Secondary battery
A secondary battery with a silicon-based and carbon-based active material ratio of 40:60 to 90:10 addresses the challenges of volumetric expansion, enhancing capacity, rapid charging, and life characteristics by optimizing the use of tailored binders and conductive materials.
Patent Information
- Application Number
- JP2022557957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-20
- Filing Date
- 2021-05-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-05-17
AI Technical Summary
Existing lithium secondary batteries face challenges in achieving high capacity, rapid charging characteristics, and long life due to the volumetric expansion of silicon-based active materials and the need for thick carbon-based active material coatings, which lead to cracking and detachment of electrodes.
A secondary battery design incorporating a first negative electrode with a silicon-based active material and a second negative electrode with a carbon-based active material, with a specific weight ratio of 40:60 to 90:10, allowing for optimized use of binders and conductive materials tailored to each active material's characteristics, thereby reducing volumetric expansion and enhancing charging potential.
The battery achieves improved capacity, rapid charging, and extended life characteristics by leveraging the advantages of both silicon-based and carbon-based active materials, minimizing volumetric expansion and maintaining structural integrity.
Smart Images

Figure 0007580818000005 
Figure 0007580818000001 
Figure 0007580818000002
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0060532, filed on May 20, 2020, and all contents disclosed in the documents of this Korean patent application are incorporated herein by reference.
[0002] The present invention relates to a secondary battery, and more particularly to a secondary battery having improved capacity characteristics, life characteristics, and rapid charging characteristics. [Background technology]
[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are in the spotlight as a driving power source for portable devices because of their light weight and high energy density. As a result, research and development efforts to improve the performance of lithium secondary batteries are being actively carried out.
[0004] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. In addition, the positive electrode and the negative electrode may have an active material layer including a positive electrode active material or a negative electrode active material formed on a current collector. In general, a lithium-containing metal oxide such as LiCoO2 or LiMn2O4 is used as a positive electrode active material in the positive electrode, and a lithium-free carbon-based active material or a silicon-based active material is used as a negative electrode active material in the negative electrode.
[0005] Among negative electrode active materials, silicon-based active materials have attracted attention because they have a capacity about 10 times higher than carbon-based active materials and have excellent high-speed charging characteristics. However, silicon-based active materials have a problem of volume expansion during charging and discharging, which leads to a decrease in life characteristics. If a large amount of binder is used to suppress this, it is difficult to realize the desired high-capacity electrode, and therefore they are not widely used.
[0006] Meanwhile, carbon-based active materials such as artificial graphite and natural graphite show relatively stable life performance compared to silicon-based active materials, but when the carbon-based active material is thickly coated to manufacture a high-capacity electrode, problems such as cracking, warping, and detachment of the electrode occur.
[0007] In order to overcome the shortcomings of the carbon-based and silicon-based active materials, a technology for manufacturing an electrode in which a carbon-based active material and a silicon-based active material are mixed has been developed. However, in order to reduce the effect of the silicon-based active material on the volume expansion, the proportion of the silicon-based active material in the negative electrode cannot be increased to a desired level, making it difficult to improve the capacity characteristics and fast charging characteristics of the negative electrode. In addition, when the proportion of the silicon-based active material is increased, the binder content must also be increased in order to suppress the volume expansion of the active material, making it difficult to realize a high capacity negative electrode.
[0008] Korean Patent No. 10-0794192 relates to a method for manufacturing a carbon-coated silicon-graphite composite negative electrode material for a lithium secondary battery and a method for manufacturing a secondary battery including the same, but there is a limit to how much the above-mentioned problems can be solved. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent No. 10-0794192 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a secondary battery that exhibits improved capacity characteristics, life characteristics, and rapid charging characteristics. [Means for solving the problem]
[0011] The present invention provides a secondary battery comprising: one or more positive electrodes including a positive electrode active material layer; a plurality of negative electrodes including a first negative electrode including a silicon-based active material and a second negative electrode including a carbon-based active material; a separator; and an electrolyte; the positive electrodes and the negative electrodes are alternately stacked with the separator sandwiched between them, and a weight ratio of the silicon-based active material contained in the first negative electrode and the carbon-based active material contained in the second negative electrode is 40:60 to 90:10. Effect of the Invention
[0012] The secondary battery of the present invention includes a first negative electrode including a silicon-based active material and a second negative electrode including a carbon-based active material, and the weight ratio of the silicon-based active material included in the first negative electrode to the carbon-based active material included in the second negative electrode is controlled to a specific ratio. According to the secondary battery of the present invention, since individual negative electrodes including different active materials having different properties are used, it is possible to use a binder and a conductive material suitable for the properties of each active material in a preferred amount, and it is possible to maximize the advantages of each of the silicon-based active material and the carbon-based active material, and it is possible to realize a secondary battery having high capacity and life characteristics.
[0013] In addition, the secondary battery of the present invention is characterized in that the silicon-based active material contained in the first negative electrode and the carbon-based active material contained in the second negative electrode are adjusted to a specific weight ratio, thereby making it possible to lower the charging potential of the silicon-based active material to an appropriate level, reduce the degree of stress on the silicon-based active material due to abrupt changes in voltage during charging and discharging, and improve high-speed charging characteristics. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a diagram for illustrating a secondary battery of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The terms and words used in this specification and the claims should not be interpreted limited to their ordinary and dictionary meanings, but should be interpreted in a way that is consistent with the technical ideas of the present invention, based on the principle that the inventor himself / herself can appropriately define the concepts of terms in order to explain the invention in the best possible way.
[0016] The terms used in this document are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression may include a plural expression unless the context clearly indicates otherwise.
[0017] In this specification, terms such as "comprise", "comprise", or "have" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0018] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and provides results with high reproducibility and high resolution.
[0019] Hereinafter, the secondary battery of the present invention will be described in detail with reference to the drawings. In describing the present invention, if it is determined that a detailed description of a known configuration or function may obscure the gist of the present invention, the detailed description may be omitted.
[0020] <Secondary battery> The present invention relates to a secondary battery 1, specifically, a lithium secondary battery.
[0021] As shown in FIG. 1, the secondary battery 1 of the present invention includes at least one positive electrode 100 including a positive electrode active material layer 120; a plurality of negative electrodes 200, 300 including a first negative electrode 200 including a silicon-based active material and a second negative electrode 300 including a carbon-based active material; a separator 400; and an electrolyte (not shown). The positive electrode 100 and the negative electrodes 200, 300 are alternately stacked with the separator 400 sandwiched therebetween, and a weight ratio of the silicon-based active material included in the first negative electrode 200 to the carbon-based active material included in the second negative electrode 300 is 40:60 to 90:10.
[0022] Conventionally, silicon-based active materials have the advantages of high capacity and rapid charging characteristics, but the degree of volume expansion / contraction during charging / discharging is large, which causes a problem of rapid deterioration of life characteristics. Meanwhile, negative electrodes that combine silicon-based active materials and carbon-based active materials have been developed, but the proportion of silicon-based active materials used in the negative electrodes must be reduced in order to control the volume expansion of the silicon-based active materials, making it difficult to realize the high capacity and rapid charging characteristics of silicon-based active materials.
[0023] In order to solve these problems, the secondary battery of the present invention is characterized in that the weight ratio of the silicon-based active material contained in the first anode 200 and the carbon-based active material contained in the second anode 300 is adjusted to the above-mentioned range. By using the silicon-based active material in the first anode 200 and the carbon-based active material in the second anode 300 in the above-mentioned weight ratio, the secondary battery of the present invention can lower the charging potential of the silicon-based active material to a preferred level by the carbon-based active material, thereby mitigating the degree of volumetric expansion / contraction of the silicon-based active material during charging / discharging, and can fully exhibit the high capacity and rapid charging characteristics of the silicon-based active material.
