Semiconductor film and method for producing same
By optimizing gas flow and positioning in the HVPE apparatus, the method reduces killer defects in β-Ga2O3 semiconductor films, leading to high-yield semiconductor devices with superior electrical characteristics.
Patent Information
- Application Number
- JP2020072460
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-04-14
AI Technical Summary
HVPE-based β-Ga2O3 single crystal films suffer from killer defects that significantly degrade device characteristics, and the causes and methods to reduce these defects have not been adequately addressed.
A method for manufacturing β-Ga2O3 semiconductor films involves controlling the flow direction and positioning of gases in the HVPE apparatus, such as Ga chloride, oxygen-containing, and dopant-containing gases, to minimize the formation and adherence of Ga oxide grains on the substrate, thereby reducing killer defects.
The method results in β-Ga2O3 semiconductor films with reduced killer defects, enabling the production of semiconductor devices with improved forward current and reverse leakage characteristics, such as Schottky barrier diodes, with high yield and excellent performance.
Smart Images

Figure 0007580708000001 
Figure 0007580708000002 
Figure 0007580708000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor film and a method for manufacturing the same. [Background technology]
[0002] Conventionally, a technique for growing a β-Ga2O3-based single crystal film by the HVPE (Halide Vapor Phase Epitaxy) method is known (see, for example, Patent Document 1). According to the technique described in Patent Document 1, a gallium source gas, an oxygen source gas, and a dopant source gas are flowed into an area in which a Ga2O3-based substrate is placed in a reaction chamber of a vapor phase growth apparatus, and a β-Ga2O3-based single crystal film is epitaxially grown on the Ga2O3-based substrate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5984069 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when growing a β-Ga2O3-based single crystal film by HVPE, there is a problem that killer defects, which are severe defects that significantly degrade device characteristics, are more likely to occur than when growing single crystal films of other nitride semiconductors such as GaN by HVPE. Until now, the cause of killer defects and methods for reducing them have not been clarified.
[0005] Therefore, an object of the present invention is to provide a semiconductor film made of β-Ga2O3-based single crystal with few killer defects, and a method for manufacturing the same. [Means for solving the problem]
[0006] In order to achieve the above object, one aspect of the present invention provides the following semiconductor film manufacturing methods [1] to [4] and the following semiconductor film [5].
[0007] [1] A method for epitaxially growing a semiconductor film made of a β-Ga2O3-based single crystal on the growth surface of the semiconductor substrate by injecting Ga chloride gas, oxygen-containing gas, and dopant-containing gas into a space in the reaction chamber in which the semiconductor substrate is placed, the method comprising the steps of: placing a semiconductor substrate made of a β-Ga2O3-based single crystal in a reaction chamber of an HVPE apparatus with a growth surface facing upward or downward; and epitaxially growing a semiconductor film made of a β-Ga2O3-based single crystal on the growth surface of the semiconductor substrate by injecting Ga chloride gas, oxygen-containing gas, and dopant-containing gas into the space in which the semiconductor substrate is placed, the method comprising the steps of: a position of the inlet of the Ga chloride gas into the space is higher than a position of the inlet of the oxygen-containing gas into the space, and a position of the inlet of the Ga chloride gas into the space is higher than a position of the inlet of the dopant-containing gas into the space, and when the semiconductor substrate is placed with the growth base surface facing downward, a position of the inlet of the dopant-containing gas into the space is higher than a position of the inlet of the Ga chloride gas into the space, and a position of the inlet of the oxygen-containing gas into the space is higher than a position of the inlet of the dopant-containing gas into the space. [2] The method for producing a semiconductor film according to [1] above, wherein the Ga chloride gas is GaCl gas, the oxygen-containing gas is O2 gas, and the dopant-containing gas is SiCl4 gas. [3] The method for manufacturing a semiconductor film according to [1] or [2] above, wherein in the step of placing the semiconductor substrate, the semiconductor substrate is placed in the reaction chamber with the growth surface facing downward. [4] The method for producing a semiconductor film according to [3] above, wherein in the step of epitaxially growing the semiconductor film, the Ga chloride gas, the oxygen-containing gas, and the dopant-containing gas are flowed into the space at a flow rate of 110 cm / s or more. [5] It consists of β-Ga2O3-based single crystals containing Cl. The thickness is 1000 nm to 1000 μm, and is measured by emission microscopy using a circular anode electrode with a diameter of 500 μm formed on the surface. The in-plane density of defects that continue from the front to the back in the thickness direction is 10 / cm 2The semiconductor film is as follows: Effect of the Invention
