Methods for SI Gap Filling by PECVD

PECVD-based deposition and removal cycles for amorphous silicon layers address the challenge of void-free filling in high aspect ratio structures, achieving high-quality gap-filling without additional processing steps and improving throughput.

JP7580540B2Active Publication Date: 2024-11-11APPLIED MATERIALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023117932
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-09
Filing Date
2023-07-20
Publication Date
2024-11-11
Estimated Expiration
2039-03-07

AI Technical Summary

Technical Problem

Existing deposition processes struggle to void-free fill high aspect ratio structures in semiconductor manufacturing due to limitations in depositing high-quality gap-filling materials, often requiring subsequent processes like annealing to improve material quality.

Method used

A method involving plasma enhanced chemical vapor deposition (PECVD) is used to form amorphous silicon layers on substrates, where a deposition and removal cycle is repeated until the feature is filled, ensuring seamless filling without voids, using controlled plasma power and etching to maintain layer quality.

Benefits of technology

The method achieves void-free filling of high aspect ratio structures with improved amorphous silicon quality, eliminating the need for subsequent curing and annealing processes, and enhances substrate throughput by minimizing ion bombardment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580540000001
    Figure 0007580540000001
  • Figure 0007580540000002
    Figure 0007580540000002
  • Figure 0007580540000003
    Figure 0007580540000003
Patent Text Reader

Abstract

To provide a method for SI gap fill by plasma enhanced chemical vapor deposition (PECVD).SOLUTION: A process for filling trenches in a substrate 100 is a PECVD process for depositing a first amorphous silicon layer 108 and a second amorphous silicon layer. The process includes: flowing a silicon-containing precursor into a process chamber; forming a plasma in the process chamber; removing the second amorphous silicon layer from a surface 101 of the substrate; after removing the second amorphous silicon layer, performing a second PECVD process to form a third amorphous silicon layer 116 on the first amorphous silicon layer, and forming a fourth amorphous silicon layer on the surface; removing the fourth amorphous silicon layer from the surface; and depositing additional amorphous silicon layers 124, 126, 128 on the third amorphous silicon layer.SELECTED DRAWING: Figure 1F
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THE DISCLOSURE

[0001] Embodiments of the present disclosure relate to a method for forming a gap fill material on a substrate. [Background technology]

[0002]

[0002] In semiconductor processing, devices are being manufactured with continuously decreasing feature dimensions. Often, the features utilized to manufacture devices at these advanced technology nodes include high aspect ratio structures, and it is often necessary to fill the gaps between the high aspect ratio structures with a gap-filling material, such as an insulating material. Examples of where insulating materials are utilized for gap-filling applications include shallow trench isolation (STI), intermetal dielectric layers (ILD), premetal dielectrics (PMD), passivation layers, and patterning applications. As device geometries shrink and thermal budgets decrease, void-free filling of high aspect ratio spaces becomes increasingly difficult due to limitations of existing deposition processes.

[0003]

[0003] Gap-fill materials can be deposited by a variety of deposition processes, such as flowable chemical vapor deposition (FCVD). As-deposited gap-fill materials by FCVD are typically of poor quality, characterized by high wet etch rate ratios (WERR) and high stress, and require subsequent processes, such as curing and / or annealing, to improve the quality of the gap-fill material.

[0004]

[0004] Therefore, there is a need for improved processes for forming gap-fill materials. Summary of the Invention

[0005]

[0005] An embodiment of the present disclosure relates to a method of forming a gap fill material on a substrate. In one embodiment, the method includes heating a substrate disposed in a process chamber to a temperature ranging from about 150°C to about 650°C, flowing a silane-containing precursor into the process chamber, depositing a first amorphous silicon layer at a bottom of a feature formed in the substrate and depositing a second amorphous silicon layer on a surface of the substrate. A first portion of each sidewall of the feature is in contact with the first amorphous silicon layer and a second portion of each sidewall is exposed. The method further includes removing the second amorphous silicon layer.