[0024] The secondary battery of the present invention includes a first negative electrode 200 containing a silicon-based active material and a second negative electrode 300 containing a carbon-based active material. Specifically, the secondary battery of the present invention uses different negative electrodes containing different active materials, so that each negative electrode can contain components with a suitable composition, and even if the proportion of the silicon-based active material used in the secondary battery is increased, the high capacity characteristics and rapid charging characteristics of the silicon-based active material can be fully exhibited without deteriorating the life characteristics.
[0025] The secondary battery 1 of the present invention includes one or more positive electrodes 100. The positive electrodes 100 include a positive electrode active material layer 120.
[0026] Specifically, the positive electrode 100 may include a positive electrode current collector 110 and a positive electrode active material layer 120 formed on at least one surface of the positive electrode current collector 110 .
[0027] The positive electrode current collector 110 is not particularly limited as long as it has high conductivity without causing a chemical change in the battery. Specifically, the positive electrode current collector 110 may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy.
[0028] The positive electrode current collector 110 may usually have a thickness of 3 to 500 μm.
[0029] The positive electrode current collector 110 may have a fine unevenness on its surface to strengthen the binding force of the negative electrode active material. For example, the positive electrode current collector 110 may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0030] The positive electrode active material layer 120 is formed on at least one surface of the positive electrode current collector 110. Specifically, the positive electrode active material layer 120 may be formed on one surface or both surfaces of the positive electrode current collector 110.
[0031] The positive electrode active material layer 120 may include a positive electrode active material.
[0032] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, a lithium transition metal composite oxide containing at least one transition metal selected from the group consisting of nickel, cobalt, manganese, and aluminum and lithium, preferably, a lithium transition metal composite oxide containing a transition metal containing nickel, cobalt, and manganese and lithium may be included.
[0033] More specifically, examples of the lithium transition metal composite oxide include lithium-manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium-cobalt-based oxides (e.g., LiCoO2, etc.), lithium-nickel-based oxides (e.g., LiNiO2, etc.), lithium-nickel-manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), lithium-nickel-cobalt-based oxides (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), lithium-manganese-cobalt-based oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1), or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are the atomic fractions of independent elements, respectively, with 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc.) etc. may be mentioned, and one or more of these compounds may be included. Among these, in terms of being able to enhance the capacity characteristics and stability of the battery, the lithium transition metal composite oxide is LiCoO2, LiMnO2, LiNiO2, lithium-nickel-manganese-cobalt oxide (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.), etc. may be, and considering the remarkable improvement effect by controlling the types and content ratios of the constituent elements forming the lithium transition metal composite oxide, the lithium transition metal composite oxide is Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc. may be, and one or more of these mixtures may be used.
[0034] The positive electrode active material may be contained in the positive electrode active material layer at 80% to 99% by weight, preferably 92% to 98.5% by weight, considering sufficient capacity display of the positive electrode active material, etc.
[0035] The positive electrode active material layer 120 may further include a positive electrode binder and / or a positive electrode conductive material in addition to the positive electrode active material.
[0036] The positive electrode binder is a component that assists in binding between the active material and the conductive material and between the active material and the current collector, and specifically may include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, and may include preferably polyvinylidene fluoride.
[0037] The positive electrode binder may be contained in the positive electrode active material layer in an amount of 1 wt % to 20 wt %, preferably 1.2 wt % to 10 wt %, in order to ensure sufficient binding strength between components such as the positive electrode active material.
[0038] The positive electrode conductive material may be used to assist and improve the conductivity of the secondary battery, and is not particularly limited as long as it has conductivity without causing a chemical change. Specifically, the positive electrode conductive material may include at least one selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives, and preferably includes carbon black in terms of improving conductivity.
[0039] The positive electrode conductive material is preferably a conductive material having a specific surface area of 80 m2 or less, which facilitates dispersion of the positive electrode conductive material during preparation of a slurry for forming a positive electrode active material layer and further improves electrical conductivity. 2 / g~200m 2 / g, preferably 100m 2 / g~150m 2 / g.
[0040] In order to ensure sufficient electrical conductivity, the positive electrode conductive material may be contained in the positive electrode active material layer in an amount of 1% by weight to 20% by weight, preferably 1.2% by weight to 10% by weight.
[0041] The thickness of the positive electrode active material layer 120 may be 30 μm to 400 μm, and preferably 40 μm to 110 μm. In this specification, the thickness of the positive electrode active material layer may be the thickness of one positive electrode active material layer formed on one surface of the positive electrode current collector 110.
[0042] The porosity of the positive electrode 100 may be 20% to 35%, and preferably 20% to 28%. The porosity of the positive electrode 100 may be measured using a porosity measuring method represented by the following Equation 1.
[0043] [Formula 1] Positive electrode porosity (%) = {1-(positive electrode density / positive electrode true density)} x 100
[0044] In Equation 1, the true density of the positive electrode is the density of the positive electrode active material layer measured when a positive electrode is cut into a certain size and pressed with a press until the thickness of the positive electrode stops changing, and the electrode density of the positive electrode is the density of the positive electrode active material layer measured when a positive electrode is cut into a certain size.
[0045] The positive electrode 100 may be manufactured by coating a positive electrode slurry including a positive electrode active material, and optionally a binder, a conductive material, and a solvent for forming a positive electrode slurry, on the positive electrode current collector 110, followed by drying and rolling.
[0046] The solvent for forming the positive electrode slurry may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material and, optionally, a binder and a conductive material are included. For example, the solvent for forming the positive electrode slurry may be included in the positive electrode slurry so that the concentration of solids including the positive electrode active material and, optionally, a binder and a conductive material is 50 wt % to 95 wt %, preferably 70 wt % to 90 wt %.
[0047] The negative electrode is a plurality of negative electrodes, and includes a first negative electrode 200 and a second negative electrode 300. The first negative electrode 200 and the second negative electrode 300 may each be included in one or more, specifically, in a plurality, in the negative electrode.
[0048] The first negative electrode 200 includes a silicon-based active material, and the second negative electrode 300 includes a carbon-based active material, and a weight ratio of the silicon-based active material contained in the first negative electrode 200 to the carbon-based active material contained in the second negative electrode 300 is 40:60 to 90:10. Specifically, when the first negative electrode 200 is multiple, "the weight of the silicon-based active material contained in the first negative electrode 200" may mean the total weight of the silicon-based active material contained in the multiple first negative electrodes 200, and when the second negative electrode 300 is multiple, "the weight of the carbon-based active material contained in the second negative electrode 300" may mean the total weight of the carbon-based active material contained in the multiple second negative electrodes 300. In this case, the weight ratio of the silicon-based active material contained in the first negative electrode 200 to the carbon-based active material contained in the second negative electrode 300 may be the ratio of the total weight of the silicon-based active material contained in the multiple first negative electrodes 200 to the total weight of the carbon-based active material contained in the multiple second negative electrodes 300.
[0049] The secondary battery of the present invention is characterized in that the weight ratio of the silicon-based active material contained in the first anode 200 and the carbon-based active material contained in the second anode 300 is adjusted to the above-mentioned range. In general, silicon-based active materials are known to have a higher charging potential and excellent rapid charging characteristics compared to carbon-based active materials. However, due to the high charging potential of the silicon-based active material, the voltage of the silicon-based active material changes significantly during charging and discharging, which causes a sudden volume expansion / contraction, resulting in a sudden decrease in life characteristics. The secondary battery of the present invention uses the silicon-based active material in the first anode 200 and the carbon-based active material in the second anode 300 in the above-mentioned weight ratio, so that the charging potential of the silicon-based active material can be lowered to a preferred level by the carbon-based active material, thereby mitigating the degree of volume expansion / contraction of the silicon-based active material during charging and discharging, and can fully exhibit the high capacity and rapid charging characteristics of the silicon-based active material.