[0008] According to the present invention, it is possible to provide a semiconductor film made of a β-Ga2O3-based single crystal with few killer defects and a method for manufacturing the same. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a vertical sectional view of a crystal layered structure according to a first embodiment of the present invention. [Diagram 2] Fig. 2(a) is a schematic diagram showing the placement of the semiconductor substrate 10 and the introduction positions of the source gas according to the first embodiment of the present invention, and Fig. 2(b) is a schematic diagram showing the placement of the semiconductor substrate 10 and the introduction positions of the source gas according to a comparative example. [Diagram 3] FIG. 3 is a schematic diagram showing a placement state of a semiconductor substrate 10 and an introduction position of a source gas according to the second embodiment of the present invention. [Figure 4] Fig. 4(a) is an emission microscope image of a semiconductor film formed by the method according to the second embodiment, and Fig. 4(b) is an emission microscope image of a semiconductor film formed by a conventional method as a comparative example. [Diagram 5] Fig. 5(a) is an optical microscope image of the surface of a semiconductor film formed by the method according to the second embodiment, on which etch pits appear, and Fig. 5(b) is an optical microscope image of the surface of a semiconductor film formed by a conventional method, on which etch pits appear, as a comparative example. [Figure 6] FIG. 6 is a vertical cross-sectional view of a Schottky barrier diode used for evaluating the characteristics of the Schottky barrier diode described later. [Figure 7] Fig. 7(a) is a graph showing the reverse leakage characteristics of a Schottky barrier diode having a semiconductor film formed by the method according to the first embodiment, and Fig. 7(b) is a graph showing the reverse leakage characteristics of a Schottky barrier diode having a semiconductor film formed by the method according to the second embodiment. [Figure 8] FIG. 8 is a graph showing the reverse leakage characteristics of a Schottky barrier diode including a semiconductor film formed by a conventional method as a comparative example. [Figure 9] 9(a) to 9(c) are diagrams showing the distribution of breakdown voltage characteristics of Schottky barrier diodes on a 2-inch wafer before being divided into individual Schottky barrier diodes each having a semiconductor film formed by the method according to the second embodiment. [Figure 10] 10(a) and (b) are graphs showing the reverse and forward characteristics, respectively, of a Schottky barrier diode having a semiconductor film formed by the method according to the second embodiment and a square anode electrode measuring 2.3 mm on each side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In order to investigate the cause of killer defects that occur in β-Ga2O3-based single crystal films grown by the HVPE method, the inventors grew β-Ga2O3 single crystal films by a conventional method using the HVPE method, fabricated multiple Schottky barrier diodes with different element sizes, and evaluated their reverse breakdown voltage characteristics.
[0011] As a result, when the element size (the size of the circular anode electrode) was 400 μm or less in diameter, elements with near-ideal characteristics in which reverse leakage current was suppressed could be obtained with a yield of about 80%. However, as the element size increased, the number of elements with large reverse leakage current increased, and the yield for elements with a diameter of 1 mm was almost 0%.
[0012] Since the element characteristics depend on the element size, it was presumed that killer defects exist in the crystal film. Based on the yield and the area of the anode electrode, the killer defect density in the β-Ga2O3 crystal film grown by the conventional method was 200 / cm 2The killer defect density has a direct effect on the size of elements that can be manufactured, i.e., the maximum current rating of the device, and with β-Ga2O3 crystal films manufactured by conventional methods, it was only possible to manufacture Schottky barrier diodes with a rated current (current value when a forward voltage of about 1.5 to 2.5 V is applied) of approximately 1 A or less.
[0013] As a result of intensive research, the inventors have found that the main cause of killer defects in β-Ga2O3-based crystal films is Ga oxide particles formed in the gas phase in the reaction chamber of the HVPE device. In the growth of β-Ga2O3-based single crystal films by the HVPE method, the reaction rate between oxygen and Ga chloride gas is very fast, so a reaction occurs in the gas phase to form Ga oxide particles, which then adhere to the Ga2O3-based substrate. When these Ga oxide particles are incorporated into the epitaxially grown β-Ga2O3-based single crystal film, the periodicity of the crystal is disturbed, and as a result, many killer defects that can become leak paths are generated in the thickness direction of the film, from the front surface to the back surface.
[0014] It has been confirmed that when GaN-based crystal films are grown by the HVPE method, many killer defects do not occur, as occurs when β-Ga2O3-based crystal films are grown. This is thought to be because the reaction rate between ammonia gas and Ga chloride gas is relatively slow, so there is almost no generation of GaN-based compound particles in the gas phase.
[0015] The present invention relates to a method for manufacturing a semiconductor film made of β-Ga2O3-based single crystal, which is formed in the gas phase in a reaction chamber of an HVPE apparatus, and which can reduce the amount of Ga oxide particles adhering to a Ga2O3-based substrate and reduce killer defects, and to a semiconductor film made of β-Ga2O3-based single crystal with few killer defects manufactured by the manufacturing method.
