Ammonia decomposition catalyst and exhaust gas treatment method using the same

The ammonia decomposition catalyst with a dual-layer structure of noble metal, inorganic oxide, and ion-exchanged CHA-type zeolite addresses low-temperature performance issues, ensuring sustained ammonia decomposition and denitrification efficiency.

JP7580756B2Active Publication Date: 2024-11-12NIKKI UNIVERSAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021000436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-05
Publication Date
2024-11-12
Estimated Expiration
2041-01-05

AI Technical Summary

Technical Problem

Existing ammonia decomposition catalysts exhibit low processing performance under low-temperature conditions and high space velocity, necessitating improvements in ammonia decomposition ability and activity.

Method used

An ammonia decomposition catalyst comprising a noble metal, inorganic oxide, and CHA-type zeolite with ion-exchanged Cu, Co, or Fe ions in two layers, which enhances low-temperature activity and durability.

Benefits of technology

The catalyst maintains excellent ammonia decomposition ability over a long period, even at low temperatures, with improved denitrification performance and reduced noble metal usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580756000006
    Figure 0007580756000006
  • Figure 0007580756000007
    Figure 0007580756000007
  • Figure 0007580756000008
    Figure 0007580756000008
Patent Text Reader

Abstract

To provide an ammonia-decomposing catalyst that can maintain excellent ammonia-decomposing capability for a long time and can express excellent low-temperature activity.SOLUTION: The inventive ammonia-decomposing catalyst is to treat exhaust containing ammonia and moisture and comprises a first layer including a noble metal, an inorganic oxide, a first protic zeolite or a first ion-exchange zeolite having been ion-exchanged with Cu, Co or Fe ions, and a second layer that is provided on the surface of the first layer and includes a second protic zeolite or a second ion-exchange zeolite having been ion-exchanged with Cu, Co or Fe ions. The first and second protic zeolites, and the first and second ion-exchange zeolites have CHA type structures.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an ammonia decomposition catalyst for treating exhaust gas containing ammonia and moisture, and an exhaust gas treatment method using the same. [Background technology]

[0002] Catalysts that decompose ammonia contained in exhaust gas are known. Patent Document 1 discloses an ammonia decomposition catalyst having a lower layer and an upper layer. The lower layer contains a precious metal, an inorganic oxide, phosphorus, and a specific zeolite. On the other hand, the upper layer contains a specific zeolite. Patent Document 2 discloses an ammonia decomposition catalyst that contains copper oxide, a zeolite, a precious metal, and phosphorus. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2015 / 099024 [Patent Document 2] International Publication No. 2009 / 075311 Summary of the Invention [Problem to be solved by the invention]

[0004] According to the investigations of the present inventors, although the ammonia decomposition catalyst described in Patent Document 1 can maintain an excellent ammonia decomposition ability for a long period of time, there is room for improvement in the treatment ability under low temperature conditions of 300°C or less and in the treatment under higher space velocity (SV) conditions.

[0005] The present disclosure provides an ammonia decomposition catalyst capable of maintaining excellent ammonia decomposition ability for a long period of time and exhibiting excellent low-temperature activity, and an exhaust gas treatment method using the same. [Means for solving the problem]

[0006] One aspect of the present disclosure relates to an ammonia decomposition catalyst. This ammonia decomposition catalyst is for treating exhaust gas containing ammonia and moisture, and comprises a first layer containing a noble metal, an inorganic oxide, and a first proton type zeolite or a first ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions, and a second layer provided on the surface of the first layer and containing a second proton type zeolite or a second ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions, and the first and second proton type zeolites and the first and second ion-exchanged zeolites have a CHA structure.

[0007] One aspect of the present disclosure relates to an exhaust gas treatment method, which includes a step of contacting exhaust gas containing ammonia and moisture with the ammonia decomposition catalyst according to the present disclosure to decompose the ammonia into nitrogen and water. Effect of the Invention

[0008] According to the present disclosure, there are provided an ammonia decomposition catalyst capable of maintaining excellent ammonia decomposition ability for a long period of time and exhibiting excellent low-temperature activity, and an exhaust gas treatment method using the same. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view that illustrates the progress of an ammonia decomposition reaction in an ammonia decomposition catalyst according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a graph showing the results of a durability test on catalyst A-4 (inlet temperature: 340° C., SV: 10,000 h-1, NH3 concentration: 1%). [Diagram 3] FIG. 3 is a graph showing the results of a durability test on catalyst B-6 (inlet temperature: 340° C., SV: 10,000 h-1, NH3 concentration: 1%). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Terminology> The terms used in this specification have the following meanings unless otherwise specified. Ammonia decomposition rate: The ratio (%) of the ammonia concentration in the exhaust gas before and after contact with the catalyst. ·NO X Production rate: The ratio of NO produced in the exhaust gas after contact with the catalyst to the ammonia concentration in the exhaust gas before contacting the catalyst. X Represents the concentration ratio (%). N 2 O production rate: The ratio of N produced in the exhaust gas after contact with the catalyst to the ammonia concentration in the exhaust gas before contacting the catalyst. 2 Represents the percentage of O. Nitrogen oxides: NO X and N 2 Refers to both O and NO X It is sometimes expressed as: N 2 Selectivity: The ammonia decomposition rate is determined by the NO in the exhaust gas after contact with the catalyst. X In other words, the amount of ammonia before contacting the catalyst is N 2 is the proportion of