[0006] In another embodiment, a method includes heating a substrate disposed in a process chamber to a temperature in a range of about 200° C. to about 550° C., flowing silane or disilane into the process chamber, forming a plasma in the process chamber, and depositing a first amorphous silicon layer at a bottom of a feature formed in the substrate and a second amorphous silicon layer on a surface of the substrate, wherein a first portion of each sidewall of the feature is in contact with the first amorphous silicon layer and a second portion of each sidewall is exposed.

[0007]

[0007] In another embodiment, a method includes depositing a first amorphous silicon layer on a bottom of a feature formed in a substrate and depositing a second amorphous silicon layer on a surface of the substrate. A first portion of each sidewall of the feature is in contact with the first amorphous silicon layer and a second portion of each sidewall is exposed. Depositing the first and second amorphous silicon layers includes heating a substrate disposed in a process chamber to a temperature in a range of about 150°C to about 650°C and flowing a silane-containing precursor into the process chamber. The method further includes removing the second amorphous silicon layer, repeating the steps of depositing the first and second amorphous silicon layers and removing the second amorphous silicon layer until the feature is filled with amorphous silicon.

[0008]

[0008] In order to allow the above features of the present disclosure to be understood in detail, a more particular description of the present disclosure briefly summarized above can be made by referring to embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the accompanying drawings show only typical embodiments of the present disclosure, and therefore should not be considered as limiting the scope of the present disclosure, since other equally effective embodiments can be recognized. [Brief description of the drawings]

[0009] [Figure 1A] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. [Figure 1B] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. [Figure 1C] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. [Figure 1D] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. [Figure 1E] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. [Figure 1F] 1 illustrates a schematic diagram of a method for forming a gap fill material on a substrate according to one embodiment described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010]

[0010] To facilitate understanding, identical elements common to the figures have been designated using the same reference numerals whenever possible. It is contemplated that an element disclosed in one embodiment may be beneficially utilized in other embodiments without specific recitation thereof.

[0011]

[0011] An embodiment of the present disclosure relates to a process for filling a trench. The process includes depositing a first amorphous silicon layer on a surface of a layer and depositing a second amorphous silicon layer in a portion of a trench formed in the layer, with a portion of the trench sidewall being exposed. The first amorphous silicon layer is removed. The process further includes depositing a third amorphous silicon layer on the surface of the layer and depositing a fourth amorphous silicon layer on the second amorphous silicon layer. The third amorphous silicon layer is removed. The deposition / removal cycle process can be repeated until the trench is filled with an amorphous silicon layer. Because the amorphous silicon layer is formed from bottom to top, the amorphous silicon layer forms a seamless amorphous silicon gap fill in the trench.

[0012]

[0012] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which a film treatment is performed during a manufacturing process. For example, substrate surfaces on which treatment can be performed include materials such as silicon, silicon oxide, strained silicon, silicon on insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys, and other conductive materials depending on the application. Substrates include, but are not limited to, semiconductor wafers. Substrates may be exposed to pretreatment processes to polish, etch, reduce, oxidize, hydroxylate, anneal, and / or bake the substrate surface. In addition to film treatment directly on the surface of the substrate, any of the disclosed film treatment steps may be performed on an underlayer formed on the substrate, as disclosed in more detail below, and the term "substrate surface" is intended to include the underlayer as the context indicates. Thus, for example, when a film / layer or partial film / layer is deposited on a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface.

[0013] 1A-1F are schematic diagrams illustrating a process for forming a gap-fill material on a substrate according to one embodiment described herein. As shown in FIG. 1A, a substrate 100 includes a feature 102. The figure shows a substrate with a single feature for illustrative purposes, but one skilled in the art will understand that there may be more than one feature. The shape of the feature 102 may be any suitable shape, including, but not limited to, a trench and a cylindrical via. As used in this regard, the term "feature" refers to any intentional surface irregularity. Suitable examples of features include, but are not limited to, trenches and vias having a bottom and two sidewalls. The feature may have any suitable aspect ratio (ratio of the depth of the feature to the width of the feature). In some embodiments, the aspect ratio is about 5:1 or more, about 10:1 or more, about 15:1 or more, about 20:1 or more, about 25:1 or more, about 30:1 or more, about 35:1 or more, or about 40:1 or more.