[0016] First Embodiment (Structure of Crystalline Layer Structure) FIG. 1 is a vertical cross-sectional view of a crystal laminate structure 1 according to a first embodiment of the present invention. The crystal laminate structure 1 includes a semiconductor substrate 10 made of a β-Ga2O3 single crystal, and a semiconductor film 12 made of a β-Ga2O3 single crystal formed by epitaxial crystal growth on a growth bottom surface 11 of the semiconductor substrate 10.
[0017] Here, the β-Ga2O3 single crystal refers to a β-Ga2O3 single crystal having a β-type crystal structure, or a β-Ga2O3 single crystal to which an element such as Al or In is added. For example, it may be a (Ga x Al y In (1-x-y) )2O3 (0 < x ≤ 1, 0 ≤ y ≤ 1, 0 < x + y ≤ 1) single crystal. When Al is added, the bandgap widens, and when In is added, the bandgap narrows. Further, the semiconductor substrate 10 may contain a dopant such as Si.
[0018] The plane orientation of the growth bottom surface 11 of the semiconductor substrate 10 is, for example, (001), (010), (100), (011), (-201), or (101).
[0019] The semiconductor substrate 10 is formed, for example, by slicing a bulk crystal of a Ga2O3 single crystal grown by a melt growth method such as the FZ (Floating Zone) method or the EFG (Edge Defined Film Fed Growth) method and polishing the surface.
[0020] The semiconductor film 12 contains, as dopants, Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, Ba, Sc, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Re, Fe, Ru, Os, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Hg, B, Al, In, Tl, C, Si, Ge, Sn, Pb, N, P, As, Sb, Bi, S, Se, Te, etc., which are doped in parallel with the crystal growth.
[0021] The concentration of the dopant contained in the semiconductor film 12 is, for example, 1×10 13 atoms / cm 3 5×10 or more 20 atoms / cm 3 Preferably, it is 6.5×10 or less. 15 atoms / cm 3 More than 2.1×10 20 atoms / cm 3 The carrier density generated by adding a dopant is, for example, 1x10 15 cm -3 Over 1x10 20 cm -3 The following is the result.
[0022] The semiconductor film 12 has a concentration of 5×10 16 atoms / cm 3 This is because the semiconductor film 12 is formed by the HVPE method using a Cl-containing gas. Normally, when a β-Ga2O3-based single crystal film is formed by a method other than the HVPE method, a Cl-containing gas is not used, so the β-Ga2O3-based single crystal film does not contain Cl, and at least 1×10 16 cm -3 It will never contain more than 100 Cl.
[0023] In addition, the semiconductor film 12 can be formed thick, for example, to a thickness of 1000 nm or more, because it is formed by the HVPE (Halide Vapor Phase Epitaxy) method, which has a high crystal growth rate. The growth rate of a β-Ga2O3-based single crystal film by industrial HVPE is generally 200 μm / h, and in this case, a film can be formed in a realistic time if the thickness is up to 1000 μm. That is, the semiconductor film 12 can be formed to a thickness of 1000 nm or more and 1000 μm or less. Note that the crystal growth rate of a β-Ga2O3-based single crystal film when the MBE method is used is about 120 nm / h, and it takes 8 hours or more to form a film to a thickness of 1000 nm or more, which is not realistic in the production field.
[0024] In addition, the in-plane density of killer defects that continue from the front surface to the back surface in the thickness direction of the semiconductor film 12 is 10 / cm according to the manufacturing method of the semiconductor film 12 described later. 2 The in-plane density of killer defects contained in the semiconductor film 12 can be measured by observing the semiconductor film 12 with an emission microscope under the condition of an anode bias of −200V.
[0025] (Structure of HVPE equipment) An example of the structure of an HVPE apparatus used to grow the semiconductor film 12 according to the first embodiment of the present invention will be described below.
[0026] The method for manufacturing a semiconductor film according to the first embodiment of the present invention uses an HVPE apparatus 2 whose vertical cross sections are shown in Figures 2(a) and (b). The HVPE apparatus 2 is a vapor phase growth apparatus for the HVPE method, and has a space 24 in which a semiconductor substrate 10 is placed, and a reaction chamber 20 having a first gas introduction port 21, a second gas introduction port 22, and a third gas introduction port 23 for introducing source gases for growing a semiconductor film 12 into the space 24. The reaction chamber 20 is made of, for example, quartz glass.
[0027] The HVPE apparatus 2 also has a heating means (not shown) that is installed around the reaction chamber 20 and heats the space 24 within the reaction chamber 20. This heating means is, for example, a resistance heating type or radiation heating type heating device.
[0028] In the reaction chamber 20, source gases for growing the semiconductor film 12 are introduced into a space 24 through a first gas introduction port 21, a second gas introduction port 22, and a third gas introduction port .
