for example, oxygen. In particular, when using oxide target materials, process control is simplified while higher coating speeds and higher process stability are possible. Furthermore, many coating equipment already installed are designed only for depositing metal layers of metal sputtering targets, and therefore cannot supply oxygen to the sputtering gas. The versatility of such sputtering equipment can be increased by using oxide target materials. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent No. 2013020347 [Patent Document 2] US Patent Application Publication No. 2006 / 0165572 [Patent Document 3] DE 102012112739 [Patent Document 4] European Patent Application Publication No. 0852266 Summary of the Invention [Problem to be solved by the invention]

[0010] It is therefore an object of the present invention to provide a molybdenum oxide-containing sputtering target with which a stable sputtering process for producing high-quality layers can be set up, which sputtering target should be producible cheaply and process-reliably on an industrial scale, has a higher bending fracture strength, thermal conductivity and temperature diffusivity and therefore can be sputtered at higher powers, thus allowing higher deposition rates and thereby a cheaper process, and wherein the layers deposited when using the target show improved properties in terms of etching properties and at the same time show acceptable values ​​of reflectivity and electrical conductivity.

[0011] This problem is solved by a sputtering target according to claim 1, by the use of a sputtering target according to claim 14 and by the use of the produced layer according to claim 15. Advantageous developments of the invention are described in the dependent claims, which can be freely combined with one another. [Means for solving the problem]

[0012] In accordance with the present invention, there is provided a sputtering target having a molybdenum-based conductive oxide target material, wherein the target material contains a MoO2 phase and at least one sub-stoichiometric metal oxide phase, at least one metal of which is molybdenum, and in the target material the atomic ratio of oxygen to molybdenum is in the range of 2.1-2.5, with the proviso that the total oxygen content of the target material is less than 71 atomic %.

[0013] Surprisingly, it has been found that when the atomic ratio of O to molybdenum in the target material is in the range of 2.1 to 2.5, a relatively low reflectivity value of the layer sputtered using the target is achieved, as compared to the higher values ​​of >2.5 to 2.9 that have been focused on up until now, and at the same time an increase in the electrical conductivity of the layer is achieved. Furthermore, the target material has a significantly better thermal conductivity and a significantly better bending strength, as compared to comparable target materials with a higher oxygen content.

[0014] "Sputtering", also called cathodic atomization, is a physical process in which atoms or molecules are released from a solid (target material) into the gas phase by the impact of energetic ions (e.g. noble gas ions of the process gas). To produce thinner layers, the atomized target material is deposited on a substrate, where it forms a solid layer. This coating process, sometimes called sputtering deposition, is one of the PVD methods (PVD: physical vapor deposition), hereinafter also called "sputtering". The target material is the sputtering target material present as a solid material that is intended to be atomized and layered during the sputtering process (optionally together with further material from the process gas and / or of the further sputtering target). The sputtering target may be formed only by the target material, i.e., consist of the target material, or may further have further components connected directly or indirectly (i.e., via at least one further component) with the target material, such as back plate(s), support tube(s), connector(s), insert(s), etc. Here, the sputtering target (and correspondingly the target material) can be provided in various shapes, in particular as planar sputtering targets having various basic shapes, such as square, rectangular, circular, etc., or also as tubular sputtering targets. In particular, the target material forms a macroscopic solid extending along at least one spatial direction of at least 0.03 m (meters).

[0015] By "oxide" target material, it is understood that the metals contained in the target material are present substantially completely as oxides. In particular, the proportion of metal phases in the target material is <1% by volume, with respect to its ground cross section. In particular, the proportion of metal phases in the target material is below the detection limit by Raman measurements, which are used here and will be explained in more detail below. A target material is called "conductive" if it has a conductivity of at least 80 S / m, measured by a resistance measuring stand (Ulvac ZEM3) in the four-point measurement method. By "phase" of a target material is understood that spatial region, within which there is a uniform chemical composition and a uniform crystal structure, the orientation of the individual crystal grains in the phase may vary. By "mixed oxide" is understood an oxide having a crystal structure whose crystal lattice is composed of oxygen ions and cations of several elements, here in particular Mo and optionally the doping element Me.