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present invention is not limited to the following embodiments.

[0012] [Ammonia decomposition catalyst] 1 is a cross-sectional view showing a schematic diagram of the progress of the ammonia decomposition reaction in the ammonia decomposition catalyst according to the present embodiment. The ammonia decomposition catalyst 10 shown in this figure includes a support S, a lower layer 1 (first layer) provided on the surface of the support S, and an upper layer 2 (second layer) provided on the surface of the lower layer 1.

[0013] <Support> The support S preferably has a shape that generates a small differential pressure during gas flow and has a large contact area with the gas. Specific examples of the support S include honeycomb, sheet, mesh, fiber, pipe, filter, sphere, etc. The material of the support is, for example, a known catalyst carrier such as cordierite or alumina, carbon fiber, metal fiber, glass fiber, ceramic fiber, or metal such as titanium, aluminum, or stainless steel.

[0014] <lower layer> The lower layer 1 contains a precious metal, an inorganic oxide, and a first proton-type zeolite or a first ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions. The lower layer 1 is provided on the surface of the support S. The thickness of the lower layer 1 is preferably 10 to 200 μm, and more preferably 30 to 100 μm. In the lower layer 1, an oxidation reaction represented by the following formula (1) mainly proceeds, and a denitrification reaction represented by the following formula (2) also proceeds. Oxidation reaction:NH 3 +O 2 →NO X +N 2 O+H 2 O+N 2 (1) Denitrification reaction: NO X +NH 3 +O 2 →N 2 +O 2 (2)

[0015] (Precious metals) The lower layer 1 contains a precious metal. Examples of the precious metal include Pt, Pd, Ir, Rh, and compounds thereof. Among these, Pt is preferred because of its high decomposition activity and N 2 This is particularly preferred since it has a large effect of improving the selectivity.

[0016] The content of the precious metal is preferably 0.3 to 10 mass %, more preferably 0.5 to 8 mass %, based on the total amount of the precious metal, inorganic oxide, and zeolite contained in the lower layer 1. The amount of the precious metal supported is preferably 0.03 to 1 g / L, more preferably 0.1 to 0.9 g / L, and even more preferably 0.15 to 0.8 g / L, relative to the catalyst volume. When the amount of the precious metal is within the above range, the ammonia decomposition rate, NO X Production rate and N 2 Better results are obtained in terms of O production rate.

[0017] (Inorganic oxides) The lower layer 1 contains an inorganic oxide. The inorganic oxide is titania (TiO 2 ), zirconia (ZrO 2 ), silica (SiO 2 ), alumina, and ceria-zirconia composite oxides and solid solutions (CeO 2 ZrO 2 and CeO 2 :ZrO 2 The molar ratio is 1:3 to 3:1. Of these, one may be used alone, or two or more may be used in combination. The inorganic oxide contributes to the action of the precious metal, that is, to improving the decomposition activity, and in particular to improving the sustainability of the decomposition activity during long-term use. Among the above inorganic oxides, TiO 2 , ZrO 2 and ceria-zirconia (composite oxide or solid solution) have an excellent effect of sustaining the decomposition activity during long-term use. The content of the inorganic oxide is preferably 5 to 50 mass %, more preferably 10 to 35 mass %, based on the total amount of the precious metal, inorganic oxide, and zeolite contained in the lower layer 1. The amount of the inorganic oxide supported is preferably 1 to 50 g / L, more preferably 5 to 20 g / L, relative to the catalyst volume. When the amount of the inorganic oxide is within the above range, the ammonia decomposition rate, NO X Production rate and N 2 Better results are obtained in terms of O production rate.

[0018] It is particularly effective to incorporate the inorganic oxide in the catalyst in a state in which the precious metal is supported. For example, TiO 2 The particles are added with 0.1 to 10 mass% (TiO 2 (based on the mass of Pt) 2 The catalyst composition containing the precious metal and the inorganic oxide can be prepared by preparing the particles of the inorganic oxide and mixing them with other components.