[0029] The inlet 21a of the first gas introduction port 21 into the space 24, the inlet 22a of the second gas introduction port 22 into the space 24, and the inlet 23a of the third gas introduction port 23 into the space 24 are different in height (position in a direction perpendicular to the growth base surface 11 of the placed semiconductor substrate 10), with the inlet 22a being disposed above the inlet 23a and the inlet 21a being disposed above the inlet 22a. In addition, in order to prevent variation in the state of the semiconductor film 12 in the in-plane direction of the growth base surface 11, the horizontal positions (position in a direction perpendicular to the paper surface of FIG. 2) of the inlets 21a, 22a, and 23a in a direction perpendicular to the traveling direction of the source gas are substantially equal.
[0030] The raw material gas for growing the semiconductor film 12 includes a gallium raw material gas which is a Ga chloride gas such as GaCl gas, GaCl2 gas, GaCl3 gas, or (GaCl3)2 gas, an oxygen raw material gas which is an oxygen-containing gas such as O2 gas or H2O gas, and a dopant raw material gas which is a dopant-containing gas such as SiCl4 gas, GeCl4 gas, SnCl4 gas, or PbCl2 gas.
[0031] Each source gas is flowed into the reaction chamber 20 using an inert gas such as Ar gas or N2 gas as a carrier gas.
[0032] (Method of manufacturing semiconductor film) The method for manufacturing a semiconductor film 12 according to the first embodiment of the present invention includes the steps of placing a semiconductor substrate 10 made of a β-Ga2O3-based single crystal in a reaction chamber 20 of an HVPE apparatus 2, and flowing Ga chloride gas, an oxygen-containing gas, and a dopant-containing gas into a space 24 in the reaction chamber 20 in which the semiconductor substrate 10 is placed, to epitaxially grow a semiconductor film 12 made of a β-Ga2O3-based single crystal on a growth base surface 11 of the semiconductor substrate 10.
[0033] In this embodiment, the semiconductor substrate 10 is placed on the bottom side of the space 24 in the reaction chamber 20 with the growth base surface 11 facing upward. Here, the growth base surface 11 facing upward refers to a state in which the growth base surface 11 faces the opposite side to the earth's surface and the angle that the growth base surface 11 makes with the horizontal plane is in the range of -5 to +5 degrees.
[0034] The Ga chloride gas, oxygen-containing gas, and dopant-containing gas flowing in from the inlets 21a, 22a, and 23a are mixed in the space 24. Then, the growth surface 11 of the semiconductor substrate 10 is exposed to the mixed gas, and the semiconductor film 12 is epitaxially grown.
[0035] In the step of epitaxially growing the semiconductor film 12, the pressure in the space 24 is maintained at, for example, 1 atm. In addition, in order to grow the semiconductor film 12, the growth temperature must be 900° C. or higher. If the temperature is lower than 900° C., there is a risk that a single crystal will not be obtained.
[0036] Here, it is preferable to use GaCl gas as the Ga chloride gas, which is the raw material gas for gallium. Among Ga chloride gases, GaCl gas is a gas that can maintain the driving force for the growth of Ga2O3 crystals up to the highest temperature. In order to obtain high-purity, high-quality Ga2O3 crystals, growth at a high growth temperature is effective, so it is preferable to use GaCl gas, which has a high driving force for growth at high temperatures.
[0037] In addition, as the dopant-containing gas, which is the source gas of the dopant, it is preferable to use a chloride-based gas in order to suppress the inclusion of other unintended impurities, and for example, when the dopant is Si, Ge, Sn, or Pb, which is a group 14 element among the above-mentioned dopants, a chloride-based gas such as SiCl4, GeCl4, SnCl4, or PbCl2 is used. In addition, the chloride-based gas is not limited to a gas that is compounded with only chlorine, and for example, a silane-based gas such as SiHCl3 may be used.
[0038] Dopants such as Si are doped in parallel with the growth of the β-Ga2O3-based single crystal.
[0039] Furthermore, if the atmosphere in which the semiconductor film 12 is grown contains hydrogen, the flatness of the surface of the semiconductor film 12 and the driving force for crystal growth will decrease, so it is preferable to use O2 gas that does not contain hydrogen as the oxygen-containing gas, which is the source gas for oxygen.
[0040] The method for manufacturing a semiconductor film 12 according to the first embodiment of the present invention is characterized by the positional relationship between the semiconductor substrate 10 and the inlets for the gallium source gas, oxygen source gas, and dopant source gas within the reaction chamber 20 of the HVPE apparatus 2.
[0041] Fig. 2(a) is a schematic diagram showing the placement of the semiconductor substrate 10 and the introduction positions of the source gas according to the first embodiment of the present invention, and Fig. 2(b) is a schematic diagram showing the placement of the semiconductor substrate 10 and the introduction positions of the source gas according to a comparative example.
