Precipitation hardening stainless steel with high fracture toughness and strength
Patent Information
- Application Number
- JP2022551277
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-26
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-02-26
Smart Images

Figure 0007580480000008 
Figure 0007580480000009 
Figure 0007580480000001
Abstract
Description
[Technical field]
[0001] BACKGROUND OF THEINVENTION (Technical field to which the invention pertains) The present invention relates to a precipitation hardened martensitic stainless steel alloy capable of exhibiting very high strength and fracture toughness together with corrosion resistance. The excellent combination of fracture toughness and strength with corrosion resistance makes the alloy particularly suitable for aerospace components, particularly aircraft landing gear. The alloy may be used in the manufacture of other articles requiring the combination of high strength and fracture toughness exhibited by the alloy. [Background technology]
[0002] Description of Related Art The aerospace industry has been searching for a high strength stainless steel alloy for use in aircraft landing gear for many years. Currently, 300M alloy is known as an alloy used in commercial aircraft landing gear applications. 300M alloy exhibits an ultimate tensile strength of approximately 280 ksi (1930 MPa) and good ductility, represented by elongation of greater than 10%, which can be quenched and tempered. 300M alloy also has a K of 50 to 60 ksi√in (55 to 66 MPa√m). Ic It has fracture toughness. However, 300M alloy does not have effective corrosion resistance. This has required landing gear components to be plated with corrosion-resistant metals such as cadmium. Cadmium is highly toxic and carcinogenic, and the manufacture and maintenance of aircraft landing gear and other exposed components using 300M alloy has posed significant health and environmental risks. The corrosion resistance required for aircraft landing gear applications includes general corrosion resistance, pitting corrosion resistance, and stress corrosion cracking resistance.
[0003] Additionally, for critical applications requiring high strength and toughness, such as aircraft landing gear cases, the relevant material specifications require design based on critical flaw size. Many of these specifications are governed by the ratio of fracture toughness to ultimate tensile strength, K, that a qualified material must meet.Ic 300M ...
[0004] Therefore, there is a need for a corrosion resistant steel alloy that can be qualified as a direct replacement for 300M alloy without significant design changes in terms of mechanical functionality, and that exhibits the combination of strength and fracture toughness required for aerospace landing gear applications and previously exhibited by 300M alloy. Summary of the Invention [Problem to be solved by the invention]
[0005] BRIEF SUMMARY OF THEINVENTION According to a first aspect of the present invention, there is provided a precipitation hardenable martensitic stainless steel having the following broad, intermediate and recommended compositions, in weight percent: TIFF0007580480000001.tif10492
[0006] The balance of the alloy is iron and normal impurities found in commercial grades of precipitation hardenable martensitic stainless steels, as known to those skilled in the art of melting such steels.
[0007] The foregoing table is provided as a convenient summary and is not intended to limit the lower and upper limits of ranges of individual elements of the alloys of this invention for use in combination with each other, or to limit ranges of elements for use only in combination with each other. Thus, one or more of the ranges of elements of a broad composition may be used with one or more of the other ranges of the remaining elements of a preferred composition. Furthermore, a minimum or maximum value for an element of a broad, intermediate, or recommended embodiment may be used with a maximum or minimum value for that element from another broad, intermediate, or recommended embodiment. Furthermore, alloys according to this invention may comprise, consist essentially of, or consist of the constituent elements described above and throughout this specification.
[0008] In accordance with another aspect of the invention, there is provided a method of manufacturing a metallic part or component comprised of the martensitic precipitation hardenable stainless steel alloy described above. The method includes obtaining an ingot having the martensitic precipitation hardenable stainless steel alloy composition described above. The method also includes heating the ingot at a temperature of about 2000°F (1093°C) to about 2400°F (1315°C) for a time sufficient to homogenize the ingot. The homogenized ingot is then hot worked to obtain a near net shape part or intermediate product form. The method further includes heat treating the part or intermediate product form by annealing the near net shape part by heating the part or product form at a temperature of about 1700°F (927°C) to about 1900°F (1038°C) for a preselected period of time. The part or product form is then quenched from the annealing temperature to below about -100°F (-73°C) to ensure complete martensitic transformation of the alloy matrix. The method further includes age hardening the quenched part by heating at a temperature of 900°F (482°C) to about 1150°F (621°C) for a selected time to obtain a combination of high tensile strength, good fracture toughness, and good corrosion resistance.
[0009] According to a further aspect of the invention, there is provided an article of manufacture made from the alloy set forth in the preceding table, characterized in that it has high strength and high fracture toughness, along with good corrosion resistance. Articles according to the invention, in the solution annealed and age hardened condition, exhibit an ultimate tensile strength of at least about 280 ksi (1930 MPa), a plane strain fracture toughness of at least about 60 ksi√in (65 MPa√m), and a fracture toughness to tensile strength ratio of about 0.25 to 0.3√in (√m).