[0016] The different phases and their volume ratios, as well as the density of the target material, are determined on the basis of a representative cross-section of the sample, where an isotropic structure can be assumed, and the volume data are derived from the area ratios measured at the cut surface (i.e. the volume ratios correspond to the measured area ratios). For this purpose, metallographic grindings of the sample are produced by dry preparation, whereby Raman spectroscopy with a Raman microscope is applied to determine the spatial resolution of the different metal oxide phases. As described in more detail below, in Raman spectroscopy, the sample surface of the target material to be analyzed is scanned point-wise with a laser beam, and a complete Raman spectrum is created for each measurement point ("Raman mapping"). By comparing the Raman spectrum obtained for each measurement point with the corresponding reference spectra of the different metal oxides, the corresponding phases are assigned to each measurement point, whereby a two-dimensional representation of the phase composition of the sample is created, from which the area ratios (or volume ratios) of the different phases are calculated. The volume data (or equivalent area data) of the different metal oxide phases are normalized and are relative to the total volume (or total area) occupied by the material particles of the target material. The volume (or equivalent area) occupied by the pores of the target material is excluded from this total volume (or total area). The volume data (or equivalent area data) of the individual metal oxide phases therefore add up to 100% without including the pore volume.

[0017] In a preferred embodiment, the atomic ratio of O to Mo in the target material is in the range of 2.1 to 2.48, more preferably 2.1 to 2.45, more preferably 2.1 to 2.42, and even more preferably 2.2 to 2.4. Particularly preferably, the atomic ratio of O to Mo in the target material is 2.375.

[0018] According to the present invention, the total oxygen content of the target material is less than 71 atomic %. Preferably, the total oxygen content is in the range of 67.7 atomic % to 71 atomic %.

[0019] Molybdenum exists in different oxidation states, specifically in the form of MoO2, MoO3, as well as several substoichiometric oxides, MoO y , e.g., MoO 11 (y=2.75), Mo 17 O 47 (y=2.76), MoO 14 (y=2.8), MoO 23 (y=2.875), Mo9O 26 ((y=2.89) high temperature transformation) and Mo 18 O 52 (y=2.89) low temperature transformation.

[0020] As shown in the table below, the layer system (glass substrate / MoO x (50 nm) / aluminum (200 nm)) has a reflectance of 13.9% at a wavelength of 550 nm, a reflectance value that is too high for the applications focused on here (e.g., electronic displays for televisions, mobile phones, and touch screens). x The sheet resistivity of a single layer is 2200 μΩ cm. In contrast, MoO 2.75 MoO sputtering target x A comparable layer system with a layer exhibits a reflectance of 5.5% at a wavelength of 550 nm, while the layer resistance of the single layer is 43600 μΩ·cm. Surprisingly, (according to the invention) MoO 2.375 MoO deposited from a sputtering target x The layer system comprising the layers has a very low reflectivity of 5.5% at 550 nm, and at the same time the individual layers have a low electrical resistivity of 22500 μΩ·cm.

[0021] [Table 1]

[0022] According to the present invention, the target material is a mixture of MoO2 phase and at least one substoichiometric MoO xThe MoO2 phase is preferably contained in the target material at a ratio of 4 to 85% by volume, more preferably 22 to 42% by volume (measured using a Raman microscope) with respect to each ground cross section.

[0023] According to a preferred embodiment, the proportion of MoO3 in the target material, with respect to its ground cross section (measured using a Raman microscope), is in the range of 0-2% by volume, i.e. this proportion is ≦2% by volume. MoO3 is electrically insulating (conductivity 1×10 -5 The proportion of MoO3 must be kept as low as possible, since the MoO3 content is less than 0.05 S / m, which can lead to the formation of particles during the coating process. Furthermore, MoO3 is water-soluble, which is a disadvantage in terms of mechanical processing and storage of the target. Preferably, MoO3 in the target material is not detectable at all by Raman spectroscopy (i.e. the proportion is 0% by volume) or, if it cannot be completely avoided, is kept in a proportion in the range of 0.1-1.0% by volume.

[0024] The invention is based on the realization that, with regard to the process stability of the sputtering process, it is advantageous if the oxygen content of the target material is identical or substantially identical to the oxygen content of the layer to be produced. Preferably, the oxygen content (wt%) of the target material and the oxygen content (wt%) of the layer to be produced differ from each other by a maximum of ±2 wt%. Thus, no or only a small supply of oxygen via the process gas is required, which suppresses hysteresis effects and simplifies the process control.

[0025] Pure molybdenum oxide layers have attractive electro-optical properties. However, they are less resistant to alkaline media, for example to the strong base tetramethylammonium hydroxide (TMAH). Surprisingly, however, layers deposited from the target material according to the invention have substoichiometric MoO with an x ​​range of >2.5 to 2.98. xIt has been found that the layer deposited from the target material having the composition has a lower, i.e., more favorable, etch rate with respect to TMAH than the layer deposited from the target material having the composition.

[0026] Therefore, in a preferred embodiment, doping element In this embodiment, MoO 11 The phase fraction in the target material and on its ground cross section is in the range of 22-77 volume % (as measured using a Raman microscope), the phase fraction in the target material and on its ground cross section is in the range of 23-78 volume % (as measured using a Raman microscope), and the total oxygen content is ≦71.4 atomic %.