[0042] In the first embodiment of the present invention, as shown in FIG. 2(a), Ga chloride gas and a carrier gas (GaCl gas and Ar gas are shown as examples) are introduced into the first gas introduction port 21, a dopant-containing gas and a carrier gas (SiCl4 gas and Ar gas are shown as examples) are introduced into the second gas introduction port 22, and an oxygen-containing gas and a carrier gas (O2 gas and Ar gas are shown as examples) are introduced into the third gas introduction port 23.
[0043] On the other hand, in the comparative example shown in Figure 2(b), similar to the conventional method of growing β-Ga2O3-based single crystals by HVPE, an oxygen-containing gas and a carrier gas (O2 gas and Ar gas are shown as examples) are introduced from the first gas introduction port 21, a dopant-containing gas and a carrier gas (SiCl4 gas and Ar gas are shown as examples) are introduced from the second gas introduction port 22, and Ga chloride gas and a carrier gas (GaCl gas and Ar gas are shown as examples) are introduced from the third gas introduction port 23.
[0044] As a result of extensive research, the inventors of the present invention have found that by setting the source gas introduction position at the position shown in Fig. 2(a), the number of killer defects contained in the growing semiconductor film 12 is reduced compared to when the position is set at the position shown in Fig. 2(b). It is believed that by making it easiest for the oxygen-containing gas to reach the growth substrate 11 and making it most difficult for the Ga chloride gas to reach the growth substrate 11, the amount of Ga oxide particles that are generated in the gas phase and adhere to the growth substrate 11 for some reason is reduced.
[0045] That is, when the semiconductor substrate 10 is placed with the growth surface 11 facing upward, the position of the inlet of the dopant-containing gas into the space 24 is made higher than the position of the inlet of the oxygen-containing gas into the space 24, and the position of the Ga chloride gas inlet into the space 24 is made higher than the position of the dopant-containing gas inlet into the space 24, thereby reducing the number of killer defects contained in the growing semiconductor film 12.
[0046] Second Embodiment The second embodiment of the present invention is different from the first embodiment in the orientation of the semiconductor substrate 10 placed in the reaction chamber 20 of the HVPE apparatus 2. Note that the description of the same points as those in the first embodiment may be omitted or simplified.
[0047] (Method of manufacturing semiconductor film) In the method for manufacturing a semiconductor film 12 according to the second embodiment of the present invention, the semiconductor substrate 10 is placed on the upper surface side of the space 24 in the reaction chamber 20 with the growth surface 11 facing downward. Here, the growth surface 11 facing downward refers to a state in which the growth surface 11 faces toward the earth's surface and the angle that the growth surface 11 makes with the horizontal plane is in the range of -5 to +5 degrees.
[0048] FIG. 3 is a schematic diagram showing a placement state of a semiconductor substrate 10 and an introduction position of a source gas according to the second embodiment of the present invention.
[0049] In the second embodiment of the present invention, as shown in FIG. 3, the semiconductor substrate 10 is placed so that the growth surface 11 faces downward, and therefore an oxygen-containing gas and a carrier gas (O2 gas and Ar gas are shown as examples) are introduced from the first gas introduction port 21, a dopant-containing gas and a carrier gas (SiCl4 gas and Ar gas are shown as examples) are introduced from the second gas introduction port 22, and Ga chloride gas and a carrier gas (GaCl gas and Ar gas are shown as examples) are introduced from the third gas introduction port 23.
[0050] That is, the position of the inlet of the dopant-containing gas into the space 24 is set higher than the position of the inlet of the Ga chloride gas into the space 24, and the position of the inlet of the oxygen-containing gas into the space 24 is set higher than the position of the inlet of the dopant-containing gas into the space 24. This makes it easiest for the oxygen-containing gas to reach the growth substrate 11 and most difficult for the Ga chloride gas to reach the growth substrate 11, thereby reducing the number of killer defects contained in the growing semiconductor film 12.
[0051] Furthermore, since the Ga oxide grains generated in the gas phase move downward due to gravity, by placing the semiconductor substrate 10 so that the growth base surface 11 faces downward, the Ga oxide grains are less likely to adhere to the growth base surface 11. Therefore, according to the semiconductor film manufacturing method of the present embodiment, it is possible to further reduce the number of killer defects contained in the semiconductor film 12 compared to the semiconductor film manufacturing method of the first embodiment.
[0052] As mentioned above, when growing a GaN-based crystal film by HVPE, the reaction rate between ammonia gas and Ga chloride gas is relatively slow, so that GaN compound particles are hardly generated in the gas phase. Therefore, when growing a GaN-based crystal film, many killer defects are not generated as in the case of growing a β-Ga2O3-based crystal film, and there is almost no effect of reducing killer defects by facing the growth surface of the substrate downward. There is a known technology for growing a GaN-based crystal film by HVPE with the growth surface of the substrate facing downward (Patent Publication No. 3376809), but this is intended to grow a uniform thin film by suppressing the generation of thermal convection of the source gas near the substrate.
