Semiconductor device manufacturing method
By employing a silicon nitride film with controlled refractive index and thickness as a surface protection film, the method addresses thermal damage in semiconductor devices, improving surface morphology and reducing contact resistance, thereby enhancing device reliability and efficiency.
Patent Information
- Application Number
- JP2023510131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-02
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-04-02
AI Technical Summary
The high-temperature ion implantation process in semiconductor devices causes thermal damage to the nitride semiconductor layer, leading to surface morphology deterioration and increased contact resistance, while conventional surface protection films either reduce device reliability or require additional manufacturing steps.
A method involving the use of a silicon nitride film with specific refractive index and thickness as a surface protection sacrificial film, applied via plasma chemical vapor deposition, to mitigate thermal damage during ion implantation and activation processes.
This approach effectively suppresses thermal damage and nitrogen desorption, maintaining the nitride semiconductor layer's integrity, reducing contact resistance, and enhancing device reliability and manufacturing efficiency.
Smart Images

Figure 0007580576000001 
Figure 0007580576000002 
Figure 0007580576000003
Abstract
Description
[Technical field]
[0001] The present application relates to a method for manufacturing a semiconductor device. [Background technology]
[0002] In general, semiconductor devices such as high electron mobility transistors (HEMTs) that use compound semiconductors such as nitride semiconductors for high frequency operation undergo a resistance reduction process for ohmic electrodes such as source-drain (SD) electrodes in order to improve their electrical characteristics. An ion implantation process is a typical example of a resistance reduction process.
[0003] In the ion implantation process, ionized impurities are implanted into the nitride semiconductor layer to form impurity regions in the nitride semiconductor layer, and then an activation process is performed. The ion implantation process significantly reduces the contact resistance between the nitride semiconductor layer and the electrode metal.
[0004] Specifically, the activation process after ion implantation is a heat treatment of the nitride semiconductor layer at 1000° C. or higher. In the heat treatment of the nitride semiconductor layer, the heat treatment temperature needs to be raised to a temperature range close to the epitaxial growth conditions of gallium nitride (GaN) or the like. Since the surface of the nitride semiconductor layer is damaged during such high-temperature heat treatment, it has been common practice to reduce the damage by forming a cap film (a sacrificial film for surface protection) on the surface of the nitride semiconductor layer.
[0005] However, when using an oxide film such as silicon oxide (SiO: Silicon Oxide), which is a typical material for a surface protection sacrificial film, it is difficult to completely suppress adverse effects of the above-mentioned activation process, such as a decrease in reliability of the semiconductor device or a deterioration in the surface morphology of the nitride semiconductor layer.
[0006] As a countermeasure against such problems, for example, Patent Document 1 discloses a method for manufacturing a semiconductor device in which a thermally damaged nitride semiconductor surface layer is removed, and Patent Document 2 discloses a method for manufacturing a semiconductor device in which the conditions for forming a cap film (a sacrificial film for surface protection) during heat treatment are specified. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-079287 A [Patent Document 2] JP 2017-079288 A Summary of the Invention [Problem to be solved by the invention]
[0008] The main heat treatment process in the manufacture of HEMTs made of nitride semiconductors is the ion implantation process, which causes thermal damage at over 1000° C. Thermal damage to the nitride semiconductor layer that occurs during the ion implantation process, i.e., deterioration of surface morphology, can be suppressed by simply lowering the heat treatment temperature, but the problem is that contact resistance worsens (increases) as the heat treatment temperature decreases.
[0009] In addition, for example, when the reliability of the semiconductor device is ensured by removing the damaged layer on the nitride semiconductor surface caused by thermal damage after performing heat treatment at the same heat treatment temperature as in the conventional method as disclosed in Patent Document 1, the number of manufacturing steps increases, and there is a concern that the nitride semiconductor layer under the gate electrode may be damaged, which may have a significant effect on the transistor characteristics. Furthermore, there is a concern that a step portion may be generated on the surface of the nitride semiconductor layer between the source and drain electrodes and the gate electrode, and that this step portion may cause unexpected electric field concentration on the surface of the nitride semiconductor layer, formation of a leak path, etc.