[0027] In addition, according to the invention, by adding doping elements to the substoichiometric molybdenum oxide-containing layer (and correspondingly the target material of the sputtering target), the etching rate in common wet etching media (e.g. PAN etching based on phosphoric acid, nitric acid and acetic acid for structuring aluminum metallizations, H2O2-based etching for structuring Cu) can be further reduced without significantly changing the electro-optical properties.

[0028] Thus, in a preferred embodiment, the target material contains a doping element Me from the group consisting of groups IVa, Va and VIa of the periodic table, with Ti, Zr, Hf, V, Nb, Ta, Cr and W being particularly preferred here.

[0029] In a further preferred embodiment, the target material contains a doping element Me from the group consisting of tantalum (Ta), niobium (Nb), vanadium (V) and titanium (Ti), where the group consisting of Ta and Nb is particularly preferred, and Ta is even more preferred.

[0030] In a further embodiment, the proportion of the doping element Me in atomic % to the total content of Mo and the doping element Me combined in atomic % in the target material is in the range of 0.02 to 0.15, preferably in the range of 0.05 to 0.12.

[0031] In this embodiment, in addition to the MoO2 phase, a mixed oxide phase (Mo 1-x Me x )5O 14 is present in the target material in a phase fraction in the range of 50-78% by volume (measured using a Raman microscope) with respect to its ground cross section. In this embodiment, Ta is the preferred doping element.

[0032] It is further advantageous that the sputtering targets according to the invention can be produced on an industrial scale as dense components (e.g., at least 1 kg of dense target material per target segment) having high relative density and high phase purity within short process times (e.g., typically holding times of less than 12 hours), as described in more detail below.

[0033] The target material may contain manufacturing-related "impurities" (both metallic and non-metallic), such as sodium (Na), potassium (K), antimony (Sb), iron (Fe), carbon (C), boron (B) and nitrogen (N). The total content of such impurities is typically <1000 μg / g.

[0034] According to one development, in the target material, the oxygen content in wt.% is in the range of 25.9-29.5 wt.%. Since the oxygen content in the deposition layer affects the light reflection, preferably an approximately corresponding oxygen content, typically in the above-mentioned range, is adjusted in the target material. Furthermore, within this range, sufficient electrical conductivity is achieved, which allows DC (direct current) sputtering processes (whereas electrically insulating targets have to be sputtered in RF (RF: radio frequency, i.e. radio frequency) sputtering processes (i.e. alternating current), which is associated with increased costs (especially with regard to the design of the sputtering equipment). Here, the oxygen content can be adjusted in the manufacturing process by weighing the corresponding oxide-containing powder, as will be explained in further more detail below, whereby the weighed oxygen ratio (relative to the weighed metal ratio) corresponds to the desired oxygen content of the target material. Since the exact occupancy of the various lattice sites in the metal oxide phase can also be varied as required in a temperature-dependent manner, it is reasonable to only take into account the total oxygen content in the target material. Here, the total oxygen content in the target material is determined by carrier gas thermal extraction (detection of oxygen as CO or CO2 by an infrared measuring cell, for example with a LECO RO300 or LECO 836 device).

[0035] For the target material itself, the proportions of the metals contained and the ratio Me / (Mo+Me) can be determined by chemical analysis, in particular ICP-MS (Inductively Coupled Plasma Mass Spectrometry; Mass Spectrometry with Inductively Coupled Plasma) or by ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometry; Optical Emission Spectrometry with Inductively Coupled Plasma).

[0036] According to one development, the target material has a relative density of 95% or more (i.e. in the range of 95-99.9%), in particular ≧97% (i.e. in the range of 97-99.9%), preferably ≧98% (i.e. in the range of 98-99.9%). The density is determined by dry preparation of a sample of the target material, which is explained more precisely below. Dense target materials with high relative density are important for the quality of the deposited layer, since less dense target materials can cause flash discharges ("arcs") and particle formation during sputtering. The relative density is determined by digital image analysis based on optical microscope images of metallographic grindings of the target material, in which the relative area ratio of pores "FA" (FA: area ratio of pores to the total area to be examined) is evaluated. The relative density corresponds to this value (1-FA), whereby the relative density is calculated as the arithmetic mean of three such porosity measurements. This procedure is explained in detail below.

[0037] According to one development, the target material has a conductivity of ≧100 S / m at 25° C. This allows DC sputtering and also results in a sufficient conductivity in the produced layers, where the conductivity is measured by a resistance measuring stand (e.g. Ulvac ZEM3) in the four-point measurement method.