[0053] It has also been confirmed that when the semiconductor substrate 10 is placed so that the growth surface 11 faces downward, the dopant incorporation rate is higher than when the semiconductor substrate 10 is placed so that the growth surface 11 faces upward. By placing the semiconductor substrate 10 so that the growth surface 11 faces downward, the donor concentration in the semiconductor film 12 becomes approximately equal to the amount of dopant charged, making it easier to control the donor concentration.
[0054] Furthermore, by increasing the flow rates of the Ga chloride gas, the oxygen-containing gas, and the dopant-containing gas, it becomes easier to wash away the Ga oxide particles generated in the gas phase by these source gases, and therefore the amount of Ga oxide particles adhering to the growth substrate surface 11 can be reduced.
[0055] For example, when growing the semiconductor film 12 on a circular semiconductor substrate 10 having a diameter of 2 inches, the number of killer defects contained in the semiconductor film 12 can be significantly reduced by flowing the Ga chloride gas, oxygen-containing gas, and dopant-containing gas into the space 24 at a flow rate of 110 cm / s or more, and can be further reduced by flowing the gases into the space 24 at a flow rate of 165 cm / s or more.
[0056] (Effects of the embodiment) According to the above embodiment, it is possible to reduce the amount of Ga oxide particles formed in the gas phase in the reaction chamber of the HVPE apparatus and adhering to the semiconductor substrate 10, and to reduce killer defects in the semiconductor film 12 made of a β-Ga2O3-based single crystal. By using the semiconductor film 12 with fewer killer defects, it is possible to manufacture semiconductor devices with excellent characteristics, for example, Schottky barrier diodes with excellent forward current characteristics and reverse leakage current characteristics, with a high yield. EXAMPLES
[0057] Fig. 4(a) is an emission microscope observation image of a semiconductor film 12 formed by the method according to the second embodiment illustrated in Fig. 3. Fig. 4(b) is an emission microscope observation image of a semiconductor film as a comparative example formed by the conventional method illustrated in Fig. 2(b).
[0058] The emission microscope images in Figures 4(a) and (b) were obtained by forming anode electrodes and cathode electrodes on the surface of semiconductor film 12 and the surface of semiconductor substrate 10, respectively, so that they do not overlap each other, and photographing the area where the anode electrodes are formed from the semiconductor substrate 10 side with a CCD camera. The images are a superposition of a pattern image of a circular anode electrode with a diameter of 500 μm, photographed by irradiating light with no voltage applied between the two electrodes, and an emission image photographed with a reverse voltage of 200 V (positive voltage on the cathode electrode side and negative voltage on the anode electrode side) applied between the two electrodes.
[0059] The black dots seen in the circle in Figure 4(b) are leak paths that emit light when a reverse voltage is applied, and indicate the location of the killer defect that becomes the leak path. The emission microscope image in Figure 4(a) does not show as many conspicuous light-emitting points as in the emission microscope image in Figure 4(b), and when the density of the light-emitting points was estimated using multiple anode electrodes, it was found to be 10 / cm 2 That is, the density of killer defects in the semiconductor film 12 according to the second embodiment was 10 / cm 2 The results were as follows.
[0060] Fig. 5(a) is an optical microscope image of the surface on which etch pits appear of the semiconductor film 12 formed by the method according to the second embodiment illustrated in Fig. 3. Fig. 5(b) is an optical microscope image of the surface on which etch pits appear of the semiconductor film as a comparative example formed by the conventional method illustrated in Fig. 2(b).
[0061] Etch pits are depressions that occur when etching a crystal surface due to the difference in etching rate between defective and other parts, and observing the etch pits makes it possible to know the location and density of defects. The etch pits shown in Figures 5(a) and (b) were formed by immersing a semiconductor film 12 grown on a semiconductor substrate 10 in hot phosphoric acid for one hour.
[0062] According to the observation image of FIG. 5(b), the etch pit density of the semiconductor film of the comparative example is approximately 10,000 / cm 2 On the other hand, according to the observation image of FIG. 5(a), the etch pit density of the semiconductor film 12 was about 2500 / cm 2 This was approximately 1 / 4 of the etch pit density of the semiconductor film of the comparative example.
[0063] FIG. 6 is a vertical cross-sectional view of a Schottky barrier diode 3 used for evaluating the characteristics of the Schottky barrier diode described later.