[0050] The secondary battery of the present invention includes a first negative electrode 200 containing a silicon-based active material and a second negative electrode 300 containing a carbon-based active material. Specifically, the secondary battery of the present invention uses different negative electrodes containing different active materials, so that each negative electrode can contain components with a suitable composition, and even if the proportion of the silicon-based active material used in the secondary battery is increased, the high capacity characteristics and rapid charging characteristics of the silicon-based active material can be fully exhibited without deteriorating the life characteristics.
[0051] If the weight of the silicon-based active material is less than 40 wt % and the weight of the carbon-based active material is more than 60 wt % based on the total weight of the silicon-based active material contained in the first anode 200 and the carbon-based active material contained in the second anode 300, the proportion of the carbon-based active material in the entire anode is high. In this case, if the proportion of the carbon-based active material in the entire anode is high, the capacity of the anode is reduced and the overall N / P ratio (N / P ratio) of the secondary battery (to be described later) is reduced. all / P all Ratio(N all / P allAs a result, the ratio of silicon-based active material used during charging and discharging of the negative electrode becomes higher, and the volume expansion / contraction of the silicon-based active material has a large effect on the secondary battery, which may result in a decrease in life performance. In addition, the potential of the carbon-based active material becomes very low during high-speed charging, for example, a negative (-) potential may be formed, and if the ratio of carbon-based active material used in the entire negative electrode becomes high, lithium deposition may occur, which is not good in terms of life performance during high-speed charging.
[0052] If the weight of the silicon-based active material exceeds 90 wt % and the weight of the carbon-based active material is less than 10 wt % based on the total weight of the silicon-based active material contained in the first negative electrode 200 and the carbon-based active material contained in the second negative electrode 300, the proportion of the silicon-based active material is high, which may cause serious problems in volume expansion / contraction due to charging / discharging, and may result in a decrease in life performance. In addition, if the usage rate of the silicon-based active material in the entire negative electrode is too high, the positive electrode 100 forms a high potential due to the high potential of the silicon-based active material during battery operation, which may cause an increase in resistance in the positive electrode 100, and therefore may result in a decrease in life performance.
[0053] In the secondary battery of the present invention, the weight ratio of the silicon-based active material contained in the first negative electrode 200 to the carbon-based active material contained in the second negative electrode 300 may be 40:60 to 90:10, preferably 60:40 to 75:25. When the weight ratio is within this range, the rapid charging characteristics, capacity, and life characteristics of the secondary battery can be further improved.
[0054] In the secondary battery of the present invention, the weight ratio of the silicon-based active material contained in the first anode 200 and the carbon-based active material contained in the second anode 300 may be realized by adjusting the amount of active material contained in the first anode 200 and the second anode 300, or by adjusting the number of the first anode 200 and the second anode 300, as shown in Fig. 1. Meanwhile, the first anode 200 and the second anode 300 in Fig. 1 are arbitrarily illustrated, and the number of the first anode and the second anode is not limited to that shown in Fig. 1.
[0055] The first negative electrode 200 includes a silicon-based active material. Specifically, the first negative electrode 200 may include only a silicon-based active material as an active material, and may not include a carbon-based active material.
[0056] The first negative electrode 200 includes a first negative electrode current collector 210 and a first negative electrode active material layer 220 formed on at least one surface of the first negative electrode current collector 210, and the first negative electrode active material layer 220 may include the silicon-based active material.
[0057] The first negative electrode current collector 210 may include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may preferably include copper.
[0058] The first negative electrode current collector 210 may have a thickness of usually 3 μm to 500 μm, preferably 5 μm to 30 μm.
[0059] The first negative electrode current collector 210 may have fine projections and recesses on its surface to strengthen the binding force of the negative electrode active material. For example, the first negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0060] The first negative electrode active material layer 220 is formed on at least one surface of the first negative electrode current collector 210. Specifically, as shown in FIG 1, the first negative electrode active material layer 220 may be formed on one surface or both surfaces of the first negative electrode current collector 210.
[0061] The first negative electrode active material layer 220 may include the silicon-based active material.
[0062] The silicon-based active material is SiO x (0≦x<2) In the case of SiO2, it does not react with lithium ions and cannot store lithium, so x is preferably within the above range.
[0063] Specifically, the silicon-based active material may contain Si. Conventionally, Si is advantageous in that its capacity is about 2.5 to 3 times higher than that of silicon oxide (for example, SiO x (0 < x < 2)). However, since the degree of volume expansion / contraction due to charge / discharge of Si is much larger than that of silicon oxide, commercialization is not easier. However, in the case of the secondary battery of the present invention, even when using a silicon-based active material containing Si, the charging potential of the active material can be lowered to a preferable level, so that while preventing a decrease in life characteristics, the high capacity and rapid charging characteristics of the silicon-based active material can be improved. Specifically, the silicon-based active material may mostly consist of Si, and more specifically, the silicon-based active material may consist of Si.
[0064] The average particle size (D 50 ) of the silicon-based active material is 1 μm to 10 μm, preferably 2 μm to 6 μm, in terms of being able to more smoothly form a conductive network for maintaining electrical conductivity based on the structural stability of the active material during charge / discharge, or making it easier to approach a binder for binding the active material and the current collector.
[0065] The silicon-based active material may be contained in the first negative electrode active material layer at 60% to 90% by weight, preferably 70% to 80% by weight, in terms of sufficiently embodying the high capacity of the silicon-based active material in the secondary battery while minimizing the influence of volume expansion / contraction of the silicon-based active material on the battery.
[0066] The first negative electrode active material layer 220 may further contain a first negative electrode binder and a first negative electrode conductive material together with the silicon-based active material.
[0067] The first negative electrode binder may be used to improve the adhesive force between the silicon-based active material and the negative electrode current collector or to enhance the binding force between the silicon-based active materials.
[0068] Specifically, the first negative electrode binder may include at least one selected from the group consisting of styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, acrylic rubber, butyl rubber, fluoro rubber, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyethylene glycol (PEG), polyacrylonitrile (PAN), and polyacryl amide (PAM).
[0069] Preferably, the first negative electrode binder may contain at least one selected from the group consisting of polyvinyl alcohol, polyacrylic acid, polyacrylonitrile, and polyacrylamide, preferably polyvinyl alcohol and polyacrylic acid, in terms of having high strength, excellent resistance to volume expansion / contraction of the silicon-based active material, and excellent flexibility to the negative electrode binder to prevent distortion and warping of the electrode. When the first negative electrode binder contains polyvinyl alcohol and polyacrylic acid, the first negative electrode binder may be a copolymer of polyvinyl alcohol and polyacrylic acid, specifically, a copolymer of polyvinyl alcohol and polyacrylic acid containing a unit derived from vinyl alcohol and a unit derived from acrylic acid in a weight ratio of 50:50 to 90:10, preferably a weight ratio of 55:45 to 80:20.
[0070] The first negative electrode binder may include hydrogen atoms in the first negative electrode binder substituted with Li, Na, Ca, or the like in order to allow the first negative electrode binder to be better dispersed in an aqueous solvent such as water and to more smoothly coat the active material and improve binding strength when a slurry for forming a negative electrode active material layer is prepared.
[0071] The first negative electrode binder may be included in the first negative electrode active material layer in an amount of 5 wt % to 30 wt %, preferably 10 wt % to 20 wt %, and when the amount is within this range, the silicon-based active material can be smoothly bound to minimize a problem of volume expansion of the active material, and at the same time, when a slurry for forming a negative electrode active material layer is prepared, the negative electrode binder can be easily dispersed, and the coatability and phase stability of the slurry can be improved.
[0072] The first negative electrode conductive material may be used to assist and improve the conductivity of the secondary battery, and is not particularly limited as long as it has conductivity without causing a chemical change. Specifically, the first negative electrode conductive material may include at least one selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives, and preferably includes carbon black in terms of realizing high conductivity.