[0010] As used herein, the term "percent" or the symbol "%" means percent by weight or percent by mass, unless otherwise specified. The term "tensile strength" means ultimate tensile strength as that property is commonly defined and understood by those skilled in the art. With respect to fracture toughness, the symbol "K Ic " refers to fracture toughness measured primarily under linear elastic, plane strain conditions. The symbol "K Q " means fracture toughness measured under predominantly linear elastic conditions. Under the applied experimental conditions, the difference between these two quantities is approximately the same as the reproducibility standard deviation of this method (ASTM E399). Therefore, in this specification, the term "fracture toughness" is used interchangeably with "K Ic " and "K Q " is used as a general term to refer to both. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 shows a graph of fracture toughness (MPa√m) as a function of ultimate tensile strength (MPa) for example alloys described in US2016 / 02899805A1 and example alloys according to the present invention. [Diagram 2] FIG. 2 shows a graph of fracture toughness (ksi√in) as a function of ultimate tensile strength (ksi) for example alloys according to the present invention and example alloys described in US2016 / 02899805A1, US8097098B2, US2016 / 0319406A1, and US5855844. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Detailed Description) The alloy according to the invention contains at least about 10.50% nickel because nickel contributes to the stabilization of the austenite phase. The stable austenite phase promotes the transformation to dislocation dense martensite during quenching while avoiding the formation of delta ferrite in the alloy. A sufficient concentration of nickel is also necessary because nickel is involved in the formation of the first strengthening phase, Ni3Ti. Furthermore, nickel ensures good toughness by promoting the formation of reverse austenite, interlath austenite and retained austenite during aging and quenching of the alloy. Nickel also lowers the ductile brittle transition temperature (DBTT) well below room temperature, imparting good impact toughness to the alloy. Preferably, the alloy contains at least about 11.0% nickel, and more preferably at least about 11.4% nickel. Too much nickel suppresses the martensitic transformation start temperature (Ms) undesirably below room temperature and inhibits sufficient transformation to obtain the desired mechanical properties. Thus, the alloy contains no more than about 12.5% nickel. Preferably, the alloy contains up to about 12.2% nickel, and more preferably up to about 12.0% nickel.
[0013] The alloy includes at least about 1.0%, preferably at least about 1.5%, and more preferably at least about 2.0% cobalt. Cobalt improves the properties of the alloy in several important ways. More specifically, cobalt retards the recovery of dislocations that occur during the aging heat treatment of the alloy. The retardation of the dislocation recovery phenomenon favors the heterogeneous nucleation of a fine dispersion of strengthening precipitates in the alloy matrix. In addition, cobalt can interact with molybdenum to reduce the solubility of molybdenum in the alloy and improve the coherency between the matrix and the precipitates. This improved coherency improves the fracture toughness of the alloy. In addition, cobalt stabilizes austenite in the alloy at high temperatures and contributes to the solid solution strengthening of the alloy. On the other hand, when cobalt is present in the alloy in an amount greater than about 6%, it adversely affects the corrosion resistance of the alloy. Cobalt interacts with chromium to form a chromium-rich phase during the aging heat treatment, thereby depleting chromium from the base metal. Therefore, in this alloy, cobalt is limited to not more than about 6.0%, preferably not more than about 5.5%, and for best results, not more than about 5.0%.
[0014] The alloy contains at least about 1.5% titanium to increase the strength of the alloy. Titanium combines with nickel during age hardening heat treatment to form the primary strengthening phase, Ni3Ti. Preferably, the alloy contains at least about 1.55% titanium, and for best results, at least about 1.6% titanium. Too much titanium undesirably increases the melting temperature of the Laves phases formed in the alloy, and the Laves phases cannot be sufficiently dissolved without undesirable grain growth. Therefore, the alloy is limited to not more than about 2.0%, preferably not more than about 1.8%, and for best results, not more than about 1.75% titanium.
[0015] Chromium favors the corrosion resistance of the alloy of the present invention. To that end, the alloy contains at least about 8.5% chromium. Preferably, the alloy contains at least about 8.75%, more preferably at least about 9.0% chromium. Too much chromium reduces the Ms temperature of the alloy and inhibits the formation of martensite in the alloy matrix upon quenching, thereby adversely affecting the tensile strength of the alloy. Therefore, chromium is limited to not more than about 11.5% of the alloy. Preferably, the alloy contains not more than about 10.5%, more preferably not more than about 10.0% chromium.
[0016] At least about 1.0% molybdenum is included in the alloy because molybdenum participates in the precipitation of strengthening phases such as R-phase during age hardening to increase the strength of the alloy. Molybdenum also contributes to the pitting and crevice corrosion resistance of the alloy. For these purposes, the alloy preferably contains at least about 2.0%, and for best results, at least about 2.25% molybdenum. Too much molybdenum reduces the Ms temperature and inhibits complete martensitic transformation. In addition, too much molybdenum can promote the formation of Mo-rich topological closed pack (TCP) phases, reducing the usefulness of molybdenum for localized corrosion resistance. Therefore, the alloy contains no more than about 4.0%, more preferably no more than about 3.0%, and even more preferably no more than about 2.75% molybdenum.