[0010] When the film used as the thermal cap film (surface protection sacrificial film) disclosed in Patent Document 2 is deposited by plasma-enhanced chemical vapor deposition (PECVD), it is necessary to transform it into a film with fewer hydrogen bonds like a sputtered film deposited by a sputtering method. According to Patent Document 2, it is necessary to add a highly damaging heat treatment at a heat treatment temperature of 800°C to 1000°C for a heat treatment time of 30 to 60 minutes. This increases the number of manufacturing steps or increases unnecessary thermal damage to the nitride semiconductor layer, and is highly likely to damage the quality of the nitride semiconductor layer.
[0011] The present disclosure discloses a technique for solving the problems described above, and aims to provide a manufacturing method capable of preventing deterioration of the surface morphology of a nitride semiconductor layer during an ion implantation process and preventing the formation of a damaged layer. [Means for solving the problem]
[0012] A method for manufacturing a semiconductor device disclosed in the present application includes the steps of: ion-implanting impurities into source / drain electrode formation regions in a nitride semiconductor layer formed on a substrate, where source and drain electrodes are to be formed; depositing a silicon nitride film having a refractive index of 1.80 or more and less than 1.88 and a thickness of 100 nm or more and 500 nm or less as a surface protection sacrificial film on a surface of the nitride semiconductor layer by plasma enhanced chemical vapor deposition; and heat-treating the nitride semiconductor layer on which the surface protection sacrificial film has been deposited. Effect of the Invention
[0013] According to the manufacturing method of a semiconductor device disclosed in the present application, it is possible to suppress thermal damage or detachment of nitrogen atoms (N) from the nitride semiconductor layer, thereby preventing deterioration of the surface morphology of the nitride semiconductor layer and preventing the formation of a damaged layer. [Brief description of the drawings]
[0014] [Figure 1]1 is a cross-sectional view showing a manufacturing step A of the method for manufacturing the semiconductor device according to the first embodiment. [Diagram 2] 4 is a cross-sectional view showing a manufacturing step B of the method for manufacturing the semiconductor device according to the first embodiment. FIG. [Diagram 3] 10 is a cross-sectional view showing a manufacturing step C of the method for manufacturing the semiconductor device according to the first embodiment. FIG. [Figure 4] 10 is a cross-sectional view showing a manufacturing step D in the method for manufacturing the semiconductor device according to the first embodiment. [Diagram 5] 10 is a cross-sectional view showing a manufacturing step E in the method for manufacturing the semiconductor device according to the first embodiment. [Figure 6] 4 is a cross-sectional view showing a manufacturing step F of the method for manufacturing the semiconductor device according to the first embodiment. FIG. [Figure 7] 10 is a cross-sectional view showing a manufacturing step G of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 8] 4 is a diagram showing the relationship between the thickness of a silicon nitride film and the defect density in the surface of a nitride semiconductor layer in the manufacturing method of the semiconductor device according to the first embodiment. FIG. [Figure 9] FIG. 11 is a cross-sectional view showing a manufacturing step E-1 in the method for manufacturing a semiconductor device according to the second embodiment. [Figure 10] FIG. 11 is a cross-sectional view showing a manufacturing step E-2 in the method for manufacturing a semiconductor device according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Embodiment 1 A method for manufacturing the semiconductor device according to the first embodiment will be described below. The method for manufacturing the semiconductor device according to the first embodiment includes at least the following manufacturing steps A to G. Moreover, the method for manufacturing a semiconductor device according to the first embodiment particularly relates to an ion implantation process, which is one of the manufacturing processes with the highest temperatures among all the manufacturing processes for manufacturing a semiconductor device that is the subject of the present disclosure.