[0073] The first negative electrode conductive material is a material having a specific surface area of 80 m2 or less, which facilitates dispersion of the negative electrode conductive material during preparation of a slurry for forming a negative electrode active material layer and further improves electrical conductivity. 2 / g~200m 2 / g, preferably 100m 2 / g~150m 2 / g.
[0074] The first negative electrode conductive material may be contained in the first negative electrode active material layer in an amount of 5 wt % to 20 wt %, preferably 7 wt % to 15 wt %, and this range is preferable in that an excellent conductive network can be formed while mitigating an increase in resistance due to the negative electrode binder.
[0075] The first negative electrode active material layer 220 may have a thickness of 10 μm to 100 μm, and preferably 20 μm to 50 μm. In this specification, the thickness of the first negative electrode active material layer 220 may be the thickness of one first negative electrode active material layer 220 formed on one surface of the first negative electrode current collector 210.
[0076] The porosity of the first negative electrode 200 may be 28% to 50%, preferably 32% to 40%, and within this range, the porosity can appropriately accommodate the volume expansion / contraction of the silicon-based active material while maintaining the degree of contact between the active materials at an appropriate level, thereby improving the conductivity.
[0077] In this specification, the porosity of the first negative electrode 200 can be calculated by the following Equation 2.
[0078] [Formula 2] Porosity of first negative electrode (%)={1-(electrode density of first negative electrode / true density of first negative electrode)}×100
[0079] In Equation 2, the true density of the first negative electrode is the density of the first negative electrode active material layer measured when a negative electrode of a certain size is cut and pressed in a press until the thickness of the negative electrode stops changing, and the electrode density of the first negative electrode is the density of the first negative electrode active material layer measured when a first negative electrode of a certain size is cut and pressed in a press until the thickness of the negative electrode stops changing.
[0080] In the first negative electrode 200, the N1 / P ratio calculated by the following formula a may be 2.2 to 3.0, preferably 2.4 to 2.8.
[0081] [Formula a] N1 / P ratio={(discharge capacity per unit area of one first negative electrode active material layer in the first negative electrode) / (discharge capacity per unit area of one positive electrode active material layer in the positive electrode)}
[0082] By adjusting the N1 / P ratio for the first negative electrode within this range, the usage rate of the silicon-based active material during operation of the first negative electrode can be reduced to an appropriate level, thereby minimizing the effect of volume expansion of the silicon-based active material on the secondary battery.
[0083] The N1 / P ratio can be calculated by preparing a half-cell of each of the first negative electrode 200 and the positive electrode 100, calculating the discharge capacity per unit area of the first negative electrode 200 and the positive electrode 100, and then substituting the results into Equation a.
[0084] The first negative electrode 200 may be manufactured by coating a negative electrode slurry including a silicon-based active material and, optionally, a first negative electrode binder, a first negative electrode conductive material, and a solvent for forming a negative electrode slurry on the first negative electrode current collector, followed by drying and rolling.
[0085] The solvent for forming the negative electrode slurry may include, for example, at least one selected from the group consisting of distilled water, ethanol, methanol, and isopropyl alcohol, preferably distilled water, in order to facilitate dispersion of the negative electrode active material, the negative electrode binder, and / or the negative electrode conductive material.
[0086] The solvent for forming the negative electrode slurry may be contained in the negative electrode slurry so that the concentration of the solids in the negative electrode slurry is 15% by weight to 45% by weight, preferably 20% by weight to 30% by weight, taking into consideration the viscosity, coating property, dispersibility, and the like of the negative electrode slurry.
[0087] The second negative electrode 300 includes a carbon-based active material. Specifically, the second negative electrode 300 may include only a carbon-based active material as an active material, and may not include a silicon-based active material. By including a carbon-based active material, the second negative electrode 300 can reduce the overall charging potential of the negative electrode, and can prevent a sudden volume expansion of the silicon-based active material in the first negative electrode.
[0088] Specifically, the second negative electrode 300 includes a second negative electrode current collector 310 and a second negative electrode active material layer 320 formed on at least one surface of the second negative electrode current collector 310, and the second negative electrode active material layer 320 may include the carbon-based active material.
[0089] The second negative electrode current collector 310 may include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may preferably include copper.
[0090] The second negative electrode current collector 310 may have a thickness of usually 3 μm to 500 μm, preferably 5 μm to 30 μm.
[0091] The second negative electrode current collector 310 may have a fine unevenness on its surface to strengthen the binding force of the negative electrode active material. For example, the second negative electrode current collector 310 may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0092] The second negative electrode active material layer 320 is formed on at least one surface of the second negative electrode current collector 310. Specifically, the second negative electrode active material layer 320 may be formed on one surface or both surfaces of the second negative electrode current collector 310.
[0093] The second negative electrode active material layer 320 may include the carbon-based active material.
[0094] Specifically, the carbon-based active material may include at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and may include preferably at least one of artificial graphite and natural graphite, more preferably artificial graphite and natural graphite.
[0095] The average particle size (D 50 ) may be 10 μm to 30 μm, preferably 15 μm to 25 μm, from the viewpoint of reducing side reactions with the electrolyte based on structural stability during charging and discharging.
[0096] In order to fully utilize the capacity of the carbon-based active material, the carbon-based active material may be contained in the second negative electrode active material layer in an amount of 90% by weight to 99% by weight, preferably 92% by weight to 98% by weight.
[0097] The second negative electrode active material layer 320 may further include a second negative electrode binder and a second negative electrode conductive material in addition to the carbon-based active material.
[0098] The second negative electrode binder may be used to improve the adhesive strength between the carbon-based active material and the negative electrode current collector or to increase the binding strength between the carbon-based active materials.
[0099] Specifically, the second negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer rubber (EPDM rubber), styrene-butadiene rubber (SBR), and fluororubber, and preferably includes styrene-butadiene rubber (SBR) in terms of improving the adhesive strength between the carbon-based active material and the current collector to an excellent level.
[0100] The second negative electrode binder may be contained in the second negative electrode active material layer in an amount of 0.5% by weight to 10% by weight, preferably 1% by weight to 5% by weight, and more preferably 1.5% by weight to 3.5% by weight.
[0101] The second negative electrode conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0102] The second negative electrode conductive material may be contained in the second negative electrode active material layer in an amount of 0.5% by weight to 5% by weight.
[0103] The second negative electrode conductive material is a conductive material having a specific surface area of 80 m2 or less, which facilitates dispersion of the negative electrode conductive material during preparation of a slurry for forming a negative electrode active material layer and further improves electrical conductivity. 2 / g~200m 2 / g, preferably 100m 2 / g~150m 2 / g.
[0104] The second negative electrode active material layer 320 may have a thickness of 20 μm to 200 μm, and preferably 60 μm to 120 μm. In this specification, the thickness of the second negative electrode active material layer 320 may be the thickness of one second negative electrode active material layer 320 formed on one surface of the negative electrode current collector 31.
[0105] The porosity of the second negative electrode 300 may be 20% to 40%, and preferably 21% to 30%, and being in this range is preferable in that it can improve the wettability of the electrolyte while also improving the energy density to a preferred level.
[0106] The porosity of the second negative electrode 300 may be calculated by applying Equation 2 to the porosity of the first negative electrode 200.
[0107] In the second negative electrode 300, the N2 / P ratio calculated by the following formula b may be 1.0 to 1.3, preferably 1.05 to 1.1.
[0108] [Formula b] N2 / P ratio={(discharge capacity per unit area of one second negative electrode active material layer in the second negative electrode) / (discharge capacity per unit area of one positive electrode active material layer in the positive electrode)}.
[0109] Adjusting the N2 / P ratio for the second negative electrode within this range is preferable in that stable performance can be obtained while using the entire potential range of the second negative electrode 300 and the positive electrode 100.
[0110] The N2 / P ratio can be calculated by preparing a half-cell of the second negative electrode 300 or the positive electrode 100, calculating the discharge capacity per unit area of the second negative electrode 300 and the positive electrode 100, and then substituting the results into Equation b.