[0017] Aluminum may be present in the alloy at about 0.5% or less, or about 0.3% or less, as a residual from deoxidizing additions during primary melting of the alloy. Aluminum may improve the fluidity of the alloy during casting. Small amounts of aluminum are believed to help raise the Ms temperature of the alloy and ensure complete transformation to the martensite phase. The alloy may optionally contain at least about 0.15% aluminum to improve the yield and tensile strength of the alloy. Too much aluminum impairs the fracture toughness of the alloy. Therefore, when added intentionally, aluminum is limited to about 0.25% or less, and preferably to about 0.20% or less. For applications requiring maximum toughness, the alloy contains about 0.025% or less aluminum.
[0018] Other elements such as boron, manganese, and silicon may be present in controlled amounts to favor other desirable properties of the alloy. More specifically, about 0.01% or less boron, more preferably about 0.005% or less boron, and preferably about 0.0035% or less boron may be present in the alloy to favor the hot workability of the alloy. At least about 0.001%, preferably at least about 0.0015% boron is present in the alloy to obtain the desired effect. About 1.0% or less manganese, more preferably about 0.5% or less, and even more preferably about 0.25% or less manganese may be present in the alloy as residual from charge additions during melting. About 0.75% or less silicon, more preferably about 0.5% or less, and even more preferably about 0.25% or less silicon may be present in the alloy as residual from scrap charge material or deoxidizing additions. Such additions are beneficial when the alloy is not vacuum melted. Manganese and / or silicon are desirably kept at low levels because they can adversely affect the toughness and corrosion resistance of the alloy. Too much manganese and / or silicon also adversely affects the austenite-martensite phase balance in the base metal. Thus, manganese and silicon are preferably limited to about 0.10% or less each in this alloy. Additionally, the amount of Nb is preferably limited to about 0.10% or less to reduce the adverse effect that Nb has on the alloy's toughness and to promote high temperature Laves phases, which increases the alloy's tendency to segregate.
[0019] The balance of the alloy is essentially iron and normal impurities found in commercial grades of alloys intended for similar service or use, the levels of such elements being controlled so as not to adversely affect the property combination exhibited by the alloy.
[0020] In particular, too much carbon and / or nitrogen impairs corrosion resistance and adversely affects the toughness of the alloy. Thus, not more than about 0.03%, more preferably not more than about 0.02%, and even more preferably not more than about 0.015% carbon is present in the alloy. Also, not more than about 0.030%, more preferably not more than about 0.015%, and even more preferably not more than about 0.010% nitrogen is present in the alloy. When present in high amounts, the carbon and / or nitrogen combine with titanium to form titanium-rich nonmetallic inclusions. This reaction inhibits the formation of nickel-titanium rich phases which are the primary cause of the high strength of the alloy.
[0021] Also, due to the alloying additions made during the primary melting, phosphorus and sulfur are inevitably present. However, the amounts of phosphorus and sulfur are controlled. In particular, phosphorus is maintained at low levels due to its adverse effect on the toughness and corrosion resistance properties exhibited by the alloy. In this regard, not more than about 0.04%, more preferably not more than about 0.015%, and even more preferably not more than about 0.01% phosphorus is present in the alloy. Sulfur is limited to not more than about 0.020%, more preferably not more than about 0.01%, and preferably not more than about 0.005% in the alloy. Higher amounts of sulfur promote the formation of titanium-rich nonmetallic inclusions, reducing the titanium available for the formation of the primary strengthening phase during age-hardening heat treatment, thereby inhibiting the strengthening effect of titanium. Also, amounts of sulfur exceeding the limiting values adversely affect the hot workability and corrosion resistance of the alloy. Furthermore, such amounts of sulfur adversely affect the toughness of the alloy, especially in the direction perpendicular to the rolling direction.
[0022] Sulfur and phosphorus, when present, tend to segregate to the grain boundaries of the alloy. Such segregation reduces the grain boundary adhesion and adversely affects the fracture toughness, notch toughness, and notch tensile strength of the alloy. Approximately 0.7 inches 2 (4cm 2) or larger cross-sections do not undergo sufficient thermomechanical treatment to homogenize the alloy and neutralize the deleterious effects of sulfur and phosphorus concentrating at the grain boundaries. In products of such large cross-section sizes, cerium is preferably added in small amounts during melting to bind with the sulfur and phosphorus and facilitate their removal from the alloy, thereby beneficially affecting the fracture toughness, notch toughness, and notch tensile strength of the alloy. To fully remove sulfur and phosphorus from the alloy, the ratio of the amount of cerium to the amount of sulfur present in the alloy (Ce:S) should be at least about 1:1, better at least about 2:1, and preferably at least about 3:1. To realize the benefits of the cerium addition, it is necessary to retain only trace amounts of cerium in the alloy (i.e., <0.001%). However, to ensure that sufficient cerium is added and to prevent significant residual sulfur and phosphorus in the final product, it is preferred that at least about 0.001%, and more preferably at least about 0.002%, of cerium be present in the alloy. Too much cerium can adversely affect the hot workability of the alloy and its fracture toughness. Thus, cerium is limited to about 0.025% or less in the alloy, more preferably about 0.015% or less, and even more preferably about 0.010% or less. Alternatively, the cerium to sulfur ratio of the alloy is about 15:1 or less, better about 12:1 or less, and preferably about 10:1 or less. Other rare earth metals, such as lanthanum and yttrium, as well as calcium and magnesium, can be present in the alloy in place of some or all of the cerium.