[0038] The target material is ≥ 2 mm at 25°C. 2 s -1 The sputtering target according to any one of the preceding claims, characterized in that it has a thermal diffusivity of 0.1 to 0.5%, which can be determined by Laser Flash Analysis (LFA).

[0039] 10. The sputtering target of any one of the preceding claims, wherein the target material has a thermal conductivity of ≧3.5 W / mK at 25° C.

[0040] According to one development, the target material is present as a (macroscopic) solid produced by powder metallurgy. The powder metallurgical production route allows the target material to be produced inexpensively on an industrial scale as a dense component (e.g. at least 1 kg of dense target material per target segment) with high relative density and high phase purity within a short process time (e.g. typically less than 12 hours of holding time). Powder metallurgical production is understood here as the compaction of corresponding starting powders (in the case of multiple powders, appropriately mixed beforehand) by application of pressure and / or temperature. Here, powder metallurgical production results in a characteristic microstructure of the target material, in particular a multiphase and fine-grained structure. Powder metallurgical production is easily recognizable from the target material by the skilled person on the basis of ground cross sections, by optical microscope, by scanning electron microscope (SEM) or by Raman microscope.

[0041] As the starting powder 、M oO2 、 MoO3 , if necessary, a small proportion, especially Mo 4 O 11 Substoichiometric molybdenum oxides such as A powder mixture with one or more oxides of the doping element Me is preferably formed. Different powder fractions are weighed to adjust the desired quantitative ratio of the elements Mo, Me and O. MoO2 and MoO3 are readily available, cheap, thermodynamically stable under ambient conditions and easy to handle raw materials. Substoichiometric oxides can be produced by reducing MoO3 powder in a suitable atmosphere such as H2.

[0042] It should be noted that the mixing of the powders is preferably carried out in an intensive mixer or by means of a plowshare mixer, which ensures very good mixing of the powders.

[0043] Compaction can be carried out in particular by hot pressing, hot isostatic pressing, spark plasma sintering (SPS) or press sintering. Here, compaction is carried out in particular at temperatures of 600-800 ° C and pressing pressures of 15-110 MPa. Preferably, compaction is carried out in a vacuum or protective gas atmosphere (for example argon), especially when high temperatures are set. In the case of SPS, compaction is carried out by applying pressure and temperature, whereby heat is generated internally by an electric current passing through the powder mixture. In the case of hot pressing, compaction is likewise carried out by applying pressure and temperature, whereby heat is supplied from the outside via a heated mold. In the case of hot isostatic pressing, the starting powder is in a closed capsule and compaction is carried out by applying pressure and temperature to the capsule. In the case of compaction by press sintering, the starting powder is pressed into a green body, which is subsequently sintered by heat treatment below the melting temperature.

[0044] During the compaction process, the starting powder is converted into the target material by solid-state reaction or even liquid-phase or multi-phase reaction (e.g. solid-liquid) depending on the chemical composition and process conditions. After compaction, mechanical post-processing may be performed, for example by cutting tools, to obtain the desired final shape or for surface post-treatment (adjustment of the desired surface roughness). The target material according to the invention shows improved processability, for example, during machining (less material chipping) and during joining (less tendency to crack formation), due to increased bending fracture strength and higher thermal conductivity. If necessary, further components such as, for example, backplate(s), support tube(s), connector(s), insert(s) must be further attached to complete the sputtering target.

[0045] The present invention further relates to the use of a sputtering target according to the invention, which can be further formed by one or more of the above-mentioned developments and variants, for depositing a molybdenum oxide-containing layer, in which the sputtering process is carried out as a DC or pulsed DC sputtering process in a noble gas atmosphere without oxygen or alternatively with up to 20% by volume of oxygen supplied as reactive gas. In direct current or DC sputtering, a direct voltage is applied between the sputtering target connected as a cathode and the anode (usually a shielding steel plate in the housing and / or vacuum chamber of the coating installation). Here, the DC or pulsed DC sputtering process is carried out non-reactively in a noble gas atmosphere, in particular an argon gas atmosphere, preferably without additional oxygen supply. The layer deposited here may have a slightly lower oxygen content than the target material used due to slight oxygen deficiency during the coating process (removal of formed oxygen by the drawn-in process gas), which may vary slightly depending on the coating installation and the operating method. To produce a molybdenum oxide-containing layer having a higher oxygen content than that of the target material, the target material can also be subjected to reactive sputtering under a supply of oxygen of up to 20% by volume (relative to the composition of the reactive gas), preferably less than 10% by volume, even more preferably less than 5% by volume, where the amount of oxygen supplied can be kept relatively low by using an oxide target material, and thus the disadvantages of reactive sputtering (hysteresis effects, potential non-uniformity of the deposited layer) do not affect as strongly.