[0014]

[0014] The substrate 100 includes a surface 101, and the feature 102 is an opening formed in the surface 101. In one embodiment, the substrate 100 includes an STI region made of a dielectric material such as silicon oxide or silicon nitride, and the feature 102 is formed in the STI region. The feature 102 includes a bottom 104 and a sidewall 106. Then, as shown in FIG. 1B, a first amorphous silicon layer 108 is deposited on the bottom 104 of the feature 102, and a second amorphous silicon layer 110 is deposited on the surface 101 of the substrate 100. The first amorphous silicon layer 108 and the second amorphous silicon layer 110 are deposited by a plasma enhanced chemical vapor deposition (PECVD) process.

[0015] In one embodiment, the PECVD process for depositing the first amorphous silicon layer 108 and the second amorphous silicon layer 110 includes flowing a silicon-containing precursor into a process chamber and forming a plasma in the process chamber. In one embodiment, the process chamber is a Producer® XP Precision™ chamber available from Applied Materials Inc., Santa Clara, Calif. The plasma may be formed in situ or may be formed at a remote location and then flowed into the process chamber. The silicon-containing precursor may be a silane-containing precursor, such as silane, disilane, trisilane, or tetrasilane. In one embodiment, the silicon-containing precursor is a lower order silane-containing precursor, such as silane or disilane. The plasma power density is about 0.14 W / cm. 2 to about 2.83 W / cm 2 and the process temperature, i.e., the temperature of the substrate during processing, ranges from about 150° C. to about 650° C., for example, from 200° C. to about 550° C. It has been discovered that when a silane-containing precursor, such as a low-order silane-containing precursor, is used at the process conditions described above, the deposited first amorphous silicon layer 108 and second amorphous silicon layer 110 are not flowable. Because the first amorphous silicon layer 108 and second amorphous silicon layer 110 are not flowable, material is not placed on the sidewall 106 during the deposition process, reducing the possibility of bridging (and corresponding void formation) of the sidewall material. The deposited first amorphous silicon layer 108 and second amorphous silicon layer 110 have improved quality compared to flowable amorphous silicon layers. Furthermore, no subsequent curing and / or annealing processes are required.

[0016]

[0016] Unlike conformal layers formed by atomic layer deposition (ALD) processes, which mostly or completely cover the sidewalls 106 during deposition, the first amorphous silicon layer 108 is formed on the bottom 104 of the feature 102 and in contact with a first portion 112 of each sidewall 106. A second portion 114 of each sidewall 106 is exposed and not covered by the first amorphous silicon layer 108. Similarly, a second amorphous silicon layer 110, which is formed simultaneously with the first amorphous silicon layer 108, is formed on the surface 101 and not on the second portion 114 of each sidewall 106 of the feature 102. The first amorphous silicon layer 108 and the second amorphous silicon layer 110 are formed on the bottom 104 and the surface 101, respectively, with the bottom 104 being approximately parallel to the surface 101. Thus, the first amorphous silicon layer 108 and the second amorphous silicon layer 110 are formed on substantially parallel surfaces and have roughly the same thickness or approximately the same thickness. In other words, the first amorphous silicon layer 108 and the second amorphous silicon layer 110 are formed on horizontal surfaces but not on vertical surfaces. The only part of the sidewall 106 (vertical surface) that is covered is the part that corresponds to the thickness of the first amorphous silicon layer 108 that is disposed on the bottom 104.

[0017]