[0023] The melting, casting and mechanical processing of the alloy of the present invention does not require any special techniques. The alloy of the present invention is preferably produced by vacuum induction melting (VIM). If desired, the alloy can also be refined by a double melting process, where a VIM ingot is remelted by electroslag remelting (ESR) or vacuum arc remelting (VAR). In the most important applications, a triple melting process consisting of VIM followed by ESR and then VAR can be used. Alternatively, a melting process consisting of VIM followed by multiple VAR melts, or any combination of ESR and VAR melts in the appropriate sequence as known to the skilled person, can be used.
[0024] The alloys may be cast as ingots which may then be hot worked to obtain near net shape product forms such as billets or bars. The alloys of the present invention may be hot worked or cold worked, with cold working improving the mechanical strength of the alloy. Prior to hot working, the alloy ingot is preferably homogenized by heating to a temperature of about 2000°F to about 2400°F for a time selected to equalize the temperature of the ingot.
[0025] Hot working is preferably carried out from the homogenization temperature to a finishing temperature of about 1900°F (1038°C). If further reduction in cross-sectional area is required, the alloy can be reheated to about 1900°F to 2400°F (1038°C to 1315°C) before further hot working. Hot working can be carried out by techniques such as press forging or rotary forging.
[0026] The precipitation hardened alloy of the present invention is solution treated and then age hardened to develop the desired strength. The solution treatment temperature must be high enough to dissolve enough titanium and molybdenum to cause the desired hardening reaction during the aging heat treatment. However, if the solution treatment temperature is too high, excessive grain growth will be promoted, thereby compromising the fracture toughness of the alloy. Typically, the alloy of the present invention is solution treated at about 1700°F to 1900°F (927°C to 1038°C) for 1 hour, and then quenched. Quenching can be performed with any known medium, including, but not limited to, water, oil, or inert gas. Preferably, the quenching medium is selected to achieve a quenching rate of about 60°C / second (°C / s), more preferably about 80°C / s, and more preferably about 100°C / s.
[0027] Preferably, the alloy is subjected to a deep chill treatment after quenching to further improve the high strength of the alloy. Deep chilling involves cooling the alloy to a temperature well below the martensitic finish temperature (Mf) to ensure the completion of the martensitic transformation. Typically, deep chilling is performed by cooling the alloy to below about -100°F (-73°C) for about one hour. However, the need for deep chilling is at least partially determined by the martensitic finish temperature of the alloy. If the martensitic finish temperature is high enough, the transformation to martensitic structure will proceed without deep chilling. Furthermore, the need for deep chilling may also depend on the cross-sectional size of the part being manufactured. As the cross-sectional size increases, segregation in the alloy becomes more pronounced, making deep chilling more beneficial. Furthermore, larger parts may require longer cooling times to complete the transformation to martensite. For example, parts with large cross-sectional areas (i.e., 0.7 in. 2 In the above, it has been found that deep cooling for about 8 to 16 hours is preferable in order to develop the high strength that is a characteristic of this alloy.
[0028] The alloy of the present invention is age hardened according to techniques known to those skilled in the art and used for known precipitation hardening, stainless steel alloys. For example, the alloy may be aged at a temperature between about 900°F (482°C) and about 1150°F (621°C) for about 4 hours to about 24 hours. After aging, the material is cooled in a medium selected to produce a cooling rate of about 60°C / sec, preferably about 80°C / sec, and more preferably about 100°C / sec. Slower cooling rates may be utilized, but mechanical properties are not guaranteed. The alloy of the present invention is capable of exhibiting an ultimate tensile strength of at least about 280 ksi and a fracture toughness of at least about 60 ksi in the solution-treated and age-hardened condition. The alloy is further characterized by good resistance to common corrosion as measured by salt spray testing (ASTM B117).
[0029] The alloy of the present invention can be formed into a variety of product forms for a wide variety of applications and is suitable for forming billets, bars, rods, wires, or plates using conventional methods. In the solution-annealed condition, the alloy is workable and has sufficient ductility to be processed into small gauge plates and strips. Furthermore, cold working into plates or strips and subsequent aging treatments improves mechanical strength but at the expense of some toughness and ductility properties. Furthermore, the alloy can be produced by powder metallurgy techniques. Metal powders produced from the alloy of the present invention can be processed into complex semi-finished products that approximate the final product, as known to those skilled in the art. At that point, the metal powders can be processed or manufactured into semi-finished products by powder metallurgy or additive manufacturing techniques.