[0016] A method for manufacturing a semiconductor device according to a first embodiment will be described with reference to Figures 1 to 7. Figures 1 to 7 show a cross-sectional structure around a gate electrode in an active layer region of a nitride semiconductor transistor 100, which is an example of a semiconductor device made of a nitride semiconductor.
[0017] (Manufacturing process A) First, a nitride semiconductor layer 2 consisting of a buffer layer, a channel layer, an electron supply layer, and a cap layer (none of which are shown) that constitute a semiconductor device is epitaxially grown on a substrate 1. A cross section after epitaxial growth is shown in FIG. 1. Specific examples of the substrate 1 include silicon (Si), silicon carbide (SiC), GaN, and sapphire substrates. In the following manufacturing steps, a case where a GaN on SiC substrate is used as the substrate 1 will be described.
[0018] As described above, the buffer layer, the channel layer, the electron supply layer, and the cap layer are all made of a nitride semiconductor, specific examples of which include GaN and aluminum gallium nitride (AlGaN).
[0019] 1, the area where the ion implantation region 3 is to be formed and the area where the source electrode formation region and the drain electrode formation region (hereinafter referred to as the source / drain electrode formation region 4) are to be formed are indicated by dotted lines. The area of the ion implantation region 3 is preset to be larger than the area of the source / drain electrode formation region 4.
[0020] The reason for this setting is that the most dominant portion of the contact resistance component of a semiconductor device is the end portion, i.e., the edge, of the source / drain electrode formation region 4, and it is important to at least implant ions into this end portion in order to obtain good contact resistance.
[0021] (Manufacturing process B) 2, a through injection film 5 that functions to protect the surface of the nitride semiconductor layer 2 during ion implantation is formed on the GaN on SiC substrate 1. As a method (a film forming apparatus) for forming the through injection film 5, a film forming method such as a sputtering method or a PECVD method may be used to form a nitride film such as a silicon nitride (SiN) film or an oxide film such as a SiO film. In one example of the method for manufacturing the semiconductor device according to the first embodiment, a SiN film is used as the through injection film 5.
[0022] (Manufacturing process C) Next, as shown in the cross-sectional view of FIG. 3, the surface of the through implantation film 5 is patterned with a resist to form a resist mask 6 having an opening only in the ion implantation region 3. After the resist mask 6 is formed, ion implantation is performed. In the ion implantation, ionized impurities such as Si are irradiated. The impurities that penetrate the through implantation film 5 by the ion implantation reach the inside of the nitride semiconductor layer 2 and form the ion implantation region 3.
[0023] (Manufacturing process D) 4, after the formation of the ion implantation region 3, the resist mask 6 and the through implantation film 5 are removed. In this removal, in order to remove the resist mask 6 that has hardened during ion implantation together with the through implantation film 5, a wet etching process using hydrofluoric acid or the like as an etchant is used, but other removal methods such as dry etching may also be used.
[0024] (Manufacturing process E) Next, as shown in the cross-sectional view of Fig. 5, a surface protection sacrificial film 7 is formed on the surface of the nitride semiconductor layer 2 before performing a heat treatment to activate the impurities in the ion implantation region 3. The surface protection sacrificial film 7 functions to suppress thermal damage to the surface of the nitride semiconductor layer 2. The PECVD method is applied as a method for forming the surface protection sacrificial film 7. This is because a film formed by the PECVD method generally has a lower stress than a film formed by the sputtering method.
[0025] A SiN film is used as the material of the surface protection sacrificial film 7. This is because the SiN film functions to suppress the detachment of nitrogen atoms (N) from the nitride semiconductor layer 2 caused by damage during heat treatment. With regard to the film quality of the SiN film as the surface protection sacrificial film 7, it is desirable that the SiN film is N-rich with respect to stoichiometry, that is, that has an excess of nitrogen (N). When the film quality of the surface protection sacrificial film 7 is specified as a refractive index, it is desirable that the refractive index be less than 1.88, which is an N-rich SiN film, compared to the stoichiometric refractive index of 1.88.