[0019] The inorganic oxide is preferably particulate in order to more effectively exert the function of the precious metal component in the catalyst composition. The average particle size of the inorganic oxide is, for example, 0.1 to 100 μm. Here, the particle size refers to the size of the secondary particles, and is the length of the major axis when observed with a SEM. The average particle size refers to the average value when the major axis is measured using a SEM for at least 10 particles.

[0020] Inorganic oxides include TiO 2 When particles are used, TiO 2 The BET specific surface area of ​​the particles is preferably 5 to 200 m 2 / g, more preferably 10 to 150m 2 / g. As inorganic oxide, ZrO 2 When particles are used, the specific surface area is 10 m 2 / g or more of porous ZrO 2 It is preferable to use ZrO particles. 2 ZrO may be of any of monoclinic, tetragonal and cubic systems. 2 (For example, ZrO 2 ·nCeO 2 , ZrO 2 nSiO 2 , ZrO 2 nTiO 2 (wherein n is generally 0.25 to 0.75) may be used as the inorganic oxide. 2 When using a zeolite, it is preferable to use a high silica zeolite having a zeolite structure (eg, mordenite).

[0021] (Zeolite) The lower layer 1 contains zeolite having a CHA type structure. The CHA type structure has a three-dimensional pore structure. As the zeolite having the CHA type structure, in addition to the proton type (H type), ion-exchanged zeolite ion-exchanged with Cu, Co or Fe can be used. One of these zeolites may be used alone, or two or more of them may be used in combination.

[0022] The zeolite is preferably particulate. The average particle size of the zeolite is, for example, 0.1 to 5.0 μm. Here, the particle size refers to the size of the zeolite crystals, and is the length of the major axis when observed with a SEM. The average particle size refers to the average value when the major axis of at least 10 particles is measured using a SEM.

[0023] NO X From the viewpoint of suppression performance and durability, it is preferable to use Cu ion-exchanged CHA-type zeolite as the zeolite having a CHA-type structure, and it is more preferable to use Cu ion-exchanged SSZ zeolite (SSZ-13) or Cu ion-exchanged SAPO-34 zeolite. The silica-alumina ratio (SAR, Si / Al) of the Cu ion-exchanged SSZ zeolite is preferably 10 to 50, more preferably 10 to 20. If the SAR is less than 10, the NOx reduction ability increases but the resistance under hydrothermal conditions tends to decrease, while if it exceeds 50, the resistance under hydrothermal conditions increases but the NOx reduction ability tends to decrease. The amount of aluminum phosphate relative to silica in the Cu ion-exchanged SAPO zeolite (Al+P) / Si is preferably 1 to 30, more preferably 5 to 30. If the (Al+P) / Si ratio is less than 1, the durability under hydrothermal conditions tends to decrease, while if it exceeds 30, the NOx reduction performance tends to decrease.

[0024] Cu ion-exchanged zeolite NH 3 By NO XThe reduction performance (denitrification performance) tends to be better as the Cu dispersibility is higher, and the more solid acid the zeolite holds. In general, the acid amount of zeolite is higher as the SAR is lower, but zeolites with low SAR have high hydrophilicity and tend to be easily dealuminated under high temperature and high moisture conditions, so that the acid amount decreases over time and the denitrification performance tends to decrease. Similarly, it can be assumed that SAPO-based zeolites also have a similar tendency, with the acid amount increasing as the (Al+P) / Si ratio decreases. The Cu ion-exchanged SSZ zeolite (SSZ-13) or Cu ion-exchanged SAPO zeolite (SAPO-34) in this embodiment has high hydrothermal stability structurally, and can be catalyzed with a composition with a higher acid amount than β zeolite (SAR: 35), so that the reduction performance is improved. X It is assumed that this product has both excellent suppression performance and durability.

[0025] The content of the CHA-type zeolite in the lower layer 1 is preferably 40 to 95 mass %, more preferably 50 to 90 mass %, based on the total amount of the precious metal, inorganic oxide, and zeolite in the lower layer 1. The amount of the CHA-type zeolite supported in the lower layer 1 is preferably 5 to 95 g / L, more preferably 10 to 90 g / L, relative to the catalyst volume. When the amount of zeolite in the lower layer 1 is within the above range, the ammonia decomposition rate, NO X Production rate and N 2 Better results are obtained in terms of O production rate.