[0030] The alloys of the present invention are useful in a wide range of commercial applications requiring alloys with a good combination of corrosion resistance, high strength and good toughness. In particular, the alloys of the present invention can be used for the manufacture of aircraft structural components, such as, but not limited to, landing gear components, flap tracks, fasteners, etc. The alloys of the present invention are also suitable for medical and dental applications, such as dental tools, medical scrapers, cutters, and suture needles. They are also suitable for consumer sports applications, such as golf club heads. EXAMPLES
[0031] (Example) To demonstrate the novel combination of high strength and fracture toughness exhibited by the alloys of the present invention, Examples 1-13 embodying the alloys of the present invention were subjected to vacuum induction melting (VIM). The compositions of Examples 1-13 are shown in weight percent in Table 1 below.
[0032] [Table 1]
[0033] The balance in each example was iron and normal impurities. In Examples 1-13, the impurities included less than 0.01% manganese, up to 0.01% silicon, less than 0.005% phosphorus, less than 0.001% sulfur, 0.002-0.004% carbon, less than 0.01% nitrogen, and less than 0.01% niobium.
[0034] Examples A-W correspond to examples described in issued U.S. patents and published U.S. patent applications. The alloys corresponding to Examples A-W in the various publications are identified in Table 2 below.
[0035] [Table 2]
[0036] The heats of Examples 1-13 were cast into 4-inch (10.2 cm) tapered rectangular ingots. The ingots were homogenized at 2300°F (1260°C) for 24 hours. They were then heated to 2000°F (1093°C) for a time sufficient to homogenize the temperature, and then cooled to 2000°F (1093°C). 1 The steel bars were press forged into 1 / 4 inch (5.7 cm) square bars. The forged bars were cut and reheated to 2000°F (1093°C). 1 The bars were pressed into 1 / 4 inch (3.175 cm) square bars, cut, and reheated to 2000°F (1093°C) to equalize temperature. They were then one-end press forged into 11 / 16 inch (17.5 mm) square bars and cooled in air to room temperature. They were then stress relieved at 1250°F (677°C) for four hours and cooled in air to room temperature.
[0037] After overaging heat treatment, longitudinal test specimens were roughly machined from the bars for smooth tensile testing, Charpy V-notch impact (CVN) testing, and four-point bend fracture toughness testing. The test specimens of Examples 1-13 were solution treated at temperatures ranging from 1750 to 1900°F (927 to 1030°C) for 1 hour, then quenched in oil to room temperature. After solution treatment, they were deep-chilled at -100°F (-73°C) for at least 8 hours, then warmed to room temperature. The test specimens were then finish-polished to their respective sizes, and heated at 925°F (496°C) for 12 hours and water-cooled to room temperature before testing.
[0038] Examples A-W were prepared, heat treated, and tested as described in the respective patents and published patent applications identified in Table 2.
[0039] Mechanical test results are reported in terms of 0.2% offset yield strength (YS) and ultimate tensile strength (ksi), elongation (%El.), reduction in area (%RA), Charpy V-notch impact energy (CVN) (ft-lbs), and fracture toughness in ksi√in (K Q / K Ic ) are shown in Table 3 below. Table 3 also shows the ratio of fracture toughness to ultimate tensile strength in each example in √in (ratio).
[0040] [Table 3]
[0041] Salt spray corrosion testing was performed on two of the solution treated and age hardened specimens of Examples 1-13. All samples were aged at 925°F (496°C) for 12 hours and then water cooled to room temperature prior to testing. The samples were tested in accordance with ASTM B117 at 5% NaCl concentration, natural pH, and 95°F for the times shown in Table 4 below. The samples were surface polished with SiC paper finish, 1200 grit for Examples 1-3 and 120 grit for Examples 4-13, prior to salt spray exposure. The results of the salt spray testing are shown in Table 4 below, including the solution treatment parameters, surface finish abrasive, test time, and a visual inspection of the specimens. The rating scale is as follows: 1=no rust, 2=1-3 spots of rust, 3=rust up to 5% of the surface, 4=rust on 5-10% of the surface, 5=rust on 10-20% of the surface, 6=rust on 20-24% of the surface.
[0042] [Table 4]
[0043] Example 1 above exhibited the best combination of tensile strength, fracture toughness, and corrosion resistance. Therefore, 400 pounds of heat having essentially the same chemical composition as Example 1 was vacuum induction melted (VIM) and cast into 6 inch (15.2 cm) VAR electrodes. The weight percent composition of this heat is shown in Table 5 below, in weight percent, as Example 14.