[0064] The Schottky barrier diode 3 has an effective carrier concentration (donor concentration N d to the acceptor concentration N a minus) is approximately 1 × 10 18 / cm 3 The semiconductor substrate 10 is made of a β-Ga2O3 single crystal having a thickness of about 600 μm, and the effective carrier concentration is about 1×10 16 / cm 3 The semiconductor device includes a semiconductor film 12 made of a β-Ga2O3 single crystal having a thickness of approximately 6 μm, an anode electrode 31 having a Ni / Au laminated structure formed on the surface of the semiconductor film 12, and a cathode electrode 32 having a Ti / Ni / Au laminated structure formed on the entire surface of the semiconductor substrate 10.
[0065] Fig. 7(a) is a graph showing the reverse leakage characteristics of a Schottky barrier diode 3 including a semiconductor film 12 formed by the method according to the first embodiment described in Fig. 2(a). Fig. 7(b) is a graph showing the reverse leakage characteristics of a Schottky barrier diode 3 including a semiconductor film 12 formed by the method according to the second embodiment described in Fig. 3. Fig. 8 is a graph showing the reverse leakage characteristics of a Schottky barrier diode 3 including a semiconductor film as a comparative example formed by the conventional method described in Fig. 2(b) instead of the semiconductor film 12.
[0066] The anode electrode 31 of the Schottky barrier diode 3 according to FIGS. 7(a), 7(b) and 8 is a circular electrode having a diameter of 500 μm.
[0067] In Fig. 7(a), (b), and Fig. 8, when a voltage of -200 V is applied to the anode electrode, the magnitude of the leakage current is 1×10 -4 A / cm 2 "Good" is below 1×10 -4 A / cm 2 Anything above this is marked as “Bad.”
[0068] If the yield is defined as the proportion of "Good" out of the total, the yield of the Schottky barrier diodes 3 having the semiconductor film 12 formed by the method according to the first embodiment illustrated in FIG. 2(a) was 78%, the yield of the Schottky barrier diodes 3 having the semiconductor film 12 formed by the method according to the second embodiment illustrated in FIG. 3 was 89%, and the yield of the Schottky barrier diodes 3 having a semiconductor film as a comparative example formed by the conventional method illustrated in FIG. 2(b) was 11%.
[0069] 9(a) to 9(c) are diagrams showing the distribution of breakdown voltage characteristics of Schottky barrier diodes 3 in a 2-inch wafer (a crystalline laminated structure 1 having a plurality of anode electrodes 31 and cathode electrodes 32 formed thereon) before being diced into individual Schottky barrier diodes 3 having semiconductor films 12 formed by the method according to the second embodiment illustrated in FIG.
[0070] 9(a) to (c) are views of the semiconductor film 12 of the wafer viewed vertically from above, with the values shown indicating the withstand voltage of the Schottky barrier diode 3 at that location (the voltage when a leakage current of 1 μA flows), and negative values indicating reverse voltage. Note that since the measurement limit for withstand voltage is -200V, the withstand voltage of the Schottky barrier diode 3 at the "-200" location in the figure is -200V or less. It can be determined that the Schottky barrier diode 3 at the "-200" location in the figure has sufficient withstand voltage.
[0071] The semiconductor film 12 in Fig. 9(a) was grown by flowing source gases (Ga chloride gas, oxygen-containing gas, and dopant-containing gas) into the space 24 at a flow rate of 55 cm / s, the semiconductor film 12 in Fig. 9(b) was grown by flowing source gases into the space 24 at a flow rate of 110 cm / s, and the semiconductor film 12 in Fig. 9(c) was grown by flowing source gases into the space 24 at a flow rate of 165 cm / s. The directions of the arrows in the figures indicate the flow directions of the source gases.
[0072] 9(a) to (c) show that the higher the flow rate of the source gas, the larger the area in the wafer where Schottky barrier diodes 3 with excellent breakdown voltage can be obtained. This is believed to be because the higher the flow rate of the source gas, the easier it is to sweep away the Ga oxide particles generated in the gas phase, reducing the amount of Ga oxide particles adhering to the growth base surface 11 and reducing killer defects in the semiconductor film 12.
[0073] 9(a) to (c), when the diameter of the wafer is 2 inches, the number of killer defects in the semiconductor film 12 can be significantly reduced by flowing the source gas into the space 24 at a flow velocity of 110 cm / s or more, and can be further reduced by flowing the source gas into the space 24 at a flow velocity of 165 cm / s or more.
[0074] However, as the flow rate of the source gas is increased, the amount of source gas that flows away without contributing to the growth of the semiconductor film 12 increases, decreasing the efficiency of use of the source gas and ultimately increasing the manufacturing cost of the semiconductor film 12. For this reason, it is preferable to set the upper limit of the flow rate to a value that allows a Schottky barrier diode 3 with excellent withstand voltage to be obtained over the entire region of the wafer.