[0026] The ammonia decomposition catalyst described in Patent Document 1 contains a specific phosphorus in the lower layer from the viewpoint of improving hydrothermal resistance. In contrast, the lower layer 1 of the ammonia decomposition catalyst according to the present embodiment has excellent hydrothermal resistance due to the CHA-type structure zeolite, so the lower layer 1 does not need to contain phosphorus. Even if the lower layer 1 contains phosphorus, the content thereof (based on the total of the noble metal, inorganic oxide, phosphorus, and zeolite contained in the lower layer 1) may be less than 0.05 mass % or may be less than 0.01 mass %. Evaluation tests conducted by the present inventors have experimentally shown that the low-temperature activity of the lower layer 1 is improved by not incorporating phosphorus into the lower layer 1 (see Examples 1 and 13).

[0027] <Upper layer> The upper layer 2 contains a second proton type zeolite or a second ion-exchanged zeolite that has been ion-exchanged with Cu, Co or Fe ions. The upper layer 2 is provided on the surface of the lower layer 1. The thickness of the upper layer 2 is preferably 10 to 200 μm, and more preferably 30 to 100 μm. In the upper layer 2, a denitrification reaction represented by the following formula (2) mainly proceeds. Denitrification reaction: NO X +NH 3 +O 2 →N 2 +O 2 (2)

[0028] The zeolite contained in the upper layer 2 has a CHA type structure, similar to the zeolite contained in the lower layer 1. As the zeolite having a CHA type structure, in addition to the proton type (H type), ion-exchanged zeolite ion-exchanged with Cu, Co or Fe can be used. One of these zeolites may be used alone, or two or more of them may be used in combination. The zeolite contained in the upper layer 2 is preferably a Cu ion-exchanged CHA type zeolite, similar to the lower layer 1, and more preferably a Cu ion-exchanged SSZ zeolite (SSZ-13) or a Cu ion-exchanged SAPO zeolite (SAPO-34). The zeolite contained in the upper layer 2 may be the same as or different from the zeolite contained in the lower layer 1.

[0029] The amount of the zeolite having a CHA structure supported in the upper layer 2 is preferably 20 to 150 g / L, more preferably 30 to 130 g / L, relative to the catalyst volume. When the amount of zeolite in the upper layer 2 is within the above range, the ammonia decomposition rate, NO X Production rate and N 2 Better results are obtained in terms of O production rate.

[0030] The amount of zeolite contained in the upper layer 2 (the total amount of proton type zeolite and ion-exchange type zeolite) is preferably 20 to 400 parts by mass, and more preferably 50 to 150 parts by mass, relative to 100 parts by mass of the total amount of the precious metal, inorganic oxide, and zeolite contained in the lower layer 1. When this amount is 50 parts by mass or more, the amount of NOx generated by the denitrification reaction in the upper layer 2 is reduced. X On the other hand, when the amount is 150 parts by mass or less, ammonia tends to come into contact with the lower layer 1 efficiently and be decomposed.

[0031] [Method of manufacturing ammonia decomposition catalyst] The method for producing the ammonia decomposition catalyst of the present embodiment will be described below, although the method is not limited to the method described below.

[0032] First, put a precious metal-containing aqueous solution into a container and add an inorganic oxide to it. After the inorganic oxide is sufficiently impregnated with the precious metal-containing aqueous solution, heat it while stirring to evaporate the water and dry it. After that, heat it further in a dryer, and the resulting powder is calcined in air to obtain inorganic oxide particles carrying a predetermined amount of precious metal (as metal content).

[0033] This powder is mixed with deionized water, and then a predetermined amount of inorganic binder and the above-mentioned zeolite are mixed therein to prepare a slurry composition for the lower layer. This slurry is applied to the support S, and the excess is blown off with an air blower. Thereafter, the support S is heated and dried, and further fired in a high-temperature furnace under air circulation, thereby forming the lower layer 1 on the surface of the support S. Examples of inorganic binders that can be mixed into the slurry include colloidal silica, silica sol, alumina sol, silicic acid sol, titania sol, boehmite, white clay, kaolin, and sepiolite. An organic binder may be used instead of the inorganic binder.

[0034] Deionized water, a predetermined amount of inorganic binder, and the above-mentioned zeolite are mixed together to prepare a slurry for the upper layer. This slurry is applied onto the surface of the lower layer 1, and the excess is blown off with an air blower. Thereafter, drying and firing are carried out in the same manner as above. As a result, an ammonia decomposition catalyst 10 consisting of two layers, the lower layer 1 and the upper layer 2, is obtained.

[0035] [Exhaust gas treatment method] The exhaust gas treatment method according to this embodiment includes a step of decomposing ammonia into nitrogen and water by contacting exhaust gas containing ammonia and moisture with an ammonia decomposition catalyst 10. Specific examples of exhaust gas containing ammonia (ammonia exhaust gas) include exhaust gas generated by the treatment of ammonia water in factories such as semiconductor factories, coke oven exhaust gas, leak gas from a flue gas denitrification process, and stripping of ammonia-containing wastewater from sewage treatment plants, sludge treatment facilities, etc.