[0017] Next, as shown in FIG. 1C, the second amorphous silicon layer 110 is removed from the surface 101. The removal process may be a plasma etching process performed in the same process chamber in which the first and second amorphous silicon layers 108, 110 are formed. The chamber pressure of the plasma etching process may be the same as the chamber pressure during the PECVD process or may be different from the chamber pressure during the PECVD process. The process temperature may be the same as the PECVD process that deposits the first and second amorphous silicon layers 108, 110. Utilizing the same process temperature for the deposition and etching processes facilitates a rapid transition between the deposition and etching processes, thereby increasing substrate throughput. The plasma power density is about 0.14 W / cm2 to about 2.83 W / cm 2 Under the process conditions described above, the second amorphous silicon layer 110 is removed, but the first amorphous silicon layer 108 is substantially unaffected because the plasma ions lose energy by colliding with the sidewalls 106, the radicals are suppressed / lost before reaching the bottom 104, and / or the plasma power density is controlled to minimize ion bombardment on the bottom 104. The etchant used in the removal process can be any suitable etchant. In one embodiment, the removal process is a physical plasma etching process, and the etchant used is helium. In another embodiment, the removal process is a chemical plasma etching process using a halogen-containing etchant, such as a fluorine or chlorine-containing etchant, or hydrogen gas as the etchant, and the plasma is formed at a remote location. The halogen-containing etchant and hydrogen gas have a high selectivity for etching amorphous silicon over the material of the substrate 100, such as silicon oxide. In yet another embodiment, the removal process is a physical and chemical plasma etching process using a halogen-containing etchant or hydrogen gas as the etchant, where the plasma is formed in situ, such as a capacitively coupled plasma.

[0018]

[0018] After removing the second amorphous silicon layer 110, a second PECVD process is performed to form a third amorphous silicon layer 116 on the first amorphous silicon layer 108 and a fourth amorphous silicon layer 118 on the surface 101, as shown in Figure 1D. The second PECVD process can be performed under the same process conditions as the PECVD process for forming the first and second amorphous silicon layers 108, 110. The third amorphous silicon layer 116 is in contact with a portion 120 of each sidewall 106, and a portion 122 of each sidewall 106 is exposed. The third and fourth amorphous silicon layers 116, 118 have the same properties as the first and second amorphous silicon layers 108, 110, respectively.

[0019] 1E, the fourth amorphous silicon layer 118 is removed from the surface 101. The removal process may be the same as the removal process for removing the second amorphous silicon layer 110. In one embodiment, the feature 102 is filled with the first amorphous silicon layer 108 and the third amorphous silicon layer 116. In other words, the entire bottom 104 is in contact with the first amorphous silicon layer 108 and the entire sidewall 106 is in contact with the first amorphous silicon layer 108 and the third amorphous silicon layer 116. In other embodiments, additional deposition / removal cycle processes can be performed to fill the feature 102. In one embodiment, as shown in FIG. 1F, additional amorphous silicon layers 124, 126, 128 are deposited on the third amorphous silicon layer 116, and as a result of the removal process following each deposition process, no amorphous silicon layer remains on the surface 101. The plasma power for the removal process is low, so that ion bombardment into the feature 102 is minimized. Furthermore, the feature 102 is overfilled with the last deposition process of the deposition / removal cycle, and the last removal process removes the amorphous silicon layer on the surface 101 and beyond the feature 102. For each deposition / removal cycle (one cycle includes one deposition process and one removal process), the ratio of deposition time to etch time can range from about 1:3 to about 1:15. In such an example, the etch time is significantly longer than the deposition time. The number of cycles depends on the depth of the feature 102 and / or the thickness of each amorphous silicon layer deposited in the feature 102. In one embodiment, the number of deposition / removal cycles ranges from about 50 to about 200, and the thickness of each amorphous silicon layer formed during each deposition cycle is between about 250 Angstroms and about 1000 Angstroms. The multiple amorphous silicon layers 108, 116, 124, 126, 128 formed in the feature 102 are formed from bottom up. Thus, no seams or voids are formed in the amorphous silicon layers 108, 116, 124, 126, 128.

[0020]

[0020] By using the deposition / removal cycle process, features such as trenches can be seamlessly filled from bottom to top. Furthermore, the amorphous silicon layer formed in the feature is not flowable, so the quality of the amorphous silicon layer is improved over conventional flowable amorphous silicon gapfill. Furthermore, subsequent curing and / or annealing processes that are typically performed after forming a flowable amorphous silicon gapfill are not required.

[0021]

[0021] While the above is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the disclosure, the scope of the present disclosure being determined by the claims that follow.