[0044] [Table 5]
[0045] The electrode ingot was vacuum arc remelted (VAR) into an 8 inch (20.3 cm) ingot. The VAR ingot was homogenized at 2300°F (1260°C) for 36 hours and then soaked at 2000°F (1093°C). The 8 inch (20.3 cm) ingot was press forged from 2000°F (1093°C) into a 6 inch (15.2 cm) square billet. The billet was reheated to 2000°F (1093°C), soaked to temperature, and press forged into a 3.75 inch (9.5 cm) square bar. The 3.75 inch (9.5 cm) bar was further reduced into a 1.5 inch by 2.75 inch (3.8 cm by 6.9 cm) slab.
[0046] Standard longitudinal smooth tensile and longitudinal Charpy V-notch impact (CBN) specimens were prepared from the 3.75 inch (9.5 cm) square bars (Examples 14A and 14B) and 1.5 inch by 2.75 inch (3.8 cm by 6.9 cm) slabs (Examples 14C and 14D). Standard longitudinal 1 inch (2.54 cm) fracture toughness blocks were prepared from the bars and slabs according to ASTM Standard Test Method E399. The tensile, CVN, and fracture toughness specimens of Examples 14A, 14B, 14C, and 14D were solution treated as described in Table 5 below. The specimens were age hardened by heating at 925°F (496°C) for 12 hours and then water quenched.
[0047] Room temperature mechanical testing results for Examples 14A, 14B, 14C, and 14D were as follows: 0.2% offset yield strength (YS) and ultimate tensile strength (ksi), elongation (%El.), percent reduction in area (%RA), Charpy V-notch impact energy in ft-lbs (CVN), and fracture toughness in ksi√in (K Ic ) are shown in Table 6 below. Table 5 also shows the fracture toughness-ultimate tensile strength ratio (ratio) for each example in √in.
[0048] [Table 6]
[0049] Important advantages exhibited by Applicant's claimed alloys are illustrated in Figures 1 and 2. Figure 1 is a graph of fracture toughness as a function of ultimate tensile strength exhibited by claimed alloy Examples 14A-14D (▲) and exemplary alloys described in US2016 / 0289805 (◯). Figure 2 is a graph of fracture toughness as a function of ultimate tensile strength exhibited by claimed alloy Examples 14A-14D (▲), Comparative Examples U, V, and W (X), Comparative Examples K and N (◇), Comparative Examples A-H (◯), and Comparative Examples Q and R (-).
[0050] Salt spray corrosion testing according to ASTM B117 was performed on two coupon samples sliced to a thickness of 0.25 in. (6.35 mm) from a 3.75 in. square bar. The salt spray specimens were surface polished and then exposed to a 5% salt water mist at 35°C. After 200 hours of exposure, no rust formation was observed on any of the coupon samples.
[0051] The terms and expressions used in this specification are used as terms of description and not of limitation. The use of such terms and expressions is not intended to exclude any equivalents of the features shown or described or portions thereof. It is recognized that various modifications are possible within the scope of the invention described and claimed herein. The disclosure of this specification may include the following aspects. (Aspect 1) A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance, comprising, in weight percent, essentially: Ni: about 10.5 to about 12.5, Co: about 1.0 to about 6.0, Mo: approx. 1.0 to approx. 4.0, Ti: about 1.5 to about 2.0, Cr: about 8.5 to about 11.5, Al: about 0.5 or less, Mn: about 1.0 or less, Si: approx. 0.75 or less, B: about 0.01 or less, and Balance of Alloy: Essentially iron and normal impurities including not more than about 0.03% carbon, not more than about 0.03% nitrogen, not more than about 0.04% phosphorus, and not more than about 0.020% sulfur. A martensitic precipitation hardening stainless steel alloy consisting of (Aspect 2) 2. The alloy of embodiment 1, containing at least about 0.15% aluminum. (Aspect 3) The alloy of embodiment 1 comprising at least about 11.0% nickel. (Aspect 4) The alloy of embodiment 1, comprising at least about 1.5% cobalt. (Aspect 5) The alloy of embodiment 4 comprising up to about 5.5% cobalt. (Aspect 6) The alloy of embodiment 1 containing at least about 2.0% molybdenum. (Aspect 7) 7. The alloy of embodiment 6 comprising up to about 3.0% molybdenum. (Aspect 8) 2. The alloy of embodiment 1, comprising at least about 1.55% titanium. (Aspect 9) The alloy of embodiment 8, comprising up to about 1.8% Titanium. (Aspect 10) The alloy of embodiment 1 comprising at least about 8.75% chromium. (Aspect 11) 11. The alloy of embodiment 10, comprising up to about 10.5% chromium. (Aspect 12) A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance properties, comprising, in weight percent, essentially: Ni: about 11.0 to about 12.2, Co: about 1.5 to about 5.5, Mo: about 2.0 to about 3.0, Ti: about 1.55 to about 1.8, Cr: approx. 8.75 ~ approx. 10.5, Al: about 0.3 or less, Mn: approx. 0.25 or less, Si: approx. 