[0111] In the secondary battery of the present invention, the positive electrode 100 and the negative electrodes 200, 300 may be stacked alternately. For example, as shown in Fig. 1, the positive electrode 100 may be disposed between the negative electrodes 200, 300, and in this case, the first negative electrode 200 and the second negative electrode 300 may be stacked alternately or in any order.
[0112] In the secondary battery of the present invention, N calculated by the following formula c all / P all The ratio may be 2 to 3, preferably 2.2 to 2.8, and more preferably 2.40 to 2.55. When the ratio is within this range, the high capacity and rapid charging characteristics of the silicon-based active material can be exhibited, while the effect of the volume expansion / contraction of the silicon-based active material on the battery can be minimized, thereby further improving the life characteristics of the secondary battery.
[0113] [Formula C] N all / P all Ratio = {(total amount of discharge capacity per unit area of negative electrodes present in secondary battery) / (total amount of discharge capacity per unit area of positive electrodes present in secondary battery)}
[0114] N all / P all Specifically, the ratio is obtained by measuring the discharge capacity per unit area of each of a plurality of negative electrodes present in the secondary battery, calculating the total amount thereof, measuring the discharge capacity per unit area of each of a plurality of positive electrodes present in the secondary battery, calculating the total amount thereof, and then substituting the values obtained from the above into formula c.
[0115] 1, the separator 400 is interposed between the positive electrode 100 and the negative electrodes 200, 300. Specifically, the positive electrode 100 and the negative electrodes 200, 300 are alternately stacked with the separator 400 interposed therebetween.
[0116] The separator 400 separates the negative electrode 200, 300 from the positive electrode 100 to provide a passage for lithium ions to move. Any separator generally used in lithium secondary batteries may be used without any particular limitation. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte impregnation ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, a separator coated with a ceramic component or a polymer material may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.
[0117] The electrolyte (not shown) may be, but is not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, or the like that can be used when manufacturing a secondary battery.
[0118] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0119] The organic solvent may be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent that may be used include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond-oriented ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant capable of enhancing the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, and the electrolyte exhibits excellent performance.
[0120] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within a range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0121] The secondary battery may be manufactured by inserting a separator between the negative electrode and the positive electrode and then injecting an electrolyte into the separator according to a conventional method for manufacturing a secondary battery.
[0122] The secondary battery according to the present invention is useful in portable devices such as mobile phones, notebook computers, and digital cameras, and in the field of electric vehicles such as hybrid electric vehicles (HEVs), and may be particularly preferably used as a constituent battery of medium- to large-sized battery modules.
[0123] Such a medium- to large-sized battery module may be preferably applied to power sources that require high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.
[0124] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the exemplary embodiments set forth herein.
[0125] Working Example Example 1: Manufacture of secondary battery <Production of positive electrodes> As a positive electrode active material, Li[Ni 0.6 Co0.2 Mn 0.2 ]O2(average particle size (D 50 The positive electrode slurry was prepared by adding carbon black (product name: Super C65, manufacturer: Timcal) as a positive electrode conductive material, and polyvinylidene fluoride (PVdF) as a positive electrode binder in a weight ratio of 97:1.5:1.5 to N-methyl-2-pyrrolidone (NMP) as a solvent for forming the positive electrode slurry (solid concentration 78 wt%).
[0126] The positive electrode current collector was an aluminum current collector (thickness: 12 μm) and the positive electrode slurry was applied to both sides at 454 mg / 25 cm. 2 The coated positive electrode was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a positive electrode active material layer (thickness: 54 μm), which was used as the positive electrode according to Example 1 (positive electrode thickness: 120 μm, porosity: 24%). A plurality of positive electrodes (20 pieces) were prepared.
[0127] <Production of negative electrodes> 1. Preparation of the first negative electrode Silicon-based active material Si (average particle size (D 50 :3μm), carbon black (product name: Super C65, manufacturer: Timcal) as the first negative electrode conductive material, and a copolymer of polyvinyl alcohol and polyacrylic acid (containing vinyl alcohol-derived units and acrylic acid-derived units in a ratio of 66:34, weight average molecular weight: about 360,000g / mol) as the first negative electrode binder in a weight ratio of 75:10:15 were added to distilled water as a solvent for forming a negative electrode slurry to prepare a negative electrode slurry (solid concentration: 25% by weight).
[0128] The negative electrode current collector was a copper current collector (thickness: 15 μm). The negative electrode slurry was applied to both sides of the copper current collector at a rate of 91.8 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a first negative electrode active material layer (thickness: 26.5 μm), which was used as the first negative electrode A (negative electrode thickness: 68 μm, negative electrode porosity: 34%). A plurality of first negative electrodes A (17 pieces) were prepared.
[0129] The negative electrode slurry was applied to one side of a copper current collector (thickness: 15 μm) at a rate of 91.8 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a first negative electrode active material layer (thickness: 26.5 μm), which was used as the first negative electrode B (negative electrode thickness: 41.5 μm, negative electrode porosity: 34%). A plurality of first negative electrodes B (2 pieces) were prepared.
[0130] The first negative electrode A and the first negative electrode B were used as a first negative electrode.
[0131] 2. Fabrication of the second negative electrode As a carbon-based active material, artificial graphite (average particle size (D 50 ): 15 μm) and natural graphite (average particle size (D 50 A mixture of 18μm (18μm) and 100μm (18μm) in a weight ratio of 90:10, carbon black (product name: Super C65, manufacturer: Timcal) as the second negative electrode conductive material, styrene-butadiene rubber (SBR) as the second negative electrode binder, and carboxymethyl cellulose (CMC) as the thickener in a weight ratio of 95.65:0.75:1.1:2.5 was added to distilled water as a solvent for forming the negative electrode slurry to prepare the negative electrode slurry (solid concentration: 48% by weight).
[0132] The negative electrode slurry was applied to both sides of a copper current collector (thickness: 8 μm) at a rate of 298 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a second negative electrode active material layer (thickness: 74 μm), which was used as a second negative electrode (negative electrode thickness: 156 μm, negative electrode porosity: 27%). A plurality of second negative electrodes (2 pieces) were prepared.
[0133] <Secondary battery manufacturing> 1. Manufacturing of secondary batteries The negative electrodes (first and second negative electrodes) and the positive electrodes were alternately stacked with a polyethylene separator between them, and an electrolyte was injected to manufacture a secondary battery. The two first negative electrodes B were disposed at the outermost shell of the secondary battery, with the first negative electrode active material layer facing the positive electrode active material layer of the positive electrode. The first negative electrode A and the second negative electrode were alternately stacked with the positive electrode, with the negative electrode active material layer facing the positive electrode active material layer of the positive electrode.
[0134] The electrolyte was an organic solvent made by mixing fluoroethylene carbonate (FEC) and diethyl carbonate (DMC) in a volume ratio of 30:70, to which was added 3 wt% vinylene carbonate based on the total weight of the electrolyte, and LiPF6 was added as a lithium salt at a concentration of 1M.
[0135] The secondary battery contained 17 first negative electrodes A, 2 first negative electrodes B, 2 second negative electrodes, and 20 positive electrodes. The weight ratio of the silicon-based active material contained in the first negative electrodes (first negative electrodes A and first negative electrodes B) to the carbon-based active material in the second negative electrodes was 68.5:31.5. Meanwhile, the weight ratio of the total weight of the first negative electrodes to the total weight of the second negative electrodes was 90:10.