[0036] The ammonia concentration of the ammonia exhaust gas is, for example, 10 ppm by volume to 5% by volume. The ammonia exhaust gas and air are brought into contact with the ammonia decomposition catalyst 10 to convert the ammonia into harmless nitrogen gas and water, and oxidatively decompose the ammonia. The oxidative decomposition temperature is appropriately determined depending on the properties of the exhaust gas (water vapor concentration and ammonia concentration), reaction conditions (temperature, space velocity), degree of catalyst deterioration, etc., and is usually selected from a temperature range of 200 to 500°C, preferably 250 to 450°C. The water vapor concentration of the ammonia exhaust gas is, for example, 10% by volume or more, and may be 20 to 50% by volume.

[0037] The space velocity (SV) of the exhaust gas to be treated against the catalyst is set to 100 to 100,000 h , taking into consideration the properties of the gas (ammonia concentration and moisture concentration) and the target value of the ammonia decomposition rate. -1 The ammonia concentration in the gas supplied to the catalytic reactor is preferably adjusted to 3% by volume or less, and more preferably 2% by volume or less. If the ammonia concentration exceeds 3% by volume, the heat generated by the reaction will cause the temperature of the catalyst layer to rise too high, which will easily cause the catalyst to deteriorate.

[0038] When treating exhaust gas that does not contain enough oxygen required for the decomposition reaction, air or an oxygen-containing gas may be mixed from the outside so that the ratio of oxygen amount / theoretical required oxygen amount at the inlet of the catalytic reactor is, for example, 1.03 or more (preferably 2.0 or more). Here, the theoretically required oxygen amount is the stoichiometric oxygen amount obtained from the following formula (3), and when the ammonia concentration at the inlet of the reactor is 1.0 volume %, the oxygen concentration is, for example, 0.77 or more (preferably 0.83 volume % or more). 4NH 3 +3O 2 →6H 2 O+2N 2 (3)

[0039] Instead of the ammonia decomposition catalyst 10 having the lower layer 1 and the upper layer 2, a first catalyst having a similar configuration to the lower layer 1 and a second catalyst having a similar configuration to the upper layer 2 may be prepared, and these catalysts may be alternately installed and sequentially contacted with the exhaust gas to decompose the ammonia contained in the exhaust gas. That is, the exhaust gas treatment method may include a step of contacting the exhaust gas with the first catalyst, and a step of contacting a product gas generated by contacting the exhaust gas with the first catalyst with the second catalyst.

[0040] Below, we will introduce an example of ammonia stripping exhaust gas. The pH of wastewater containing ammonia (for example, cleaning fluid in semiconductor manufacturing, sulfuric acid scrubber fluid that has captured ammonia, dehydrated sewage sludge fluid) is adjusted to around 10 using sodium hydroxide or similar, heated to 50°C to 90°C, and then air, nitrogen, and steam are fed in to release the ammonia into the gas phase. After that, steam (exhaust gas) containing high concentrations of moisture and ammonia is introduced into a catalytic reaction device, and the required amount of air is separately introduced from outside, and the ammonia is decomposed into nitrogen and water vapor upon contact with the catalyst, and detoxified.

[0041] According to the ammonia decomposition catalyst of this embodiment, even if the amount of precious metal carried is reduced compared to the conventional catalyst, excellent ammonia decomposition ability is exhibited. This is presumably due to the fact that the CHA-structured zeolite contained in the lower and upper layers has excellent denitrification performance. In addition, since the CHA-structured zeolite has excellent hydrothermal resistance, excellent ammonia decomposition ability is maintained for a long period of time. Furthermore, since the phosphorus content in the ammonia decomposition catalyst is sufficiently low or substantially free of phosphorus, excellent ammonia decomposition ability is exhibited even under low-temperature conditions of about 300°C. According to the study by the present inventors, phosphorus improves the hydrothermal resistance of the ammonia decomposition catalyst, but has the effect of lowering low-temperature activity. EXAMPLES

[0042] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.