[0046] Furthermore, the present invention relates to molybdenum oxide containing layers deposited by the above uses.The advantages of these layers, such as low reflectivity, low layer resistance, have already been discussed based on the previous table.

[0047] Further advantages and benefits of the present invention will become apparent on the basis of the following description of examples with reference to the attached drawings. [Brief description of the drawings]

[0048] [Figure 1] FIG. 1 is a plot of bending fracture strength (determined in a 4-point bending test and reported in MPa (megapascals)) for a molybdenum oxide according to the invention (Example 1) and two molybdenum-tantalum oxide sputtering targets according to the invention (Examples 2 and 3) as well as three comparative examples (MoOx, x=2.75 in the O portion; 0, 3 and 6 Mol% Ta2O5). [Diagram 2] FIG. 1 is a plot of thermal conductivity (in W / m·K (Watts per meter per Kelvin)) for a molybdenum oxide according to the invention (Example 1) and two molybdenum-tantalum oxide sputtering targets according to the invention (Examples 2 and 3) as well as three comparative examples (MoOx, x=2.75 in the O portion; 0, 3 and 6 Mol% Ta2O5). [Diagram 3] FIG. 1 shows a plot of reflectivity (%) versus wavelength (nm) (nanometers) for layer systems deposited in sputtering tests using a molybdenum oxide according to the invention (Example 1) and a molybdenum-tantalum oxide sputtering target according to the invention (Example 3) as well as two comparative examples (MoOx, x=2.75 in the O portion; 0 and 6 Mol% Ta2O5). [Figure 4] FIG. 1 shows plots of the minimum reflectance (%) for a wavelength of 550 nm (@550 nm; nanometers) for layer systems deposited in sputtering tests using a molybdenum oxide according to the invention (Example 1) and a molybdenum-tantalum oxide sputtering target according to the invention (Example 3) as well as two comparative examples (MoOx, x=2.75 in the O portion; 0 and 6 Mol% Ta2O5). [Diagram 5]FIG. 1 is a plot of the specific electrical resistivity (determined in a 4-point measurement and reported in μΩ·cm (microohms per centimeter)) for layers deposited in sputtering tests using a molybdenum oxide according to the invention (Example 1) and two molybdenum-tantalum oxide sputtering targets according to the invention (Examples 2, 3) as well as three comparative examples (MoOx, x=2.75 in the O portion; 0, 3 and 6 Mol% Ta2O5). [Figure 6] FIG. 1 is a plot of etch rates (specified in a 2.36% aqueous TMAH (tetramethylammonium hydroxide) solution and reported in nm / min (nanometers per minute)) for layers deposited in sputtering tests using a molybdenum oxide according to the invention (Example 1) and a molybdenum-tantalum oxide sputtering target according to the invention (Example 2) as well as two comparative examples (MoOx, x=2.75 in the O portion; 0 and 3 Mol % Ta2O5). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0049] Manufacturing example: Example 1: MoO 2.375 MoO2 powder (Plansee SE) is sieved through a sieve with a mesh size of 63 μm. The 62 Mol% MoO2 powder so obtained is mixed with 38 Mol% MoO3 powder (Molymet) in an intensive mixer (Eirich) for 20 minutes, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ 250 mm and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 25 MPa, a temperature of 800 °C and a holding time of 120 minutes. The relative density of the densified component is 98.1%. The bulk of the obtained target material is composed of Mo4O3 with a proportion of 95.2% by volume. 11 Furthermore, the target material has a MoO2 phase with a proportion of 4.8% by volume.

[0050] Example 2: MoO 2.375 +3Mol% Ta2O5 MoO2 powder (Plansee SE) is sieved through a sieve with a mesh size of 63 μm. The 76 Mol% MoO2 powder thus obtained is mixed with 21 Mol% MoO3 powder (Molymet) and 3 Mol% tantalum pentoxide powder (HC Starck, Ta2O5) in an intensive mixer (Eirich) for 20 minutes, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ 250 mm and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 25 MPa, a temperature of 800 °C and a holding time of 120 minutes. The relative density of the densified component is 98.1%. The bulk of the target material obtained is composed of (MoO3) powder with a proportion of 69% by volume. 0.93 Ta 0.07 )5O 14 Furthermore, the target material is composed of 29% by volume of MoO2 phase and 2% by volume of Mo4O 11 It has a phase.