0.25 or less, B: 0.001 to 0.005, and Balance of Alloy: Essentially iron and the usual impurities including not more than about 0.02% carbon, not more than about 0.015% nitrogen, not more than about 0.015% phosphorus, and not more than about 0.01% sulfur. A martensitic precipitation hardening stainless steel alloy consisting of (Aspect 13) 13. The alloy of embodiment 12, comprising at least about 0.15% aluminum. (Aspect 14) 13. The alloy of embodiment 12, comprising at least about 11.4% nickel. (Aspect 15) 13. The alloy of embodiment 12, comprising at least about 2.0% cobalt. (Aspect 16) 16. The alloy of embodiment 15 comprising up to about 5.0% cobalt. (Aspect 17) 13. The alloy of embodiment 12, comprising at least about 2.25% molybdenum. (Aspect 18) 18. The alloy of embodiment 17 comprising up to about 2.75% molybdenum. (Aspect 19) 13. The alloy of embodiment 12, comprising at least about 1.60% titanium. (Aspect 20) 20. The alloy of embodiment 19, comprising up to about 1.75% titanium. (Aspect 21) 13. The alloy of embodiment 12, comprising at least about 9.0% chromium. (Aspect 22) 22. The alloy of embodiment 21 comprising up to about 10.0% chromium. (Aspect 23) A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance properties, comprising, in weight percent, essentially: Ni: about 11.4 to about 12.0, Co: about 2.0 to about 5.0, Mo: about 2.25 to about 2.75, Ti: about 1.60 to about 1.75, Cr: approx. 9.0~10.0, Al: about 0.2 or less, Mn: about 0.10 or less, Si: approx. 0.10 or less, B: 0.0015 to 0.0035, and Balance of Alloy: Essentially iron and the usual impurities including not more than about 0.015% carbon, not more than about 0.010% nitrogen, not more than about 0.01% phosphorus, and not more than about 0.005% sulfur. A martensitic precipitation hardening stainless steel alloy consisting of (Aspect 24) 24. The alloy of embodiment 23, comprising at least about 0.15% aluminum. (Aspect 25) 2. A method of manufacturing a metallic part or component made from the martensitic precipitation hardenable stainless steel alloy of embodiment 1, thereby exhibiting a novel combination of corrosion resistance, high strength, and high fracture toughness, said method comprising the steps of: Obtaining an ingot having the composition of the martensitic precipitation hardening stainless steel alloy according to embodiment 1 by melting and casting said alloy; heating the ingot to a temperature of about 2000°F (1093°C) to about 2400°F (1315°C) for a time sufficient to homogenize the ingot; hot working the homogenized ingot to obtain a near net shape part; annealing the near net shape part by heating the part at a temperature of about 1700°F (927°C) to about 1900°F for a preselected time; quenching the annealed component to below about -100°F (-73°C) from the annealing temperature to ensure complete martensitic transformation of the alloy matrix; and Age hardening is accomplished by heating the quenched parts at temperatures between 900°F (482°C) and about 1150°F (621°C) for times selected to obtain a combination of tensile strength, fracture toughness, and corrosion resistance. (Aspect 26) 26. The method of embodiment 25, wherein the consolidation step is performed by a powder metallurgy consolidation process. (Aspect 27) 26. The method of embodiment 25, wherein the consolidation step is performed by an additive manufacturing process. (Aspect 28) 2. An article of manufacture produced from the alloy of embodiment 1, wherein the article of manufacture has a tensile strength of at least 280 ksi (1930 MPa), a plane strain fracture toughness of at least 60 ksi√in (66 MPa√m), and a general corrosion resistance characterized by a rating of about 1 when tested in accordance with ASTM Standard Test Procedure B117. (Aspect 29) 29. The article of manufacture of claim 28, wherein the article is a structural member for an aircraft. (Aspect 30) 30. The article of manufacture of embodiment 29, wherein the structural member is selected from the group consisting of landing gear, landing gear parts, flap tracks, and fasteners. (Aspect 31) 29. The article of manufacture of embodiment 28, wherein the article is a medical or dental device. (Aspect 32) 32. The article of manufacture of embodiment 31, wherein the medical or dental device is selected from the group consisting of dental tools, medical scrapers, and cutters, and suture needles. (Aspect 33) 30. The article of manufacture of claim 28, wherein the article comprises sports equipment. (Aspect 34) 34. The article of manufacture of claim 33, wherein the sports equipment comprises a golf club head.
Claims
1. A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance comprising, in weight percent: Ni: 10.5-12.5, Co: 1.0-6.0, Mo: 1.0 to 4.0, Ti: 1.5-2.0, Cr:8.5-11.5, Al: 0.2 or less, Mn: 1.0 or less, Si: 0.75 or less, B: 0.01 or less, C: 0.03% or less, N: 0.03% or less, P: 0.04% or less, and S: 0.020% or less; A martensitic precipitation hardenable stainless steel alloy, the balance of the alloy being iron and incidental impurities.