[0026] On the other hand, if the SiN film is too N-rich, the nitrogen (N) becomes too excessive, and the function as the surface protection sacrificial film 7 is deteriorated. From this viewpoint, the refractive index of the SiN film is desirably 1.80 or more. Therefore, the refractive index of the SiN film is preferably 1.80 or more and less than 1.88.
[0027] The thickness of the surface protection sacrificial film 7 is desirably 100 nm or more. This is because, as the amount of nitrogen atoms (N) desorbed from the surface of the nitride semiconductor layer 2 increases due to the high-temperature heat treatment, the volume of the surface protection sacrificial film 7 that functions as an inhibitory film must be increased. Therefore, the thickness of the surface protection sacrificial film 7 must be at least 30 nm or more even if the heat treatment temperature during the heat treatment is 1000° C. or less. This is also because the heat treatment temperature during the heat treatment in the ion implantation process in the first embodiment is as very high as 1000° C. to 1200° C.
[0028] On the other hand, the thickness of the surface protection sacrificial film 7 is preferably 500 nm or less. If the thickness of the surface protection sacrificial film 7 is made thicker than necessary, the time required for film formation will be longer and the amount of film formation material used will also increase, resulting in a problem of increased manufacturing costs. Therefore, the thickness of the surface protection sacrificial film (SiN film) 7 is preferably 100 nm or more and 500 nm or less.
[0029] In addition, in order to obtain an activation rate equivalent to that obtained by heat treatment under the conditions of a heat treatment temperature of 1200°C and a heat treatment time of 5 minutes, a heat treatment at a lower temperature, for example, when the heat treatment temperature is 1150°C, a thermal history of 10 minutes or more is required. The heat treatment conditions may be changed to some extent depending on the desired activation rate.
[0030] After the surface protection sacrificial film 7 is formed, a heat treatment is carried out to activate the impurities in the ion implantation region 3. The heat treatment is carried out at a temperature in the range of 1000°C to 1200°C, whereby the impurities ion-implanted in the nitride semiconductor layer 2 are activated and good contact resistance is obtained. In general, the higher the heat treatment temperature, the lower the resistance of the contact, i.e., the better the electrical connection.
[0031] Generally, damage to the nitride semiconductor layer 2 increases with increasing heat treatment temperature and heat history such as longer heat treatment time, resulting in deterioration of surface morphology due to detachment of nitrogen atoms (N) from the surface of the nitride semiconductor layer 2 and an increase in potential crystal defects in the epitaxial crystal growth layer, i.e., the nitride semiconductor layer 2. However, in the method for manufacturing a semiconductor device according to the first embodiment, the application of the above-mentioned surface protection sacrificial film 7 in the ion implantation process makes it possible to significantly suppress the occurrence of the above-mentioned problems.
[0032] (Manufacturing process F) After the heat treatment, the surface protection sacrificial film 7 is removed. A cross-sectional view after the removal of the surface protection sacrificial film 7 is shown in FIG. 6. The surface protection sacrificial film 7 can be removed by a wet etching process. Although the surface protection sacrificial film 7 can also be removed by dry etching, dry etching of the active layer region is not recommended due to concerns that it may damage the surface of the nitride semiconductor layer 2.
[0033] (Manufacturing process G) After carrying out the above-mentioned manufacturing steps A to F, a semiconductor device is completed through transistor formation steps such as formation of source electrode 8a and drain electrode 8b (hereinafter, source electrode 8a and drain electrode 8b are collectively referred to as source-drain electrodes 8), formation of gate electrode 9, formation of first gate protective film 10 (first gate passivation) and second gate protective film 11 (second gate passivation), and formation of wiring 12 by a general manufacturing method. A cross-sectional view of a nitride semiconductor transistor 100, which is an example of a semiconductor device, is shown in FIG.