[0051] Example 3: MoO 2.375 +6Mol% Ta2O5 MoO2 powder (Plansee SE) is sieved through a sieve with a mesh size of 63 μm. The 88 Mol% MoO2 powder so obtained is mixed with 8 Mol% MoO3 powder (Molymet) and 6 Mol% tantalum pentoxide powder (HC Starck, Ta2O5) in an intensive mixer (Eirich) for 20 minutes, ensuring a homogeneous distribution between the powder components. The resulting powder mixture is placed in a graphite mold with dimensions of φ 250 mm and height 50 mm and compressed in a hot press under vacuum at a pressing pressure of 25 MPa, a temperature of 800 °C and a holding time of 120 minutes. The relative density of the densified component is 99.7%. The bulk of the obtained target material is composed of (MoO3) powder with a proportion of 57% by volume. 0.93 Ta 0.07 )5O 14 Furthermore, the target material has a MoO2 phase with a volume percentage of 41% and a Ta2O5 phase with a volume percentage of 2%.

[0052] Physical and mechanical properties: In the course of a series of tests, a molybdenum-tantalum oxide sputtering target (MoO x , x=2.75 in the O portion) of the molybdenum-tantalum oxide sputtering targets (MoO x , x=2.375 for the O moiety) were investigated, where the Ta2O5 content in the powder mixtures used to prepare the sputtering targets was different and was 0, 3 or 6 Mol%.

[0053] FIG. 1 shows the bending fracture strength (determined by four-point bending test) of different molybdenum oxide and molybdenum-tantalum oxide sputtering targets. The sputtering targets produced according to Examples 1 to 3 (MoO x , x=2.375 in the O portion) is a sputtering target not according to the present invention (MoO x , x=2.75 for the O portion), all of the compositions examined have higher bending fracture strengths.

[0054] FIG. 2 shows the thermal conductivity (determined by laser flash analysis) of different molybdenum oxide and molybdenum-tantalum oxide sputtering targets. The sputtering targets produced according to Examples 1 to 3 (MoO x , x=2.375 in the O portion) is a sputtering target not according to the present invention (MoO x , O portion (x=2.75)) have higher thermal conductivities for all compositions examined.

[0055] Sputtering Test: In the course of a series of tests, a molybdenum-tantalum oxide sputtering target (MoO x , x=2.75 in the O portion) compared with the molybdenum oxide and molybdenum-tantalum oxide target materials (MoO xThe non-reactive sputtering was performed on the O portion (x=2.375) under the specified process conditions. Here, the sputtering power was 200 W and the -3 A process pressure of argon of 1000 MPa (22 sccm; sccm: standard cubic centimetres per minute) was used.

[0056] The reflectance of the prepared layer was used as the evaluation criterion. To determine the reflectance, a glass substrate (Corning Eagle XG, 50 × 50 × 0.7 mm 3 ) were coated with molybdenum oxide or molybdenum-tantalum oxide and a cover layer of 200 nm Al (aluminum). The reflection was measured through the glass substrate over the specified wavelength range using a Perkin Elmer Lambda 950 spectrophotometer. The layer thickness of the molybdenum oxide or molybdenum-tantalum oxide was varied in the range of 40-60 nm in order to obtain the lowest possible reflectance. The results from this series of tests are shown in Fig. 3 and Fig. 4. In Fig. 3 the reflectance in (%) is plotted against the wavelength in (nm; nanometers), respectively. Here, the reflectance curves from Example 1 and Example 3 are depicted as curves drawn in black, dashed for Example 1 and dashed-dotted for Example 3, and are in the range of equivalence (almost identical) to the reflectance curves of the reference layer systems not according to the invention (described by the curves drawn in grey as solid or dotted lines). The minimum of the measured reflectance curves is, for the layers from Example 1 and Example 3, the reflectance curves of the reference not according to the invention (MoO x , which is almost the same value as the minimum value of the reflectance curve at x=2.75 in part O.

[0057] In FIG. 4, the absolute values ​​of the measured minimum reflectance in (%) for a wavelength of 550 nm are plotted depending on the molybdenum oxide or molybdenum-tantalum oxide sputtering target used, respectively. All reflectance curves determined for sputtered molybdenum oxide and molybdenum-tantalum oxide layers with layer thicknesses of 40 to 60 nm were evaluated here. As can be seen from the comparison of FIG. 4, the reflectance curves determined for the sputtering targets according to the invention according to examples 1 and 3 are significantly lower than those determined for sputtering targets not according to the invention (MoO x , a minimum reflectance equivalent to that of the O moiety at x = 2.75; 0 and 6 Mol% Ta2O5) is achieved.

[0058] Furthermore, the sputtering targets (MoO x The specific electrical resistivity (four-point measurement, Keithley 2400 Source Meter) was determined for 50 nm thick sputtered molybdenum oxide and molybdenum-tantalum oxide layers deposited using a sputtering target not according to the invention (MoO x 5. As can be seen from the comparison in FIG. 5, using the sputtering targets according to the invention according to examples 1-3 a lower specific electrical resistivity of the layer is achieved than when using sputtering targets not according to the invention.