2. 2. The alloy of claim 1 containing at least 11.0% nickel.
3. 10. The alloy of claim 1 comprising at least 1.5% cobalt.
4. 4. The alloy of claim 3 containing up to 5.5% cobalt.
5. 10. The alloy of claim 1 containing at least 2.0% molybdenum.
6. 6. The alloy of claim 5 containing up to 3.0% molybdenum.
7. 10. The alloy of claim 1 comprising at least 1.55% titanium.
8. 8. The alloy of claim 7 containing up to 1.8% titanium.
9. 10. The alloy of claim 1 comprising at least 8.75% chromium.
10. 10. The alloy of claim 9 containing up to 10.5% chromium.
11. A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance properties comprising, in weight percent: Ni: 11.0-12.2, Co: 1.5-5.5, Mo: 2.0-3.0, Ti: 1.55 to 1.8, Cr:8.75-10.5, Al: 0.2 or less, Mn: 0.25 or less, Si: 0.25 or less, B: 0.001 to 0.005, C: 0.02% or less, N: 0.015% or less, P: 0.015% or less, and S: 0.01% or less; A martensitic precipitation hardenable stainless steel alloy, the balance of the alloy being iron and incidental impurities.
12. 12. The alloy of claim 11 comprising at least 11.4% nickel.
13. 12. The alloy of claim 11 comprising at least 2.0% cobalt.
14. 14. The alloy of claim 13 containing up to 5.0% cobalt.
15. 12. The alloy of claim 11 comprising at least 2.25% molybdenum.
16. 16. The alloy of claim 15 containing up to 2.75% molybdenum.
17. 12. The alloy of claim 11 comprising at least 1.60% titanium.
18. 20. The alloy of claim 17 containing up to 1.75% titanium.
19. 12. The alloy of claim 11 containing at least 9.0% chromium.
20. 20. The alloy of claim 19 containing up to 10.0% chromium.
21. A martensitic precipitation hardenable stainless steel alloy having a novel combination of fracture toughness, strength and corrosion resistance properties comprising, in weight percent: Ni: 11.4-12.0, Co:2.0-5.0, Mo: 2.25-2.75, Ti: 1.60 to 1.75, Cr:9.0-10.0, Al: 0.2 or less, Mn: 0.10 or less, Si: 0.10 or less, B: 0.0015 to 0.0035, C: 0.015% or less, N: 0.010% or less, P: 0.01% or less, and S: 0.005% or less; A martensitic precipitation hardenable stainless steel alloy, the balance of the alloy being iron and incidental impurities.
22. 22. A method for manufacturing a metallic part or component made from a martensitic precipitation hardenable stainless steel alloy according to any one of the preceding claims, said method comprising the steps of: Obtaining an ingot having the composition of the martensitic precipitation hardening stainless steel alloy according to any one of claims 1 to 21 by melting and casting said alloy; heating said ingot at a temperature of 2000°F (1093°C) to 2400°F (1315°C) for a time sufficient to homogenize said ingot; hot working the homogenized ingot to obtain a near net shape part; annealing the near net shape part by heating the part at a temperature of 1700°F (927°C) to 1900°F (1038°C) for one hour; quenching the annealed part from the annealing temperature in a quenching medium providing a quenching rate of 60°C / sec to 100°C / sec; and Age hardening by heating the quenched parts at temperatures between 900°F (482°C) and 1150°F (621°C) for 4 to 24 hours.
23. 23. The method of claim 22, further comprising deep chill treating the quenched component to below -100°F (-73°C) to ensure a complete martensitic transformation of the alloy matrix, said deep chill treating occurring after said quenching and prior to said age hardening.
24. 24. The method of claim 23, wherein the deep cooling is carried out for 8 to 16 hours.
25. 22. An article of manufacture produced from the alloy of any of the preceding claims, said article of manufacture having a tensile strength of at least 280 ksi (1930 MPa), a plane strain fracture toughness of at least 60 ksi√in (66 MPa√m), and a general corrosion resistance characterized by a rating of about 1 when tested in accordance with ASTM standard test procedure B117.
26. 26. The article of manufacture of claim 25, wherein the article is a structural member for an aircraft.
27. 27. The article of manufacture of claim 26, wherein the structural member is selected from the group consisting of landing gear, landing gear parts, flap tracks, and fasteners.
28. 26. The article of manufacture of claim 25, wherein the article is a medical or dental device.
29. 30. The article of manufacture of claim 28, wherein the medical or dental device is selected from the group consisting of dental tools, medical scrapers, and cutters, and suture needles.
30. 26. The article of manufacture of claim 25, wherein the article comprises sports equipment.
31. The article of manufacture of claim 30 , wherein the sports equipment comprises a golf club head.
Citation Information
Patent Citations
Precipitation-hardened stainless steel and process for production thereof
WO2012002208A1