[0075] Furthermore, when the size of the wafer from which the Schottky barrier diodes 3 are cut is increased, the flow rate of the source gas can be further increased to ensure a wide region in which Schottky barrier diodes 3 with excellent pressure resistance can be obtained. For example, when forming a wafer with a diameter of 4 inches, the flow rate of the source gas can be doubled compared to when forming a wafer with a diameter of 2 inches. By injecting the source gas into the space 24 at a flow rate of 220 cm / s or more, the number of killer defects contained in the semiconductor film 12 can be significantly reduced, and by injecting the source gas into the space 24 at a flow rate of 330 cm / s or more, the number of killer defects can be further reduced.
[0076] 10(a) and 10(b) are graphs showing the reverse and forward characteristics of a Schottky barrier diode 3 having a semiconductor film 12 formed by the method according to the second embodiment described in FIG. 3 and a square anode electrode 31 of 2.3 mm on each side. The dotted line in FIG. 10(a) indicates the measurement limit. The forward characteristics in FIG. 10(b) were measured by applying a pulse voltage with a pulse width of 1 ms.
[0077] Figure 10(a) shows that excellent reverse leakage characteristics were obtained, with the leakage current being less than 1 μA even when the applied voltage was -460 V. Figure 10(b) shows that a current of 10 A or more flows when the applied voltage is 2.1 V or higher, indicating that excellent large current characteristics are obtained.
[0078] Although the embodiment and examples of the present invention have been described above, the present invention is not limited to the above embodiment and examples, and various modifications are possible without departing from the spirit of the invention. Furthermore, the components of the above embodiment and examples can be combined in any manner without departing from the spirit of the invention.
[0079] In addition, the above-described embodiments and examples do not limit the scope of the invention according to the claims. It should be noted that not all of the combinations of features described in the embodiments and examples are necessarily essential to the means for solving the problems of the invention. [Explanation of symbols]
[0080] REFERENCE SIGNS LIST 1...crystalline laminated structure, 2...HVPE apparatus, 3...Schottky barrier diode, 10...semiconductor substrate, 11...growth surface, 12...semiconductor film, 20...reaction chamber, 21...first gas inlet port, 22...second gas inlet port, 23...third gas inlet port, 24...space, 31...anode electrode, 32...cathode electrode
Claims
1. In the reaction chamber of the HVPE apparatus, β-Ga is placed with the growth surface facing upward or downward. 2 O 3 providing a semiconductor substrate made of a GaN-based single crystal; Ga chloride gas, oxygen-containing gas, and dopant-containing gas are introduced into the reaction chamber in a space in which the semiconductor substrate is placed, and β-Ga is grown on the growth surface of the semiconductor substrate. 2 O 3 epitaxially growing a semiconductor film made of a nitride-based single crystal; Including, When the semiconductor substrate is placed with the growth surface facing upward, a position of an inlet of the dopant-containing gas into the space is higher than a position of an inlet of the oxygen-containing gas into the space, and a position of an inlet of the Ga chloride gas into the space is higher than a position of an inlet of the dopant-containing gas into the space, When the semiconductor substrate is placed so that the growth surface faces downward, a position of an inlet of the dopant-containing gas into the space is set higher than a position of an inlet of the Ga chloride gas into the space, and a position of an inlet of the oxygen-containing gas into the space is set higher than a position of an inlet of the dopant-containing gas into the space. A method for manufacturing a semiconductor film.
2. the Ga chloride gas is GaCl gas, The oxygen-containing gas is O 2 It is a gas, The dopant-containing gas is SiCl 4 It is a gas, The method for producing a semiconductor film according to claim 1 .
3. In the step of placing the semiconductor substrate, the semiconductor substrate is placed in the reaction chamber with the growth surface facing downward. The method for producing a semiconductor film according to claim 1 or 2.
4. In the step of epitaxially growing the semiconductor film, the Ga chloride gas, the oxygen-containing gas, and the dopant-containing gas are flowed into the space at a flow rate of 110 cm / s or more. The method for producing a semiconductor film according to claim 3 .
5. β-Ga containing Cl 2 O 3 It is made of single crystals of the The thickness is 1000 nm or more and 1000 μm or less, The in-plane density of defects continuing from the front surface to the back surface in the thickness direction is 10 / cm, as measured by emission microscope observation with a circular anode electrode having a diameter of 500 μm formed on the surface. 2 Below is the Semiconductor film.
Citation Information
Patent Citations
storehouse
JP1984084069A
Semiconductor substrate and method of manufacture
JP1997027489A
Semiconductor substrate and manufacture thereof
JP2001077024A
Silicon carbide schottky diode and manufacturing method therefor
JP2002134760A
Silicon carbide semiconductor device and method for manufacturing the same
JP2003332562A