[0034] 8 is a diagram showing the relationship between the thickness of the SiN film used as the surface protection sacrificial film 7 and the defect density on the surface of the nitride semiconductor layer 2 in the manufacturing method of the semiconductor device according to the first embodiment. The refractive index of the SiN film is 1.85. As can be seen from FIG. 8, when the thickness of the SiN film is 50 nm or less, the defect density on the surface of the nitride semiconductor layer 2 is 31.0 / cm. 2 It has a high density. On the other hand, when the thickness of the SiN film is 100 nm or more and 150 nm or less, the defect density on the surface of the nitride semiconductor layer 2 is 10.6 / cm 2 Even when the thickness of the SiN film is 200 nm, the defect density on the surface of the nitride semiconductor layer 2 is 14.3 / cm 2 and maintains a low density.
[0035] As described above, in the manufacturing method of the semiconductor device according to the first embodiment, a surface protection sacrificial film made of a SiN film having a refractive index of 1.80 or more and less than 1.88 and a thickness of 100 nm or more and 500 nm or less is formed on the surface of the nitride semiconductor layer after ion implantation, and then a heat treatment after ion implantation is performed. This makes it possible to suppress thermal damage to the nitride semiconductor layer or detachment of nitrogen atoms (N), thereby preventing deterioration of the surface morphology of the nitride semiconductor layer and preventing the formation of a damaged layer.
[0036] The above-mentioned effects enable activation heat treatment after ion implantation at a higher temperature (or with a sufficient temperature margin) than before, which results in a reduction in the contact resistance of the semiconductor device. Furthermore, the effects of reducing the appearance defect rate of the semiconductor device, preventing initial malfunctions of the semiconductor device, and improving the reliability of the semiconductor device are also achieved.
[0037] Embodiment 2 The manufacturing method of a semiconductor device according to embodiment 2 differs from that according to embodiment 1 in that the surface protection sacrificial film 17 is composed of two layers: a lower-layer surface protection sacrificial film 17a in contact with the nitride semiconductor layer 2, and an upper-layer surface protection sacrificial film 17b on the surface side. The following describes a method for manufacturing a semiconductor device according to the embodiment 2. Note that manufacturing steps A to D, F and G are the same as those in the method for manufacturing a semiconductor device according to the embodiment 1, and therefore descriptions thereof will be omitted.
[0038] (Manufacturing process E-1) 9, before performing a heat treatment for activating impurities in the ion implantation region 3, a lower surface protection sacrificial film 17a of the two-layer surface protection sacrificial film 17 is first formed on the surface of the nitride semiconductor layer 2. The lower surface protection sacrificial film 17a functions to suppress thermal damage to the surface of the nitride semiconductor layer 2.
[0039] The PECVD method is used as a method for forming the lower surface protection sacrificial film 17a. A SiN film is used as the material for the lower surface protection sacrificial film 17a. This is because the SiN film functions to suppress the detachment of nitrogen atoms (N) from the nitride semiconductor layer 2 caused by damage during heat treatment. The SiN film constituting the lower surface protection sacrificial film 17a has a refractive index of 1.80 or more and less than 1.88, and a thickness of 30 nm or more.
[0040] (Manufacturing process E-2) Next, as shown in the cross-sectional view of Fig. 10, an upper-layer surface protection sacrificial film 17b is formed on the surface of the lower-layer surface protection sacrificial film 17a. As described above, the surface protection sacrificial film 17 is composed of two layers, the lower-layer surface protection sacrificial film 17a and the upper-layer surface protection sacrificial film 17b.
[0041] The upper surface protection sacrificial film 17b may be a film formed by any film forming method, such as sputtering and atomic layer deposition (ALD), but is not limited to these methods.