[0059] Furthermore, the sputtering targets (MoO x The wet etching rates were determined in a 2.36% TMAH (tetramethylammonium hydroxide) aqueous solution for 100 nm thick sputtered molybdenum oxide and molybdenum-tantalum oxide layers deposited using a sputtering target not according to the invention (MoO x6. The etching rate of the layer sputtered using the sputtering targets according to the invention according to Examples 1 and 2 is compared with that of the layer sputtered using the sputtering targets according to the invention (x=2.75 in the O portion). As can be seen from the comparison in FIG. 6, a lower etching rate is achieved using the sputtering targets according to the invention according to Examples 1 and 2 than when using sputtering targets not according to the invention.

[0060] Furthermore, the sputtering targets according to the invention have the further advantages explained above.In particular, due to their increased thermal conductivity and increased bending fracture strength, the sputtering targets according to the invention show a reduced tendency to crack when joining or a more favorable sputtering behavior when sputtering the target material according to the invention (uniform sputtering rate and less particle formation while avoiding arcing), which has a favorable effect on the layer quality (uniform layer composition; uniform layer thickness; less layer defects).The sputtering layers deposited using the sputtering targets according to the invention have a low specific electrical resistivity and a low wet etching rate, which is advantageous in combination with aluminum or copper layers.

[0061] Sample preparation: To determine the volume ratio of the phases contained in the target material and the density of the target material, a sample of approximately 10-15 x 10-15 mm 2 Metallographic grindings from representative sample parts were produced by dry preparation, by cutting samples with an area of ​​100 nm in a dry cutting process (diamond wire saw, band saw, etc.), cleaning with compressed air, followed by embedding in warm and conductive (C-doped) phenolic resin, grinding and polishing. Dry preparation is important, since the optionally present MoO3 phase fraction is water soluble. The grindings so obtained were then analyzed by optical microscopy.

[0062] Determination of phase proportions by Raman spectroscopy: To determine the spatial resolution of the phases contained in the target material, a confocal optical microscope (Olympus BX41) combined with a Raman spectrometer (Horiba LabRAM HR800) was used, where the surface to be analyzed was imaged on a 1 × 1 mm2 area using a focused laser beam (He-Ne laser, wavelength λ = 632.81 nm, total power 15 mW). 2 An area of ​​201 × 201 was scanned point by point with a step size of 5 μm (the sample surface to be examined was fixed on a motorized XYZ table, which was moved). For each individual measurement point of the 201 × 201 measurement points, a complete Raman spectrum was generated ("Raman mapping"). The Raman spectrum was generated by scanning the sample with an optical grating (300 lines / mm, spectral resolution: 2.6 cm -1 ) and is obtained from the backscattered radiation recorded using a CCD detector (1024 × 256 pixel multichannel CCD, spectral range: 200-1050 nm). A microscope objective with a magnification of 100x and a numerical aperture of NA0.9, which serves to focus the laser beam from the Raman spectrometer, provides a 0.7 μm 2 The theoretical measurement spot size of 1000 nm was achieved. 2 ) is chosen to be sufficiently low to avoid phase transformations in the sample. The penetration depth of the excitation radiation is limited to a few micrometers for molybdenum oxide (for pure MoO3 it is, for example, about 4 μm). For each measurement point, the Raman signal was averaged in time over an acquisition time of 1 s, whereby a sufficiently good signal-to-noise ratio was obtained. By automatic evaluation of these Raman spectra (evaluation software Horiba LabSpec 6), a two-dimensional representation of the surface composition of the sample is produced, from which the area sizes, area ratios, etc. of the various phases are quantitatively determined. To precisely identify the molybdenum oxide phase, a reference spectrum of a previously synthesized reference sample or a reference spectrum of a relatively large homogeneous sample area is recorded, where it should be noted that the reference spectrum corresponds to exactly one metal oxide phase. Figures 1-6 show the Raman spectra of (Mo 0.93 Ta 0.07 )5O 14(Fig. 1), Ta2O5 (Fig. 2), Mo 18 O 52 (Fig. 3), MoO2 (Fig. 4), MoO3 (Fig. 5), Mo4O 11 The reference spectra used in (Figure 6) are shown (in the individual spectra, the Raman shift (cm -1 ) versus the scattered light intensity (number). Here, the analysis and assignment of the Raman spectra is carried out by the "multivariate analysis module" of the evaluation software mentioned above using the CLS method (Classical Least Squares). For this purpose, the sample spectrum S is multiplied by the individual normalized reference spectra R i is expressed as a linear combination of i are the respective weighting coefficients, Δ is the offset value, and S = Σc i R i Then, a color corresponding to the metal oxide phase is assigned to each measurement point, with the color assignment being weighted by the largest weighting factor c i Only phases with weighting coefficient c i The magnitude (amount) of determines the brightness of the measurement point. This approach is justified because the spectrum of a measurement point can usually be unambiguously assigned to a single metal oxide phase.