[0136] 2.N / P ratio (1)N1 / P ratio A negative electrode for measuring the N / P ratio was manufactured in the same manner as in the manufacturing method of the first negative electrode A, except that the negative electrode active material layer was formed only on one side of the copper current collector. A coin-shaped half-cell including the negative electrode for measuring the N / P ratio, a lithium metal counter electrode facing the negative electrode for measuring the N / P ratio, and a polyethylene separator and electrolyte interposed between the negative electrode for measuring the N / P ratio and the lithium metal counter electrode was manufactured, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was multiplied by the loading amount (91.8 mg / 25 cm). 2 =3.67mg / cm 2 =0.00367g / cm 2 ) to calculate the "discharge capacity per unit area of one first negative electrode active material layer in the first negative electrode" (unit: mAh / cm 2 ).
[0137] A positive electrode for measuring the N / P ratio was manufactured in the same manner as the positive electrode manufacturing method, except that the positive electrode active material layer was formed only on one side of the aluminum current collector. A coin-shaped half-cell including the positive electrode for measuring the N / P ratio, a lithium metal counter electrode facing the positive electrode for measuring the N / P ratio, a polyethylene separator and an electrolyte interposed between the positive electrode for measuring the N / P ratio and the lithium metal counter electrode was manufactured, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was multiplied by the loading amount (454 mg / 25 cm). 2 =18.16mg / cm 2 =0.01816g / cm 2 ) to calculate the "discharge capacity per unit area of one positive electrode active material layer in the positive electrode" (unit: mAh / cm 2 ).
[0138] The N1 / P ratio was calculated by the following formula a, and the N1 / P ratio of the secondary battery of Example 1 was 2.69.
[0139] [Formula a] N1 / P ratio=(discharge capacity per unit area of one first negative electrode active material layer in the first negative electrode / discharge capacity per unit area of one positive electrode active material layer in the positive electrode).
[0140] (2)N2 / P ratio A negative electrode for measuring the N / P ratio was manufactured in the same manner as the manufacturing method of the second negative electrode, except that the negative electrode active material layer was formed only on one side of the copper current collector. A coin-shaped half-cell including the negative electrode for measuring the N / P ratio, a lithium metal counter electrode facing the negative electrode for measuring the N / P ratio, and a polyethylene separator and electrolyte interposed between the negative electrode for measuring the N / P ratio and the lithium metal counter electrode was manufactured, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was multiplied by the loading amount (298 mg / 25 cm 2 =11.92mg / cm 2 =0.01192g / cm 2 ) to obtain the "discharge capacity per unit area of one second negative electrode active material layer in the second negative electrode" (unit: mAh / cm 2 ).
[0141] A positive electrode for measuring the N / P ratio was manufactured in the same manner as the positive electrode manufacturing method, except that the positive electrode active material layer was formed only on one side of the aluminum current collector. A coin-shaped half-cell including the positive electrode for measuring the N / P ratio, a lithium metal counter electrode facing the positive electrode for measuring the N / P ratio, a polyethylene separator and an electrolyte interposed between the positive electrode for measuring the N / P ratio and the lithium metal counter electrode was manufactured, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was multiplied by the loading amount (454 mg / 25 cm 2 =18.16mg / cm 2 =0.01816g / cm 2 ) to calculate the "discharge capacity per unit area of one positive electrode active material layer in the positive electrode" (unit: mAh / cm 2 ).
[0142] The N2 / P ratio was calculated by the following formula b, and the N2 / P ratio of the secondary battery of Example 1 was 1.08.
[0143] [Formula b] N2 / P ratio=(discharge capacity per unit area of one second negative electrode active material layer in the second negative electrode / discharge capacity per unit area of one positive electrode active material layer in the positive electrode).
[0144] (3)N all / P all ratio N all / P all The ratio was calculated in the following way.
[0145] The "discharge capacity per unit area of one first negative electrode active material layer in the first negative electrode" obtained in (1) above was multiplied by the number of first negative electrode active material layers in the secondary battery of Example 1 to obtain the total discharge capacity of the first negative electrode. The "discharge capacity per unit area of one second negative electrode active material layer in the second negative electrode" obtained in (2) above was multiplied by the number of second negative electrode active material layers in the secondary battery of Example 1 to obtain the total discharge capacity of the second negative electrode. The total discharge capacity of the first negative electrode and the total discharge capacity of the second negative electrode were added together to obtain the total discharge capacity of the negative electrodes present in the secondary battery of Example 1.
[0146] The "discharge capacity per unit area of one positive electrode active material layer in the positive electrode" obtained in (1) above was multiplied by the number of positive electrode active material layers in the secondary battery of Example 1 to determine the total discharge capacity of the positive electrodes present in the secondary battery of Example 1.
[0147] According to the following formula c, N all / P all The ratio was calculated and N all / P all The ratio was 2.53.
[0148] [Formula C] N all / P all Ratio = (total amount of discharge capacity per unit area of negative electrodes present in the secondary battery / total amount of discharge capacity per unit area of positive electrodes present in the secondary battery).
[0149] Example 2: Manufacture of secondary battery The secondary battery of Example 2 was manufactured in the same manner as in Example 1, except that 15 first negative electrodes A, 2 first negative electrodes B, 4 second negative electrodes, and 20 positive electrodes were prepared to manufacture the secondary battery.
[0150] In Example 2, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 49.2:50.8, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 80:20.
[0151] In the secondary battery of Example 2, N all / P all The ratio was 2.37.
[0152] Example 3: Manufacture of secondary battery The secondary battery of Example 3 was manufactured in the same manner as in Example 1, except that 18 first negative electrodes A, 2 first negative electrodes B, 1 second negative electrode, and 20 positive electrodes were prepared to manufacture the secondary battery.
[0153] In Example 3, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 82.1:17.9, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 95:5.
[0154] In the secondary battery of Example 3, N all / P all The ratio was 2.61.
[0155] Comparative Example 1: Manufacturing of secondary batteries A secondary battery of Comparative Example 1 was produced in the same manner as in Example 1, except that no second negative electrode was used, and 19 first negative electrodes A, 2 first negative electrodes B, and 20 positive electrodes were alternately stacked.
[0156] In Comparative Example 1, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 100:0, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 100:0.
[0157] In the secondary battery of Comparative Example 1, N all / P all The ratio was 2.69.
[0158] Comparative Example 2: Manufacturing of secondary batteries A secondary battery of Comparative Example 2 was manufactured in the same manner as in Example 1, except that 11 first negative electrodes A, 2 first negative electrodes B, 8 second negative electrodes, and 20 positive electrodes were prepared to manufacture the secondary battery.
[0159] In Comparative Example 2, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 26.6:73.4, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 60:40.
[0160] In the secondary battery of Comparative Example 2, N all / P all The ratio was 2.04.
[0161] Comparative Example 3: Manufacturing of secondary battery The secondary battery of Comparative Example 3 was manufactured in the same manner as in Example 1, except that 7 first negative electrodes A, 2 first negative electrodes B, 12 second negative electrodes, and 20 positive electrodes were prepared to manufacture the secondary battery.
[0162] In Comparative Example 3, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 13.9:86.1, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 40:60.
[0163] In the secondary battery of Comparative Example 3, N all / P all The ratio was 1.72.
[0164] Comparative Example 4: Manufacture of secondary battery The secondary battery of Comparative Example 4 was manufactured in the same manner as in Example 1, except that no first negative electrode was used and a second negative electrode active material layer was formed on only one side, not both sides, of the battery. Two negative electrodes manufactured in the same manner as the second negative electrode were arranged on the outermost shell, and 19 second negative electrodes and 20 positive electrodes were alternately stacked between them.
[0165] In Comparative Example 4, the weight ratio of the silicon-based active material in the first negative electrode to the carbon-based active material in the second negative electrode was 0:100, and the weight ratio of the total weight of the first negative electrode to the total weight of the second negative electrode was 0:100.
[0166] In the secondary battery of Comparative Example 1, N all / P all The ratio was 1.08.
[0167] Comparative Example 5: Manufacture of secondary battery <Production of negative electrodes> The negative electrode active material is silicon-based active material Si (average particle size (D 50 The carbon-based active material was a mixture of artificial graphite (average particle size (D):3 μm) and a carbon-based active material in a weight ratio of 68.5:31.5. 50 ): 15 μm) and natural graphite (average particle size (D 50 ):18 μm) in a weight ratio of 90:10 was used.