[0042] Materials constituting the upper surface protection sacrificial film 17b include a nitride film, an oxide film, etc., but are not limited to these films, and any film can be used. For example, an aluminum nitride (AlN) film formed by a sputtering method, an SiO film formed by a PECVD method, an aluminum oxide (AlO) film formed by an ALD method, etc. can be used without any problems. However, there is a restriction that the upper surface protection sacrificial film 17b is under excessive stress relative to the lower surface protection sacrificial film 17a, so that peeling of the film does not occur.
[0043] As described above, the thickness of the lower surface protection sacrificial film 17a must be 30 nm or more. The thickness of the entire surface protection sacrificial film 17 must be 100 nm or more and 500 nm or less. This thickness is necessary for the surface protection sacrificial film 17 to function as a film for suppressing the detachment of nitrogen atoms (N) from the surface of the nitride semiconductor layer 2 due to high-temperature treatment, but if the film thickness is too thick, the manufacturing cost will increase.
[0044] As described above, in the manufacturing method of the semiconductor device according to the second embodiment, a lower surface protection sacrificial film in contact with the surface of the nitride semiconductor layer after ion implantation is formed on the surface of the nitride semiconductor layer, the lower surface protection sacrificial film being made of a SiN film having a refractive index of 1.80 or more and less than 1.88 and a thickness of 30 nm or more, and the total thickness including the upper surface protection sacrificial film is 100 nm or more and 500 nm or less, so that it is possible to suppress thermal damage to the nitride semiconductor layer or detachment of nitrogen atoms (N), thereby preventing deterioration of the surface morphology of the nitride semiconductor layer and preventing formation of a damaged layer. Such effects further reduce the appearance failure rate of the semiconductor device, prevent initial malfunction of the semiconductor device, or improve reliability.
[0045] Embodiment 3 The method for manufacturing a semiconductor device according to the third embodiment differs from the method for manufacturing a semiconductor device according to the first embodiment in that a specific metal material is used as the material for source / drain electrodes 8. The following describes a method for manufacturing a semiconductor device according to the third embodiment. Note that manufacturing steps A to F are the same as those in the method for manufacturing a semiconductor device according to the first embodiment, and therefore descriptions thereof will be omitted.
[0046] (Manufacturing process G-1) After carrying out the above-mentioned manufacturing steps A to F, a transistor formation process is carried out by a general manufacturing method, including the formation of source / drain electrodes 8, the formation of gate electrode 9, the formation of first gate protective film 10 (first gate passivation) and second gate protective film 11 (second gate passivation), and the formation of wiring 12.
[0047] In forming the source / drain electrodes 8, the electrode material for the source / drain electrodes 8 does not include aluminum (Al)-based materials, and may be, for example, a metal material such as titanium (Ti), niobium (Nb), platinum (Pt), gold (Au), etc., or a combination of two or more of these metal materials.
[0048] In the case of source / drain electrodes 8 made of an Al-based material, even if the above-mentioned ion implantation process is not used, by using highly reactive Al as the electrode material, the Al mixes with the underlying nitride semiconductor layer 2 through heat treatment (ohmic sintering), making it possible to obtain good ohmic contact resistivity.
[0049] However, Al strongly mixes with the underlying nitride semiconductor layer 2 as well as with metal materials other than Al used to form the source / drain electrodes, raising concerns that this may cause surface roughening and contact failure of the source / drain electrodes 8. Therefore, it is desirable not to include Al-based materials as metal materials constituting the source / drain electrodes 8, i.e., to exclude them. This is because, when using the above-mentioned ion implantation process, if an Al-based material is selected as the electrode material for the source / drain electrodes 8, it is difficult to avoid surface roughening of the nitride semiconductor layer 2 itself.
[0050] In the method for manufacturing a semiconductor device according to the third embodiment, even when Al is not used as the metal material of the source / drain electrodes 8, the use of the above-mentioned ion implantation process makes it possible to prevent electrode roughness in the source / drain electrodes 8. Furthermore, the use of the above-mentioned ion implantation process makes it possible to prevent the surface roughness of the nitride semiconductor layer 2.