[0043] [Catalyst preparation] <Catalyst A-1> In an evaporating dish, an aqueous solution of dinitrodiamine platinum (Pt concentration: 4.5 mass%) was added to TiO 2 Powder (Ishihara Sangyo Kaisha, average particle size 1 μm, BET specific surface area: 60 m 2 / g) was added, and TiO 2 The powder was thoroughly impregnated with the aqueous solution. After that, the water was evaporated while stirring at a temperature of 80 to 90°C, and the powder was dried. After that, it was further heated to 150°C in a dryer. The obtained powder was calcined in air at a temperature of 500°C for 1 hour, and TiO2 carrying 5.0 mass% of Pt (as metal) was obtained. 2 Particles (which are called Pt(5.0) / TiO 2The powder was mixed with 64.4 g of deionized water to prepare a slurry. The slurry was mixed with 249 g of silica sol (Nissan Chemical Industries, Snowtex C) and 142.3 g of Cu ion-exchanged SSZ zeolite (Zeolyst, hereinafter also referred to as "Cu-SSZ-13") to prepare a lower layer slurry. The lower layer slurry was applied to a support of 200 cells of cordierite honeycomb (cell number: 200 cells / square inch, length 50 mm x width 50 mm x height 50 mm, volume: 0.125 liters), and the excess was blown off with an air blower. The catalyst was then dried for 4 hours in a dryer at 150°C, and further calcined for 4 hours at 500°C in a high-temperature furnace under air circulation to obtain a lower layer catalyst. The amount of Pt was 0.5 g per liter of catalyst, and the amount of Cu ion-exchanged SSZ zeolite was 70 g.

[0044] Next, 64.4 g of deionized water, 249 g of silica sol (Nissan Chemical Industries, Snowtex C), and 142.3 g of Cu ion-exchanged SSZ zeolite (Zeolyst) were mixed together to prepare an upper layer slurry (Cu-SSZ slurry). This slurry was applied onto the lower layer catalyst, and the excess was blown off with an air blower. Thereafter, drying and firing were carried out in the same manner as above, to obtain a two-layered catalyst A-1. The amount of Cu ion-exchanged SSZ zeolite supported in the upper layer at this time was 64 g per 1 liter of catalyst volume.

[0045] <Catalyst A-2> The amount of Pt was changed to Pt(5.0) / TiO 2 (0.5 g / L) to Pt(3.0) / TiO 2 Catalyst A-2 was obtained in the same manner as Catalyst A-1, except that the concentration of the catalyst was changed to 0.3 g / L.

[0046] <Catalyst A-3> The amount of Pt was changed to Pt(5.0) / TiO 2 (0.5 g / L) to Pt(7.5) / TiO 2 Catalyst A-2 was obtained in the same manner as Catalyst A-1, except that the concentration of the catalyst was changed to 0.75 g / L.

[0047] <Catalyst A-4> Catalyst A-4 was obtained in the same manner as Catalyst A-1, except that the thickness of the lower layer was adjusted so that the mass per unit area of ​​the lower layer was half that of Catalyst A-1.

[0048] <Catalyst A-5> Catalyst A-5 was obtained in the same manner as Catalyst A-1, except that the thickness of the lower layer was adjusted so that the mass per unit area of ​​the lower layer was 1.5 times that of Catalyst A-1.

[0049] <Catalyst A-6> Catalyst A-6 was obtained in the same manner as Catalyst A-1, except that the amount of the catalyst supported in the upper layer of Catalyst A-1 was changed from 64 g / L to 50 g / L.

[0050] <Catalyst A-7> Catalyst A-6 was obtained in the same manner as Catalyst A-1, except that the amount supported in the upper layer was changed from 64 g / L to 100 g / L.

[0051] <Catalyst A-8> Catalyst A-8 was obtained in the same manner as Catalyst A-4, except that the amount of the catalyst supported in the upper layer was changed from 64 g / L to 50 g / L.

[0052] <Catalyst A-9> Catalyst A-9 was obtained in the same manner as Catalyst A-4, except that the amount of the catalyst supported in the upper layer was changed from 64 g / L to 100 g / L.

[0053] <Catalyst A-10> Catalyst A-10 was obtained in the same manner as Catalyst A-1, except that Fe ion-exchanged SSZ (H-type SSZ-13 manufactured by Zeolyst Co., Ltd., in which Fe ion-exchanged SSZ was used instead of Cu ion-exchanged SSZ zeolite, hereinafter also referred to as "Fe-SSZ-13").

[0054] <Catalyst A-11> The inorganic oxide in the lower layer is TiO 2 Instead of powder, ZrO 2 Catalyst A-11 was obtained in the same manner as Catalyst A-1, except that powder was used.

[0055] <Catalyst A-12> Catalyst A-12 was obtained in the same manner as Catalyst A-1, except that Cu ion-exchanged SAPO-34 (H-type SAPO-34 manufactured by UOP Corporation, in which Cu is supported by ion exchange), hereinafter sometimes referred to as "Cu-SAPO-34") was used instead of Cu ion-exchanged SSZ zeolite to form the lower and upper layers.