[0063] With the objective lens used, sample spectra were obtained from all 201 × 201 measurement points, even when measuring in the pores. In this case, the signal originated from the deeper regions below the pores. If a Raman spectrum is not available for an individual measurement point, for example because of pores, this Raman spectrum may be excluded from the determination of the area ratio, i.e. the volume occupied by the pores of the target material is excluded from the total volume. The volume data of the individual molybdenum oxide phases therefore sum to 100% without including the pore volume.

[0064] The analytical methods described herein are very well suited for determining the relative phase proportions of the phases of interest here.

[0065] Determination of relative density: The relative density of the target material is determined by digital image analysis of optical microscope images of metallographic grindings, in which the relative area ratio of pores "FA" is identified. For that purpose, after preparation of the sample, three bright field images, each with a size of 1 × 1 mm, were taken at 100x magnification, avoiding as much as possible zones of obvious chipping or other damage patterns such as scratches due to dry preparation. The obtained images were evaluated with the aid of digital image processing software implemented in the IMAGIC image database. For that purpose, the pore areas (dark areas) were marked on the images based on a histogram as a function of the grayscale. The lower limit of the interval was set to 0 (= black). In contrast to that, the upper limit has to be subjectively evaluated based on the grayscale intensity histogram (255 = white). The image area to be measured was set (ROI) to exclude the scale bar. The result is an image colored corresponding to the relative area ratio of the pores (in percent) "FA" and the selected grayscale interval (coloring means that this pixel was included in the measurement and therefore counted as a pore). The value for relative density (1-FA) was determined as the arithmetic mean of three such porosity measurements.

Claims

1. 1. A sputtering target comprising a molybdenum-based conductive oxide target material, The target material has a MoO content of 22-42% by volume based on a ground cross section of the target material measured by Raman microscopy. 2 phase, at least one substoichiometric metal oxide phase, at least one metal being molybdenum, and 0-2 volume % MoO 3 based on a ground cross section of said target material as measured by Raman microscopy, wherein the atomic ratio of oxygen to molybdenum in said target material is in the range of 2.1-2.5, with the proviso that the total oxygen content of said target material is less than 71 atomic % and is 25.9-29.5 weight % as measured by carrier gas thermal extraction; The target material contains a doping element Me, the doping element Me being selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr and W, the ratio of the total content of the doping element Me to the total content of Mo and the doping element Me being in the range of 0.02-0.15 atomic %, and further the target material contains a mixed oxide phase (Mo1-xMex)5O14 with a phase fraction of 50-78 volume % based on the ground cross section of the target material measured by Raman microscopy. A sputtering target comprising:

2. The sputtering target of claim 1, wherein the doping element is a doping element selected from the group consisting of tantalum (Ta), niobium (Nb), vanadium (V) and titanium (Ti).

3. A sputtering target as described in claim 2, wherein the doping element is tantalum (Ta).

4. The sputtering target according to any one of claims 1 to 3, characterized in that the target material has a relative density of ≧95%.

5. 5. The sputtering target of claim 1, wherein the target material has an electrical conductivity of ≧100 S / m at 25° C.

6. The target material has a thickness of ≧2 mm at 25° C. 2 s -1 The sputtering target according to any one of claims 1 to 5, characterized in that it has a thermal diffusivity of

7. 7. The sputtering target of claim 1, wherein the target material has a thermal conductivity of ≧3.5 W / mK at 25° C.

8. A method for producing a molybdenum oxide-containing layer, comprising using the sputtering target according to any one of claims 1 to 7, and forming a molybdenum oxide-containing layer by either a DC sputtering method or a pulsed DC sputtering method in an oxygen-free rare gas atmosphere or in a rare gas atmosphere in which 20 volume % or less of oxygen is supplied as a reactive gas.

Citation Information

Patent Citations

  • Light-absorbing layer system and its fabrication, as well as a suitable sputtering target

    DE102012112739A1

  • Target, process for production thereof, and method of forming highly refractive film

    EP0852266A1

  • Method for producing MoO2 powder, products produced from MoO2 powder, attachment of MoO2 thin films, and methods for using such materials.

    JP2007500661A

  • Touch panel and touch panel manufacturing method

    JP2013020347A

  • Light-absorbing layer system and its production and sputter targets suitable therefor

    JP2016502592A