[0051] Therefore, in the method for manufacturing a semiconductor device according to the third embodiment, the metal material for the source / drain electrodes 8 does not include an Al-based material, and may be, for example, a metal material such as titanium (Ti), niobium (Nb), platinum (Pt), gold (Au), or a combination of two or more of these metal materials.
[0052] Although the present disclosure describes various exemplary embodiments and examples, the various features, aspects, and functions described in one or more embodiments are not limited to application to a particular embodiment, but may be applied to the embodiments alone or in various combinations.
[0053] Therefore, countless modifications not exemplified are assumed within the scope of the technology disclosed in the present specification, including, for example, modifying, adding, or omitting at least one component, and further, extracting at least one component and combining it with a component of another embodiment. [Explanation of symbols]
[0054] REFERENCE SIGNS LIST 1 substrate, 2 nitride semiconductor layer, 3 ion implantation region, 4 source / drain electrode formation region, 5 through implantation film, 6 resist mask, 7, 17 surface protection sacrificial film, 8 source / drain electrode, 8a source electrode, 8b drain electrode, 9 gate electrode, 10 first gate protection film, 11 second gate protection film, 12 wiring, 17a lower surface protection sacrificial film, 17b upper surface protection sacrificial film, 100 nitride semiconductor transistor
Claims
1. A step of ion-implanting impurities into a source / drain electrode formation region in which a source electrode and a drain electrode are to be formed in a nitride semiconductor layer formed on a substrate; forming a silicon nitride film having a refractive index of 1.80 or more and less than 1.88 and a thickness of 100 nm or more and 500 nm or less as a surface protection sacrificial film on a surface of the nitride semiconductor layer by plasma chemical vapor deposition; a step of heat-treating the nitride semiconductor layer on which the surface protective sacrificial film has been formed; A method for manufacturing a semiconductor device comprising the steps of:
2. A step of ion-implanting impurities into a source / drain electrode formation region in which a source electrode and a drain electrode are to be formed in a nitride semiconductor layer formed on a substrate; forming a silicon nitride film having a refractive index of 1.80 or more and less than 1.88 and a thickness of 30 nm or more on a surface of the nitride semiconductor layer by plasma chemical vapor deposition as the lower surface protection sacrificial film of a surface protection sacrificial film consisting of two layers, an upper surface protection sacrificial film and a lower surface protection sacrificial film; forming the upper-layer surface protection sacrificial film laminated on the lower-layer surface protection sacrificial film, the sum of the film thickness of the upper-layer surface protection sacrificial film and the film thickness of the lower-layer surface protection sacrificial film being 100 nm or more and 500 nm or less; a step of heat-treating the nitride semiconductor layer on which the surface protective sacrificial film has been formed; A method for manufacturing a semiconductor device comprising the steps of:
3. 3. The method for manufacturing a semiconductor device according to claim 1, wherein the heat treatment is performed at a temperature of 1000[deg.] C. or more and 1200[deg.] C. or less.
4. 4. The method for manufacturing a semiconductor device according to claim 1, wherein the source electrode and the drain electrode are made of an electrode material that does not contain aluminum.
5. 5. The method for manufacturing a semiconductor device according to claim 4, wherein the electrode material is made of one of titanium, niobium, platinum and gold, or a combination of two or more of them.
6. 6. The method for manufacturing a semiconductor device according to claim 1, wherein the surface protection sacrificial film is removed by wet etching.
Citation Information
Patent Citations
Method of manufacturing semiconductor element, and semiconductor element
JP2010109276A
Heterojunction field effect transistor and method of manufacturing the same
JP2012114242A
Semiconductor device and semiconductor device manufacturing method
JP2015037105A
Semiconductor device and method of manufacturing semiconductor device
JP2017079287A
Semiconductor device manufacturing method and semiconductor device
JP2017079288A