[0168] The negative electrode active material, carbon black (product name: Super C65, manufacturer: Timcal) as a negative electrode conductive material, and a copolymer of polyvinyl alcohol and polyacrylic acid (containing vinyl alcohol-derived units and acrylic acid-derived units in a ratio of 66:34, weight average molecular weight: about 360,000 g / mol) as a negative electrode binder were added in a weight ratio of 75:10:15 to distilled water as a solvent for forming a negative electrode slurry to prepare a negative electrode slurry (solid concentration: 25 wt%).
[0169] The negative electrode current collector was a copper current collector (thickness: 15 μm) and the negative electrode slurry was applied to both sides at 100.5 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 29.5 μm), which was used as the first negative electrode (negative electrode thickness: 44.5 μm, negative electrode porosity: 32.8%). A plurality of first negative electrodes (21 pieces) were prepared.
[0170] <Secondary battery manufacturing> A secondary battery of Comparative Example 5 was manufactured in the same manner as in Example 1, except that the negative electrode prepared above was used instead of the first negative electrode and the second negative electrode, and 21 negative electrodes and 20 positive electrodes prepared above were prepared to manufacture a secondary battery.
[0171] In the secondary battery of Comparative Example 5, N all / P all The ratio was 2.68.
[0172] Comparative Example 6: Manufacture of secondary battery <Production of negative electrodes> The negative electrode active material is silicon-based active material Si (average particle size (D 50 The carbon-based active material was a mixture of artificial graphite (average particle size (D):3 μm) and a carbon-based active material in a weight ratio of 68.5:31.5. 50 ): 15 μm) and natural graphite (average particle size (D 50 ):18 μm) in a weight ratio of 90:10 was used.
[0173] The negative electrode active material, carbon black (product name: Super C65, manufacturer: Timcal) as a negative electrode conductive material, styrene butadiene rubber as a negative electrode binder, and carboxymethyl cellulose as a thickener were added in a weight ratio of 95.65:0.75:1.1:2.5 to distilled water as a solvent for forming a negative electrode slurry to prepare a negative electrode slurry (solid concentration: 48 wt%).
[0174] The negative electrode current collector was a copper current collector (thickness: 15 μm) on both sides of which the negative electrode slurry was applied at 81.8 mg / 25 cm. 2 The coated negative electrode was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 23 μm), which was used as the first negative electrode (negative electrode thickness: 61 μm, negative electrode porosity: 35.4%). A plurality of negative electrodes (21 pieces) were prepared.
[0175] <Secondary battery manufacturing> A secondary battery of Comparative Example 6 was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used instead of the first negative electrode and the second negative electrode, and 21 negative electrodes and 20 positive electrodes manufactured as described above were prepared to manufacture a secondary battery.
[0176] In the secondary battery of Comparative Example 6, N all / P all The ratio was 2.78.
[0177] [Table 1]
[0178] Experimental Example 1: Evaluation of initial efficiency and capacity retention rate The secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 to 6 were evaluated for initial efficiency and capacity retention rate using an electrochemical charger / discharger.
[0179] The secondary battery was 1) charged (0.2C CC / CV charge, 4.2V, 0.05C cut) and discharged (0.2C CC discharge, 3.2V cut), which was the first cycle, and 2) charged and discharged under the conditions of 1.0C CC / CV charge, 4.2V, 0.05C cut) and discharge (0.5C CC discharge, 3.0V cut) from the second cycle to the 100th cycle.
[0180] The capacity retention rate was evaluated according to the following formula, and the results are shown in Table 2 below.
[0181] Capacity retention rate (%) = {(discharge capacity at 100th cycle) / (discharge capacity at 1st cycle)} x 100
[0182] [Table 2]
[0183] Referring to Table 2, it can be seen that the secondary batteries of Examples 1 to 3, which include a first negative electrode containing a silicon-based active material and a second negative electrode containing a carbon-based active material, and in which the silicon-based active material and the carbon-based active material contained in the first negative electrode and the second negative electrode are contained in a specific weight ratio, exhibit excellent capacity, initial efficiency, and life performance.
[0184] However, in the case of Comparative Example 1, since the negative electrode contains only a silicon-based active material as an active material, the positive electrode active material also forms a high potential due to the high potential of the silicon-based active material in the same operating voltage range as in the Examples. Therefore, in the case of Comparative Example 1, a problem occurs in which the resistance of the positive electrode increases as the potential of the positive electrode increases, and Comparative Example 1 is judged to show a lower life performance than the Examples.
[0185] In addition, in the case of Comparative Example 2 and Comparative Example 3, the proportion of the carbon-based active material used in the negative electrode is high, and the overall N / P ratio (N all / P allSince the ratio of the negative electrode active material involved in charging and discharging in the negative electrode becomes low, the proportion of the negative electrode active material involved in charging and discharging in the negative electrode increases, and the impact of the volume expansion / contraction of the silicon-based active material on the secondary battery becomes greater, resulting in a decrease in life performance.
[0186] In Comparative Example 4, since the negative electrode uses only a carbon-based active material as the active material, the life performance is not significantly reduced compared to the Examples. However, as will be described later, Comparative Example 4 has a significantly reduced energy density and high-speed charging performance, and is therefore not suitable for use in secondary batteries that require high-speed charging characteristics and high energy density.
[0187] In the case of Comparative Example 5, the ratio of the binder in the negative electrode composition is high, so that the volume expansion of the silicon-based active material can be controlled to some extent, but as the ratio of the binder in the negative electrode composition is high, the carbon-based active material generates high resistance, resulting in poor life performance. On the other hand, in the case of Comparative Example 6, the ratio of the binder in the negative electrode composition is low, so that the volume expansion / contraction of the silicon-based active material is difficult to control, resulting in poor life performance. Therefore, the secondary batteries of Comparative Examples 5 and 6 contain both the silicon-based active material and the carbon-based active material in one negative electrode, so that the composition of the negative electrode cannot be adjusted according to the characteristics of each active material, and therefore show poor life performance compared to the secondary batteries of the Examples.
[0188] Experimental example 2: Evaluation of fast charging life The capacity retention rate during high-speed charging was evaluated using an electrochemical charger / discharger for the secondary batteries manufactured in Examples 1 to 3 and Comparative Examples 1 to 6. The secondary batteries were 1) charged (0.2C CC / CV charge, 4.2V, 0.05C cut) and discharged (0.2C CC discharge, 3.2V cut), which was the first cycle, and 2) charged and discharged from the second cycle to the 100th cycle under the conditions of charge (2.0C CC / CV charge, 4.2V, 0.05C cut) and discharge (0.5C CC discharge, 3.2V cut).
[0189] The capacity retention rate was evaluated according to the following formula, and the results are shown in Table 3 below.
[0190] Capacity retention rate (%) = {(discharge capacity at 100th cycle) / (discharge capacity at 1st cycle)} x 100
[0191] [Table 3]
[0192] Referring to Table 3, it can be seen that the secondary batteries of Examples 1 to 3, which include a first negative electrode including a silicon-based active material and a second negative electrode including a carbon-based active material, and in which the silicon-based active material and the carbon-based active material included in the first negative electrode and the second negative electrode are present in a specific weight ratio, exhibit excellent life performance during fast charging.
[0193] However, in the case of Comparative Example 1, since the negative electrode contains only a silicon-based active material as an active material, the positive electrode active material also forms a high potential due to the high potential of the silicon-based active material in the same operating voltage range as in the Examples. Therefore, in the case of Comparative Example 1, a problem occurs in which the resistance of the positive electrode increases as the potential of the positive electrode increases, and it is therefore determined that Comparative Example 1 exhibits a lower fast charge life performance than the Examples.