Claims

1. 1. A method for use in semiconductor manufacturing, comprising: heating a substrate disposed in a process chamber to a temperature in the range of 200° C. to 550° C.; flowing silane or disilane into the process chamber; forming a plasma in the process chamber; depositing a first amorphous silicon layer over a bottom of a feature formed in the substrate; the feature has one or more sidewalls, the first amorphous silicon layer contacting a first portion of each sidewall of the feature and exposing a second portion of each sidewall; the first amorphous silicon layer is deposited by a plasma enhanced chemical vapor deposition process; A method wherein the plasma power density of said plasma enhanced chemical vapor deposition process ranges from 0.14 W / cm 2 to 2.83 W / cm 2 .

2. The method of claim 1 , wherein the first portion of each sidewall corresponds to a thickness of the first amorphous silicon layer.

3. 10. The method of claim 1, wherein the first amorphous silicon layer is deposited to a thickness of 250 Angstroms to 1000 Angstroms.

4. The method of claim 1 , wherein the substrate includes a region formed from a dielectric material in which the feature is to be formed.

5. The method of claim 1 , wherein a second amorphous silicon layer is deposited in the feature and over the first amorphous silicon layer.

6. 1. A method for use in semiconductor manufacturing, comprising: depositing a first amorphous silicon layer on a bottom of a feature formed in a substrate and depositing a second amorphous silicon layer on a surface of the substrate, wherein a first portion of each sidewall of the feature is in contact with the first amorphous silicon layer and a second portion of each sidewall is exposed, depositing the first and second amorphous silicon layers; heating the substrate disposed in a process chamber to a temperature in the range of 150° C. to 650° C.; flowing a silane precursor into the process chamber; depositing first and second amorphous silicon layers, comprising: removing the second amorphous silicon layer; repeating the depositing of the first and second amorphous silicon layers and removing the second amorphous silicon layer until the feature is filled with amorphous silicon; Including, removing the second amorphous silicon layer comprises an etching process; The method of claim 1, wherein a ratio of a deposition time during depositing the first amorphous silicon layer and the second amorphous silicon layer to an etching time during the etching process is from 1:3 to 1:

15.

7. The method of claim 6 , wherein the first and second amorphous silicon layers are deposited by a plasma enhanced chemical vapor deposition process.

8. The method of claim 6 , wherein the silane precursor is a silane or a disilane.

9. The method of claim 6 , wherein the first amorphous silicon layer and the second amorphous silicon layer are formed simultaneously.

10. The method of claim 9 , wherein the surface of the substrate is outside the feature.

11. The method of claim 6, wherein the first amorphous silicon layer is deposited by a plasma enhanced chemical vapor deposition process.

12. The method of claim 11, wherein the plasma power density of the plasma enhanced chemical vapor deposition process is in the range of 0.14 W / cm 2 to 2.83 W / cm 2 .

13. 1. A method for use in semiconductor manufacturing, comprising: heating a substrate disposed in a process chamber to a temperature in the range of 150° C. to 650° C.; flowing a silane precursor into the process chamber; forming a plasma in the process chamber; depositing a first amorphous silicon layer over a bottom of a feature formed in the substrate; the feature has one or more sidewalls, the first amorphous silicon layer contacting a first portion of each sidewall of the feature and exposing a second portion of each sidewall; the first amorphous silicon layer is deposited by a plasma enhanced chemical vapor deposition process; A method wherein the plasma power density of said plasma enhanced chemical vapor deposition process ranges from 0.14 W / cm 2 to 2.83 W / cm 2 .

14. The method of claim 13 , wherein the silane precursor is a silane or a disilane.

15. 14. The method of claim 13, wherein the temperature is from 200°C to 550°C.

16. The method of claim 13 further comprising etching the substrate.

17. The method of claim 16 , wherein etching the substrate is performed at 150° C. to 650° C.

18. The etching is performed at a frequency of 0.14 W / cm 2 to 2.83 W / cm 2 20. The method of claim 17, comprising a plasma etch process having a plasma power density of

Citation Information

Patent Citations

  • Surface treatment device

    JP1994291063A

  • Fabrication of semiconductor device

    JP1995297136A

  • Method for forming silicon film and apparatus for forming silicon film

    JP2013239717A

  • Low-temperature selective epitaxy method

    JP2014512669A

  • Method for filling recessed part and processing apparatus