[0056] <Catalyst A-13> First, a lower layer was formed on the surface of a cordierite honeycomb in the same manner as in the case of catalyst A-1. Next, a phosphorus solution was applied to the surface of the lower layer, and the excess liquid was blown off with an air blower. After that, the upper layer was formed in the same manner as for catalyst A-1. Note that the phosphorus solution used was a mixture of 50 g of 85% phosphoric acid solution and 500 g of deionized water.

[0057] <Comparative catalyst B-1> Pt(5.0) / TiO 2 The powder, deionized water, and silica sol were mixed to prepare a slurry. This slurry was applied to a 200-cell cordierite honeycomb support, and the excess was blown off with an air blower. After that, it was dried in a dryer at 150°C for 4 hours, and further calcined in a high-temperature furnace at 500°C for 4 hours under air circulation to obtain comparative catalyst B-1.

[0058] <Comparative catalyst B-2> Pt(5.0) / TiO 2 The powder, deionized water, silica sol, and Cu ion-exchanged β zeolite (manufactured by Clariant Catalyst, hereinafter sometimes referred to as "Cuβ") were mixed together to form a slurry. Comparative catalyst B-2 was obtained in the same manner as comparative catalyst B-1, except that a slurry containing Cuβ was used.

[0059] <Comparative catalyst B-3> A lower layer was formed on the surface of the cordierite support in the same manner as in Comparative Catalyst B-2. Next, 50 g of 85% phosphoric acid solution was mixed with 500 g of deionized water to prepare a phosphorus solution. This solution was applied to the surface of the lower layer, and the excess liquid was blown off with an air blower. After that, it was dried in a dryer at 150°C for 4 hours, and further calcined in a high-temperature furnace under air circulation at 500°C for 4 hours to obtain Comparative Catalyst B-3.

[0060] <Comparative catalyst B-4> 64.4g of deionized water, 249g of silica sol (Nissan Chemical Industries, Snowtex C), and 142.3g of Cu ion-exchanged β zeolite (Clariant Catalysts) were mixed together to prepare a slurry (Cuβ slurry). This slurry was applied onto comparative catalyst B-2, and the excess was blown off with an air blower. It was then dried for 4 hours in a 150°C dryer, and further calcined for 4 hours at 500°C in a high-temperature furnace under air circulation to obtain comparative catalyst B-4.

[0061] <Comparative catalyst B-5> Comparative catalyst B-5 was obtained in the same manner as comparative catalyst B-4, except that the upper layer slurry (Cuβ slurry) was applied onto comparative catalyst B-1.

[0062] <Comparative catalyst B-6> Comparative catalyst B-5 was obtained in the same manner as comparative catalyst B-4, except that the upper layer slurry (Cuβ slurry) was applied onto comparative catalyst B-3.

[0063] Table 1 shows the composition and loading amount of the lower and upper layers of each catalyst. [Table 1]

[0064] <Activity evaluation test> A cylindrical honeycomb catalyst (diameter 21 mm, length 50 mm) was taken from the honeycomb catalyst obtained as described above and packed into a flow reactor. A predetermined amount of gas was circulated by controlling the flow rate with a mass flow controller. The catalyst was heated in an electric furnace to set the catalyst inlet temperature (inlet temperature) to a predetermined temperature, and ammonia decomposition activity was evaluated. Tables 2 and 3 show the evaluation conditions and initial activity data.

[0065] <Gas analysis method> Ammonia: Gas chromatography (TCD detector) or gas detector tube ·NO X : Chemiluminescence (chemiluminescence) analyzer N 2 O: Gas chromatography (TCD detector)

[0066] <Calculation> ·NH 3 Decomposition rate (%): 100-{(Outlet NH 3 Concentration) / (Inlet NH 3 concentration)×100} ·NO X Generation rate (%): (Exit NO. X Concentration) / (Inlet NH 3 concentration)×100 N 2 O generation rate (%):{(Exit N 2 O concentration) / (inlet NH 3 concentration)}×100 N 2 Selectivity (%): 100-{(100-NH 3 decomposition rate)+NO X Generation rate +N 2 O generation rate x 2}

[0067] [Table 2]

[0068] [Table 3]

[0069] <Durability test> Durability tests were carried out using Catalyst A-4, Catalyst A-12, Catalyst A-13 and Catalyst B-6, respectively, and the results are shown in Table 4.

[0070] [Table 4]

[0071] Figure 2 shows the catalyst A-4 (inlet temperature: 340℃, SV: 10000h -1 , N.H. 3 This is a graph showing the results of a durability test for catalyst B-6 (inlet temperature: 340°C, SV: 10,000h). -1 , N.H. 3 As shown in these graphs, catalyst A-4 (a catalyst according to the embodiment) has a lower NO X The production rate could be maintained over a long period of time.