[0194] In addition, in the case of carbon-based active materials, the potential is very low during high-speed charging, for example, a negative (-) potential may be formed. Therefore, in the cases of Comparative Examples 2, 3, and 4 in which the proportion of carbon-based active materials is high, lithium plating may occur during high-speed charging, which may significantly reduce the life performance.
[0195] In the case of Comparative Example 5, the proportion of the binder in the negative electrode composition is high, so that the volume expansion of the silicon-based active material can be controlled to some extent, but as the proportion of the binder in the negative electrode composition is high, the carbon-based active material generates high resistance, resulting in poor high-speed charging life performance. Meanwhile, in the case of Comparative Example 6, the proportion of the binder in the negative electrode composition is low, so that the volume expansion / contraction of the silicon-based active material is difficult to control, resulting in poor high-speed charging life performance. Therefore, the secondary batteries of Comparative Examples 5 and 6 contain both a silicon-based active material and a carbon-based active material in one negative electrode, so that the composition of the negative electrode cannot be adjusted according to the characteristics of each active material, and therefore show poor high-speed charging life performance compared to the secondary batteries of the Examples.
[0196] Experimental example 3: Evaluation of energy density The secondary batteries produced in Examples 1 to 3 and Comparative Examples 1 to 6 were charged and discharged once under the following conditions, and the discharge capacity (unit: Wh) of the secondary batteries was determined.
[0197] At this time, after the charging was completed, the thickness of the secondary battery was measured, and the thickness thus obtained was multiplied by the area of the secondary battery to obtain the volume (unit: L (liter)) of the secondary battery.
[0198] The energy density (unit: Wh / L) was calculated by dividing the discharge capacity of the secondary battery obtained above by the volume of the secondary battery. The results are shown in Table 4 below.
[0199] <Charge and discharge conditions> Charging: CC / CV charging, 0.2C, 4.2V, 5% cut-off Discharge: CC discharge, 0.2C, 3.2V
[0200] [Table 4]
[0201] Referring to Table 4, it can be seen that the secondary batteries of Examples 1 to 3 have an excellent level of energy density because the secondary batteries contain a silicon-based active material, which may improve the capacity.
[0202] In the case of Comparative Example 1, since the negative electrode contains only silicon-based active material as the active material, the capacity may be improved, and thus the battery shows a high energy density. However, as described above, when only silicon-based active material is used as the negative electrode active material, a high potential is formed on the positive electrode due to the high potential of the silicon-based active material, so that Comparative Example 1 shows poor life performance compared to the Examples due to an increase in resistance.
[0203] Furthermore, the secondary batteries of Comparative Examples 2 to 4 contain an excessive amount of anode containing a carbon-based active material having a low energy density, and as a result, the energy density of the secondary batteries is low.
[0204] In addition, in the case of the secondary battery of Comparative Example 5, since the negative electrode contains a silicon-based active material, the energy density is increased to a certain extent. However, since the binder content in the negative electrode is high and the resistance of the carbon-based active material increases, the capacity decreases due to the increased resistance of the carbon-based active material, resulting in a low energy density.
[0205] In addition, in the case of Comparative Example 6, since the binder composition in the negative electrode is low, it is difficult to control the volume expansion of the silicon-based active material, and therefore it is not possible to control the change in thickness of the negative electrode, resulting in a problem of low energy density. [Explanation of symbols]
[0206] 1 Secondary battery 100 positive electrode 110 Positive electrode current collector 120 Cathode active material layer 200 1st negative electrode 210 First negative electrode current collector 220 First negative electrode active material layer 300 2nd negative electrode 310 Second negative electrode current collector 320 Second negative electrode active material layer 400 Separation membrane
Claims
1. one or more positive electrodes including a positive electrode active material layer; a plurality of negative electrodes including a first negative electrode including a silicon-based active material and a second negative electrode including a carbon-based active material; A separation membrane; an electrolyte; The positive electrode and one of the first negative electrode and the second negative electrode constituting the negative electrode are alternately stacked with the separation film interposed therebetween, a ratio of a total weight of the silicon-based active material contained in all of the first negative electrodes of the negative electrode to a total weight of the carbon-based active material contained in all of the second negative electrodes of the negative electrode is 40:60 to 90:10; The first negative electrode and the second negative electrode contain different active materials.
2. the first negative electrode includes a first negative electrode current collector and a first negative electrode active material layer formed on at least one surface of the first negative electrode current collector, The secondary battery according to claim 1 , wherein the first negative electrode active material layer contains the silicon-based active material.
3. the first negative electrode active material layer further includes a first negative electrode binder and a first negative electrode conductive material, 3. The secondary battery of claim 2, wherein the first negative electrode active material layer comprises 60 wt % to 90 wt % of the silicon-based active material, 5 wt % to 30 wt % of the first negative electrode binder, and 5 wt % to 20 wt % of the first negative electrode conductive material.
4. 4. The secondary battery according to claim 3, wherein the first negative electrode binder includes at least one selected from the group consisting of styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, polyvinyl alcohol, polyacrylic acid, polyethylene glycol, polyacrylonitrile, and polyacrylamide.
5. N calculated by the following formula a 1 The secondary battery according to claim 2, wherein the / P ratio is 2.2 to 3.0: [Formula a] N 1 / P ratio={(discharge capacity per unit area of one first negative electrode active material layer in the first negative electrode) / (discharge capacity per unit area of one positive electrode active material layer in the positive electrode)}.
6. The secondary battery according to claim 1 , wherein the silicon-based active material comprises a compound represented by the following chemical formula 1: [Chemical formula 1] SiOx In the above formula 1, 0≦x<2.
7. The secondary battery according to claim 1 , wherein the silicon-based active material contains Si.
8. The average particle size (D 50 8. The secondary battery according to claim 1, wherein the thickness of the first electrode is 1 μm to 10 μm.
9. the second negative electrode includes a second negative electrode current collector and a second negative electrode active material layer formed on at least one surface of the second negative electrode current collector, The secondary battery according to claim 1 , wherein the second negative electrode active material layer contains the carbon-based active material.
10. the second negative electrode active material layer further includes a second negative electrode binder and a second negative electrode conductive material, 10. The secondary battery of claim 9, wherein the second negative electrode active material layer comprises 90 wt % to 99 wt % of the carbon-based active material, 0.5 wt % to 10 wt % of a second negative electrode binder, and 0.5 wt % to 5 wt % of a second negative electrode conductive material.
11. 11. The secondary battery according to claim 10, wherein the second negative electrode binder comprises at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer rubber, styrene-butadiene rubber, and fluororubber.
12. 12. The secondary battery according to claim 1, wherein the carbon-based active material comprises at least one selected from the group consisting of artificial graphite, natural graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon.
13. The average particle size (D 50 13. The secondary battery according to claim 1, wherein the thickness of the first electrode is 10 μm to 30 μm.
14. N calculated by the following formula b 2 The secondary battery according to claim 9, wherein the / P ratio is 1.0 to 1.
3. [Formula b] N 2 / P ratio={(discharge capacity per unit area of one second negative electrode active material layer in the second negative electrode) / (discharge capacity per unit area of one positive electrode active material layer in the positive electrode)}.
15. N calculated by the following formula c all / P all The secondary battery according to any one of claims 1 to 14, wherein the ratio is 2 to 3: [Formula c] N all / P all Ratio={(total amount of discharge capacity per unit area of negative electrodes present in the secondary battery) / (total amount of discharge capacity per unit area of positive electrodes present in the secondary battery)}.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2013178913A
Lithium ion secondary battery
JP2016058236A
Nonaqueous electrolyte secondary battery, and negative electrode unit
JP2018055952A
Method for fabricating carbon-coated silicon / graphite composite anode material for lithium secondary battery and method for fabricating secondary battery comprising the same
KR100794192B1
Lithium-ion secondary cell provided with negative electrode for high energy density cell
WO2018155609A1