[0072] <Performance evaluation under high SV conditions> The performance tests were carried out under high SV conditions using Catalyst A-1, Catalyst A-4 and Catalyst B-6, respectively, and the results are shown in Table 5.

[0073] [Table 5]

[0074] As shown in Table 5, catalysts A-1 and A-4 had a lower NO2 content than catalyst B-6 even at higher SV. X The production rate was kept low.

Claims

1. An ammonia decomposition catalyst for treating exhaust gas containing ammonia and moisture, a first layer including a precious metal, an inorganic oxide, and a first proton-type zeolite or a first ion-exchanged zeolite ion-exchanged with Cu, Co, or Fe ions; a second layer provided on the surface of the first layer and including a second proton-type zeolite or a second ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions; Equipped with The first and second proton type zeolites and the first and second ion-exchange type zeolites have a CHA type structure; When the total amount of the precious metal, the inorganic oxide, and the zeolite in the first layer is taken as 100 parts by mass, the contents of the precious metal, the inorganic oxide, and the zeolite in the first layer are within the following ranges, respectively: Precious metal: 0.3 to 10 parts by mass Inorganic oxide: 5 to 50 parts by mass Zeolite: 40 to 95 parts by mass the amount of zeolite in the second layer is 20 to 400 parts by mass relative to 100 parts by mass in total of the precious metal, inorganic oxide, and zeolite in the first layer; An ammonia decomposition catalyst, wherein the first layer has a phosphorus content of less than 0.05 parts by mass relative to 100 parts by mass of the total of the precious metal, the inorganic oxide and the zeolite contained in the first layer.

2. 2. The ammonia decomposition catalyst according to claim 1, wherein the noble metal is at least one selected from the group consisting of Pt, Pd, Ir and Rh.

3. 3. The ammonia decomposition catalyst according to claim 1, wherein the inorganic oxide is at least one selected from the group consisting of titania, zirconia, ceria zirconia, alumina and silica.

4. The ammonia decomposition catalyst according to any one of claims 1 to 3, wherein at least one of the first and second ion-exchanged zeolites is a Cu ion-exchanged CHA-type zeolite.

5. The ammonia decomposition catalyst according to any one of claims 1 to 4, wherein at least one of the first and second ion-exchanged zeolites is a Cu ion-exchanged SSZ zeolite.

6. The ammonia decomposition catalyst according to any one of claims 1 to 4, wherein at least one of the first and second ion-exchanged zeolites is a Cu ion-exchanged SAPO zeolite.

7. The ammonia decomposition catalyst according to any one of claims 1 to 6, further comprising a support provided on the first layer opposite to the second layer.

8. An exhaust gas treatment method for treating exhaust gas containing ammonia and moisture, comprising: A method for treating an exhaust gas, comprising a step of contacting the exhaust gas with the ammonia decomposition catalyst according to any one of claims 1 to 7 to decompose ammonia into nitrogen and water.

9. An exhaust gas treatment method for treating exhaust gas containing ammonia and moisture, comprising: The method includes a step of sequentially contacting the exhaust gas with a first catalyst and a second catalyst that are alternately installed, The first catalyst comprises a precious metal, an inorganic oxide, and a first proton-type zeolite or a first ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions; The second catalyst comprises a second proton type zeolite or a second ion-exchanged zeolite ion-exchanged with Cu, Co or Fe ions; The first and second proton type zeolites and the first and second ion-exchange type zeolites have a CHA type structure; When the total amount of the noble metal, the inorganic oxide, and the zeolite in the first catalyst is taken as 100 parts by mass, the contents of the noble metal, the inorganic oxide, and the zeolite in the first catalyst are in the following ranges, respectively: Precious metal: 0.3 to 10 parts by mass Inorganic oxide: 5 to 50 parts by mass Zeolite: 40 to 95 parts by mass the amount of zeolite in the second catalyst is 20 to 400 parts by mass relative to 100 parts by mass of the total amount of the precious metal, inorganic oxide, and zeolite in the first catalyst; The method for treating an exhaust gas, wherein the first catalyst has a phosphorus content of less than 0.05 parts by mass relative to 100 parts by mass of the total amount of the precious metal, the inorganic oxide, and the zeolite contained in the first catalyst.

Citation Information

Patent Citations

  • Integrated scr and amox catalyst systems

    JP2016073971A

  • Ammonia-decomposing catalyst, and method for treatment of ammonia-containing exhaust gas with the catalyst

    WO2009075311A1

  • Ammonia decomposition catalyst

    WO2015099024A1

  • Catalyst, catalyst product and catalyst production method

    WO2020230639A1

  • Ammonia oxidation catalyst for diesel applications

    WO2020234375A1